Conductive sponge and preparation method thereof, sensor unit, sleep pressure sensor and intelligent pillow

By embedded printing graphene on melamine sponge, a three-dimensional conductive network is formed, which solves the mechanical rigidity and brittleness problems of flexible sensors, improves the sensitivity and stability of the sensor, is suitable for sleep pressure monitoring, and achieves efficient pressure sensing and comfort. degree increase.

CN118772482APending Publication Date: 2024-10-15BEIJING GRAPHENE TECH RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410710966.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing flexible sensors are difficult to maintain high sensitivity and long-term stability due to mechanical rigidity and brittleness during use, and are especially prone to damage during repeated compression processes. In addition, existing sleep sensors have insufficient sensitivity and poor comfort, which affects the accuracy of sleep data. and user experience.

Method used

Embedded printing technology is used to assemble and pattern graphene on a porous melamine sponge to form an embedded three-dimensional graphene conductive network. Combining the porous characteristics of the sponge and the conductivity of graphene, a product with excellent softness and fatigue resistance is prepared. and highly sensitive conductive sponges used to build sensor units and sleep pressure sensors.

Benefits of technology

It achieves high softness and deformability of the conductive sponge, improves the comfort and pressure sensing capabilities of the sensor, enhances the stability and sensitivity of the sensor, is suitable for pressure sensing and sleep monitoring, reduces material consumption and cost, and at the same time The complexity and hardness increase issues of the soaking method are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772482A_ABST
    Figure CN118772482A_ABST
Patent Text Reader

Abstract

The invention provides a conductive sponge and a preparation method thereof, a sensor unit, a sleep pressure sensor and an intelligent pillow, the conductive sponge comprises a melamine sponge and a three-dimensional graphene conductive network, the melamine sponge has a porous structure, and the three-dimensional graphene conductive network is embedded in the melamine sponge. The three-dimensional graphene conductive network in the conductive sponge is embedded in the melamine sponge, and the conductive sponge combines the porous characteristic of the sponge and the excellent conductivity of graphene, has excellent softness, fatigue resistance, deformability, stability and high-sensitivity pressure sensing characteristic, and is very suitable for being used as a conductive material of a sensor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of sensor technology, and in particular to a conductive sponge and a preparation method thereof, a sensor unit, a sleep pressure sensor and a smart pillow. Background Art

[0002] In recent years, flexible sensors have attracted increasing attention due to their potential applications in motion detection, health monitoring, human-machine interface, electronic skin, etc. Conductive materials are the main components to realize the functions of flexible sensors. Due to the diversity of external stimuli, the performance parameters of conductive materials such as sensitivity, softness, and stability are key factors to consider when preparing advanced sensors.

[0003] Designing conductive materials with three-dimensional structures has been proven to be an effective way to improve sensitivity. Nanofunctional materials such as carbon nanotubes, graphene, and MXene can be directly assembled into three-dimensional conductive materials by catalytic chemical vapor deposition or freeze-drying. However, the inherent mechanical rigidity and brittleness of conductive materials limit the deformability of sensors, making such materials composed only of nanofunctional materials susceptible to irreversible damage during compression. Since flexible sensors are inevitably subjected to repeated compression during use, enhancing the deformation ability and stability of conductive materials while maintaining their high sensitivity is an urgent problem to be solved. Summary of the invention

[0004] Based on this, the present application provides a conductive sponge with high sensitivity and excellent deformation ability and stability, and a preparation method thereof, a sensor unit, a sleep pressure sensor and a smart pillow.

[0005] A first aspect of the present application provides a conductive sponge, comprising a melamine sponge and a three-dimensional graphene conductive network, wherein the melamine sponge has a porous structure, and the three-dimensional graphene conductive network is embedded in the interior of the melamine sponge.

[0006] In some embodiments, the material of the three-dimensional graphene conductive network includes reduced graphene oxide.

[0007] The second aspect of the present application provides a method for preparing a conductive sponge, comprising the following steps:

[0008] Printing graphene ink on the surface of a melamine sponge having a porous structure to perform patterning on the melamine sponge;

[0009] Air-drying the patterned melamine sponge;

[0010] The air-dried melamine sponge is subjected to vacuum heat treatment to reduce graphene to reduced graphene oxide, thereby preparing the conductive sponge;

[0011] The conductive sponge comprises a melamine sponge and a three-dimensional graphene conductive network, wherein the three-dimensional graphene conductive network is embedded in the melamine sponge.

[0012] In some embodiments, the step of printing graphene ink on the surface of the melamine sponge having a porous structure comprises:

[0013] The graphene ink is printed on the surface of the melamine sponge with a porous structure according to a predetermined printing path and printing speed using a printing device.

[0014] In some embodiments, the printing pressure is 5psi-20psi; and / or

[0015] Printing speed is 5mm / s-30mm / s; and / or

[0016] The diameter of the nozzle used in printing is 150μm-420μm.

[0017] In some embodiments, the concentration of the graphene ink is 0.5 mg / mL-4 mg / mL.

[0018] In some embodiments, the air-drying treatment is performed at a temperature of 20°C-30°C and for a time of 12h-24h.

[0019] In some embodiments, the vacuum heat treatment is performed at a temperature of 150° C. to 300° C. for a time of 12 h to 24 h.

[0020] The third aspect of the present application provides a sensor unit, which includes the conductive sponge of the first aspect of the present application or the conductive sponge prepared by the preparation method of the second aspect of the present application.

[0021] In some embodiments, the sensor unit also includes a PET gasket and a PET base film, the PET gasket has a pore structure, and interdigitated electrodes are attached to the surface of the PET base film. The conductive sponge, the PET gasket and the PET base film are stacked in sequence, and the three-dimensional graphene conductive network of the conductive sponge, the pore structure of the PET gasket and the projection of the interdigitated electrodes on the PET base film overlap.

[0022] In some embodiments, the cross-section of the sensor unit is circular, and the diameter of the cross-section is 10 mm-20 mm.

[0023] In some embodiments, the cross section of the sensor unit is a square, and the side length of the cross section is 10 mm-20 mm.

[0024] A fourth aspect of the present application provides a sleep pressure sensor, which includes the sensor unit provided in the third aspect of the present application.

[0025] In some embodiments, the sleep pressure sensor includes a plurality of sensor units, and the plurality of sensor units are arranged in an array.

[0026] The fifth aspect of the present application provides a smart pillow, which includes the sleep pressure sensor provided by the fourth aspect of the present application.

[0027] The three-dimensional graphene conductive network in the conductive sponge provided above is embedded in the interior of the melamine sponge. The conductive sponge combines the porous characteristics of the sponge and the excellent conductivity of graphene. It has excellent softness, fatigue resistance, deformation ability, stability and highly sensitive pressure sensing characteristics, and is very suitable as a conductive material for sensors.

[0028] The method for preparing the conductive sponge provided above has at least the following beneficial effects:

[0029] (1) The embedded printing technology can precisely control the assembly and patterning of graphene oxide on the sponge, realizing the construction of complex circuits while avoiding the problems of difficulty in controlling complex patterns and increased costs in the immersion method.

[0030] (2) Compared with the immersion method, the printing method is an environmentally friendly and sustainable alternative that can reduce the excessive consumption of raw materials and solvents and meet the requirements of sustainable development.

[0031] (3) The printed graphene oxide selectively penetrates into the internal structure of the porous sponge through capillary action, maximizing the softness of the sponge, avoiding the problem of increased modulus and hardness caused by large loads of conductive materials through immersion, and improving the overall comfort of the material.

[0032] (4) Due to the strong π-π interaction between graphene oxide, the graphene oxide infiltrated into the sponge will form an embedded three-dimensional interconnected conductive network through self-assembly. The resulting conductive sponge has high softness, deformability and conductivity, and can be used as a pressure sensor to quickly sense pressure. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.

[0034] FIG1 is a flow chart of printing and preparing a conductive sponge according to an embodiment of the present application and a corresponding microscopic image of the internal structure of the sponge;

[0035] FIG2 is a diagram showing the mechanism of printing and preparing conductive sponge;

[0036] Figure 3 A schematic diagram of the structure of a sensor unit provided in one embodiment of the present application;

[0037] Figure 4 A sleep pressure sensor and a smart pillow provided in one embodiment;

[0038] Figure 5 A schematic diagram of the working mechanism of a sleep pressure sensor provided in one embodiment;

[0039] Figure 6 This is an optical top view image of the conductive sponge prepared in Example 1;

[0040] Figure 7 This is a microscopic morphology of the conductive sponge obtained in Example 1;

[0041] Figure 8 The penetration state of the printing process of Example 3 and Example 4;

[0042] Fig. 9 is a graph showing the relationship between the concentration of graphene ink and the printed line width in Examples 1-5;

[0043] Fig.10 is a graph showing the relationship between the concentration of graphene ink and the penetration depth in melamine sponge in Examples 1-5;

[0044] Fig.11 The compression behavior test results of the conductive sponge prepared in Example 1 and the GO / Sponge composite material prepared in Comparative Example 1;

[0045] Fig.12 The relative current change of the conductive sponge prepared in Example 1 during 5 loading-unloading cycles;

[0046] Fig.13 is the sensitivity fitting curve of the sensor unit prepared in Experimental Example 1 within different pressure ranges;

[0047] Fig.14 The relative current change curve of the sensor unit prepared in Experimental Example 1 after the sensor unit is repeatedly compressed 2500 times under a pressure of 9.5 kPa;

[0048] Fig.15 Schematic diagram of the array distribution of sensor units in the sleep pressure sensor of the experimental example and the corresponding schematic diagram of the pressure distribution on the head of the sleeper;

[0049] Fig.16 The relative current change curves of the smart pillow in the application example are monitored in real time in the supine and lateral positions;

[0050] Fig.17 This is a schematic diagram of the electrical signal distribution of the smart pillow in the application example, which monitors different lateral positions including right side lying position and left side lying position in real time;

[0051] Fig.18 The relative current change curve of the smart pillow in the application example that monitors the human body's breathing behavior in real time during sleep;

[0052] Fig.19 Schematic diagram of the electrical signal distribution of the smart pillow in the application example, which monitors different breathing behaviors including deep breathing (a), snoring (b) and coughing (c) during sleep in real time. DETAILED DESCRIPTION

[0053] For ease of understanding of the present invention, the application will be described more fully below with reference to relevant embodiments. The following provides preferred embodiments of the application. However, the application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the application more thorough and comprehensive.

[0054] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0055] The terms "and / or", "or / and", and "and / or" used herein include any one of two or more related listed items, and also include any and all combinations of the related listed items, wherein the any and all combinations include any combination of two related listed items, any more related listed items, or all related listed items. It should be noted that when at least three items are connected by at least two conjunctions selected from "and / or", "or / and", and "and / or", it should be understood that in the present application, the technical solution undoubtedly includes technical solutions connected by "logical and", and also undoubtedly includes technical solutions connected by "logical or".

[0056] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0057] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0058] Only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and likewise any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.

[0059] The temperature parameters in this application, unless otherwise specified, allow both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.

[0060] In this application, unless otherwise specified, the size, particle size, and diameter generally refer to the average value. In this application, "particle size" and "particle size" have the same definition, both representing the average particle size of a sphere or a spheroid.

[0061] Herein, the “suitable” mentioned in “suitable combination”, “suitable method”, “any suitable method”, etc., shall be based on the ability to implement the technical solution of this application, solve the technical problems of this application, and achieve the expected technical effects of this application.

[0062] In the description of the application, "plurality" means at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0063] If there is no special description, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution. If there is no special description, all technical features and optional technical features of the present application can be combined with each other to form a new technical solution.

[0064] If there is no special explanation, all the steps of the present application can be performed sequentially or randomly, preferably sequentially.

[0065] In recent years, the application demand of flexible sensors in various fields has been increasing, and the performance of conductive materials plays a vital role in the function of flexible sensors. Designing conductive materials with three-dimensional structures has been proven to be an effective way to improve sensitivity. However, since flexible sensors are inevitably subjected to repeated compression during use, enhancing the deformation ability and long-term stability of conductive materials while maintaining their high sensitivity is an urgent problem to be solved.

[0066] In the related technology, the method of using sponge as a template to soak conductive fillers has made some progress, but there are still many challenges, such as increased costs, difficulty in forming complex patterns, and problems affecting the comfort of the sensor.

[0067] Sleep disorders have become a common global problem. Long-term sleep disorders can cause a series of serious physiological and psychological diseases, seriously affecting people's physical and mental health. Continuous and real-time sleep monitoring is essential for improving sleep quality and preventing sleep-related health problems. At present, many studies are devoted to monitoring long-term sleep behavior through pressure detection, including monitoring sleep posture and physiological analysis. However, although great progress has been made in sleep sensors, existing sleep sensors still have a series of problems. For example, the insufficient sensitivity of the sensor makes it unable to accurately feedback subtle pressure changes, thus affecting the accuracy of sleep data. Secondly, poor comfort may make users feel uncomfortable during sleep, affecting the natural state of sleep. In addition, poor long-term stability is also a more serious problem, because long-term sleep monitoring requires the sensor to maintain stable performance for a long time, and existing sensors perform poorly in this regard.

[0068] Based on the above problems, the present application provides a direct printing technology to prepare a conductive sponge with an embedded three-dimensional graphene conductive network. The preparation of the conductive sponge is achieved by precisely assembling and patterning graphene on a hydrophilic porous melamine sponge. During the printing process, graphene penetrates into the structure inside the sponge, and forms a strong three-dimensional interconnected conductive network through hydrogen bonding and self-assembly. The prepared conductive sponge combines the porous properties of the sponge and the excellent conductivity of graphene, and has excellent softness, fatigue resistance and highly sensitive pressure sensing properties, which is very suitable as a conductive material for sensors.

[0069] One or more embodiments of the present application provide a conductive sponge, including a melamine sponge and a three-dimensional graphene conductive network, wherein the melamine sponge has a porous structure, and the three-dimensional graphene conductive network is embedded in the interior of the melamine sponge.

[0070] It can be understood that the three-dimensional graphene conductive network in the conductive sponge provided by the present application is embedded in the interior of the melamine sponge. The conductive sponge combines the porous characteristics of the sponge and the excellent conductivity of graphene. It has excellent softness, fatigue resistance, deformation ability, stability and highly sensitive pressure sensing characteristics, and is very suitable as a conductive material for sensors.

[0071] In some embodiments, the material of the three-dimensional graphene conductive network includes reduced graphene oxide.

[0072] One or more embodiments of the present application provide a method for preparing a conductive sponge, which can be used to prepare the conductive sponge described above. The preparation method specifically includes:

[0073] Printing graphene ink on the surface of a melamine sponge with a porous structure to pattern the melamine sponge;

[0074] Air-drying the patterned melamine sponge;

[0075] The air-dried melamine sponge is subjected to vacuum heat treatment to reduce graphene to reduced graphene oxide to prepare a conductive sponge;

[0076] The conductive sponge comprises a melamine sponge and a three-dimensional graphene conductive network, and the three-dimensional graphene conductive network is embedded in the melamine sponge.

[0077] It should be noted that during the air-drying process, the graphene ink can penetrate into the interior of the melamine sponge and achieve self-assembly; after the subsequent vacuum heat treatment process, the graphene oxide can be reduced to reduced graphene oxide, thereby obtaining a three-dimensional graphene conductive network.

[0078] It can be understood that the preparation method of the conductive sponge provided in the present application has at least the following beneficial effects:

[0079] (1) The embedded printing technology can precisely control the assembly and patterning of graphene oxide on the sponge, realizing the construction of complex circuits while avoiding the problems of difficulty in controlling complex patterns and increased costs in the immersion method.

[0080] (2) Compared with the immersion method, the printing method is an environmentally friendly and sustainable alternative that can reduce the excessive consumption of raw materials and solvents and meet the requirements of sustainable development.

[0081] (3) The printed graphene oxide selectively penetrates into the internal structure of the porous sponge through capillary action, maximizing the softness of the sponge, avoiding the problem of increased modulus and hardness caused by large loads of conductive materials through immersion, and improving the overall comfort of the material.

[0082] (4) Due to the strong π-π interaction between graphene oxide, the graphene oxide infiltrated into the sponge will form an embedded three-dimensional interconnected conductive network through self-assembly. The resulting conductive sponge has high softness, deformability and conductivity, and can be used as a pressure sensor to quickly sense pressure.

[0083] Referring to FIG. 1 , in some embodiments, the flow of preparing the conductive sponge by embedded printing is as follows:

[0084] First, the graphene (GO) ink is printed onto a hydrophilic melamine sponge (MS) substrate. Due to the porous nature of the sponge, the printed graphene ink will continue to penetrate into the sponge through capillary action, and form a graphene composite sponge after air drying. The graphene composite sponge is then placed in an oven for vacuum heat treatment, and the graphene oxide is reduced to reduced graphene oxide. As the brown graphene oxide inside the sponge turns dark black, a conductive sponge is obtained.

[0085] Referring to Figure 2, the mechanism of printing and preparing conductive sponge is as follows: During the printing process, the graphene oxide that penetrates into the melamine sponge will self-assemble into a three-dimensional structure using the sponge frame as a template. On the one hand, the graphene oxide containing abundant hydrophilic groups (hydroxyl, carboxyl) will form hydrogen bonds with the hydrophilic melamine sponge (MS), thereby forming a strong connection between the graphene oxide and the sponge. On the other hand, the strong π-π interaction between graphene oxide and graphene oxide will cause the graphene oxide dispersed inside the sponge to assemble into a three-dimensional interconnected structure, forming a solid conductive sponge.

[0086] As a non-limiting example, the method for preparing the graphene ink may include: concentrating the graphene oxide dispersion in a water bath at 60° C., and then diluting the concentrated paste with deionized water to obtain graphene inks of different concentrations.

[0087] In some embodiments, the step of printing graphene ink on the surface of a melamine sponge having a porous structure comprises:

[0088] The graphene ink is printed on the surface of the melamine sponge with a porous structure according to a predetermined printing path and printing speed using a printing device.

[0089] As a possible implementation, the printing pressure when printing the graphene ink is 5psi-20psi; for example, it may be but not limited to 5psi, 6psi, 7psi, 8psi, 9psi, 10psi, 11psi, 12psi, 13psi, 14psi, 15psi, 16psi, 17psi, 18psi, 19psi, 20psi or a range between any two of the above pressures, etc. When the printing pressure is within the above range, it is beneficial to control the graphene ink to form an expected straight line and to ensure the continuity of the line.

[0090] In some optional embodiments, the printing speed is 5 mm / s-30 mm / s; for example, it can be but not limited to 5 mm / s, 6 mm / s, 7 mm / s, 8 mm / s, 9 mm / s, 10 mm / s, 11 mm / s, 12 mm / s, 13 mm / s, 14 mm / s, 15 mm / s, 16 mm / s, 17 mm / s, 18 mm / s, 19 mm / s, 20 mm / s, 21 mm / s, 22 mm / s, 23 mm / s, 24 mm / s, 25 mm / s, 26 mm / s, 27 mm / s, 28 mm / s, 29 mm / s, 30 mm / s or a range between any two of the above speeds. When the printing speed is within the above range, it is beneficial to control the graphene ink to form an expected straight line and to ensure the continuity of the line.

[0091] In some exemplary embodiments, the diameter of the nozzle used in printing is 150 μm-420 μm; for example, it can be but not limited to 150 μm, 160 μm, 170 μm, 200 μm, 210 μm, 230 μm, 250 μm, 260 μm, 280 μm, 300 μm, 330 μm, 340 μm, 350 μm, 380 μm, 400 μm, 420 μm, or a range between any two of the above diameters. When the diameter of the nozzle used in printing is within the above range, it is beneficial to better match the rheological properties of the graphene ink and smoothly print out the circuit pattern of the required characteristic size.

[0092] It should be noted that the printing pressure, printing speed and nozzle diameter can be combined in any suitable manner, and the three can be selected from any printing pressure, printing speed and nozzle diameter described in this document.

[0093] As a non-limiting example, the printing device includes a syringe, a nozzle, and an air-powered fluid dispenser; when printing, the syringe containing graphene ink is connected to the nozzle. Appropriate pressure is applied by the air-powered fluid dispenser to control the extrusion and flow of the graphene ink in the syringe. Finally, the graphene ink is printed onto the sponge substrate according to a predetermined printing path and speed.

[0094] In some exemplary embodiments, the concentration of the graphene ink is 0.5 mg / mL-4 mg / mL; for example, it can be but not limited to 0.5 mg / mL, 1 mg / mL, 1.5 mg / mL, 2 mg / mL, 2.5 mg / mL, 3 mg / mL, 3.5 mg / mL, 4 mg / mL or a range between any two of the above concentrations. When the concentration of the graphene ink is within the above range, it is conducive to stable printing operation on the melamine sponge, and the ink can fully penetrate into the sponge and assemble to form a three-dimensional structure.

[0095] As a possible implementation manner, the temperature of the air-drying treatment is 20°C-30°C; for example, it can be but not limited to 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C or a range between any two of the above temperatures.

[0096] As a non-limiting example, the air-drying time is 12h-24h; for example, it can be but not limited to 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h or a range between any two of the above times. When the air-drying time is within the above range, the graphene sheets undergo uniform self-assembly behavior as the ink dries, and the graphene sheets form stable connections with each other and with the sponge matrix by relying on intermolecular interactions such as hydrogen bonds and π-π stacking.

[0097] It should be noted that the temperature and time of the air-drying treatment can be combined in any appropriate manner, and both can be selected from any temperature and time of the air-drying treatment described in this article.

[0098] In some embodiments, the temperature of the vacuum heat treatment is 150°C-300°C; for example, it can be but not limited to 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C, 300°C or a range between any two of the above temperatures. When the temperature of the vacuum heat treatment is within the above range, it is beneficial to reduce the graphene oxide to reduced graphene oxide and form a three-dimensional graphene conductive network.

[0099] In some exemplary embodiments, the time for vacuum heat treatment is 12h-24h; for example, it can be but not limited to 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h or a range between any two of the above times, etc.

[0100] One or more embodiments of the present application provide a sensor unit, which includes the above-mentioned conductive sponge or the conductive sponge prepared by the above-mentioned preparation method.

[0101] The sensor unit including the conductive sponge has excellent softness, fatigue resistance, deformation ability, stability and highly sensitive pressure sensing characteristics.

[0102] As a possible implementation, the sensor unit also includes a PET gasket and a PET base film, the PET gasket has a pore structure, and interdigitated electrodes are attached to the surface of the PET base film. The conductive sponge, PET gasket and PET base film are stacked in sequence, and the three-dimensional graphene conductive network of the conductive sponge, the pore structure of the PET gasket and the projection of the interdigitated electrodes on the PET base film overlap.

[0103] refer to Figure 3 The sensor unit includes a conductive sponge 1, a PET gasket 2 with a pore structure and a PET base film, a surface of the PET base film is attached with a forked electrode 2, the conductive sponge 1, the PET gasket 2 and the PET base film are stacked in sequence, and the three-dimensional graphene conductive network of the conductive sponge 1, the pore structure of the PET gasket 2 and the projection of the forked electrode 3 on the PET base film overlap.

[0104] As a non-limiting example, the method for preparing the sensor unit includes: seamlessly integrating a conductive sponge with a PET gasket and a PET base film containing interdigital electrodes in sequence, wherein the PET gasket has a pore structure to display a printed circuit pattern, and overlapping the three-dimensional graphene conductive network of the conductive sponge, the pore structure of the PET gasket, and the interdigital electrodes.

[0105] In some exemplary embodiments, the interdigitated electrodes use a silver electrode as a current collector.

[0106] In some optional embodiments, the cross-section of the sensor unit is circular, and the diameter of the cross-section is 10 mm-20 mm; for example, it can be but not limited to 10 mm, 11 mm, 12 mm, 13 mm, 14 mm, 15 mm, 16 mm, 17 mm, 18 mm, 19 mm, 20 mm or a range between any two of the above values.

[0107] In some exemplary embodiments, the cross-section of the sensor unit is square, and the side length of the cross-section is 10 mm-20 mm; for example, it can be but not limited to 10 mm, 11 mm, 12 mm, 13 mm, 14 mm, 15 mm, 16 mm, 17 mm, 18 mm, 19 mm, 20 mm or a range between any two of the above values, etc.

[0108] One or more embodiments of the present application provide a sleep pressure sensor, which includes the above-mentioned sensor unit. The sleep pressure sensor not only has excellent comfort, but also has a wide pressure sensing capability and high pressure sensing sensitivity, and is therefore very suitable for sleep monitoring.

[0109] As a possible implementation, the sleep pressure sensor includes a plurality of the sensor units, and the plurality of sensor units are arranged in an array.

[0110] One or more embodiments of the present application provide a smart pillow, which includes the sleep pressure sensor provided above, and the sleep pressure sensor is attached to the pillow base.

[0111] refer to Figure 4 , Figure 4 The left side of the picture shows a smart pillow, and the right side shows a sleep pressure sensor. Figure 4 It can be seen that the sleep pressure sensor includes a plurality of sensor units arranged in an array; the sleep pressure sensor is integrated with a commercial square pillow to obtain a smart pillow.

[0112] refer to Figure 5 The working mechanism of the sleep pressure sensor is: when the posture and breathing behavior of the human body change during sleep, the muscles from the back of the head to the neck will change slightly, and this change will be transmitted to the sensor unit, thereby generating a changing current signal. Therefore, the array sensor unit integrated into the pillow can monitor the changes in human posture during sleep.

[0113] The technical scheme of the present invention is described in detail below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods for which specific conditions are not specified in the following embodiments are preferably referred to the guidance given in the present invention, and can also be carried out according to the experimental manual or conventional conditions in the art, or according to the conditions recommended by the manufacturer, or with reference to experimental methods known in the art.

[0114] In the following specific embodiments, the measured parameters of raw material components may have slight deviations within the range of weighing accuracy unless otherwise specified. For temperature and time parameters, acceptable deviations caused by instrument test accuracy or operation accuracy are allowed.

[0115] 1. Preparation of Conductive Sponge

[0116] Example 1

[0117] S1. Concentrate the graphene oxide dispersion in a water bath at 60° C. Then, dilute the concentrated paste with deionized water to obtain a graphene ink with a concentration of 2 mg / mL.

[0118] S2. Using a multi-axis inkjet system as a printing device, a syringe filled with graphene ink is connected to a micro nozzle, and 7.5 psi pressure is applied through an air-powered fluid dispenser to control the extrusion and flow of the graphene ink in the syringe; finally, the graphene ink is printed onto a melamine sponge substrate according to a predetermined printing path and speed to pattern the sponge.

[0119] S3. Air-dry the printed pattern at 25°C for 12 h to achieve the infiltration and assembly of graphene oxide.

[0120] S4. The patterned GO sponge was vacuum heat treated at 200°C to reduce the graphene oxide to reduced graphene oxide (rGO) by mild thermal reduction, thereby obtaining a conductive sponge with an embedded three-dimensional graphene conductive network.

[0121] The optical top view image of the conductive sponge prepared in Example 1 is as follows: Figure 6 shown by Figure 6 It can be seen that graphene oxide can be embedded into the sponge structure during the printing process and form complex circuit patterns.

[0122] The microscopic morphology of the conductive sponge obtained in Example 1 is as follows: Figure 7 shown by Figure 7 It can be seen that the printed graphene oxide will penetrate into the interior of the sponge structure and assemble to form a conductive network with embedded three-dimensional interconnections.

[0123] Example 2

[0124] The difference between Example 2 and Example 1 is that the concentration of the graphene ink prepared in step S1 of Example 2 is 0.5 mg / mL, and the others are the same.

[0125] Example 3

[0126] The difference between Example 3 and Example 1 is that the concentration of the graphene ink prepared in step S1 of Example 3 is 1 mg / mL, and the others are the same.

[0127] Example 4

[0128] The difference between Example 4 and Example 1 is that the concentration of the graphene ink prepared in step S1 of Example 4 is 3 mg / mL, and the others are the same.

[0129] Example 5

[0130] The difference between Example 5 and Example 1 is that the concentration of the graphene ink prepared in step S1 of Example 4 is 4 mg / mL, and the others are the same.

[0131] Comparative Example 1

[0132] The difference between Comparative Example 1 and Example 1 is that the conductive sponge is prepared by an impregnation method in Comparative Example 1; specifically, as follows:

[0133] S1. Concentrate the graphene oxide dispersion in a water bath at 60° C. Then, dilute the concentrated paste with deionized water to obtain a graphene ink with a concentration of 2 mg / mL.

[0134] S2. Put graphene ink in a beaker, completely immerse the melamine sponge in it, squeeze it repeatedly to make it fully soaked, and let it stand for 2 hours.

[0135] S3. Take out the soaked sponge from the beaker and air-dry it at 25° C. for 24 hours to achieve volatilization and drying of the liquid in the sponge and assembly of graphene oxide.

[0136] S4. The dried GO sponge is subjected to vacuum heat treatment at 200°C, and the graphene oxide is reduced to reduced graphene oxide (rGO) by mild thermal reduction, thereby obtaining a bulk-structured graphene conductive sponge.

[0137] The penetration state of the printing process of Example 3 and Example 4 is as follows Figure 8 As shown, Figure 8 a is the penetration state of the printing process of Example 3, Figure 8 b is the penetration state of the printing process of Example 4. Figure 8 It can be seen that at low concentrations, the ink will quickly penetrate into the interior of the sponge, and as the concentration increases, the viscosity of the ink increases, resulting in a lower degree of penetration, and gradually tends to gather on the surface of the sponge.

[0138] The relationship between the graphene ink concentration and the printed line width in Examples 1-5 is as follows: Fig. 9 As shown. Fig. 9 It can be seen that with the increase of graphene oxide concentration in graphene ink, the printed line width gradually decreases. This may be because the low-concentration graphene oxide solution has a lower viscosity and is easy to spread and diffuse when printed on the sponge, forming wider lines.

[0139] The relationship between the concentration of graphene ink and the penetration depth in melamine sponge in Examples 1-5 is as follows: Fig.10 shown by Fig.10 It can be seen that with the increase of graphene oxide concentration, the penetration depth of graphene oxide after printing gradually decreases.

[0140] The compression behaviors of the pure sponge, the conductive sponge prepared in Example 1 and the GO / Sponge composite material prepared in Comparative Example 1 were compared by a loading-unloading test. The test results are shown in FIG. Fig.11 shown by Fig.11It can be seen that compared with the GO / Sponge composite material obtained by the impregnation method in Comparative Example 1, the compression hysteresis curves of the conductive sponge prepared in Example 1 and the pure sponge are almost overlapped, indicating that the conductive sponge provided in the present application maintains the original compression characteristics of the sponge to a large extent. This may be because the selective assembly and patterning of the graphene ink on the sponge can be better regulated by printing, thereby not changing the original mechanical properties of the sponge.

[0141] The relative current change of the conductive sponge prepared in Example 1 during 5 loading-unloading cycles is as follows: Fig.12 shown by Fig.12 It can be seen that when the conductive sponge is connected to the circuit, the conductive sponge can have a good electrical response to different pressures, and repeated and stable current responses can be monitored.

[0142] 2. Experimental Example: Preparation of Sensor Unit

[0143] The conductive sponge prepared in Example 1, the PET gasket with a pore structure, and the PET film containing interdigital electrodes are sequentially stacked and seamlessly integrated together, and the three-dimensional graphene conductive network of the conductive sponge, the pore structure of the PET gasket, and the interdigital electrodes overlap to prepare a sensor unit. The interdigital electrodes use silver electrodes as current collectors.

[0144] The sensitivity fitting curves of the sensor unit prepared in the test example in different pressure ranges are as follows: Fig.13 As shown. Fig.13 It can be seen that the sensitivity fitting curve of the sensor unit shows four partial linear fitting areas, with sensitivities ranging from 0 to 65 kPa, 206.85 kPa and -1 , 114.94 kPa in the range of 65-175 kPa -1 , 71.40 kPa in the range of 175-475 kPa -1 and 32.73 kPa in the range of 475-1000 kPa -1 .

[0145] After the sensor unit prepared in the test example was repeatedly compressed 2500 times under a pressure of 9.5 kPa, the relative current change curve of the sensor unit is as follows: Fig.14 As shown. Fig.14 It can be seen that during the 2500 times of repeated compression, the sensor unit can monitor repeated and stable electrical signals.

[0146] 3. Application example: Preparation of smart pillow

[0147] The sensor unit arrays prepared in the 18 test examples are arranged as follows Figure 4The sleep pressure sensor shown in b is seamlessly integrated into a commercial square pillow to obtain a sleep pressure sensor as shown in Figure 4 The smart pillow shown in middle a.

[0148] The schematic diagram of the array distribution of the sensor units in the sleep pressure sensor and the schematic diagram of the corresponding pressure distribution on the sleeper's head are shown in FIG. Fig.15 shown.

[0149] The volunteers were tested for sleep stress using a smart pillow. The test results are as follows:

[0150] The smart pillow monitors the relative current change curves of volunteers in supine and lateral positions in real time. Fig.16 As shown. Fig.16 It can be seen that the sleep pressure sensor can monitor the current signal of the human body in the right side lying position and the left side lying position respectively. From the relative current change curve, it can be seen that the right side lying position and the left side lying position have specific peak values ​​and waveforms respectively.

[0151] The smart pillow monitors the electrical signal distribution of different lateral positions, including right and left lateral positions, in real time. Fig.17 As shown. Fig.17 It can be seen that when the volunteer lies on the left side, the electrical signal is concentrated in the left sensor channel, and vice versa.

[0152] The relative current change curve of the smart pillow that monitors the human body's breathing behavior during sleep in real time is as follows Fig.18 As shown. Fig.18 It can be seen that the sleep pressure sensor can monitor the current signals of the human body during deep breathing, snoring and coughing.

[0153] The smart pillow monitors the electrical signal distribution of different breathing behaviors including deep breathing (a), snoring (b) and coughing (c) during sleep in real time. Fig.19 As shown. Fig.19 It can be seen that: Figure 19 describes the two-dimensional distribution diagram of pressure signals under different breathing behaviors. Among them, the pressure is mainly concentrated in the upper area of ​​the back of the head during deep breathing; the pressure is mainly concentrated in the transition area between the back of the head and the neck during snoring, and the pressure in the upper area of ​​the back of the head is reduced; the pressure signal changes during coughing are concentrated in channels 5, 7, 8 and 9.

[0154] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0155] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A conductive sponge, characterized in that: The invention comprises a melamine sponge and a three-dimensional graphene conductive network. The melamine sponge has a porous structure, and the three-dimensional graphene conductive network is embedded in the melamine sponge.

2. The conductive sponge according to claim 1, characterized in that The material of the three-dimensional graphene conductive network includes reduced graphene oxide.

3. A method for preparing a conductive sponge, characterized in that: The steps include: Printing graphene ink on the surface of a melamine sponge having a porous structure to perform patterning on the melamine sponge; Air-drying the patterned melamine sponge; The air-dried melamine sponge is subjected to vacuum heat treatment to reduce graphene to reduced graphene oxide, thereby preparing the conductive sponge; The conductive sponge comprises a melamine sponge and a three-dimensional graphene conductive network, wherein the three-dimensional graphene conductive network is embedded in the melamine sponge.

4. The preparation method according to claim 3, characterized in that: The step of printing graphene ink on the surface of the melamine sponge having a porous structure comprises: The graphene ink is printed on the surface of the melamine sponge with a porous structure according to a predetermined printing path and printing speed using a printing device.

5. The preparation method according to claim 4, characterized in that: Printing pressure is 5psi-20psi; and / or Printing speed is 5mm / s-30mm / s; and / or The diameter of the nozzle used in printing is 150μm-420μm.

6. The preparation method according to claim 3, characterized in that: The concentration of the graphene ink is 0.5 mg / mL-4 mg / mL.

7. The preparation method according to any one of claims 3 to 6, characterized in that: The air-drying treatment is performed at a temperature of 20°C-30°C and for a time of 12h-24h.

8. The preparation method according to any one of claims 3 to 6, characterized in that: The temperature of the vacuum heat treatment is 150° C.-300° C., and the time is 12 h-24 h.

9. A sensor unit, characterized in that: The conductive sponge comprises the conductive sponge as claimed in any one of claims 1 to 2 or the conductive sponge prepared by the preparation method as claimed in any one of claims 3 to 8.

10. The sensor unit according to claim 9, characterized in that The sensor unit also includes a PET gasket and a PET base film, the PET gasket has a pore structure, and interdigitated electrodes are attached to the surface of the PET base film. The conductive sponge, the PET gasket and the PET base film are stacked in sequence, and the three-dimensional graphene conductive network of the conductive sponge, the pore structure of the PET gasket and the projection of the interdigitated electrodes on the PET base film overlap.

11. The sensor unit according to any one of claims 9 to 10, characterized in that The cross section of the sensor unit is circular, and the diameter of the cross section is 10 mm-20 mm.

12. The sensor unit according to any one of claims 9 to 10, characterized in that The cross section of the sensor unit is a square, and the side length of the cross section is 10 mm-20 mm.

13. A sleep pressure sensor, characterized in that: Comprising a sensor unit as claimed in any one of claims 9 to 12.

14. The sleep pressure sensor according to claim 13, characterized in that: The sleep pressure sensor includes a plurality of sensor units, and the plurality of sensor units are arranged in an array.

15. A smart pillow, characterized in that: The sleep pressure sensor comprises the sleep pressure sensor as claimed in any one of claims 13 to 14, wherein the sleep pressure sensor is attached to a pillow base.