Full-biological enzyme degradation packaging film and packaging bag
By using materials such as starch, N-methylol acrylamide, modified carboxymethyl cellulose and polylactic acid to prepare fully biological enzyme-degradable packaging films, the problems of biodegradability and process complexity of plastic packaging films have been solved and achieved High toughness and rapid biodegradation.
Patent Information
- Application Number
- CN202411262027.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-09-10
AI Technical Summary
Existing plastic packaging films are difficult to biodegrade, and the film-forming process is complex and pollutes the environment. The hygroscopicity and brittleness of starch materials limit their application.
Using materials such as starch, N-methylol acrylamide, modified carboxymethyl cellulose, modified polylactic acid and polybutylene succinate, fully biological enzymes are prepared through mechanical stirring, twin-screw extrusion and blown film processes. Degrade packaging films and improve the mechanical properties and biodegradation rate of materials.
It has realized a packaging film with high toughness and full biological enzyme degradation, improved the elongation at break and biodegradation efficiency of the packaging film, and solved the problems of biodegradability and process complexity of plastic packaging films.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biodegradable polymer materials, in particular to a fully bioenzyme-degradable packaging film and a packaging bag. Background Art
[0002] At present, the packaging films for daily use on the market are mainly polyethylene or polyvinyl chloride plastic films. Since these plastics are difficult to be decomposed by soil microorganisms and absorbed by plant roots, a large amount of plastic films are discarded in the environment after long-term use, causing adverse effects on the environment. To this end, people have used different methods to improve the performance of plastic films for daily use packaging, but none of them can fundamentally solve the problem of biodegradability of plastic films. In addition, the existing film forming method is to cast the glue solution into a saturated sodium sulfate solution. After the film is formed by this method, it must go through a long process of water washing, which is complicated. The residual inorganic salts in the washing liquid are discharged, which causes environmental pollution and other defects.
[0003] As one of the biodegradable materials, starch has been recognized by the industry as a representative of new biodegradable materials with great development potential due to its advantages such as wide raw material sources, low price and excellent degradation performance. However, since starch is a rigid natural polymer material containing multiple hydroxyls, hygroscopicity and brittleness have always hindered the application of this type of material. Therefore, improving the solubility of starch plastics and increasing the toughness of the materials have become the development direction of starch plastics. The present invention provides a fully bioenzyme-degradable packaging film and packaging bag, thereby improving the mechanical properties and biodegradation rate of the film prepared using starch. Summary of the invention
[0004] The object of the present invention is to provide a fully bio-enzyme-degradable packaging film and packaging bag to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a fully bio-enzyme-degradable packaging film and packaging bag, comprising the following preparation steps: (1) Weigh 11-13 parts of glycerol according to the weight ratio, add 1-3 parts of N-hydroxymethyl acrylamide, and mechanically stir at 200-400 rpm in a high-speed mixer for 30-60 minutes to obtain a mixed solution; slowly pour the mixed solution into 40-50 parts of starch for 10 minutes, and stir at 1000-2000 rpm to fully mix; after the stirring is completed, add 2-10 parts of modified carboxymethyl cellulose, and continue to stir at 500-800 rpm for 60-120 minutes at 100-120° C. to obtain a packaging film filler; (2) Dissolve 1 part of maleic anhydride and 0.15 parts of vulcanizing agent in 3-5 parts of acetone, mix with 40-50 parts of polylactic acid, and stir at 2000 rpm for 20 minutes; place for 24 hours, after the acetone is completely volatilized, add it to a twin-screw extruder for melt extrusion; set the temperature of each section of the twin-screw extruder barrel to 160°C, 170°C, and 180°C, respectively, and set 180°C as the reaction temperature of the third section; the head temperature is 160°C; control the main screw speed to 90-120r / min, and the feed screw speed to 10r / in; cool the extrudate to 25°C at room temperature, cut into pellets, and then dry at room temperature for 24 hours to obtain the modified polylactic acid; (3) The modified polylactic acid and polybutylene succinate are placed in a 50°C forced air oven for 12 hours; then placed in a high-speed mixer containing packaging film filler, and the blended composite polymer is prepared by a twin-screw extruder; the screw speed is 160-180 rpm, the extrusion temperature range is 145-165°C, and then extrusion blown film is used to prepare a packaging film raw material with a thickness of 30-50 μm, and then cut into packaging bags.
[0006] Furthermore, the starch in step (1) is wheat starch or corn starch.
[0007] Furthermore, the preparation method of the modified carboxymethyl cellulose in step (1) is as follows: 0.2 parts of carboxymethyl cellulose is dissolved in 100 parts of deionized water, and stirred at 100 rpm for 12 hours at 35°C to prepare a carboxymethyl cellulose solution; then 0.2 parts of sodium periodate is added to the carboxymethyl cellulose solution; a 1% sulfuric acid aqueous solution is added dropwise to adjust the pH value of the solution to 3-4, and then the solution is allowed to react for 6 hours; after the reaction is completed, an excess of ethylene glycol is added to remove unreacted sodium periodate; 1 part of ethanol is used for precipitation, and then the solution is dialyzed with pure water using a 5 μm dialysis membrane for 24 hours; 0.04-0.1 parts of malic acid are added to the dialyzed solution, a 1% sulfuric acid aqueous solution is added dropwise to adjust the pH to 7-8, the solution is stirred at 25°C at 100 rpm for 12 hours, and vacuum dried at 37°C and 0.085 MPa to constant weight to obtain modified carboxymethyl cellulose.
[0008] Furthermore, the viscosity of the carboxymethyl cellulose is 300-900 cps.
[0009] Furthermore, in step (2), the vulcanizing agent is diisopropylbenzene peroxide.
[0010] Furthermore, the polylactic acid in step (2) is polylactic acid pellets.
[0011] Furthermore, the polybutylene succinate in step (3) is AZ91TN polybutylene succinate.
[0012] Furthermore, in step (3), the mass ratio of the packaging film filler, modified polylactic acid, and polybutylene succinate is 3-4:1-2:0.5-1.5.
[0013] Furthermore, in step (3), the high-speed mixer is used for blending at a speed of 500 rpm for 5 minutes.
[0014] Furthermore, the film blowing process in step (3) is: prepared using a smooth bore single screw extruder equipped with a film blowing head with a diameter of 46 mm, the film blowing temperature range is 155-175° C., and the screw speed is 30-40 rpm.
[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: The invention uses starch as a main raw material to prepare a packaging film filler, and uses maleic anhydride to modify polylactic acid and polybutylene succinate to achieve the effects of high toughness and full bioenzyme degradation.
[0016] Firstly, N-hydroxymethyl acrylamide is a cross-linking monomer with a bifunctional group. In the present invention, N-hydroxymethyl acrylamide is used as a cross-linking agent. The unsaturated active functional groups contained therein are hydrophilic and dispersed in starch under the dissolution of glycerol, thereby improving the solubility of starch in the composite polymer. Then, modified carboxymethyl cellulose is added to cooperate with N-hydroxymethyl acrylamide to improve the mechanical properties of the packaging film after preparation, thereby improving the elongation at break while ensuring the full bioenzymatic degradation of the packaging film. Carboxymethyl cellulose is modified with malic acid. Hydroxymethyl cellulose has a large specific surface area and high surface energy, and can be grafted with more malic acid. After high-temperature reaction, malic acid and N-hydroxymethyl acrylamide form functional micro-cross-linking regions in starch, which are compatible with starch molecules, thereby achieving a synergistic capacity-enhancing effect, thereby further improving the elongation at break of the packaging film. Secondly, modified polylactic acid and polybutylene succinate are used as composite polymer raw materials, and a packaging film is prepared by melt blending and extrusion film blowing process; both modified polylactic acid and polybutylene succinate are biodegradable polymers, but the toughness of modified polylactic acid is poor, and polybutylene succinate is added to the modified polylactic acid for blending to change its mechanical properties. Since the two are incompatible systems, maleic anhydride is used for bridging grafting to achieve a miscible effect and improve the compatibility of the filler with the composite polymer; at the same time, the introduction of maleic anhydride makes the modified polylactic acid have a degradable group, which accelerates the biodegradable efficiency of the packaging film. DETAILED DESCRIPTION
[0017] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of a fully bio-enzyme-degradable packaging film prepared in the following examples are as follows: Mechanical properties: Packaging film samples were cut into sizes of 20×4×0.04mm in the longitudinal and transverse directions. 3 The size of the test is tested. According to GB / T13022-1991 plastic film tensile properties test method, 5 groups of each sample are tested and the results are averaged. The test results show the elongation at break and the elongation at break data.
[0019] Biodegradation: According to the definition, classification, marking and degradation performance requirements of degradable plastics in GB / T20197-2006.
[0020] Example 1; (1) 0.2 parts of carboxymethyl cellulose with a viscosity of 300 cps was dissolved in 100 parts of deionized water, and the mixture was stirred at 100 rpm for 12 hours at 35°C to prepare a carboxymethyl cellulose solution; 0.2 parts of sodium periodate was then added to the carboxymethyl cellulose solution; a 1% aqueous sulfuric acid solution was added dropwise to adjust the pH value of the solution to 3, and then the solution was allowed to react for 6 hours; after the reaction was completed, an excess of ethylene glycol was added to remove the unreacted sodium periodate; 1 part of ethanol was used for precipitation, and then the solution was dialyzed with pure water using a 5 μm dialysis membrane for 24 hours; 0.04 parts of malic acid was added to the dialyzed solution, and a 1% aqueous sulfuric acid solution was added dropwise to adjust the pH value to 3. 7. Stir at 100 rpm for 12 h at 25 ° C, and vacuum dry at 37 ° C and 0.085 MPa to constant weight to obtain modified carboxymethyl cellulose; weigh 11 parts of glycerol according to the weight ratio, add 1 part of N-hydroxymethyl acrylamide, and mechanically stir at 200 rpm in a high-speed mixer for 30 min to obtain a mixed solution; slowly pour all the mixed solution into 40 parts of wheat starch for 10 min, and stir at 1000 rpm to mix them thoroughly; after the stirring is completed, add 2 parts of modified carboxymethyl cellulose, and continue to stir at 500 rpm for 60 min at 100 ° C to obtain a packaging film filler; (2) Dissolve 1 part of maleic anhydride and 0.15 parts of dicumyl peroxide in 3 parts of acetone, mix with 40 parts of polylactic acid pellets, and stir at 2000 rpm for 20 min; place for 24 hours, after the acetone is completely volatilized, add it to a twin-screw extruder for melt extrusion; set the temperature of each section of the twin-screw extruder barrel to 160°C, 170°C, and 180°C, respectively, and set 180°C as the reaction temperature of the third section; the head temperature is 160°C; control the main screw speed to 90r / min, and the feed screw speed to 10r / in; cool the extrudate to 25°C at room temperature, cut it into pellets, and then dry it at room temperature for 24 hours to obtain the modified polylactic acid; (3) The modified polylactic acid and AZ91TN polybutylene succinate were placed in a 50°C forced air oven for 12 h; then placed in a high-speed mixer containing a packaging film filler, the mass ratio of the packaging film filler, the modified polylactic acid, and the polybutylene succinate was 3:1:0.5, and blended at a speed of 500 rpm for 5 min. The blended composite polymer was prepared by a twin-screw extruder; the screw speed was 160 rpm, the extrusion temperature range was 145°C, and then extrusion blown film was prepared into a packaging film raw material with a thickness of 30 μm. The film blowing process was: prepared using a smooth bore single screw extruder equipped with a film blowing head with a diameter of 46 mm, the film blowing temperature range was 155°C, and the screw speed was 30 rpm; and then cut into packaging bags.
[0021] Example 2; (1) 0.2 parts of carboxymethyl cellulose with a viscosity of 600 cps was dissolved in 100 parts of deionized water, and the mixture was stirred at 100 rpm for 12 hours at 35°C to prepare a carboxymethyl cellulose solution; 0.2 parts of sodium periodate was then added to the carboxymethyl cellulose solution; a 1% aqueous sulfuric acid solution was added dropwise to adjust the pH value of the solution to 3, and then the solution was allowed to react for 6 hours; after the reaction, an excess of ethylene glycol was added to remove the unreacted sodium periodate; 1 part of ethanol was used for precipitation, and then the solution was dialyzed with pure water using a 5 μm dialysis membrane for 24 hours; 0.07 parts of malic acid was added to the dialyzed solution, and a 1% aqueous sulfuric acid solution was added dropwise to adjust the pH value to 3. 7. Stir at 100 rpm for 12 h at 25 ° C, and vacuum dry at 37 ° C and 0.085 MPa to constant weight to obtain modified carboxymethyl cellulose; weigh 12 parts of glycerol according to the weight ratio, add 2 parts of N-hydroxymethyl acrylamide, and mechanically stir at 300 rpm in a high-speed mixer for 45 min to obtain a mixed solution; slowly pour all the mixed solution into 45 parts of wheat starch for 10 min, and stir at 1500 rpm to mix them thoroughly; after stirring, add 6 parts of modified carboxymethyl cellulose, and continue to stir at 650 rpm at 110 ° C for 90 min to obtain a packaging film filler; (2) Dissolve 1 part of maleic anhydride and 0.15 parts of dicumyl peroxide in 4 parts of acetone, mix with 45 parts of polylactic acid pellets, and stir at 2000 rpm for 20 min; place for 24 hours, after the acetone is completely volatilized, add it to a twin-screw extruder for melt extrusion; set the temperature of each section of the twin-screw extruder barrel to 160°C, 170°C, and 180°C, respectively, and set 180°C as the reaction temperature of the third section; the head temperature is 160°C; control the main screw speed to 105r / min, and the feed screw speed to 10r / in; cool the extrudate to 25°C at room temperature, cut it into pellets, and then dry it at room temperature for 24 hours to obtain the modified polylactic acid; (3) The modified polylactic acid and AZ91TN polybutylene succinate were placed in a 50°C forced air oven for 12 h; then placed in a high-speed mixer containing a packaging film filler, the mass ratio of the packaging film filler, the modified polylactic acid, and the polybutylene succinate was 3.5:1.5:1, and blended at a speed of 500 rpm for 5 min. The blended composite polymer was prepared by a twin-screw extruder; the screw speed was 170 rpm, the extrusion temperature range was 155°C, and then extrusion blown film was prepared into a packaging film raw material with a thickness of 40 μm. The film blowing process was: prepared using a smooth bore single screw extruder equipped with a film blowing head with a diameter of 46 mm, the film blowing temperature range was 165°C, and the screw speed was 35 rpm; and then cut into packaging bags.
[0022] Example 3; (1) 0.2 parts of carboxymethyl cellulose with a viscosity of 900 cps was dissolved in 100 parts of deionized water, and the mixture was stirred at 100 rpm for 12 hours at 35°C to prepare a carboxymethyl cellulose solution; 0.2 parts of sodium periodate was then added to the carboxymethyl cellulose solution; a 1% aqueous sulfuric acid solution was added dropwise to adjust the pH value of the solution to 4, and then the solution was allowed to react for 6 hours; after the reaction, an excess of ethylene glycol was added to remove the unreacted sodium periodate; 1 part of ethanol was used for precipitation, and then the solution was dialyzed with pure water using a 5 μm dialysis membrane for 24 hours; 0.1 parts of malic acid was added to the dialyzed solution, and a 1% aqueous sulfuric acid solution was added dropwise to adjust the pH value to 8, Stirring at 100 rpm for 12 h at 25° C., and vacuum drying at 37° C. and 0.085 MPa to constant weight to obtain modified carboxymethyl cellulose; weighing 13 parts of glycerol according to weight ratio, adding 3 parts of N-hydroxymethyl acrylamide, and mechanically stirring at 400 rpm in a high-speed mixer for 60 min to obtain a mixed solution; slowly pouring all the mixed solution into 50 parts of corn starch for 10 min, and stirring at 2000 rpm to fully mix; after the stirring is completed, adding 10 parts of modified carboxymethyl cellulose, and continuing to stir at 800 rpm for 120 min at 120° C. to obtain a packaging film filler; (2) Dissolve 1 part of maleic anhydride and 0.15 parts of dicumyl peroxide in 5 parts of acetone, mix with 50 parts of polylactic acid pellets, and stir at 2000 rpm for 20 minutes; place for 24 hours, after the acetone is completely volatilized, add it to a twin-screw extruder for melt extrusion; set the temperature of each section of the twin-screw extruder barrel to 160°C, 170°C, and 180°C, respectively, and set 180°C as the reaction temperature of the third section; the head temperature is 160°C; control the main screw speed to 120r / min, and the feed screw speed to 10r / in; cool the extrudate to 25°C at room temperature, cut it into pellets, and then dry it at room temperature for 24 hours to obtain the modified polylactic acid; (3) The modified polylactic acid and AZ91TN polybutylene succinate were placed in a 50°C forced air oven for 12 h; then placed in a high-speed mixer containing a packaging film filler, the mass ratio of the packaging film filler, the modified polylactic acid, and the polybutylene succinate was 4:2:1.5, and blended at a speed of 500 rpm for 5 min. The blended composite polymer was prepared by a twin-screw extruder; the screw speed was 180 rpm, the extrusion temperature range was 165°C, and then extrusion blown film was prepared into a packaging film raw material with a thickness of 50 μm. The film blowing process was: prepared using a smooth bore single screw extruder equipped with a film blowing head with a diameter of 46 mm, the film blowing temperature range was 175°C, and the screw speed was 40 rpm; and then cut into packaging bags.
[0023] Comparative Example 1: The difference between Comparative Example 1 and Example 2 is that step (1) is changed to: weigh 12 parts of ethylene glycol by weight, add 2 parts of N-hydroxymethyl acrylamide, and mechanically stir at 300 rpm in a high-speed mixer for 45 minutes to obtain a mixed solution; slowly pour the mixed solution into 45 parts of wheat starch for 10 minutes, and stir at 1500 rpm to mix them thoroughly; after stirring, add 6 parts of carboxymethyl cellulose with a viscosity of 600 cps, and continue stirring at 650 rpm at 110°C for 90 minutes to obtain a packaging film filler; the remaining steps are the same as those of Example 2.
[0024] Comparative Example 2: The difference between Comparative Example 2 and Example 2 is that step (1) is changed to: dissolve 0.2 parts of carboxymethyl cellulose with a viscosity of 600 cps in 100 parts of deionized water, and stir at 100 rpm for 12 hours at 35°C to prepare a carboxymethyl cellulose solution; then add 0.2 parts of sodium periodate to the carboxymethyl cellulose solution; dropwise add a 1% sulfuric acid aqueous solution to adjust the pH value of the solution to 3, and then allow to react for 6 hours; after the reaction is completed, add excess ethylene glycol to remove unreacted sodium periodate; use 1 part of ethanol for precipitation, and then dialyze with pure water for 24 hours using a 5 μm dialysis membrane; dialyze the dialyzed To the resulting solution, 0.07 parts of malic acid were added, and a 1% aqueous sulfuric acid solution was added dropwise to adjust the pH to 7. The mixture was stirred at 100 rpm for 12 h at 25° C., and vacuum dried at 37° C. and 0.085 MPa to constant weight to obtain modified carboxymethyl cellulose; 12 parts of glycerol were weighed according to the weight ratio, and all of them were slowly poured into 45 parts of wheat starch for 10 min, and stirred at 1500 rpm to fully mix them; after the stirring was completed, 6 parts of modified carboxymethyl cellulose were added, and the mixture was stirred at 650 rpm for 90 min at 110° C. to obtain a packaging film filler; the remaining steps were the same as those in Example 2.
[0025] Comparative Example 3: The difference between Comparative Example 3 and Example 2 is that step (1) is changed to: weigh 12 parts of ethylene glycol by weight, add 2 parts of N-hydroxymethyl acrylamide, and mechanically stir at 300 rpm in a high-speed mixer for 45 minutes to obtain a mixed solution; slowly pour the entire mixed solution into 45 parts of wheat starch for 10 minutes, and at the same time stir at 1500 rpm to fully mix them, to obtain a packaging film filler; the remaining steps are the same as Example 2.
[0026] Comparative Example 4: The difference between Comparative Example 4 and Example 2 is that there is no step (2), and step (3) is changed to: placing polylactic acid pellets and AZ91TN polybutylene succinate in a 50°C blast oven for 12 hours; using a melt blending method, placing polylactic acid and polybutylene succinate in a high-speed mixer containing a packaging film filler in step (1), the mass ratio of the packaging film filler, polylactic acid, and polybutylene succinate being 3.5:1.5:1, blending at a speed of 500 rpm for 5 minutes, and preparing a blended composite polymer by a twin-screw extruder; the screw speed is 170 rpm, the extrusion temperature range is 155°C, and then extruding and blowing a film to prepare a packaging film raw material with a thickness of 40 μm, the film blowing process is: using a smooth bore single screw extruder equipped with a film blowing head with a diameter of 46 mm, the film blowing temperature range is 165°C, and the screw speed is 35 rpm; and then cutting to prepare a packaging bag; the remaining steps are the same as in Example 2.
[0027] Comparative Example 5: The difference between Comparative Example 5 and Example 2 is that step (3) is different. Step (3) is changed to: placing the modified polylactic acid in a 50°C blast oven for 12 hours; using a melt blending method, placing the modified polylactic acid in a high-speed mixer containing a packaging film filler in step (1), the mass ratio of the packaging film filler to the modified polylactic acid being 3.5:2.5, blending at a speed of 500 rpm for 5 minutes, and preparing the blended composite polymer by a twin-screw extruder; the screw speed is 170 rpm, the extrusion temperature range is 155°C, and then extrusion blown film is used to prepare a packaging film raw material with a thickness of 40 μm, the film blowing process is: using a smooth bore single screw extruder equipped with a film blowing head with a diameter of 46 mm, the film blowing temperature range is 165°C, and the screw speed is 35 rpm; and then cutting to prepare a packaging bag; the remaining steps are the same as in Example 2.
[0028] Effect example Table 1 below shows the performance analysis results of a fully bio-enzyme-degradable packaging film using Examples 1 to 3 of the present invention and Comparative Examples 1 to 5.
[0029] Table 1
[0030] From the comparison of the experimental data of the elongation at break of the embodiment and the comparative example, it can be found that the present invention uses N-hydroxymethyl acrylamide as a crosslinking agent, and the unsaturated active functional groups contained therein are hydrophilic, and dispersed in starch under the dissolution of glycerol, thereby improving the solubility of starch in the composite polymer; then adding modified carboxymethyl cellulose, and cooperating with N-hydroxymethyl acrylamide to improve the mechanical properties of the packaging film after preparation, and improving its elongation at break; using malic acid to modify carboxymethyl cellulose, hydroxymethyl cellulose has a large specific surface area and high surface energy, and can graft more malic acid; after high temperature reaction, malic acid and N-hydroxymethyl acrylamide form functional micro-crosslinking areas in starch, and are compatible with starch molecules, achieving the effect of synergistic volume expansion, and further improving the elongation at break of the packaging film. Secondly, the present invention uses modified polylactic acid and polybutylene succinate as composite polymer raw materials, and prepares a packaging film by melt blending and extrusion film blowing process. Both modified polylactic acid and polybutylene succinate are biodegradable polymers, but the toughness of modified polylactic acid is poor. Polybutylene succinate is added to the modified polylactic acid for blending to change its mechanical properties. Since the two are incompatible systems, the present invention uses maleic anhydride for bridging grafting to achieve a miscible effect and also improve the compatibility of the filler and the composite polymer. From the comparison of the experimental data of biodegradability of the embodiment and the comparative example, it can be found that the present invention not only selects biodegradable materials in terms of raw material use, but also introduces maleic anhydride, so that the modified polylactic acid has a degradable group, which accelerates the biodegradable efficiency of the packaging film.
[0031] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A fully bio-enzyme-degradable packaging film and packaging bag, characterized in that: The method comprises the following preparation steps: (1) Weigh 11-13 parts of glycerol according to the weight ratio, add 1-3 parts of N-hydroxymethyl acrylamide, and mechanically stir at 200-400 rpm in a high-speed mixer for 30-60 minutes to obtain a mixed solution; slowly pour the mixed solution into 40-50 parts of starch for 10 minutes, and stir at 1000-2000 rpm to fully mix; after the stirring is completed, add 2-10 parts of modified carboxymethyl cellulose, and continue to stir at 500-800 rpm for 60-120 minutes at 100-120° C. to obtain a packaging film filler; (2) Dissolve 1 part of maleic anhydride and 0.15 parts of vulcanizing agent in 3-5 parts of acetone, mix with 40-50 parts of polylactic acid, and stir at 2000 rpm for 20 minutes; place for 24 hours, after the acetone is completely volatilized, add it to a twin-screw extruder for melt extrusion; set the temperature of each section of the twin-screw extruder barrel to 160°C, 170°C, and 180°C, respectively, and set 180°C as the reaction temperature of the third section; the head temperature is 160°C; control the main screw speed to 90-120r / min, and the feeding screw speed to 10r / in; cool the extrudate to 25°C at room temperature, cut into pellets, and then dry at room temperature for 24 hours to obtain modified polylactic acid; (3) The modified polylactic acid and polybutylene succinate are placed in a 50°C forced air oven for 12 hours, and then placed in a high-speed mixer containing packaging film filler, and the blended composite polymer is prepared by a twin-screw extruder; the screw speed is 160-180rpm, the extrusion temperature range is 145-165°C, and then the packaging film raw material with a thickness of 30-50μm is prepared by extrusion blown film, and then it is prepared into packaging bags by cutting.
2. A fully bio-enzyme-degradable packaging film and packaging bag according to claim 1, characterized in that: The starch in step (1) is wheat starch or corn starch.
3. A fully bio-enzyme-degradable packaging film and packaging bag according to claim 1, characterized in that: The preparation method of the modified carboxymethyl cellulose in the step (1) is as follows: 0.2 parts of carboxymethyl cellulose is dissolved in 100 parts of deionized water, and stirred at 100 rpm for 12 hours at 35°C to prepare a carboxymethyl cellulose solution; then 0.2 parts of sodium periodate is added to the carboxymethyl cellulose solution; a 1% sulfuric acid aqueous solution is added dropwise to adjust the pH value of the solution to 3-4, and then the solution is allowed to react for 6 hours; after the reaction is completed, an excess of ethylene glycol is added to remove unreacted sodium periodate; 1 part of ethanol is used for precipitation, and then the solution is dialyzed with pure water using a 5 μm dialysis membrane for 24 hours; 0.04-0.1 parts of malic acid are added to the dialyzed solution, a 1% sulfuric acid aqueous solution is added dropwise to adjust the pH to 7-8, the solution is stirred at 25°C at 100 rpm for 12 hours, and vacuum dried at 37°C and 0.085 MPa to constant weight to obtain the modified carboxymethyl cellulose.
4. A fully bio-enzyme-degradable packaging film and packaging bag according to claim 3, characterized in that: The carboxymethyl cellulose has a viscosity of 300-900 cps.
5. The fully bio-enzyme-degradable packaging film and packaging bag according to claim 1, characterized in that: In the step (2), the vulcanizing agent is dicumyl peroxide.
6. A fully bio-enzyme-degradable packaging film and packaging bag according to claim 1, characterized in that: The polylactic acid in step (2) is polylactic acid pellets.
7. The fully bio-enzyme-degradable packaging film and packaging bag according to claim 1, characterized in that: The polybutylene succinate in step (3) is AZ91TN polybutylene succinate.
8. The fully bio-enzyme-degradable packaging film and packaging bag according to claim 1, characterized in that: In the step (3), the mass ratio of the packaging film filler, the modified polylactic acid, and the polybutylene succinate is 3-4:1-2:0.5-1.
5.
9. The fully bio-enzyme-degradable packaging film and packaging bag according to claim 1, characterized in that: In step (3), the high-speed mixer is used for blending at a speed of 500 rpm for 5 minutes.
10. The fully bio-enzyme-degradable packaging film and packaging bag according to claim 1, characterized in that: The film blowing process in step (3) is as follows: the film is prepared by using a smooth bore single screw extruder equipped with a film blowing head with a diameter of 46 mm, the film blowing temperature range is 155-175° C., and the screw speed is 30-40 rpm.
Citation Information
Patent Citations
Degradable environment-friendly plastic film
CN113004607A
Starch biodegradable film and production method thereof
CN114736437A
Biodegradable material and process for producing the same
CN1871283A
Composition containing cellulose nanofiber and starch
JP2020033531A
Cited By
Biodegradable material as well as preparation method and application thereof
CN120737565A
A biodegradable material, its preparation method and its application
CN120737565B