Preparation method of semi-steel anti-slip low rolling resistance tire

By using core-shell foaming material combined with porous adhesive layer in the tire, using short fibers and microporous structures, the problem of difficult balance of grip and rolling resistance in traditional tires under slippery and dry conditions is solved, and the problem of the difficulty in balancing the grip and rolling resistance of traditional tires is achieved. Higher grip and lower rolling resistance improve vehicle safety and fuel efficiency.

CN118772501BActive Publication Date: 2024-11-22SHANDONG ZHENTAI TIRE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411260986.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-22
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

Traditional tires lack grip in slippery conditions, and rolling resistance in dry conditions is too high, making it difficult to balance the performance of both, resulting in limited vehicle safety and fuel efficiency.

Method used

The design of core-shell foaming material combined with the porous adhesive layer is adopted to form a uniform porous structure in the tire through short fibers and microporous structures, improving drainage and grip while reducing rolling resistance.

Benefits of technology

Significantly improve grip on slippery roads, reduce rolling resistance, improve vehicle safety and fuel efficiency, and enhance structural stability and fatigue resistance through fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the technical field of rubber tires, and specifically proposes a method for preparing a semi-steel anti-wet and anti-skid low rolling resistance tire. By combining short fibers with core-shell foamed particles and optimizing the rubber layer formula, significant improvements in wet grip and rolling resistance are achieved. Compared with traditional microporous tires, the core-shell structure of nylon short fibers significantly improves wet grip, especially in humid environments, and the swelling characteristics of nylon fibers further enhance the grip performance. In addition, by optimizing the ratio of carbon black and vulcanizer in the rubber layer, as well as reasonable process control, the rolling resistance is further reduced, and the wear resistance and fatigue resistance of the tire are improved. The dual optimization scheme of surface modification and annealing treatment significantly enhances the comprehensive performance of the tire while improving the bonding strength between the fiber and the rubber matrix. Finally, the scheme proposed by the present invention is superior to the traditional scheme in various performance indicators, providing a new technical path for the design of high-performance tires.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber tires, and in particular to a method for preparing a semi-steel anti-slip low rolling resistance tire. Background Art

[0002] With the continuous development of the automotive industry, consumers have higher and higher requirements for tire performance, especially grip on wet and slippery roads and low rolling resistance on dry roads. The balance of these two properties directly affects vehicle safety, fuel efficiency and driving experience. However, traditional tire materials face many challenges in optimizing these two properties.

[0003] Traditional tires usually use homogeneous rubber materials or composite materials containing fillers such as carbon black, which can provide lower rolling resistance under dry conditions, but often have difficulty providing sufficient grip under wet conditions. This is mainly because the liquid film formed on the surface of the rubber material after it comes into contact with water increases the risk of sliding between the tire and the road surface, resulting in a significant decrease in grip. In order to improve performance on wet roads, some tire manufacturers have introduced rubber materials with microporous structures. These micropores can enhance drainage and surface roughness, thereby improving grip under wet conditions. However, while such microporous structure materials improve grip, they usually reduce the overall strength of the tire and increase rolling resistance under dry conditions, resulting in reduced fuel efficiency.

[0004] Providing a tire that strikes a balance between wet grip and low rolling resistance has become a major challenge in the field of tire technology in recent years. Summary of the invention

[0005] In view of this, the present invention proposes a method for preparing a semi-steel anti-wet and low rolling resistance tire with a more reasonable structural design, aiming to balance wet grip and low rolling resistance and provide a tire with better comprehensive performance.

[0006] The technical solution of the present invention is achieved as follows: The present invention provides a method for preparing a semi-steel anti-slip low rolling resistance tire, comprising the following steps:

[0007] Preparation of core-shell foaming material: liquid styrene-butadiene rubber, short fibers, carbon black, vulcanizer, accelerator, plasticizer and diluent are uniformly mixed to obtain a coating liquid, and the coating liquid is rolled onto the surface of the foaming particles and dried to obtain a core-shell foaming material;

[0008] Preparation of porous rubber layer: Styrene-butadiene rubber, natural rubber, carbon black, vulcanizer, accelerator and plasticizer are mixed in an internal mixer at 55-65°C for 10-20 minutes to obtain a rubber layer substrate, core-shell foam material and rubber layer substrate are mixed in a mass ratio of 1: (4-9) and kneaded at 50-60°C for 10-20 minutes, molded at 110°C-130°C for 20-30 minutes into a thin sheet, and pre-vulcanized at 145-155°C for 20-40 minutes to obtain a porous rubber layer;

[0009] Preparation of semi-steel anti-skid low rolling resistance tire: laminate the porous rubber layer and the tread part of the semi-steel tire, perform final vulcanization at 165-175°C for 40-50 minutes, and then form the tire.

[0010] In the above embodiment, the foamed particles may be polyurethane foamed particles, wherein the foaming agent material is ADC. Specifically, the foamed particles may be obtained by mixing and granulating polyurethane, foaming agent ADC and bisphenol A epoxy resin in a mass ratio of 40:2:3.

[0011] In the above embodiment, a coating liquid is prepared by using a mixture of liquid styrene-butadiene rubber and short fibers, carbon black, a vulcanizer, an accelerator, a plasticizer and a diluent, and the coating liquid is roll-coated onto the surface of the foamed particles, followed by drying to obtain a core-shell foamed material. The core-shell foamed material and the adhesive layer substrate are kneaded at a specific temperature to ensure that the foamed particles are evenly distributed and form a uniform porous structure. This structure not only provides good drainage on wet and slippery roads, but also reduces rolling resistance through an optimized pore structure.

[0012] Specifically, the porous rubber layer in the tire structure is realized by introducing micropores into the rubber matrix. These micropores can act as drainage channels. When the tire contacts a wet road surface, water is quickly introduced into these micropores, thereby effectively reducing the thickness of the water film between the tire and the road surface. The microporous structure can form a certain water absorption effect between the tire and the road surface, quickly absorb and remove moisture from the contact surface, so that the tire can contact the road surface more directly. By reducing the thickness of the water film, the grip of the tire is enhanced, thereby improving the driving safety on wet roads. The micropores in the porous rubber layer not only play a role in drainage, but also attract water into the pores through capillary water absorption. This effect effectively reduces the accumulation of water on the tire surface and further reduces the formation of water film. The microporous structure reduces the surface tension of the water film by increasing the effective contact area of ​​the tire surface, making it easier to destroy and discharge water, so that the tire maintains a high grip on wet roads.

[0013] On the basis of this microporous structure, the fiber material serves as the skeleton of the microporous structure, which improves the overall rigidity and durability of the composite material. During the microporous formation process, the presence of the fiber makes the pore wall stronger and less likely to collapse or deform, thereby ensuring the structural stability of the micropores. On slippery roads, these fibers further enhance the tire's grip by increasing the contact area and surface roughness. This enhancement, in conjunction with the microporous structure, can more effectively destroy the water film and directly contact the road surface. The capillary action of the fiber material can form a more effective water removal channel in the microporous structure. When the tire contacts a slippery road, the water can be quickly guided by the fiber to the inside of the micropores and then discharged through the pores, thereby significantly improving the drainage performance of the tire. During the molding and pre-vulcanization process, a good synergistic effect is formed between the fiber and the microporous structure. The fiber-reinforced pore wall will not deform easily when subjected to pressure, maintaining the stability of the pore structure, which is very important for reducing rolling resistance. At the same time, the presence of the fiber material ensures that the material's anti-slip performance is excellent under a variety of road conditions. The good combination between the fiber material and the rubber matrix enables the microporous structure to maintain good shape and function under high pressure, further reducing rolling resistance.

[0014] In some embodiments, in the preparation of the core-shell foaming material, the mass ratio of liquid styrene-butadiene rubber, short fibers, carbon black, vulcanizer, accelerator, plasticizer and diluent is 100: (8-12): (35-45): (2-3): (1-1.5): (8-12): (10-50).

[0015] In some embodiments, the staple fibers are nylon staple fibers.

[0016] The use of nylon staple fibers is not only because nylon has excellent mechanical and chemical properties, but also because nylon fibers are hydrophilic materials. Therefore, nylon absorbs water in a wet road environment. During this water absorption period, the fiber length increases, causing the fiber structure on the tire surface to expand slightly, thereby increasing the actual contact area between the tire and the road. A larger contact area means that the tire can contact the road more directly, thereby improving grip. Nylon fibers that have been stretched by water can penetrate deeper into the water film, helping to break the water film between the tire and the road. This effect reduces the thickness of the water film, reduces the risk of sliding caused by the presence of the water film, and enhances the stability and safety of the tire on wet roads. The combination of the microporous structure and the nylon fiber allows the fibers that have been stretched by water to expand in the pores, further supporting the pore walls and enhancing the stability of the pore structure. This expansion effect not only helps to maintain the pore shape, but also further increases the drainage efficiency by physically stretching it open.

[0017] In some embodiments, the nylon staple fibers have an average diameter of 10-20 μm and an average length of 100-200 μm.

[0018] The above preferred fiber diameter and length are used to provide suitable mechanical properties and an effective support network to improve the tensile strength and tear resistance of the material. This length setting ensures that the fiber can fully exert its reinforcing effect in the composite material while maintaining good processing performance.

[0019] In some embodiments, the nylon staple fiber is surface modified, and the surface modification method includes: soaking the nylon fiber in a 1-5wt% hydroxysilane aqueous solution for 1-3 hours and then drying, then soaking in a solution containing 1-5wt% glycolic acid for 1-3 hours, washing and drying to obtain the surface modified nylon staple fiber.

[0020] Through the action of hydroxysilane, active silane groups are introduced on the surface of nylon fiber. Through the action of glycolic acid, the fiber surface is further functionalized to increase hydrophilicity and the density of active groups. Hydroxysilane molecules have a dual functional group structure, one end is an organic functional group that can react with organic materials, and the other end is a silane group that can react with inorganic materials (such as amino or carboxyl groups on the surface of nylon fibers). During the soaking process, hydroxysilane undergoes a condensation reaction with the active groups on the surface of nylon fibers through the silane groups to form a strong chemical bond. Glycolic acid (hydroxyacetic acid) is an α-hydroxy acid with good acidity and chelating ability. During the soaking process, glycolic acid can further activate the fiber surface, increase its hydrophilicity, and introduce more hydroxyl and carboxyl functional groups. These newly added functional groups can form hydrogen bonds or other secondary bonds with the active groups in the rubber matrix (such as double bonds, hydroxyl groups, etc.), thereby improving the interfacial affinity between the fiber and the matrix. The surface roughness and chemical activity of the fiber after surface modification are enhanced, which helps to improve the mechanical locking effect between the fibers. Higher friction enables the fibers to be more firmly interwoven with each other in the composite material, thus forming a stronger fiber network structure.

[0021] The hydroxysilane mentioned above may be trimethylsilanol.

[0022] In some embodiments, the nylon staple fibers are subjected to annealing treatment, and the annealing treatment method includes subjecting the nylon staple fibers to a flame burning treatment at 100-140° C., and the burning treatment time is 0.5-1.5 seconds.

[0023] The above annealing process is designed to cause slight thermoplastic deformation of the surface layer of nylon fiber, which helps to eliminate the internal stress of the fiber and improve the order of the surface molecular chain. During the annealing process, the molecular chains on the surface of nylon fiber are rearranged, resulting in increased crystallinity. Higher crystallinity increases the rigidity and strength of the fiber, which helps to enhance the overall mechanical properties of the composite material. The micro-bending structure brought by thermoplastic deformation increases the contact area and significantly enhances the friction when the fibers contact each other in the composite material. This increased friction enables the fibers to better resist relative sliding, thereby improving the tensile strength and tear resistance of the material. Due to the micro-bending structure on the fiber surface, when the fiber is subjected to external force, these bent parts will be embedded in the recessed area of ​​the adjacent fiber, forming a self-locking effect. This self-locking effect can stabilize the fiber network structure under the action of external force and reduce the possibility of fiber slippage or breakage. In the composite material, the overall strength of the fiber network depends in part on the relative position stability between the fibers. The micro-bending structure significantly improves the mutual stability between the fibers through the self-locking effect, prevents the fibers from slipping under stress, and maintains the overall mechanical properties of the material. Due to the enhanced self-locking ability between fibers, external forces can be evenly distributed in the fiber network, avoiding stress concentration in certain weak points. Uniform stress distribution helps to extend the service life of the material and improve its fatigue resistance.

[0024] In some embodiments, the method of rolling the coating liquid onto the surface of the foamed particles includes: placing the foamed particles in a drum, maintaining the drum speed at 20-40 rpm at 60-80°C, spraying the coating liquid onto the surface of the foamed particles, and after spraying, keeping the drum rotating and keeping warm and drying for 1-2 hours to obtain a core-shell type foaming material.

[0025] In some embodiments, the particle size of the foamed particles is 0.1-0.5 mm.

[0026] In some embodiments, the mass ratio of the coating liquid roller to the foamed particles is 1:(1.5-4).

[0027] In some embodiments, in the base material, the mass ratio of styrene-butadiene rubber, natural rubber, carbon black, vulcanizer, accelerator, and plasticizer is 70:30:(45-55):(1-3):(0.5-1.5):(5-10).

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The preparation method of the semi-steel anti-slip low rolling resistance tire provided by the present invention improves the grip of the tire tread part under wet and slippery road conditions by combining short fibers with a microporous structure. The microporous strength of the short fibers is higher, and on dry roads, the contact area with the road surface can be significantly reduced, thereby reducing rolling resistance. The microporous structure can effectively reduce the weight of the tire and further reduce energy loss during rolling. The addition of short fibers is beneficial to the elastic recovery performance of the microporous structure, which is beneficial to further reducing rolling resistance and improving the energy utilization rate of the vehicle. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the embodiments of the present invention belong. If the definitions set forth in this section are contrary to or otherwise inconsistent with the definitions set forth in the patents, patent applications, published patent applications, and other publications incorporated herein by reference, the definitions listed in this section take precedence over the definitions incorporated herein by reference.

[0032] Unless otherwise specified, the methods used in the following examples are all conventional methods. Unless otherwise specified, the materials, reagents and instruments used are all conventional materials, reagents and instruments in the art, and can be obtained by those skilled in the art through commercial channels.

[0033] When an amount, concentration or other value or parameter is expressed as a range, a preferred range or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including the range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described herein, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range. In the present specification and claims, range definitions can be combined and / or interchanged, and if not otherwise stated, these ranges include all subranges contained therein.

[0034] The conventional microporous tread design can theoretically reduce the overall weight of the tire and reduce energy loss on the contact surface through the buffering effect of the micropores. However, during high-pressure and high-frequency rolling, the pore wall is prone to collapse or deformation, resulting in a decrease in the stability of the microporous structure. The collapse of the pore wall will increase the contact area between the rubber matrix and the road surface, resulting in an increase in rolling resistance. In conventional rubber materials, the microporous structure is often difficult to quickly recover to its original state when subjected to repeated compression. This hysteresis effect will increase the rolling resistance of the tire because the tire cannot effectively rebound when contacting and leaving the road surface, resulting in increased energy loss.

[0035] Although some existing solutions set up microporous structures to more effectively destroy the liquid film between the tire and the road surface under slippery road conditions, thereby improving grip, when the strength of the rubber matrix material is low, these micropores are prone to shrinkage or closure of the pore walls under high pressure and slippery conditions. This not only weakens the ability of the micropores to drain water and destroy the liquid film, but may also further cause the tire to lose some grip on slippery roads.

[0036] Based on the above-mentioned deficiencies and the problems existing in the prior art, the applicant has proposed a new improvement idea, which is to overcome the problem of insufficient structural strength of micropores formed in rubber materials by enhancing the strength of the pore walls of the micropore structure. Specifically, the present application first prepares a foamed particle with a shell, wherein the shell structure includes a rubber matrix and short fibers for reinforcement, and the short fibers are interlaced and associated with each other, and supported by the foaming material, so as to form a uniform shell on the surface of the foaming material, and then the foamed particles with the shell structure are mixed with the rubber substrate to prepare a porous rubber, and the inner wall of the pores of the porous rubber has a pre-formed layered structure containing interlaced short fibers, so as to obtain a good pore structure maintenance effect. When the porous rubber is subjected to other forces such as pressure, the support of the layered structure with short fibers forms a good maintenance effect on the pore structure, and these short fibers are conducive to further increasing the destructive effect on the liquid film and the anchoring effect between the contacting ground, so as to achieve a good anti-slip effect and a low rolling resistance effect.

[0037] The semi-steel anti-skid low rolling resistance tire of the present application is described in detail below through specific embodiments.

[0038] Example 1

[0039] Preparation of a semi-steel anti-slip low rolling resistance tire:

[0040] S1. Preparation of core-shell foaming material: 100 g of liquid styrene-butadiene rubber, 10 g of nylon staple fiber (average diameter 10 μm, average length 100 μm), 40 g of carbon black N330, 2.5 g of sulfur, 1.2 g of accelerator DM, 10 g of paraffin oil and 30 g of toluene are uniformly mixed to obtain a coating liquid for use; 200 g of foaming particles with an average particle size of 0.5 mm are added into a drum, the temperature in the drum is maintained at 70°C, the rotation speed is 30 rpm, 100 g of the coating liquid is sprayed into the drum, and after spraying, the drum is kept warm and rotated to dry for 1.5 hours to obtain a core-shell foaming material.

[0041] S2. Preparation of porous adhesive layer: 70g of styrene-butadiene rubber, 30g of natural rubber, 50g of carbon black N330, 2g of sulfur, 1g of accelerator CBS and 8g of paraffin oil were mixed in an internal mixer at 60°C for 15min to obtain an adhesive layer substrate; 20g of core-shell foaming material was mixed with 100g of the adhesive layer substrate and kneaded at 55°C for 15min, and then molded at 120°C for 25min to form a thin sheet (foamed); the mixture was heated to 150°C for pre-treatment for 30min and demolded to obtain a porous adhesive layer.

[0042] S3. Preparation of a semi-steel anti-skid low rolling resistance tire: laminating the porous rubber layer with the tread part of the semi-steel tire, and vulcanizing it at 170° C. for 45 minutes to obtain a semi-steel anti-skid low rolling resistance tire.

[0043] Example 2

[0044] S1. Preparation of core-shell foaming material: 100 g of liquid styrene-butadiene rubber, 8 g of nylon staple fiber (average diameter 10 μm, average length 100 μm), 45 g of carbon black N330, 2 g of sulfur, 1 g of accelerator DM, 12 g of paraffin oil and 10 g of toluene are mixed evenly to obtain a coating liquid for use; 200 g of foaming particles with an average particle size of 0.3 mm are added into a drum, the temperature in the drum is maintained at 60°C, the rotation speed is 40 rpm, 100 g of the coating liquid is sprayed into the drum, and after spraying, the drum is kept warm and rotated to dry for 2 hours to obtain a core-shell foaming material.

[0045] S2. Preparation of porous adhesive layer: 70g of styrene-butadiene rubber, 30g of natural rubber, 50g of carbon black N330, 2g of sulfur, 1g of accelerator CBS and 8g of paraffin oil were mixed in an internal mixer at 60°C for 15min to obtain an adhesive layer substrate; 20g of core-shell foaming material was mixed with 100g of the adhesive layer substrate and kneaded at 55°C for 15min, and then molded at 120°C for 25min to form a thin sheet (foamed); the mixture was heated to 150°C for pre-treatment for 30min and demolded to obtain a porous adhesive layer.

[0046] S3. Preparation of a semi-steel anti-skid low rolling resistance tire: laminating the porous rubber layer with the tread part of the semi-steel tire, and vulcanizing it at 170° C. for 45 minutes to obtain a semi-steel anti-skid low rolling resistance tire.

[0047] Example 3

[0048] S1. Preparation of core-shell foaming material: 100 g of liquid styrene-butadiene rubber, 12 g of nylon staple fiber (average diameter 10 μm, average length 100 μm), 35 g of carbon black N330, 3 g of sulfur, 1.5 g of accelerator DM, 8 g of paraffin oil and 50 g of toluene are uniformly mixed to obtain a coating liquid for use; 200 g of foaming particles with an average particle size of 0.1 mm are added into a drum, the temperature in the drum is maintained at 80°C, the rotation speed is 20 rpm, 100 g of the coating liquid is sprayed into the drum, and after spraying, the drum is kept warm and rotated to dry for 1 hour to obtain a core-shell foaming material.

[0049] S2. Preparation of porous adhesive layer: 70g of styrene-butadiene rubber, 30g of natural rubber, 50g of carbon black N330, 2g of sulfur, 1g of accelerator CBS and 8g of paraffin oil were mixed in an internal mixer at 60°C for 15min to obtain an adhesive layer substrate; 20g of core-shell foaming material was mixed with 100g of the adhesive layer substrate and kneaded at 55°C for 15min, and then molded at 120°C for 25min to form a thin sheet (foamed); the mixture was heated to 150°C for pre-treatment for 30min and demolded to obtain a porous adhesive layer.

[0050] S3. Preparation of a semi-steel anti-skid low rolling resistance tire: laminating the porous rubber layer with the tread part of the semi-steel tire, and vulcanizing it at 170° C. for 45 minutes to obtain a semi-steel anti-skid low rolling resistance tire.

[0051] Example 4

[0052] S1. Preparation of core-shell foaming material: 100 g of liquid styrene-butadiene rubber, 10 g of nylon staple fiber (average diameter 10 μm, average length 100 μm), 40 g of carbon black N330, 2.5 g of sulfur, 1.2 g of accelerator DM, 10 g of paraffin oil and 30 g of toluene are uniformly mixed to obtain a coating liquid for use; 200 g of foaming particles with an average particle size of 0.5 mm are added into a drum, the temperature in the drum is maintained at 70°C, the rotation speed is 30 rpm, 100 g of the coating liquid is sprayed into the drum, and after spraying, the drum is kept warm and rotated to dry for 1.5 hours to obtain a core-shell foaming material.

[0053] S2. Preparation of porous adhesive layer: 70g of styrene-butadiene rubber, 30g of natural rubber, 45g of carbon black N330, 1g of sulfur, 0.5g of accelerator CBS and 5g of paraffin oil were mixed in an internal mixer at 55°C for 20min to obtain an adhesive layer substrate; 20g of core-shell foaming material was mixed with 100g of the adhesive layer substrate and kneaded at 50°C for 20min, and then molded at 130°C for 20min to form a thin sheet (foamed); the mixture was heated to 155°C for pre-treatment for 20min, and the porous adhesive layer was obtained after demolding.

[0054] S3. Preparation of a semi-steel anti-wet skid low rolling resistance tire: laminating the porous rubber layer with the tread part of the semi-steel tire, and vulcanizing it at 175° C. for 40 minutes to obtain a semi-steel anti-wet skid low rolling resistance tire.

[0055] Example 5

[0056] S1. Preparation of core-shell foaming material: 100 g of liquid styrene-butadiene rubber, 10 g of nylon staple fiber (average diameter 10 μm, average length 100 μm), 40 g of carbon black N330, 2.5 g of sulfur, 1.2 g of accelerator DM, 10 g of paraffin oil and 30 g of toluene are uniformly mixed to obtain a coating liquid for use; 200 g of foaming particles with an average particle size of 0.5 mm are added into a drum, the temperature in the drum is maintained at 70°C, the rotation speed is 30 rpm, 100 g of the coating liquid is sprayed into the drum, and after spraying, the drum is kept warm and rotated to dry for 1.5 hours to obtain a core-shell foaming material.

[0057] S2. Preparation of porous adhesive layer: 70g of styrene-butadiene rubber, 30g of natural rubber, 55g of carbon black N330, 3g of sulfur, 1.5g of accelerator CBS and 10g of paraffin oil were mixed in an internal mixer at 65°C for 10min to obtain an adhesive layer substrate; 20g of core-shell foaming material was mixed with 100g of the adhesive layer substrate and kneaded at 60°C for 10min, and then molded at 110°C for 30min to form a thin sheet (foamed); the mixture was heated to 145°C for pre-treatment for 40min and demolded to obtain a porous adhesive layer.

[0058] S3. Preparation of a semi-steel anti-skid low rolling resistance tire: laminating the porous rubber layer with the tread part of the semi-steel tire, and vulcanizing it at 165° C. for 50 minutes to obtain a semi-steel anti-skid low rolling resistance tire.

[0059] Example 6

[0060] On the basis of Example 1, other conditions remain unchanged, and the only difference is that the short fibers used are polyester short fibers.

[0061] Example 7

[0062] On the basis of Example 1, other conditions remain unchanged, and the only difference is that the short fibers used are glass short fibers.

[0063] Example 8

[0064] On the basis of Example 1, other conditions remain unchanged, and the only difference is that the short fibers used are carbon fibers.

[0065] Example 9

[0066] On the basis of Example 1, other conditions remain unchanged, except that the average diameter of the nylon staple fibers used is 15 μm and the average length is 150 μm.

[0067] Example 10

[0068] On the basis of Example 1, other conditions remain unchanged, except that the average diameter of the nylon staple fibers used is 20 μm and the average length is 200 μm.

[0069] Embodiment 11

[0070] On the basis of Example 1, other conditions remain unchanged, except that the average diameter of the nylon staple fibers used is 5 μm and the average length is 50 μm.

[0071] Example 12

[0072] On the basis of Example 1, other conditions remain unchanged, except that the average diameter of the nylon staple fibers used is 30 μm and the average length is 300 μm.

[0073] Embodiment 13

[0074] On the basis of Example 1, other conditions remain unchanged, and the only difference is that the nylon staple fibers used are pre-surface modified, and the method includes: soaking the nylon fibers in a 3wt% hydroxysilane aqueous solution for 2 hours and then drying, and then soaking them in a solution containing 3wt% glycolic acid for 2 hours, washing and drying to obtain surface-modified nylon staple fibers.

[0075] Embodiment 14

[0076] On the basis of Example 1, other conditions remain unchanged, and the only difference is that the nylon staple fibers used are pre-surface modified, and the method includes: soaking the nylon fibers in a 1wt% hydroxysilane aqueous solution for 3 hours and then drying, and then soaking them in a solution containing 1wt% glycolic acid for 3 hours, washing and drying to obtain surface-modified nylon staple fibers.

[0077] Embodiment 15

[0078] On the basis of Example 1, other conditions remain unchanged, and the only difference is that the nylon staple fibers used are pre-surface modified, and the method includes: soaking the nylon fibers in a 5wt% hydroxysilane aqueous solution for 1 hour and then drying, and then soaking them in a solution containing 5wt% glycolic acid for 1 hour, washing and drying to obtain surface-modified nylon staple fibers.

[0079] Example 16

[0080] On the basis of Example 1, other conditions remain unchanged, and the only difference is that the nylon staple fibers used are subjected to annealing treatment, and the method includes: subjecting the nylon staple fibers to a flame burning treatment at 120° C., and the burning treatment time is 1 second.

[0081] Embodiment 17

[0082] On the basis of Example 1, other conditions remain unchanged, and the only difference is that the nylon staple fibers used are subjected to annealing treatment, and the method includes: subjecting the nylon staple fibers to a flame burning treatment at 100° C., and the burning treatment time is 1.5 seconds.

[0083] Embodiment 18

[0084] On the basis of Example 1, other conditions remain unchanged, and the only difference is that the nylon staple fibers used are subjected to annealing treatment, and the method includes: subjecting the nylon staple fibers to a flame burning treatment at 140° C., and the burning treatment time is 0.5 s.

[0085] Embodiment 19

[0086] On the basis of Example 1, other conditions remain unchanged, and the only difference is that the nylon staple fibers used are simultaneously subjected to annealing treatment and surface modification treatment, and the method includes: subjecting the nylon staple fibers to a flame burning treatment at 120° C. for 1 second, soaking the annealed nylon fibers in a 3wt% hydroxysilane aqueous solution for 2 hours and then drying, and then soaking the fibers in a solution containing 3wt% glycolic acid for 2 hours, and washing and drying to obtain surface-modified nylon staple fibers.

[0087] Comparative Example 1

[0088] Preparation of a semi-steel anti-slip low rolling resistance tire:

[0089] S1. Preparation of porous rubber layer: 70g of styrene-butadiene rubber, 30g of natural rubber, 50g of carbon black N330, 2g of sulfur, 1g of accelerator CBS and 8g of paraffin oil were mixed in an internal mixer at 60°C for 15min to obtain a rubber layer substrate. 20g of foamed particles (average particle size 0.5mm) were mixed with 100g of the rubber layer substrate and kneaded at 55°C for 15min, and then molded at 120°C for 25min to form a thin sheet (foamed). The mixture was heated to 150°C for pre-treatment for 30min and demolded to obtain a porous rubber layer.

[0090] S2. Preparation of a semi-steel anti-skid low rolling resistance tire: laminating the porous rubber layer with the tread part of the semi-steel tire, and vulcanizing it at 170° C. for 45 minutes to obtain a semi-steel anti-skid low rolling resistance tire.

[0091] Comparative Example 2

[0092] S1. Preparation of porous adhesive layer: 70g of styrene-butadiene rubber, 30g of natural rubber, 50g of carbon black N330, 0.35g of nylon staple fiber (average diameter 10μm, average length 100μm), 2g of sulfur, 1g of accelerator CBS and 8g of paraffin oil were mixed in an internal mixer at 60℃ for 15min to obtain an adhesive layer substrate; 20g of foamed particles (average particle size 0.5mm) were mixed with 100g of the adhesive layer substrate and kneaded at 55℃ for 15min, and then molded at 120℃ for 25min to form a thin sheet (foamed); the mixture was heated to 150℃ for pre-treatment for 30min and demolded to obtain a porous adhesive layer.

[0093] S2. Preparation of a semi-steel anti-skid low rolling resistance tire: laminating the porous rubber layer with the tread part of the semi-steel tire, and vulcanizing it at 170° C. for 45 minutes to obtain a semi-steel anti-skid low rolling resistance tire.

[0094] The semi-steel tires prepared in the above different embodiments and comparative examples were subjected to performance tests, including wet grip test, rolling resistance test, wear resistance test and fatigue resistance test, wherein:

[0095] Wet grip test method: Use standard wet road friction test equipment to test the sliding friction coefficient of the tire on a simulated wet road. By measuring the sliding friction coefficient of the tire on a wet surface, its grip is evaluated.

[0096] Rolling resistance test method: Use a rolling resistance tester to measure the rolling resistance coefficient of the tire at a specified speed and load. The test environment should be controlled at a constant temperature and humidity to ensure the accuracy of the results.

[0097] Wear resistance test method: Use a DIN wear tester to perform a wear test under a specified load to measure the wear on the tire surface. The test should be conducted under dry road conditions to simulate the wear conditions in actual use.

[0098] Fatigue resistance test method: Use a dynamic fatigue tester to simulate the fatigue performance of tires under long-term, high-frequency loads. The test should include repeated compression, tension and bending tests until the tire material cracks or breaks.

[0099] Among them, the wet grip test results are shown in the following table:

[0100]

[0101] The above wet grip test results show that compared with the conventional microporous tire (Comparative Example 1), Examples 1-3 all have better wet grip performance. Although Comparative Example 2 also uses the same equivalent of nylon fiber, it does not use pre-prepared core-shell foamed particles. The wet grip is still slightly insufficient compared with Example 1. It can be seen that the short fiber combined with the core-shell structure foamed particles has an unexpected technical effect on the improvement of wet grip. Examples 4 and 5 respectively optimize the glue layer formula to obtain different degrees of improvement in grip effect. Examples 6-8 respectively use short fibers of different materials, and the wet grip performance shows different degrees of decline. Analysis may be because nylon fiber has a certain swelling ability when wet, which makes the short fiber grow and further improves the grip. Examples 9-12 respectively use nylon staple fibers of different sizes. It can be seen that the preferred sizes are 10-20 μm in diameter and 100-200 μm in length. Examples 13-15 use surface-modified nylon staple fibers, which have significantly improved grip compared to Example 1. Examples 16-18 use annealed nylon staple fibers, and the wet grip effect is slightly better than that of Example 1. Example 19 further uses annealing treatment on the basis of surface modification. At this time, the grip effect is significantly improved, which is better than the effect of simple surface modification treatment.

[0102] The rolling resistance test results are shown in the following table:

[0103]

[0104] According to the above rolling resistance test results, it can be known that Examples 1-3 show a reduction in rolling resistance relative to Comparative Example 1, which is mainly attributed to the combination of short fibers and core-shell foamed particles, making the microporous structure more stable and effectively reducing rolling resistance. Since Comparative Example 2 does not adopt a core-shell structure, its rolling resistance has increased, further proving the advantage of the core-shell structure in controlling rolling resistance. By optimizing the glue layer formula, Examples 4 and 5 have reduced rolling resistance to varying degrees, especially Example 4 shows a more significant effect. Due to the use of short fibers of different materials, Examples 6-8 have higher rolling resistance, indicating that nylon fibers perform better in reducing rolling resistance. Examples 9-12 show the effect of nylon short fibers of different sizes on rolling resistance, and moderate fiber size helps to reduce rolling resistance. The surface modification treatment of Examples 13-15 significantly reduces rolling resistance, and the annealing treatment of Examples 16-18 also effectively reduces rolling resistance. Example 19 shows the minimum rolling resistance through the dual optimization of surface modification and annealing treatment.

[0105] The wear resistance test results are shown in the following table:

[0106]

[0107] It can be seen from the above wear resistance test results that Examples 1-3 show lower wear than Comparative Example 1 in the wear resistance test, which is mainly due to the combination of short fibers and core-shell foamed particles, which enhances the wear resistance of the adhesive layer. Comparative Example 2 does not adopt a core-shell structure, and the wear resistance is reduced. The wear resistance of Examples 4 and 5 is improved by optimizing the adhesive layer formula, indicating that the optimized formula is effective in enhancing wear resistance. Examples 6-8 use short fibers of different materials, and the wear resistance is slightly lower than that of Example 1, which further verifies the advantage of nylon fiber in wear resistance. Examples 9-12 show the effect of nylon short fibers of different sizes on wear resistance, and moderate fiber size shows the best wear resistance. The surface modification treatment of Examples 13-15 significantly reduces the wear, and the annealing treatment of Examples 16-18 also effectively enhances the wear resistance. Example 19 combines surface modification and annealing treatment to show the smallest wear.

[0108] The anti-fatigue performance test results are shown in the following table:

[0109]

[0110] From the above fatigue resistance test, it can be seen that the fatigue resistance of Examples 1-3 is improved compared with that of Comparative Example 1, which is mainly due to the combination of staple fibers and core-shell foamed particles, which enhances the structural stability of the adhesive layer. Comparative Example 2 does not adopt a core-shell structure, and its fatigue resistance is slightly lower. The fatigue resistance of Examples 4 and 5 is improved by optimizing the adhesive layer formula, especially the performance of Example 4 is the most significant. The fatigue resistance of Examples 6-8 is slightly lower, which verifies the effect of nylon fibers in enhancing fatigue resistance. Examples 9-12 show the effect of nylon staple fibers of different sizes on fatigue resistance, and moderate fiber sizes show the best fatigue resistance. The surface modification treatment of Examples 13-15 significantly prolongs the fatigue life, and the annealing treatment of Examples 16-18 also significantly enhances the fatigue resistance. Example 19 exhibits the longest fatigue life through the dual optimization of surface modification and annealing treatment.

[0111] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a semi-steel anti-skid low rolling resistance tire, characterized in that: The steps include: Preparation of core-shell foaming material: liquid styrene-butadiene rubber, nylon staple fiber, carbon black, vulcanizer, accelerator, plasticizer and diluent are mixed uniformly in a mass ratio of 100: (8-12): (35-45): (2-3): (1-1.5): (8-12): (10-50) to obtain a coating liquid, and the coating liquid is rolled onto the surface of foaming particles and dried to obtain a core-shell foaming material, wherein the nylon staple fiber is subjected to surface modification treatment, and the surface modification treatment method comprises: immersing the nylon fiber in a 1-5wt% hydroxysilane aqueous solution, immersing for 1-3h and then drying, and then immersing in a solution containing 1-5wt% glycolic acid for 1-3h, washing and drying to obtain the surface-modified nylon staple fiber; Preparation of porous rubber layer: Styrene-butadiene rubber, natural rubber, carbon black, vulcanizing agent, accelerator and plasticizer are mixed in an internal mixer at 55-65°C for 10-20 minutes to obtain a rubber layer substrate, the core-shell foaming material and the rubber layer substrate are mixed in a mass ratio of 1:(4-9) and kneaded at 50-60°C for 10-20 minutes, molded at 110°C-130°C for 20-30 minutes into a thin sheet, and pre-vulcanized at 145-155°C for 20-40 minutes to obtain a porous rubber layer, the mass ratio of styrene-butadiene rubber, natural rubber, carbon black, vulcanizing agent, accelerator and plasticizer is 70:30:(45-55):(1-3):(0.5-1.5):(5-10); Preparation of semi-steel anti-skid low rolling resistance tire: laminate the porous rubber layer and the tread part of the semi-steel tire, perform final vulcanization at 165-175°C for 40-50 minutes, and then form the tire.

2. The method for preparing a semi-steel anti-wet skid low rolling resistance tire according to claim 1, characterized in that: The average diameter of nylon staple fibers is 10-20 μm and the average length is 100-200 μm.

3. The method for preparing a semi-steel anti-wet skid low rolling resistance tire according to claim 1, characterized in that: The nylon staple fibers are subjected to annealing treatment, wherein the annealing method comprises subjecting the nylon staple fibers to flame burning treatment at 100-140° C., and the burning treatment time is 0.5-1.5 seconds.

4. The method for preparing a semi-steel anti-wet skid low rolling resistance tire according to claim 1, characterized in that: The method of rolling the coating liquid onto the surface of the foamed particles includes: placing the foamed particles in a drum, maintaining the drum speed at 20-40rpm at 60-80°C, spraying the coating liquid onto the surface of the foamed particles, and after spraying, keeping the drum rotating and keeping warm and drying for 1-2 hours to obtain a core-shell type foamed material.

5. The method for preparing a semi-steel anti-wet skid low rolling resistance tire according to claim 1, characterized in that: The particle size of the foamed particles is 0.1-0.5 mm.

6. The method for preparing a semi-steel wet-slip resistant low rolling resistance tire according to claim 1, characterized in that: The mass ratio of the coating liquid to the foamed particles is 1:(1.5-4).