Precipitation-resistant, yellowing-resistant, low-odor and high-concentration weather-resistant master batch and preparation method thereof

Through the Lewis acid-base reaction of low-melting point hindered amine light stabilizer and UV light stabilizer to form a complex, combined with copolymerized polypropylene carrier resin and processing aids, the precipitation and yellowing of high-content, low-melting point weather-resistant masterbatch are solved. and high odor problems, a high-concentration weather-resistant masterbatch that is resistant to precipitation, yellowing, and low odor has been achieved, reducing production costs and improving product performance.

CN118772541APending Publication Date: 2024-10-15SUQIAN LIANHONG NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411100512.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing high-content, low-melting-point weather-resistant masterbatches have problems with precipitation, yellowing, and high odor during processing and use. Moreover, existing solutions increase production costs and process complexity, making it difficult to improve precipitation and yellowing resistance at the same time. and low odor.

Method used

Copolymerized polypropylene is used as the carrier resin, and the low melting point hindered amine light stabilizer HALS 3853 and the ultraviolet light stabilizer UVA 2908 generated by the reaction at 80~100°C form a complex through Lewis acid-base reaction, combined with processing aids such as N,N-bis(n-octadecane)hydroxylamine, etc., improve the compatibility and dispersion of additives to form high-concentration weather-resistant masterbatch that is resistant to precipitation, anti-yellowing, and low odor.

Benefits of technology

It effectively solves the problem of additive precipitation and yellowing, improves the thermal stability and weather resistance of the product, reduces production costs, and does not cause precipitation, caking and discoloration during summer transportation. It is suitable for traditional and underwater granulation processes. Improved throughput and product performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772541A_ABST
    Figure CN118772541A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of material processing and auxiliary agent compounding, and particularly relates to a precipitation-resistant, yellowing-resistant, low-odor and high-concentration weather-resistant master batch and a preparation method thereof. The weather-resistant master batch comprises the following components in percentage by mass: 25-50% of carrier resin polypropylene, 25-52% of a low-melting-point hindered amine light stabilizer, 10-30% of a low-melting-point ultraviolet light stabilizer and 0.5-2% of a processing aid; according to the invention, HALS 3853 and UVA 2908 are fully stirred and uniformly mixed at the temperature of 80-100 DEG C, so that the activity, thermal stability and yellowing resistance of the auxiliary agent are improved, and the problems of precipitation of the auxiliary agent and odor caused by volatilization of a small molecular auxiliary agent are effectively solved; by adopting the conventional processing equipment, the problems of precipitation, caking, difficult transportation and the like of the master batch can be solved, the productivity of the product is greatly improved, and meanwhile, the synergistic reaction among the main auxiliary components is increased at the effective reaction temperature, so that the production cost is saved, and the performance index of the product is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material processing and additive compounding, and specifically relates to a precipitation-resistant, yellowing-resistant, low-odor, high-concentration weather-resistant masterbatch and a preparation method thereof. Background Art

[0002] Polymer materials have ushered in rapid development due to their excellent performance. They have been widely used in construction, automobiles, home appliances, agriculture and other fields. With the development and progress of science and technology, people have put forward higher requirements for materials, which are mainly reflected in the need to achieve specific performance and have a long service life. Adding weathering additives is currently recognized as the most simple and efficient weathering modification solution, but most additives including antioxidants, light stabilizers, etc. will affect the mechanical properties of products when applied to plastic products. At the same time, there are also problems such as difficult dispersion, difficult processing, and large amount of dust. Functional masterbatch additives have the advantages of simplicity, safety, hygiene, and pollution-free production and processing of materials, but weathering additives are organic low molecular weight compounds, most of which have low melting points. With the increase of the amount of additives and the difference in polarity between them and the carrier resin, the additives will precipitate in large quantities, causing problems such as processing, transportation, and storage. In addition, due to the precipitation of low melting point additives, the masterbatch will become sticky or agglomerated, which is not conducive to the use of downstream customers. However, there are relatively few existing studies in China, and the processing and use problems of such masterbatches cannot be fundamentally solved.

[0003] In order to solve the precipitation problem of low-melting-point weather-resistant masterbatch during processing, the improvement is mainly from the perspective of formulation and equipment. The Chinese patent CN105218856A adopts a multi-stage TEM structure and an ultrasonic variable amplitude twin-screw extruder. From the results, it can not effectively solve the problem of additive precipitation, and the method has low production efficiency and increases production costs. Patent CN110041616A discloses an anti-precipitation light stabilizer 3853 masterbatch, which increases the carrying capacity of the carrier resin for low-melting-point additives by adding adsorbents and foaming. However, the addition of other components will affect the weather resistance of the masterbatch itself, and the chemical foaming process itself is unstable and the adsorption capacity is limited, resulting in unstable products and increased production costs. As one of the earliest companies to conduct research in this field, American Cytec Corporation's products UV-3853PP5 and UV-3808PP5 use a microencapsulation technology to improve the precipitation of low-melting-point weathering additives. A protective film is formed on the surface of the masterbatch, forming a core-shell structure to improve the product's resistance to precipitation. However, this production method has high requirements on equipment, high production costs, and difficult process control.

[0004] The above-mentioned patents for this type of products involve optimizing the weather resistance and precipitation resistance of the products, but there is almost no mention of the yellowing resistance and low odor of the products themselves. This type of weather-resistant products are mainly used in modification fields such as automotive interior and exterior decoration and small household appliances, and have extremely high requirements for the precipitation resistance, low odor, and color stain resistance of the masterbatch. Therefore, in view of the shortcomings of the existing technology, the applicant believes that it is urgent to develop a precipitation-resistant, anti-yellowing, low-odor, high-concentration weather-resistant masterbatch that can be stably produced at low cost without introducing other components and using existing equipment. Summary of the invention

[0005] In order to solve the deficiencies in the above-mentioned production and use of high-content, low-melting-point weather-resistant masterbatch technology, the present invention discloses a high-concentration weather-resistant masterbatch that is resistant to precipitation, yellowing, and low in odor, and a method for manufacturing the same.

[0006] To achieve the above object, the technical solution of the present invention is as follows: The invention provides a precipitation-resistant, yellowing-resistant, low-odor and high-concentration weather-resistant masterbatch, which comprises, by mass percentage, 25-50% of carrier resin polypropylene, 25-52% of a low-melting-point hindered amine light stabilizer, 10-30% of a low-melting-point ultraviolet light stabilizer, and 0.5-2% of a processing aid.

[0007] Furthermore, the carrier resin is a copolymer polypropylene with a melt index of 15 g / 10min to 25 g / 10min, which can effectively increase the compatibility between the additive and the carrier resin, improve the precipitation of the masterbatch, and increase the melt strength of the masterbatch.

[0008] Furthermore, the low melting point hindered amine light stabilizer is HALS 3853.

[0009] Furthermore, the low melting point ultraviolet light stabilizer is UVA 2908.

[0010] The low melting point hindered amine light stabilizer HALS3853 and the ultraviolet absorber UVA 2908 can react at 80~100℃ to generate a complex structure with better thermal stability and larger molecular weight, which effectively solves the precipitation and yellowing of additives.

[0011] Furthermore, the processing aid is one or more of N,N-bis(n-octadecyl)hydroxylamine (FS 042), triphenyl phosphate, distearate, zinc stearate and vinyl bisstearamide (EBS), which can protect the additive and play an internal lubricating role to enhance the dispersion effect of the additive.

[0012] The present invention also provides a method for preparing the above-mentioned precipitation-resistant, yellowing-resistant, low-odor, high-concentration weather-resistant masterbatch, comprising the following steps: (1) The carrier resin polypropylene and the processing aid are weighed according to the above mass percentages and added into a high-speed mixer. The speed of the high-speed mixer is adjusted to 1000-1800 rpm at room temperature and mixed at high speed for 3-5 minutes to obtain a premix 1.

[0013] (2) The two materials, the low melting point hindered amine light stabilizer and the low melting point ultraviolet light stabilizer, are weighed according to the mass percentage, placed in a heated stirring kettle provided with a liquid pump, and stirred thoroughly at 80-100° C. to obtain premix 2.

[0014] (3) The uniformly mixed premix 1 is then injected into a twin-screw extruder with a length-to-diameter ratio of 64:1 from a main feed port through a loss-in-weight scale, and the premix 2 is injected into the twin-screw extruder through a liquid pump and extruded through the twin-screw extruder at 180-220° C. After water-cooling and pelletizing, the premix enters a negative pressure homogenization tank for drying and homogenization to obtain the precipitation-resistant, anti-yellowing, low-odor, high-concentration weather-resistant masterbatch.

[0015] Copolymer polypropylene is used as a carrier. Due to the introduction of other monomers, there is a certain degree of heterogeneity in its molecular chain structure, which makes the copolymer polypropylene have better compatibility at the molecular level and can more effectively carry and disperse organic low-molecular additives. In addition, since the copolymer polypropylene has a low crystallization temperature and high molecular chain mobility, it is also conducive to the diffusion and dispersion of the additives, thereby reducing the precipitation of the additives. The technology disclosed in the existing patents mentions the addition of polyethylene wax, polypropylene wax, and styrene-ethylene-butylene-styrene (SEBS) to this type of masterbatch to achieve similar effects as the present invention, but the addition of other components increases the instability of product performance and the increase of additional costs. In addition, the technical solution of the present invention proposes to first fully stir and mix HALS 3853 and UVA 2908 at 80-100° C., so that the two main auxiliary components form a long-chain or branched structure complex through a Lewis acid-base reaction, and at the same time increase the reaction rate of the active ingredient 2,2,6,6-tetramethylpiperidinyloxy free radical (TEMPO) in the hindered amine light stabilizer with the peroxy free radical, which not only improves the activity, thermal stability and yellowing resistance of the auxiliary, but also effectively solves the problem of auxiliary precipitation and odor caused by the volatilization of small molecule auxiliary.

[0016] The beneficial effects of the present invention are: (1) The carrier resin used in this technology is copolymer polypropylene with a melt index of 15g / 10min~25g / 10min, which can increase the compatibility of the additives with the carrier resin. The effective additive content can reach more than 50%, and there will be no problems such as exhaust port spraying, difficulty in forming strips at the die mouth, and inability to cut pellets during the processing process, which facilitates high-capacity and stable production of the product.

[0017] (2) The technical solution of the present invention is to firstly stir and mix HALS 3853 and UVA 2908 at 80-100°C, so that the two main auxiliary components form a long-chain or branched structure complex through Lewis acid-base reaction, and at the same time increase the reaction rate of the active ingredient TEMPO in the hindered amine light stabilizer with peroxyl radicals, which not only improves the activity, thermal stability and yellowing resistance of the auxiliary, but also effectively solves the problem of auxiliary precipitation and odor caused by the volatilization of small molecule auxiliary.

[0018] (3) The use of copolymerized polypropylene and very conventional processing equipment can solve the problems of precipitation, agglomeration and transportation difficulties existing in this type of masterbatch. Compared with adding low-molecular wax and SEBS or even special equipment processing, it greatly improves production capacity. At the same time, it increases the synergistic reaction between the main auxiliary ingredients at the effective reaction temperature, saving production costs while effectively improving product performance indicators.

[0019] (4) The masterbatch prepared by this technical solution can fundamentally solve the technical defects of this type of product that previously existed. Even after long-term sea transportation in summer, there will be no precipitation, agglomeration or discoloration, and there is no need to use high-cost cold chain transportation.

[0020] (5) The masterbatch preparation scheme of this scheme is suitable for the traditional water-drawing process to prepare cylindrical particles, and is also suitable for the underwater granulation process to prepare spherical particles. The production process is stable and the production capacity is greatly improved, which can reach 2t / h~3t / h. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Appearance of the masterbatches prepared in Examples 1 and 4 and two competitive masterbatches on the market; (a) Competitive product 1 (imported); (b) Competitive product 2 (domestic); (c) Masterbatch 1; (d) Masterbatch 4; Figure 2 This is a diagram of comparative example 1 in which the masterbatch processing is not carried out according to the present technology, resulting in material overflow and entanglement with the cutting knife during the production process. DETAILED DESCRIPTION

[0022] The present invention will be further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the following specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Example 1

[0023] A high concentration weather-resistant masterbatch with high precipitation resistance, yellowing resistance, low odor, and the raw material ratio is as follows: Copolymer polypropylene 38.5wt%; HALS 3853 30wt%; UVA 2908 30wt%; FS 042 0.5wt%; EBS 1wt%.

[0024] A method for preparing the above-mentioned precipitation-resistant, yellowing-resistant, low-odor, high-concentration weather-resistant masterbatch comprises the following steps: (1) First, HALS 3853 and UVA 2908 were weighed according to the mass ratio and placed in a high-temperature stirring kettle equipped with an 80°C liquid pump, and stirred for 15 minutes to allow them to fully react, thereby obtaining premix 1.

[0025] (2) The copolymerized polypropylene particles, FS 042 and EBS were weighed according to the mass ratio and placed in a high-speed mixer. The speed was adjusted to 1200 rpm / min and mixed at high speed for 5 minutes so that FS 042 and EBS could fully infiltrate and coat the resin surface to obtain premix 2.

[0026] (3) The uniformly mixed premix 2 is then injected into a twin-screw extruder with a length-to-diameter ratio of 64:1 from the main feeding port through a loss-in-weight scale, and the premix 1 is injected into the twin-screw extruder through a liquid pump. The extruder feeding section temperature is 60°C, the mixing section temperature is 220-240°C, the meshing section temperature is 230°C, the conveying section temperature is 180°C, and the die section temperature is 165°C for extrusion. After water cooling and pelletizing, the premix 2 is fed into a negative pressure homogenizing tank for drying and homogenization to obtain the precipitation-resistant, anti-yellowing, low-odor, high-concentration weather-resistant masterbatch 1. Example 2

[0027] A high concentration weather-resistant masterbatch with high precipitation resistance, yellowing resistance, low odor, and the raw material ratio is as follows: Copolymer polypropylene 43.5wt%; HALS 3853 30wt%; UVA 2908 25wt%; FS 042 0.5wt%; EBS 1wt%.

[0028] A method for preparing the above-mentioned precipitation-resistant, yellowing-resistant, low-odor, high-concentration weather-resistant masterbatch comprises the following steps: (1) First, HALS 3853 and UVA 2908 were weighed according to the mass ratio and placed in a high-temperature stirring kettle equipped with an 80°C liquid pump, and stirred for 15 minutes to allow them to fully react, thereby obtaining premix 1.

[0029] (2) The copolymerized polypropylene particles, FS 042 and EBS were weighed according to the mass ratio and placed in a high-speed mixer. The speed was adjusted to 1200 rpm / min and mixed at high speed for 5 minutes so that FS 042 and EBS could fully infiltrate and coat the resin surface to obtain premix 2.

[0030] (3) The uniformly mixed premix 2 is then injected into a twin-screw extruder with a length-to-diameter ratio of 64:1 from the main feeding port through a loss-in-weight scale, and the premix 1 is injected into the twin-screw extruder through a liquid pump. The extruder feeding section temperature is 60°C, the mixing section temperature is 220-240°C, the meshing section temperature is 230°C, the conveying section temperature is 180°C, and the die section temperature is 165°C for extrusion. After water cooling and pelletizing, the premix 2 is dried and homogenized in a negative pressure homogenizing tank to obtain the precipitation-resistant, anti-yellowing, low-odor, high-concentration weather-resistant masterbatch 2. Example 3

[0031] A high concentration weather-resistant masterbatch with high precipitation resistance, yellowing resistance, low odor, and the raw material ratio is as follows: Copolymer polypropylene 43.5wt%; HALS 3853 35wt%; UVA 2908 20wt%; FS 042 0.5wt%; EBS 1wt%.

[0032] A method for preparing the above-mentioned precipitation-resistant, yellowing-resistant, low-odor, high-concentration weather-resistant masterbatch comprises the following steps: (1) First, HALS 3853 and UVA 2908 were weighed according to the mass ratio and placed in a high-temperature stirring kettle equipped with an 80°C liquid pump, and stirred for 15 minutes to allow them to fully react, thereby obtaining premix 1.

[0033] (2) The copolymerized polypropylene particles, FS 042 and EBS were weighed according to the mass ratio and placed in a high-speed mixer. The speed was adjusted to 1200 rpm / min and mixed at high speed for 5 minutes so that FS 042 and EBS could fully infiltrate and coat the resin surface to obtain premix 2.

[0034] (3) The uniformly mixed premix 2 is then injected into a twin-screw extruder with a length-to-diameter ratio of 64:1 from the main feeding port through a loss-in-weight scale, and the premix 1 is injected into the twin-screw extruder through a liquid pump. The extruder feeding section temperature is 60°C, the mixing section temperature is 220-240°C, the meshing section temperature is 230°C, the conveying section temperature is 180°C, and the die section temperature is 165°C for extrusion. After water cooling and pelletizing, the premix 2 is fed into a negative pressure homogenizing tank for drying and homogenization to obtain the precipitation-resistant, anti-yellowing, low-odor, high-concentration weather-resistant masterbatch 3. Example 4

[0035] A high concentration weather-resistant masterbatch with high precipitation resistance, yellowing resistance, low odor, and the raw material ratio is as follows: Copolymer polypropylene 38.5wt% HALS 3853 30wt% UVA 2908 30wt% FS 042 0.5wt% EBS 1wt% A method for preparing the above-mentioned precipitation-resistant, yellowing-resistant, low-odor, high-concentration weather-resistant masterbatch comprises the following steps: (1) First, HALS 3853 and UVA 2908 were weighed according to the mass ratio and placed in a high-temperature stirring kettle equipped with an 80°C liquid pump and stirred for 15 minutes to allow them to fully react, thereby obtaining premix 1.

[0036] (2) The copolymerized polypropylene particles, FS 042 and EBS were weighed according to the mass ratio and placed in a high-speed mixer. The speed was adjusted to 1200 rpm / min and mixed at high speed for 5 minutes so that FS 042 and EBS could fully infiltrate and coat the resin surface to obtain premix 2.

[0037] (3) The uniformly mixed premix 2 is then injected into a twin-screw extruder with a length-to-diameter ratio of 64:1 from the main feeding port through a loss-in-weight scale, and the premix 1 is injected into the twin-screw extruder through a liquid pump. The extruder feeding section temperature is 60°C, the mixing section temperature is 220-240°C, the meshing section temperature is 230°C, the conveying section temperature is 180°C, and the die section temperature is 165°C for extrusion. After water ring cooling, the premix 2 is fed into a negative pressure homogenizing tank for drying and homogenization to obtain the precipitation-resistant, anti-yellowing, low-odor, high-concentration weather-resistant masterbatch 4. Example 5

[0038] A high concentration weather-resistant masterbatch with high precipitation resistance, yellowing resistance, low odor, and the raw material ratio is as follows: Copolymer polypropylene 43.5wt% HALS 3853 30wt% UVA 2908 25wt% FS 042 0.5wt% EBS 1wt% A method for preparing the above-mentioned precipitation-resistant, yellowing-resistant, low-odor, high-concentration weather-resistant masterbatch comprises the following steps: (1) First, HALS 3853 and UVA 2908 were weighed according to the mass ratio and placed in a high-temperature stirring kettle equipped with an 80°C liquid pump and stirred for 15 minutes to allow them to fully react, thereby obtaining premix 1.

[0039] (2) The copolymerized polypropylene particles, FS 042 and EBS were weighed according to the mass ratio and placed in a high-speed mixer. The speed was adjusted to 1200 rpm / min and mixed at high speed for 5 minutes so that FS 042 and EBS could fully infiltrate and coat the resin surface to obtain premix 2.

[0040] (3) The uniformly mixed premix 2 is then injected into a twin-screw extruder with a length-to-diameter ratio of 64:1 from the main feeding port through a loss-in-weight scale, and the premix 1 is injected into the twin-screw extruder through a liquid pump. The extruder feeding section temperature is 60°C, the mixing section temperature is 220-240°C, the meshing section temperature is 230°C, the conveying section temperature is 180°C, and the die section temperature is 165°C for extrusion. After water ring cooling, the premix 2 is fed into a negative pressure homogenizing tank for drying and homogenization to obtain the precipitation-resistant, yellowing-resistant, low-odor, high-concentration weather-resistant masterbatch 5. Example 6

[0041] A high concentration weather-resistant masterbatch with high precipitation resistance, yellowing resistance, low odor, and the raw material ratio is as follows: Copolymer polypropylene 43.5wt% HALS 3853 35wt% UVA 2908 20wt% FS 042 0.5wt% EBS 1wt% A method for preparing the above-mentioned precipitation-resistant, yellowing-resistant, low-odor, high-concentration weather-resistant masterbatch comprises the following steps: (1) First, HALS 3853 and UVA 2908 were weighed according to the mass ratio and placed in a high-temperature stirring kettle equipped with an 80°C liquid pump, and stirred for 15 minutes to allow them to fully react, thereby obtaining premix 1.

[0042] (2) The copolymerized polypropylene particles, FS 042 and EBS were weighed according to the mass ratio and placed in a high-speed mixer. The speed was adjusted to 1200 rpm / min and mixed at high speed for 5 minutes so that FS 042 and EBS could fully infiltrate and coat the resin surface to obtain premix 2.

[0043] (3) The uniformly mixed premix 2 is then injected into a twin-screw extruder with a length-to-diameter ratio of 64:1 from the main feeding port through a loss-in-weight scale, and the premix 1 is injected into the twin-screw extruder through a liquid pump. The extruder feeding section temperature is 60°C, the mixing section temperature is 220-240°C, the meshing section temperature is 230°C, the conveying section temperature is 180°C, and the die section temperature is 165°C for extrusion. After water ring cooling, the premix 2 is fed into a negative pressure homogenizing tank for drying and homogenization to obtain the precipitation-resistant, anti-yellowing, low-odor, high-concentration weather-resistant masterbatch 6.

[0044] Performance testing: The appearance of the masterbatches prepared in Examples 1 and 4 and two competitive masterbatches on the market are as follows Figure 1As shown. From the figure, the appearance of the imported masterbatch competitor 1 is similar to that of the masterbatch 1 prepared in Example 1. Both are water-drawn processes. The surface gloss and melt strength of the masterbatch are higher than those of the competitor 1. There is powder aggregation at the cut of the competitor 1, indicating precipitation, while the masterbatch 1 does not have this phenomenon, indicating that the masterbatch 1 is superior to the competitor 1 in appearance and precipitation. The present Example 4 adopts water ring cutting, and the appearance of the particles obtained by underwater granulation is consistent with the appearance of domestically available masterbatches, and the particles of the masterbatch 4 are uniform in size, the surface is glossy, and the particles are full and round, while the particles of the competitor 2 are of different sizes, and the shape is more like an ellipse, the shape is shriveled, and there is auxiliary powder precipitated on the surface. Therefore, the masterbatch 4 prepared by Example 4 of the present technology is superior to the competitor 2 in shape, appearance and precipitation.

[0045] a. Test of precipitation resistance and discoloration resistance 10 g of competitive masterbatch and homemade masterbatch were weighed respectively, placed in a wide-mouth glass bottle, heated at 80°C for 2 h, and then left to stand at room temperature for 2 h. The test results are shown in Table 2.

[0046] b. Odor detection 10 g of the sample was placed in a transparent glass cup, sealed, and heated at 80°C for 2 h. Five testers evaluated the odor. The test results are shown in Table 2.

[0047] The odor detection standards are shown in Table 1 below: Table 1 Odor detection standards

[0048] c. Weather resistance test 0.5% of the competitive masterbatch and the homemade masterbatch were added to the polypropylene granules respectively, and the standard color plates and standard tensile specimens were injection molded and placed in a xenon lamp accelerated aging box for aging experiments. The xenon lamp aging box adopts the PV3930 standard. After aging, a desktop colorimeter was used to test the color difference and a universal tensile machine was used for testing. The test results are shown in Table 2.

[0049] Table 2 Summary of test results of the above competitive products and embodiment masterbatch

[0050] The masterbatch containing the present invention has a more uniform appearance than the competitive product, and has higher surface gloss and melt strength. By comparing the test results of precipitation, odor and weather resistance, it is found that the performance of the masterbatch prepared by this technology is better than that of the competitive product masterbatch, and after aging with a xenon lamp for 2000 hours, the color difference value at the same amount of additives is much smaller than the color plate with the competitive product added, and the mechanical property retention rate is higher than that of the imported masterbatch, while the domestic competitive product is only 78%, which is far lower than the performance of the masterbatch prepared by this technology, indicating that the masterbatch prepared by this technology not only has low odor, precipitation resistance and anti-yellowing performance, but also shows excellent weather resistance, and will not precipitate, agglomerate and yellow during use and storage and transportation, greatly reducing the customer's use cost. Comparative Example 1

[0051] A high concentration weather-resistant masterbatch with high precipitation resistance, yellowing resistance, low odor, and the raw material ratio is as follows: Copolymer polypropylene 48.5wt%; HALS 3853 25wt%; UVA 2908 25wt%; FS 042 0.5wt%; EBS 1wt%.

[0052] A method for preparing the above-mentioned precipitation-resistant, yellowing-resistant, low-odor, high-concentration weather-resistant masterbatch comprises the following steps: (1) First, the pre-melted liquid HALS 3853 is weighed according to the mass ratio and placed in an 80°C liquid pump oil hot kettle. After the twin-screw extruder is started, the liquid pump is turned on for liquid injection.

[0053] (2) Copolymer polypropylene particles with a melt index of 5 g / 10 min, UVA 2908, FS 042 and EBS were weighed according to the mass ratio and placed in a high-speed mixer. The speed was adjusted to 1200 rpm / min and mixed at high speed for 5 min so that FS 042 and EBS could fully infiltrate and coat the resin surface to obtain a uniformly mixed premix 1.

[0054] (3) The uniformly mixed premix 1 is then injected into a twin-screw extruder with a length-to-diameter ratio of 64:1 from the main feeding port through a loss-in-weight scale. Liquid HALS 3853 is injected into the twin-screw extruder through a liquid pump. The extruder feeding section temperature is 60°C, the mixing section temperature is 220-240°C, the meshing section temperature is 230°C, the conveying section temperature is 180°C, and the die section temperature is 165°C for extrusion. After water cooling and pelletizing, the premix enters a negative pressure homogenizing tank for drying and homogenization to obtain a high-concentration weather-resistant masterbatch that is resistant to precipitation, yellowing, and low in odor.

[0055] The carrier resin used in the comparative example is 5g / 10min, and HALS 3853 and UVA2908 are not fully stirred and mixed at 80-100°C and reacted according to the technical solution. In addition, compared with the examples, the content of additives in the masterbatch of comparative example 1 is lower than that of the examples, and the processing difficulty is theoretically lower than that of the examples. However, the production process is not carried out according to the technical solution, and there are material overflow and knife entanglement. The masterbatch prepared barely has uneven particle size and dispersion. Figure 2 (a) is a diagram of material bubbling out of the vacuum port, and (b) is a diagram of material entangled with the cutting knife.

[0056] It should be noted that the above content only illustrates the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications all fall within the protection scope of the claims of the present invention.

Claims

1. A high concentration weather-resistant masterbatch with high precipitation resistance, yellowing resistance, low odor, It is characterized in that Calculated by mass percentage, the composition includes 25-50% of carrier resin polypropylene, 25-52% of low melting point hindered amine light stabilizer, 10-30% of low melting point ultraviolet light stabilizer, and 0.5-2% of processing aid.

2. The precipitation-resistant, yellowing-resistant, low-odor, high-concentration weather-resistant masterbatch according to claim 1, It is characterized in that The carrier resin polypropylene is a copolymer polypropylene with a melt index of 15 g / 10min to 25 g / 10min.

3. The precipitation-resistant, yellowing-resistant, low-odor, high-concentration weather-resistant masterbatch according to claim 1, It is characterized in that The low melting point hindered amine light stabilizer is HALS 3853.

4. The precipitation-resistant, yellowing-resistant, low-odor, high-concentration weather-resistant masterbatch according to claim 1, It is characterized in that The low melting point UV stabilizer is UVA 2908.

5. The precipitation-resistant, yellowing-resistant, low-odor, high-concentration weather-resistant masterbatch according to claim 1, It is characterized in that The processing aid is one or more of N,N-bis(n-octadecyl)hydroxylamine, triphenyl phosphate, bis(hexadecyl)sulfide, zinc stearate and vinyl bisstearamide.

6. A method for preparing the precipitation-resistant, yellowing-resistant, low-odor, high-concentration weather-resistant masterbatch according to any one of claims 1 to 5, It is characterized in that The following steps are involved: (1) Adding carrier resin polypropylene and processing aid into a high-speed mixer, adjusting the speed of the high-speed mixer to 1000-1800 rpm at room temperature, and mixing at high speed for 3-5 minutes to obtain premix 1; (2) placing the low melting point hindered amine light stabilizer and the low melting point ultraviolet light stabilizer in an oil-heated stirring kettle, and stirring them thoroughly at 80-100° C. to obtain premix 2; (3) The uniformly mixed premix 1 is injected into a twin-screw extruder with a length-to-diameter ratio of 64:1 from the main feed port through a loss-in-weight scale, and the premix 2 is injected into the twin-screw extruder through a liquid pump, and is extruded through the twin-screw extruder at 180-220° C. After water-cooling and pelletizing, it enters a negative pressure homogenization tank for drying and homogenization to obtain the precipitation-resistant, anti-yellowing, low-odor, high-concentration weather-resistant masterbatch.

7. The method for preparing a precipitation-resistant, yellowing-resistant, low-odor, high-concentration weather-resistant masterbatch according to claim 6, It is characterized in that In step (2), stir thoroughly at 80-100°C for 5-8 minutes.