A tensile-resistant base film for composite current collector and preparation method thereof
By preparing a composite material containing polyester resin, triazole biphenyl functional polymer, etc., and using twin-screw extrusion and biaxial stretching processes, the performance deficiency of the composite current collector base film was solved, and a high-performance tensile base film suitable for lithium batteries was achieved.
Patent Information
- Application Number
- CN202411280303.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-13
AI Technical Summary
Existing composite current collector base films have shortcomings in terms of mechanical properties, bonding strength with surface metal layers, resistance to electrolyte swelling, and heat aging resistance, making it difficult to meet the comprehensive performance requirements of lithium batteries.
A composite material composed of polyester resin, triazole biphenyl functional polymer, reinforcing agent, coupling agent, catalyst, compatibilizer, antioxidant, lubricant and environmentally friendly plasticizer is used to prepare a tensile-resistant base film through twin-screw extrusion and biaxial stretching film-forming process, forming an interpenetrating network structure to improve performance.
The prepared composite current collector tensile base film has good mechanical properties, strong bonding with the metal layer, resistance to electrolyte swelling and heat aging, and is suitable for continuous large-scale production, thus extending its service life.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of current collectors for lithium batteries, and in particular to an anti-stretching base film for a composite current collector and a preparation method thereof. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density and power density, high operating voltage, light weight, small size, long cycle life, high operating voltage, high energy density, good safety, and green environmental protection. They have broad application prospects in portable appliances, digital products, power tools, large energy storage, electric transportation power supply, electric vehicles, etc. As one of the key components of lithium-ion batteries, the performance of the current collector directly affects the coulombic efficiency, cycle stability and rate performance of lithium batteries. It can be seen that it is particularly important to develop a current collector with excellent comprehensive performance and performance stability.
[0003] At present, composite current collectors based on polymer membranes have received extensive attention and application in the field of new energy. Compared with traditional current collectors, composite current collectors based on polymer membranes have the characteristics of low cost, light weight, and good internal insulation. These characteristics enable the composite current collector to reduce the cost of the battery, improve the energy density and safety of the battery when used in the battery. In the composite current collector, the base film is the key to determining the quality of the composite current collector. The existing base films for composite current collectors have more or less technical defects such as insufficient mechanical properties, weak bonding with the surface metal layer, poor resistance to electrolyte swelling, and heat aging resistance that needs to be further improved.
[0004] In order to solve the above problems, the Chinese invention patent with the authorization announcement number CN115521586B discloses a high mechanical strength polymer film, its manufacturing method and application, the high mechanical strength polymer film includes 95% to 99% polyester and 1% to 5% additives by mass, the number average molecular weight of the polyester is 13000Da to 20000Da, and the number of polyester molecules with a molecular weight less than 5000Da accounts for 0.5% to 5% of the total number of polyester molecules, and the molecular weight distribution index of the polyester is 1.6 to 2.4. This application can improve the mechanical strength of the polymer film in the MD direction and reduce the film breakage rate by controlling the number average molecular weight, proportion and molecular weight distribution index of the polymer film raw material, and then use the polymer film as a support film to manufacture a high mechanical strength composite current collector, and promote the application of the composite current collector in the battery. However, the resistance to electrolyte swelling and heat aging of the polymer film still needs to be further improved.
[0005] It can be seen that the field still needs a tensile-resistant base film for a composite current collector with sufficient mechanical properties, firm bonding with the surface metal layer, good resistance to electrolyte swelling, and excellent heat-aging resistance, and its preparation method meets market demand, has high market value and application prospects, and is of great significance to promoting the development of the field of composite current collectors. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a tensile-resistant base film for a composite current collector having sufficient mechanical properties, firm bonding with a surface metal layer, good resistance to electrolyte swelling, and excellent heat aging resistance, and a preparation method thereof.
[0007] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a tensile-resistant base film for a composite current collector, comprising the following raw materials in parts by weight: 100 parts of polyester resin, 20-30 parts of triazolyl biphenyl functional polymer, 15-25 parts of reinforcing agent, 3-5 parts of coupling agent, 6-8 parts of 2,6-pyridinedicarbonyl chloride, 1-3 parts of catalyst A, 1-3 parts of compatibilizer, 1-1.5 parts of antioxidant, 0.8-1.2 parts of lubricant, and 5-8 parts of environmentally friendly plasticizer; the triazolyl biphenyl functional polymer includes structural units introduced by the following monomers: 3,5-diamino-1,2,4-triazole, dimethylbiphenyl diisocyanate, and N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine.
[0008] Preferably, the polyester resin is selected from PET resin with a brand name of PET CZ-333.
[0009] Preferably, the preparation method of the triazole-based biphenyl functional polymer comprises the following steps: adding 3,5-diamino-1,2,4-triazole, dimethylbiphenyl diisocyanate, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, and catalyst B to a high boiling point solvent, stirring and reacting at 68-86° C. in an inert gas atmosphere for 3-5 hours, then heating to 90-96° C. and continuing to stir and react for 7-12 hours, then precipitating in water, washing the precipitated polymer with ethanol for 3-6 times, and then removing the residual solvent by rotary evaporation to obtain a triazole-based biphenyl functional polymer.
[0010] Preferably, the molar ratio of the 3,5-diamino-1,2,4-triazole, dimethylbiphenyl diisocyanate, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, catalyst B, and high boiling point solvent is 0.7:1:0.3:(0.8-1.2):(10-15).
[0011] Preferably, the catalyst B is at least one of dibutyltin dilaurate and stannous octoate; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is any one of nitrogen, helium, neon and argon.
[0012] Preferably, the reinforcing agent is glass fiber; the glass fiber is alkali-free glass fiber with an average diameter of 3-6 μm and a length of 1-3 mm.
[0013] Preferably, the coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570.
[0014] Preferably, the catalyst A is a mixture of anhydrous aluminum chloride and anhydrous ferric chloride in a mass ratio of 1:(3-5).
[0015] Preferably, the compatibilizer is the compatibilizer CMG9801 provided by Jiayirong Polymer (Shanghai) Co., Ltd.; the antioxidant is at least one of antioxidant 1010, antioxidant 168, and antioxidant 1076.
[0016] Preferably, the lubricant is at least one of ethylene bisstearamide and butyl stearate.
[0017] Preferably, the environmentally friendly plasticizer is epoxidized soybean oil.
[0018] Another object of the present invention is to provide a method for preparing the anti-stretching base film for the composite current collector, comprising the following steps: mixing the raw materials in parts by weight, adding them to a high-speed mixer, mixing them at a speed of 900-1200r / min for 8-12min to obtain a mixture; adding the mixture to a twin-screw extruder for melt extrusion, the material staying in the extruder for 3-5 minutes, and then passing the extruded material through a biaxial stretching film-forming machine for film formation to obtain the anti-stretching base film for the composite current collector.
[0019] Preferably, the extrusion temperature of the twin-screw extruder is 230-260°C.
[0020] Preferably, the stretching temperature of the biaxial stretching film-forming machine is 115-120° C., the stretching rate is 115-85 mm / s, the heat setting temperature is 215-235° C., and the stretching ratio is 4:1.
[0021] Due to the application of the above technical solution, the present invention has the following beneficial effects:
[0022] (1) The method for preparing the anti-stretching base film for the composite current collector disclosed in the present invention can be realized by using conventional equipment and production lines, with low capital investment, low energy consumption, high preparation efficiency and finished product qualification rate, suitable for continuous large-scale production, and high promotion and application value.
[0023] (2) The anti-stretching base film for the composite current collector disclosed in the present invention comprises the following raw materials in parts by weight: 100 parts of polyester resin, 20-30 parts of triazolyl biphenyl functional polymer, 15-25 parts of reinforcing agent, 3-5 parts of coupling agent, 6-8 parts of 2,6-pyridinedicarbonyl chloride, 1-3 parts of catalyst A, 1-3 parts of compatibilizer, 1-1.5 parts of antioxidant, 0.8-1.2 parts of lubricant, and 5-8 parts of environmentally friendly plasticizer; through the mutual cooperation and joint action of the raw materials, the anti-stretching base film for the composite current collector has sufficient mechanical properties, is firmly bonded to the surface metal layer, has good resistance to electrolyte swelling, and has excellent heat aging resistance.
[0024] (3) The anti-stretching base film for the composite current collector disclosed in the present invention, the triazole-based biphenyl functional polymer includes structural units introduced from the following monomers: 3,5-diamino-1,2,4-triazole, dimethylbiphenyl diisocyanate, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine; the triazole, biphenyl, benzotriazole and polyurethane, urea structures introduced at the same time, under the multiple effects of electronic effect, steric effect and conjugation effect, make the prepared polymer more compatible with other components, and cooperate with other raw material components to effectively improve the product's anti-stretching properties, bonding strength with metals, resistance to electrolyte swelling and heat aging, thereby effectively extending its service life.
[0025] (4) In the anti-stretching base film for the composite current collector disclosed in the present invention, the acyl chloride group on 2,6-pyridinedicarbonyl chloride can undergo Friedel-Crafts reaction with other raw material components containing benzene rings to form an interpenetrating network structure, which effectively improves the comprehensive performance and performance stability of the base film. In addition, through this component, a pyridine structure is introduced. Under the multiple effects of electronic effect, steric effect and conjugation effect, the product is endowed with more excellent anti-stretching performance, higher bonding strength with metal, better resistance to electrolyte swelling and heat aging. DETAILED DESCRIPTION
[0026] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.
[0027] Embodiment 1, a tensile-resistant base film for a composite current collector, comprising the following raw materials in parts by weight: 100 parts of polyester resin, 20 parts of triazolyl biphenyl functional polymer, 15 parts of reinforcing agent, 3 parts of coupling agent, 6 parts of 2,6-pyridinedicarbonyl chloride, 1 part of catalyst A, 1 part of compatibilizer, 1 part of antioxidant, 0.8 part of lubricant, and 5 parts of environmentally friendly plasticizer; the triazolyl biphenyl functional polymer includes structural units introduced by the following monomers: 3,5-diamino-1,2,4-triazole, dimethylbiphenyl diisocyanate, and N-[(4-methyl-1H-benzotriazol-1-yl)methyl]diethanolamine.
[0028] The polyester resin is PET resin with the brand name PET CZ-333.
[0029] The preparation method of the triazole-based biphenyl functional polymer comprises the following steps: adding 3,5-diamino-1,2,4-triazole, dimethyl biphenyl diisocyanate, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine and catalyst B to a high boiling point solvent, stirring and reacting at 68° C. for 3 hours in an inert gas atmosphere, then heating to 90° C. and continuing stirring and reacting for 7 hours, then precipitating in water, washing the precipitated polymer with ethanol for 3 times, The residual solvent is then removed by rotary evaporation to obtain a triazole-based biphenyl functional polymer; the molar ratio of the 3,5-diamino-1,2,4-triazole, dimethyl biphenyl diisocyanate, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, catalyst B, and high boiling point solvent is 0.7:1:0.3:0.8:10; the catalyst B is dibutyltin dilaurate; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is nitrogen. The M of the obtained functional polymer is measured by GPC test. n =15337 g / mol, M W / M n =1.421; calculated by elemental analysis and weight change, the molar ratio of the structural units introduced by 3,5-diamino-1,2,4-triazole, dimethylbiphenyl diisocyanate, and N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine in the triazole-based biphenyl functional polymer is approximately 0.7:1:0.3, which is the same as the theoretical value.
[0030] The reinforcing agent is glass fiber; the glass fiber is alkali-free glass fiber with an average diameter of 3 μm and a length of 1 mm; the coupling agent is silane coupling agent KH550; the catalyst A is a mixture of anhydrous aluminum chloride and anhydrous ferric chloride in a mass ratio of 1:3; the compatibilizer is compatibilizer CMG9801 provided by Jiayrong Polymer (Shanghai) Co., Ltd.; the antioxidant is antioxidant 1010; the lubricant is ethylene bisstearamide; and the environmentally friendly plasticizer is epoxidized soybean oil.
[0031] A method for preparing a stretch-resistant base film for a composite current collector comprises the following steps: mixing the raw materials in parts by weight, adding them to a high-speed mixer, mixing at a speed of 900 r / min for 8 minutes to obtain a mixture; adding the mixture to a twin-screw extruder for melt extrusion, the material stays in the extruder for 3 minutes, and then forming the extruded material into a film through a biaxial stretching film-forming machine to obtain the stretch-resistant base film for a composite current collector; the extrusion temperature of the twin-screw extruder is 230°C; the stretching temperature of the biaxial stretching film-forming machine is 115°C, the stretching rate is 115 mm / s, the heat setting temperature is 215°C, and the stretching ratio is 4:1.
[0032] Embodiment 2, a tensile-resistant base film for a composite current collector, comprising the following raw materials in parts by weight: 100 parts of polyester resin, 23 parts of triazolyl biphenyl functional polymer, 17 parts of reinforcing agent, 3.5 parts of coupling agent, 6.5 parts of 2,6-pyridinedicarbonyl chloride, 1.5 parts of catalyst A, 1.5 parts of compatibilizer, 1.2 parts of antioxidant, 0.9 parts of lubricant, and 6 parts of environmentally friendly plasticizer; the triazolyl biphenyl functional polymer includes structural units introduced by the following monomers: 3,5-diamino-1,2,4-triazole, dimethylbiphenyl diisocyanate, and N-[(4-methyl-1H-benzotriazol-1-yl)methyl]diethanolamine.
[0033] The polyester resin is PET resin with the brand name PET CZ-333.
[0034] The preparation method of the triazole-based biphenyl functional polymer comprises the following steps: adding 3,5-diamino-1,2,4-triazole, dimethyl biphenyl diisocyanate, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine and catalyst B to a high boiling point solvent, stirring and reacting at 72°C for 3.5 hours in an inert gas atmosphere, then heating to 92°C and continuing stirring and reacting for 8 hours, then precipitating in water, and washing the precipitated polymer with ethanol. 4 times, and then rotary evaporation to remove the residual solvent to obtain a triazole-based biphenyl functional polymer; the molar ratio of the 3,5-diamino-1,2,4-triazole, dimethylbiphenyl diisocyanate, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, catalyst B, and high boiling point solvent is 0.7:1:0.3:0.9:11; the catalyst B is stannous octoate; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is helium.
[0035] The reinforcing agent is glass fiber; the glass fiber is alkali-free glass fiber with an average diameter of 4 μm and a length of 1.5 mm; the coupling agent is silane coupling agent KH560; the catalyst A is a mixture of anhydrous aluminum chloride and anhydrous ferric chloride in a mass ratio of 1:3.5; the compatibilizer is compatibilizer CMG9801 provided by Jiayrong Polymer (Shanghai) Co., Ltd.; the antioxidant is antioxidant 168; the lubricant is butyl stearate; and the environmentally friendly plasticizer is epoxidized soybean oil.
[0036] A method for preparing a stretch-resistant base film for a composite current collector comprises the following steps: mixing the raw materials in parts by weight, adding them to a high-speed mixer, mixing at a speed of 1000 r / min for 9 minutes to obtain a mixture; adding the mixture to a twin-screw extruder for melt extrusion, the material stays in the extruder for 3.5 minutes, and then forming the extruded material into a film through a biaxial stretching film-forming machine to obtain a stretch-resistant base film for a composite current collector; the extrusion temperature of the twin-screw extruder is 240°C; the stretching temperature of the biaxial stretching film-forming machine is 117°C, the stretching rate is 105 mm / s, the heat setting temperature is 220°C, and the stretching ratio is 4:1.
[0037] Embodiment 3, a tensile-resistant base film for a composite current collector, comprising the following raw materials in parts by weight: 100 parts of polyester resin, 25 parts of triazolyl biphenyl functional polymer, 20 parts of reinforcing agent, 4 parts of coupling agent, 7 parts of 2,6-pyridinedicarbonyl chloride, 2 parts of catalyst A, 2 parts of compatibilizer, 1.3 parts of antioxidant, 1 part of lubricant, and 6.5 parts of environmentally friendly plasticizer; the triazolyl biphenyl functional polymer includes structural units introduced by the following monomers: 3,5-diamino-1,2,4-triazole, dimethylbiphenyl diisocyanate, and N-[(4-methyl-1H-benzotriazol-1-yl)methyl]diethanolamine.
[0038] The polyester resin is PET resin with the brand name PET CZ-333.
[0039] The preparation method of the triazole biphenyl functional polymer comprises the following steps: adding 3,5-diamino-1,2,4-triazole, dimethyl biphenyl diisocyanate, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine and catalyst B to a high boiling point solvent, stirring and reacting at 78° C. for 4 hours in an inert gas atmosphere, then heating to 93° C. and continuing stirring and reacting for 9.5 hours, then precipitating in water, and washing the precipitated polymer with ethanol for 5 minutes. The method comprises the following steps: performing the reaction mixture into a prepolymer and carrying out the step of: performing the reaction mixture into a prepolymer and carrying out the step of rotary evaporation to remove the residual solvent, and obtaining a triazole-based biphenyl functional polymer; the molar ratio of the 3,5-diamino-1,2,4-triazole, dimethylbiphenyl diisocyanate, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, catalyst B, and high boiling point solvent is 0.7:1:0.3:1:13; the catalyst B is dibutyltin dilaurate; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is neon.
[0040] The reinforcing agent is glass fiber; the glass fiber is alkali-free glass fiber with an average diameter of 4.5 μm and a length of 2 mm; the coupling agent is silane coupling agent KH570; the catalyst A is a mixture of anhydrous aluminum chloride and anhydrous ferric chloride in a mass ratio of 1:4; the compatibilizer is compatibilizer CMG9801 provided by Jiayrong Polymer (Shanghai) Co., Ltd.; the antioxidant is antioxidant 1076; the lubricant is ethylene bisstearamide; and the environmentally friendly plasticizer is epoxidized soybean oil.
[0041] A method for preparing a stretch-resistant base film for a composite current collector comprises the following steps: mixing the raw materials in parts by weight, adding them to a high-speed mixer, mixing at a speed of 1050 r / min for 10 minutes, and discharging a mixture; adding the mixture to a twin-screw extruder for melt extrusion, the material stays in the extruder for 4 minutes, and then forming the extruded material into a film through a biaxial stretching film-forming machine to obtain a stretch-resistant base film for a composite current collector; the extrusion temperature of the twin-screw extruder is 245°C; the stretching temperature of the biaxial stretching film-forming machine is 118°C, the stretching rate is 95 mm / s, the heat setting temperature is 225°C, and the stretching ratio is 4:1.
[0042] Example 4, a tensile-resistant base film for a composite current collector, comprising the following raw materials in parts by weight: 100 parts of polyester resin, 28 parts of triazolyl biphenyl functional polymer, 23 parts of reinforcing agent, 4.5 parts of coupling agent, 7.5 parts of 2,6-pyridinedicarbonyl chloride, 2.5 parts of catalyst A, 2.5 parts of compatibilizer, 1.4 parts of antioxidant, 1.1 parts of lubricant, and 7.5 parts of environmentally friendly plasticizer; the triazolyl biphenyl functional polymer includes structural units introduced by the following monomers: 3,5-diamino-1,2,4-triazole, dimethylbiphenyl diisocyanate, and N-[(4-methyl-1H-benzotriazol-1-yl)methyl]diethanolamine.
[0043] The polyester resin is PET resin with the brand name PET CZ-333.
[0044] The preparation method of the triazole biphenyl functional polymer comprises the following steps: adding 3,5-diamino-1,2,4-triazole, dimethyl biphenyl diisocyanate, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine and catalyst B to a high boiling point solvent, stirring and reacting at 84°C for 4.5 hours in an inert gas atmosphere, then heating to 95°C and continuing stirring and reacting for 11 hours, then precipitating in water, washing the precipitated polymer with ethanol for 6 times, and then rotary evaporating to remove the residual solvent. agent to obtain a triazole-based biphenyl functional polymer; the molar ratio of the 3,5-diamino-1,2,4-triazole, dimethylbiphenyl diisocyanate, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, catalyst B, and high boiling point solvent is 0.7:1:0.3:1.1:14; the catalyst B is a mixture of dibutyltin dilaurate and stannous octoate in a mass ratio of 3:5; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is argon.
[0045] The reinforcing agent is glass fiber; the glass fiber is alkali-free glass fiber with an average diameter of 5.5 μm and a length of 2.5 mm; the coupling agent is a mixture of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570 in a mass ratio of 1:2:3; the catalyst A is a mixture of anhydrous aluminum chloride and anhydrous ferric chloride in a mass ratio of 1:4.5; the compatibilizer is the compatibilizer CMG9801 provided by Jiayrong Polymer (Shanghai) Co., Ltd.; the antioxidant is a mixture of antioxidant 1010, antioxidant 168, and antioxidant 1076 in a mass ratio of 1:4:2; the lubricant is a mixture of ethylene bis stearamide and butyl stearate in a mass ratio of 3:5; and the environmentally friendly plasticizer is epoxidized soybean oil.
[0046] A method for preparing a stretch-resistant base film for a composite current collector comprises the following steps: mixing the raw materials in parts by weight, adding them to a high-speed mixer, mixing at a speed of 1100 r / min for 11 minutes to obtain a mixture; adding the mixture to a twin-screw extruder for melt extrusion, the material staying in the extruder for 4.5 minutes, and then forming the extruded material into a film through a biaxial stretching film-forming machine to obtain a stretch-resistant base film for a composite current collector; the extrusion temperature of the twin-screw extruder is 255°C; the stretching temperature of the biaxial stretching film-forming machine is 119°C, the stretching rate is 90 mm / s, the heat setting temperature is 232°C, and the stretching ratio is 4:1.
[0047] Example 5, a tensile-resistant base film for a composite current collector, comprising the following raw materials in parts by weight: 100 parts of polyester resin, 30 parts of triazolyl biphenyl functional polymer, 25 parts of reinforcing agent, 5 parts of coupling agent, 8 parts of 2,6-pyridinedicarbonyl chloride, 3 parts of catalyst A, 3 parts of compatibilizer, 1.5 parts of antioxidant, 1.2 parts of lubricant, and 8 parts of environmentally friendly plasticizer; the triazolyl biphenyl functional polymer includes structural units introduced by the following monomers: 3,5-diamino-1,2,4-triazole, dimethylbiphenyl diisocyanate, and N-[(4-methyl-1H-benzotriazol-1-yl)methyl]diethanolamine.
[0048] The polyester resin is PET resin with the brand name PET CZ-333.
[0049] The preparation method of the triazole-based biphenyl functional polymer comprises the following steps: adding 3,5-diamino-1,2,4-triazole, dimethyl biphenyl diisocyanate, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine and catalyst B to a high boiling point solvent, stirring and reacting at 86° C. for 5 hours in an inert gas atmosphere, then heating to 96° C. and continuing stirring and reacting for 12 hours, then precipitating in water, washing the precipitated polymer with ethanol for 6 times, The residual solvent is then removed by rotary evaporation to obtain a triazole-based biphenyl functional polymer; the molar ratio of the 3,5-diamino-1,2,4-triazole, dimethylbiphenyl diisocyanate, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, catalyst B, and high boiling point solvent is 0.7:1:0.3:1.2:15; the catalyst B is dibutyltin dilaurate; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is nitrogen.
[0050] The reinforcing agent is glass fiber; the glass fiber is alkali-free glass fiber with an average diameter of 6 μm and a length of 3 mm; the coupling agent is silane coupling agent KH560; the catalyst A is a mixture of anhydrous aluminum chloride and anhydrous ferric chloride in a mass ratio of 1:5; the compatibilizer is compatibilizer CMG9801 provided by Jiayrong Polymer (Shanghai) Co., Ltd.; the antioxidant is antioxidant 1076; the lubricant is ethylene bisstearamide; and the environmentally friendly plasticizer is epoxidized soybean oil.
[0051] A method for preparing a stretch-resistant base film for a composite current collector comprises the following steps: mixing the raw materials in parts by weight, adding them to a high-speed mixer, mixing them at a speed of 1200 r / min for 12 minutes, and discharging the mixture; adding the mixture to a twin-screw extruder for melt extrusion, the material stays in the extruder for 5 minutes, and then forming the extruded material into a film through a biaxial stretching film-forming machine to obtain the stretch-resistant base film for the composite current collector; the extrusion temperature of the twin-screw extruder is 260°C; the stretching temperature of the biaxial stretching film-forming machine is 120°C, the stretching rate is 85 mm / s, the heat setting temperature is 235°C, and the stretching ratio is 4:1.
[0052] Comparative Example 1, a tensile-resistant base film for a composite current collector, is basically the same as Example 1, except that a polyester resin is used instead of the modified triazole biphenyl functional polymer; the polyester resin is a PET resin with a brand number of PET CZ-333.
[0053] Comparative Example 2, a tensile-resistant base film for a composite current collector, is substantially the same as Example 1, except that 2,6-pyridinedicarbonyl chloride is not added.
[0054] In order to further illustrate the beneficial technical effects of the anti-stretching base film for the composite current collector involved in each embodiment of the present invention, the anti-stretching base film for the composite current collector involved in Examples 1-5 and Comparative Examples 1-2 was subjected to relevant performance tests, and the film thickness of the test sample was controlled to be 6 microns; the test method is as follows:
[0055] (1) Tensile properties: Tensile strength test is carried out according to GB / T 1040.1-2018.
[0056] (2) Heat aging resistance: The tensile strength-resistant base film products for each composite current collector were placed in hot air at 85°C for artificial accelerated aging for 168 hours. After cooling to room temperature, the tensile strength was measured again. The heat aging resistance was measured by the retention rate of the tensile strength. The larger the value, the better the heat aging resistance.
[0057] (3) Electrolyte tolerance: The composite current collector prepared in each example was cut into samples of 20 cm × 20 cm using a tensile base film, and the circumference of the sample was recorded as C. 1Then, place it in an electrolyte at 65℃ for 48h, and record the circumference of the sample after immersion as C. 2 The swelling degree SD of the sample is calculated according to the following formula: SD = (C 2 -C 1 ) / C 1 × 100%, the electrolyte is a mixture of ethylene carbonate, diethyl carbonate and methyl ethyl carbonate in a mass ratio of 1:2:1; the smaller the swelling degree, the better the tolerance of the electrolyte.
[0058] (4) Adhesion between the base film and the metal conductive layer: The base films of each example were placed in a magnetron sputtering chamber, and aluminum metal with a purity of 99.99% was used as the target material and argon gas was used as the gas source. A 1200 nm thick aluminum metal layer was plated on both sides of the tensile-resistant base film in the thickness direction by magnetron sputtering in the magnetron sputtering chamber to obtain a composite current collector; a layer of Permacel P-94 double-sided tape was adhered to a 1 mm thick aluminum foil, and the composite current collector was adhered on the double-sided tape. A layer of ethylene acrylic acid copolymer film (DuPont Nurcel0903, thickness of 50 μm) was covered on the composite current collector, and then a 1.3×10 5 N / m 2 , hot pressing at 120°C for 10s, cooling to room temperature, and cutting into small strips of 150mm×15mm; finally, the ethylene acrylic acid copolymer film of the small sample strip is fixed on the upper fixture of the tensile machine, and the rest is fixed on the lower fixture. After fixation, the two are peeled off at an angle of 180° and a speed of 100mm / min to test the peeling force, which is the bonding force between the base film and the metal conductive layer.
[0059]
[0060] As can be seen from Table 1, the tensile-resistant base film for the composite current collector involved in each embodiment of the present invention has better mechanical properties, more excellent heat aging resistance, electrolyte swelling resistance and adhesion to the metal conductive layer than the comparative example products, and the combined use of triazolyl biphenyl functional polymer and 2,6-pyridinedicarbonyl chloride is beneficial to improving the above properties.
[0061] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. All equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A tensile-resistant base film for a composite current collector, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of polyester resin, 20-30 parts of triazolyl biphenyl functional polymer, 15-25 parts of reinforcing agent, 3-5 parts of coupling agent, 6-8 parts of 2,6-pyridinedicarbonyl chloride, 1-3 parts of catalyst A, 1-3 parts of compatibilizer, 1-1.5 parts of antioxidant, 0.8-1.2 parts of lubricant, and 5-8 parts of environmentally friendly plasticizer; the triazolyl biphenyl functional polymer comprises structural units introduced by the following monomers: 3,5-diamino-1,2,4-triazole, dimethyl biphenyl diisocyanate, and N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine; the catalyst A is a mixture of anhydrous aluminum chloride and anhydrous ferric chloride in a mass ratio of 1:(3-5); The preparation method of the triazole-based biphenyl functional polymer comprises the following steps: adding 3,5-diamino-1,2,4-triazole, dimethyl biphenyl diisocyanate, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine and catalyst B to a high boiling point solvent, stirring and reacting for 3-5 hours at 68-86° C. in an inert gas atmosphere, then heating to 90-96° C. and continuing stirring and reacting for 7-12 hours, then precipitating in water, washing the precipitated polymer with ethanol for 3-6 times, The residual solvent is then removed by rotary evaporation to obtain a triazole-based biphenyl functional polymer; the high boiling point solvent is dimethyl sulfoxide; the catalyst B is at least one of dibutyltin dilaurate and stannous octoate; the molar ratio of the 3,5-diamino-1,2,4-triazole, dimethylbiphenyl diisocyanate, N-[(4-methyl-1H-benzotriazole-1-yl)methyl]diethanolamine, catalyst B, and high boiling point solvent is 0.7:1:0.3:(0.8-1.2):(10-15).
2. The tensile-resistant base film for a composite current collector according to claim 1, characterized in that: The polyester resin is selected from PET resin with the brand name PET CZ-333.
3. The tensile-resistant base film for a composite current collector according to claim 1, characterized in that: The inert gas is any one of nitrogen, helium, neon and argon.
4. The tensile-resistant base film for a composite current collector according to claim 1, characterized in that: The reinforcing agent is glass fiber; the glass fiber is alkali-free glass fiber with an average diameter of 3-6 μm and a length of 1-3 mm; the coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560 and silane coupling agent KH570.
5. The tensile-resistant base film for a composite current collector according to claim 1, characterized in that: The compatibilizer is compatibilizer CMG9801; the antioxidant is at least one of antioxidant 1010, antioxidant 168, and antioxidant 1076.
6. The tensile-resistant base film for a composite current collector according to claim 1, characterized in that: The lubricant is at least one of ethylene bisstearamide and butyl stearate; and the environmentally friendly plasticizer is epoxidized soybean oil.
7. A method for preparing the tensile-resistant base film for the composite current collector according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: mixing the raw materials in parts by weight, adding the raw materials into a high-speed mixer, mixing the raw materials at a speed of 900-1200 r / min for 8-12 minutes, and discharging the raw materials to obtain a mixed material; adding the mixed material into a twin-screw extruder for melt extrusion, wherein the material stays in the extruder for 3-5 minutes, and then forming the extruded material into a film by a biaxial stretching film-forming machine, so as to obtain a tensile-resistant base film for a composite current collector.
8. The method for preparing the tensile-resistant base film for the composite current collector according to claim 7, characterized in that: The extrusion temperature of the twin-screw extruder is 230-260°C; the stretching temperature of the biaxial stretching film-forming machine is 115-120°C, the stretching rate is 115-85 mm / s, the heat setting temperature is 215-235°C, and the stretching ratio is 4:1.