Anticorrosive bio-based epoxy coating as well as preparation method and application thereof

Through the combination of a high proportion of bio-based epoxy resin, modified graphene oxide, and p-aminoazobenzene, the problem of poor anti-corrosion performance of existing epoxy coatings has been solved, and the bio-based epoxy coating has achieved good acid resistance, alkali resistance, Resistant to salt water and salt spray, it has excellent protective effects and realizes the green synthesis of epoxy coatings.

CN118772736APending Publication Date: 2024-10-15XIAMEN WELDTONE TECH CO LTD

Patent Information

Application Number
CN202411014847.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing epoxy coatings mainly use petroleum-based epoxy resins as raw materials, which have poor anti-corrosion properties. The depletion of petroleum resources and environmental pollution problems force the search for bio-based material alternatives, and the synthesis of bio-based epoxy resins needs to replace fossil raw materials to achieve environmental protection. Processing and production of coatings.

Method used

A high proportion of bio-based epoxy resin is used with modified graphene oxide, p-aminoazobenzene and other materials to prepare bio-based epoxy coatings through substitution reactions and esterification reactions to improve acid and alkali resistance, salt water resistance and salt spray resistance. performance, and improve the anti-corrosion performance of the coating through the synergistic effect of modified graphene oxide and p-aminoazobenzene.

Benefits of technology

It achieves good anti-corrosion properties of bio-based epoxy coatings, reduces potential harm to human health, and has excellent protective effects, especially in the marine environment. Compared with traditional petroleum-based epoxy coatings, it achieves the greenness of epoxy coatings synthesis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004965406610000091
    Figure BDA0004965406610000091
  • Figure BDA0004965406610000131
    Figure BDA0004965406610000131
Patent Text Reader

Abstract

The invention belongs to the field of epoxy coatings, and particularly relates to an anti-corrosion bio-based epoxy coating as well as a preparation method and application thereof. The bio-based anticorrosive paint comprises epoxy resin, a curing agent, modified graphene oxide, a solvent and optional auxiliaries, the epoxy resin at least comprises bio-based epoxy resin; the bio-based epoxy resin is obtained by carrying out substitution reaction on a phenolic hydroxyl group-containing bio-based ester compound and a halogenated epoxyalkane compound under the condition of an alkaline medium and then purifying; the curing agent at least comprises a first curing agent; the first curing agent is p-aminoazobenzene; the modified graphene oxide is obtained by modifying graphene oxide with dopamine hydrochloride. The bio-based epoxy coating provided by the invention has good corrosion resistance, namely good acid resistance, alkali resistance, brine resistance and salt spray resistance, and can achieve an excellent protection effect in an environment with corrosion resistance requirements, especially in a marine environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of epoxy coatings, and in particular relates to an anticorrosive bio-based epoxy coating and a preparation method and application thereof. Background Art

[0002] Since the 21st century, with the proposal and implementation of the "ocean power" strategy, my country has further expanded the development and utilization of marine resources. However, in the process of developing and building the ocean, various metal equipment and facilities are inevitably faced with corrosion problems from the marine environment.

[0003] Among the thermosetting polymers sold in the current global market, epoxy resin has always occupied a leading position in market share. Due to its excellent mechanical properties, processability and versatility, epoxy resin is widely used in coatings, composite materials, electronic equipment and thermosetting materials in the aerospace industry. Among them, epoxy coatings have been widely used as a physical barrier to protect metal substrates from corrosive environments. However, the epoxy coatings formed by existing epoxy coatings have poor anti-corrosion properties, and the synthesis of its main component, epoxy resin, often requires petrochemical products as raw materials. The increasingly depleted oil resources and increasingly severe environmental problems force people to seek green and renewable bio-based materials to replace fossil raw materials to achieve the processing and production of environmentally friendly coatings. Among them, bisphenol A diglycidyl ether (DGEBA) and its oligomers account for 90% of the global epoxy resin production, and bis(4-hydroxyphenylene)-2,2-propane, also known as bisphenol A (BPA), is required as a raw material to synthesize epoxy resin. However, BPA is a highly toxic petrochemical raw material. Due to its chemical structure similar to hormones, BPA is considered an endocrine disruptor and carcinogenic. It not only damages the environment but also poses potential risks to human health. Therefore, replacing fossil resources with biomass raw materials to synthesize bio-based epoxy coatings with good anti-corrosion properties is more in line with the needs of sustainable development. Summary of the invention

[0004] One of the purposes of the present invention is to solve the problem that epoxy coatings in the prior art are mostly made of petroleum-based epoxy resins and have poor anti-corrosion performance, and to provide a bio-based epoxy coating that contains a higher proportion of bio-based epoxy resins and has good anti-corrosion performance (acid and alkali resistance, salt water resistance, and salt spray resistance).

[0005] Specifically, the bio-based anti-corrosion coating includes 20 to 40 parts by weight of epoxy resin, 15 to 35 parts by weight of curing agent, 0.2 to 1 part by weight of modified graphene oxide, 30 to 50 parts by weight of solvent and optional auxiliary agents; the epoxy resin includes at least bio-based epoxy resin; the bio-based epoxy resin is obtained by purifying a bio-based ester compound containing phenolic hydroxyl groups and a halogenated epoxy alkylene compound under alkaline medium conditions after substitution reaction; the curing agent includes at least a first curing agent; the first curing agent is p-aminoazobenzene; the modified graphene oxide is obtained by modifying graphene oxide with dopamine hydrochloride.

[0006] In a preferred embodiment, the epoxy resin includes bio-based epoxy resin and bisphenol F epoxy resin.

[0007] In a preferred embodiment, the mass ratio of the bio-based epoxy resin to the bisphenol F epoxy resin is 1:(0.5-2).

[0008] In a preferred embodiment, the viscosity of the bisphenol F epoxy resin at 25° C. is 1000 to 5000 mPa·s.

[0009] In a preferred embodiment, the curing agent includes a first curing agent and a second curing agent.

[0010] In a preferred embodiment, the content of the first curing agent is 5 to 10 parts by weight.

[0011] In a preferred embodiment, the second curing agent is selected from at least one of isophoronediamine, hexamethylenediamine and polyetheramine.

[0012] In a preferred embodiment, during the preparation of the bio-based epoxy resin, the amount of the bio-based ester compound containing phenolic hydroxyl groups is 5 to 10 parts by weight, the amount of the halogenated epoxy hydrocarbon compound is 20 to 30 parts by weight, and the amount of the alkaline medium is 16 to 23 parts by weight.

[0013] In a preferred embodiment, the halogenated epoxyalkylene compound is selected from epichlorohydrin and / or epichlorohydrin.

[0014] In a preferred embodiment, the alkaline medium is selected from at least one of sodium hydroxide, potassium hydroxide, magnesium hydroxide, calcium hydroxide, ammonia water, sodium carbonate and potassium carbonate.

[0015] In a preferred embodiment, the bio-based ester compounds containing phenolic hydroxyl groups are obtained by esterification reaction of phenolic hydroxyl-containing acid compounds with hydroxyl-containing alcohol compounds and derivatives and then purified.

[0016] In a preferred embodiment, in the preparation process of the bio-based ester compound containing phenolic hydroxyl groups, the amount of the acid compound containing phenolic hydroxyl groups is 15 to 25 parts by weight, and the amount of the hydroxyl-containing alcohol compound and its derivatives is 10 to 15 parts by weight.

[0017] In a preferred embodiment, the acid compound containing phenolic hydroxyl group is selected from at least one of diphenolic acid, salvianolic acid A, mycophenolic acid and mycophenolic acid d3.

[0018] In a preferred embodiment, the hydroxyl-containing alcohol compound and its derivatives are selected from at least one of 1,3-dimethoxy-2-propanol, cinnamyl alcohol, phytol and coniferyl alcohol.

[0019] In a preferred embodiment, the esterification reaction is carried out in the presence of a catalyst and / or a dehydrating agent.

[0020] In a preferred embodiment, in the preparation process of the bio-based ester compound containing phenolic hydroxyl groups, the amount of the catalyst used is 0.5 to 1.5 parts by weight, and the amount of the dehydrating agent used is 22 to 25 parts by weight.

[0021] In a preferred embodiment, the catalyst is selected from at least one of 4 (dimethylamino) pyridine, methanesulfonic acid, p-toluenesulfonic acid, concentrated sulfuric acid, tetrabutyl titanate and tin oxide.

[0022] In a preferred embodiment, the dehydrating agent is selected from at least one of N,N-dicyclohexylcarbodiimide, triethyl orthoformate, phosphorus pentoxide and p-toluenesulfonyl isocyanate.

[0023] In a preferred embodiment, the solvent is selected from at least one of methanol, ethanol, isopropanol, acetone, dimethyl sulfoxide, dimethylformamide, tetrahydrofuran, xylene, ether, dichloromethane, epichlorohydrin and carbon tetrachloride.

[0024] The second object of the present invention is to provide a method for preparing the above-mentioned anti-corrosion bio-based epoxy coating, which comprises: mixing epoxy resin, curing agent, modified graphene oxide, solvent and optional auxiliary agents and then discharging the mixture to obtain the anti-corrosion bio-based epoxy coating.

[0025] The third object of the present invention is to provide an anti-corrosion bio-based epoxy coating, which is obtained by coating the above-mentioned anti-corrosion bio-based epoxy coating on the surface of a substrate and curing it.

[0026] A fourth object of the present invention is to provide the use of the above-mentioned anticorrosive bio-based epoxy paint or the above-mentioned anticorrosive bio-based epoxy coating on the surface of a substrate with anticorrosion requirements.

[0027] The key of the present invention is to coordinate the epoxy resin, curing agent, modified graphene oxide, solvent and optional auxiliary agent with a specific ratio to obtain a bio-based epoxy coating. Due to the introduction of p-aminoazobenzene with an azo structure and graphene oxide modified by dopamine hydrochloride, the anti-corrosion performance (acid and alkali resistance, salt water resistance and salt spray resistance) of the bio-based epoxy coating is improved by synergistic effect. At the same time, due to the introduction of a higher proportion of bio-based epoxy resin (without cytotoxicity and carcinogenicity), compared with bisphenol A epoxy resin mainly from fossil resources, it has no cytotoxicity and carcinogenicity, reducing the harm that the bio-based epoxy coating may bring to human health, while also ensuring that the bio-based epoxy coating has good mechanical properties (adhesion, impact resistance). In addition, p-aminoazobenzene has a unique cis-trans isomer structure of the azo structure, so that it is responsive to changes in the external environment, such as light, acid and alkali, humidity, etc. On the one hand, it can simply and effectively confirm whether the coating is fully coated, and on the other hand, it can improve the corrosion resistance of the coating in environments such as acid and alkali. In summary, the bio-based epoxy coating provided by the present invention has good anti-corrosion properties, namely, good acid resistance, alkali resistance, salt water resistance and salt spray resistance, and can provide excellent protection in environments with anti-corrosion requirements, especially in marine environments. Compared with traditional petroleum-based epoxy anti-corrosion coatings, it realizes the green synthesis of epoxy coatings and has broad application prospects.

[0028] In a preferred embodiment, the bio-based epoxy resin has two or more benzene ring structures and two or more epoxy functional groups, which can increase the cross-linking density of the epoxy coating and further improve the anti-corrosion performance of the epoxy coating. DETAILED DESCRIPTION

[0029] The bio-based anti-corrosion coating provided by the present invention comprises epoxy resin, curing agent, modified graphene oxide, solvent and optional auxiliary agent. Wherein, the content of the epoxy resin is 20 to 40 parts by weight, such as 20, 22, 25, 28, 30, 32, 35, 38, 40 parts by weight or any value therebetween; the content of the curing agent is 15 to 35 parts by weight, such as 15, 18, 20, 22, 25, 28, 30, 32, 35 parts by weight or any value therebetween; the content of the modified graphene oxide is 0.2 to 1 part by weight, such as 0.2, 0.5, 0.8, 1 part by weight or any value therebetween; the content of the solvent is 30 to 50 parts by weight, such as 30, 32, 35, 38, 40, 42, 45, 48, 50 parts by weight or any value therebetween. The epoxy resin at least comprises a bio-based epoxy resin. The bio-based epoxy resin is obtained by purifying a bio-based ester compound containing phenolic hydroxyl groups and a halogenated epoxy alkylene compound by substitution reaction under alkaline medium conditions. The curing agent includes at least a first curing agent. The first curing agent is p-aminoazobenzene. The modified graphene oxide is obtained by modifying graphene oxide with dopamine hydrochloride.

[0030] In the present invention, the epoxy resin preferably includes a bio-based epoxy resin and a bisphenol F epoxy resin. Adding a certain amount of bisphenol F epoxy resin is beneficial to further improve the mechanical properties of the epoxy adhesive, such as shear strength. The mass ratio of the bio-based epoxy resin to the bisphenol F epoxy resin is preferably 1: (0.5-2), such as 1: 0.5, 1: 0.8, 1: 1, 1: 1.2, 1: 1.5, 1: 1.8, 1: 2 or any value therebetween. In a preferred embodiment, the content of the bio-based epoxy resin is preferably 10-20 parts by weight, such as 10, 12, 15, 18, 20 parts by weight or any value therebetween; the content of the bisphenol F epoxy resin is preferably 0-20 parts by weight, such as 10, 12, 15, 18, 20 parts by weight or any value therebetween.

[0031] In the present invention, the viscosity of the bisphenol F epoxy resin at 25° C. is 1000-5000 mPa·s, such as 1000 mPa·s, 2000 mPa·s, 3000 mPa·s, 4000 mPa·s, 5000 mPa·s or any value therebetween. Specific examples of the bisphenol F epoxy resin include, but are not limited to, at least one of EPALLOY 8220 and EPALLOY 8230 of CVC Specialty Chemicals, Inc., USA, EXA-830LV and EXA-835LV of Dainippon Ink & Printing Co., Ltd., and jER 806, jER 807 and EP-4910E of Shanghai Zhongsi Industrial Co., Ltd.

[0032] In the present invention, the curing agent preferably includes a first curing agent and a second curing agent. In a preferred embodiment, the content of the first curing agent is preferably 5 to 10 parts by weight, such as 5, 6, 7, 8, 9, 10 parts by weight or any value therebetween. The present invention does not specifically limit the type of the second curing agent, and is preferably at least one of isophorone diamine, hexamethylene diamine and polyether amine.

[0033] In addition, the terms "first" and "second" are only used to distinguish the different curing agents used, and do not represent any particular limitation on the type of the curing agent.

[0034] In the preparation process of the above-mentioned bio-based epoxy resin, the amount of the bio-based ester compound containing phenolic hydroxyl groups is preferably 5 to 10 parts by weight, such as 5, 6, 7, 8, 9, 10 parts by weight or any value therebetween; the amount of the halogenated epoxy alkylene compound is preferably 20 to 30 parts by weight, such as 20, 22, 25, 28, 30 parts by weight or any value therebetween; the amount of the alkaline medium is preferably 16 to 23 parts by weight, such as 16, 18, 20, 22, 25, 28, 30 parts by weight or any value therebetween.

[0035] In a specific embodiment, the preparation process of the bio-based epoxy resin may include: mixing a bio-based ester compound containing a phenolic hydroxyl group and a halogenated epoxy alkylene compound in an organic solvent I, then adding an alkaline medium aqueous solution dropwise to carry out a substitution reaction, and obtaining a bio-based epoxy resin after purification. The purification treatment may be a purification method commonly used in the prior art. The present invention preferably adopts the following steps for purification treatment: mixing the product obtained after the above-mentioned substitution reaction with an organic solvent II, centrifugally washing three times with deionized water, adding anhydrous magnesium sulfate to remove the remaining water, removing the organic solvent by rotary evaporation, and then purifying by vacuum distillation to obtain a bio-based epoxy resin. Wherein, the organic solvent I and the organic solvent II are each independently preferably selected from at least one of methanol, ethanol, acetone, dichloromethane, benzene, and toluene. The organic solvent II is more preferably dichloromethane, which can better dissolve the resin obtained by the reaction and remove the unreacted raw materials by oil-water separation.

[0036] In addition, "Ⅰ" and "Ⅱ" in "organic solvent Ⅰ" and "organic solvent Ⅱ" are only used to distinguish the organic solvents used in different steps, and do not represent any particular limitation on the type of organic solvent.

[0037] In the above-mentioned preparation process of bio-based epoxy resin, the conditions of the substitution reaction are not particularly limited, as long as the epoxy group can be modified to the bio-based ester compound containing phenolic hydroxyl group to obtain the bio-based epoxy resin. In a specific embodiment, the conditions of the substitution reaction include a temperature of preferably 70 to 90°C, such as 70°C, 75°C, 80°C, 85°C, 90°C or any value therebetween; and a time of preferably 15 to 40 minutes, such as 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes or any value therebetween.

[0038] In the present invention, the halogenated epoxyalkylene compound only needs to have a structure as shown in formula (1). In view of the availability of raw materials, the halogenated epoxyalkylene compound is particularly preferably epichlorohydrin and / or epichlorohydrin.

[0039] Wherein, X is a halogen, which may be fluorine, chlorine, bromine or iodine, and R is C 1 ~C 4 The alkylene group can be methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.

[0040] In the present invention, the alkaline medium can be any compound that can make the pH value of the reaction system alkaline, and specific examples thereof can be at least one of sodium hydroxide, potassium hydroxide, magnesium hydroxide, calcium hydroxide, ammonia water, sodium carbonate and potassium carbonate, and more preferably sodium hydroxide and / or potassium hydroxide.

[0041] In the present invention, the bio-based ester compound containing phenolic hydroxyl groups is preferably prepared by the following method: after esterification reaction of the acid compound containing phenolic hydroxyl groups with the alcohol compound containing hydroxyl groups and derivatives, the bio-based ester compound containing phenolic hydroxyl groups is obtained after purification. Among them, the amount of the acid compound containing phenolic hydroxyl groups is preferably 15 to 25 parts by weight, such as 15, 18, 20, 22, 25 parts by weight or any value therebetween; the amount of the alcohol compound containing hydroxyl groups and derivatives is preferably 10 to 15 parts by weight, such as 10, 11, 12, 13, 14, 15 parts by weight or any value therebetween.

[0042] In the present invention, the acid compound containing phenolic hydroxyl group is a kind of acid compound containing at least one phenolic hydroxyl group and carboxyl group from non-fossil energy, and its specific examples include but are not limited to: at least one of diphenolic acid, salvianolic acid A, mycophenolic acid and mycophenolic acid d3, more preferably diphenolic acid and / or salvianolic acid A. Among them, diphenolic acid is synthesized by levulinic acid derived from cellulose, and cellulose is the most abundant renewable material in nature. Therefore, diphenolic acid is the most promising candidate to replace petroleum-based bisphenol A. The bio-based epoxy resin prepared with diphenolic acid as a precursor has no cytotoxicity and carcinogenicity, and has two epoxy groups and a double benzene ring structure, which is more conducive to improving the network crosslinking density of the epoxy adhesive system and has a positive effect on improving the glass transition temperature and thermal stability of the polymer, thereby further improving the anti-corrosion performance of the epoxy adhesive.

[0043] In the present invention, specific examples of the hydroxyl-containing alcohol compounds and derivatives include, but are not limited to, at least one of 1,3-dimethoxy-2-propanol, cinnamyl alcohol, phytol and coniferyl alcohol.

[0044] In the present invention, the esterification reaction is preferably carried out in the presence of a catalyst and / or a dehydrating agent, which is beneficial to further improve the reaction efficiency and reduce the reaction energy consumption. The amount of the catalyst is preferably 0.5 to 1.5 parts by weight, such as 0.5, 0.8, 1, 1.2, 1.5 parts by weight or any value therebetween; the amount of the dehydrating agent is preferably 22 to 25 parts by weight, such as 22, 23, 24, 25 parts by weight or any value therebetween. The catalyst is preferably at least one selected from 4-(dimethylamino)pyridine, methanesulfonic acid, p-toluenesulfonic acid, concentrated sulfuric acid, tetrabutyl titanate and tin oxide. The dehydrating agent is preferably at least one selected from N, N-dicyclohexylcarbodiimide, triethyl orthoformate, phosphorus pentoxide and p-toluenesulfonyl isocyanate.

[0045] In a specific embodiment, the preparation process of the bio-based ester compound containing phenolic hydroxyl groups may include: dissolving the acid compound containing phenolic hydroxyl groups, the alcohol compound containing hydroxyl groups and its derivatives and the catalyst in an organic solvent III, cooling to 0° C. and then using N 2 Purging to obtain a reaction substrate, dissolving a dehydrating agent in an organic solvent III and adding the dehydrating agent dropwise to the reaction substrate, reacting for 20 to 30 hours, collecting the product and vacuum drying to obtain a solid product, separating and purifying the obtained solid product, and obtaining a bio-based ester compound containing a phenolic hydroxyl group. The organic solvent III is preferably at least one selected from methanol, ethanol, acetone, dichloromethane, benzene, and toluene, and more preferably dichloromethane.

[0046] In the present invention, the modified graphene oxide is preferably prepared by the following method: dispersing graphene oxide (GO) in a Tris buffer solution to obtain a GO dispersion, adding dopamine hydrochloride and stirring at 40 to 60°C for 24 to 48 hours, and collecting the product to obtain the modified graphene oxide. Wherein, the amount of graphene oxide is preferably such that the concentration of graphene oxide in the GO dispersion is 0.1 to 0.5 g / L, such as 0.1 g / L, 0.2 g / L, 0.3 g / L, 0.4 g / L, 0.5 g / L or any value therebetween. The amount of dopamine hydrochloride added is 0.5 to 1 times the mass of graphene oxide, such as 0.5 times, 0.6 times, 0.7 times, 0.8 times, 0.9 times, 1 times or any value therebetween. The method of collecting the product is preferably: collecting the solid product by microporous membrane filtration, washing with deionized water, and drying the product in a vacuum oven at 60 to 80°C.

[0047] The present invention does not particularly limit the type of the solvent, which can be a conventional choice in the prior art, and specific examples thereof include but are not limited to: at least one of methanol, ethanol, isopropanol, acetone, dimethyl sulfoxide, dimethylformamide, tetrahydrofuran, xylene, ether, dichloromethane, epichlorohydrin and carbon tetrachloride.

[0048] The present invention does not particularly limit the type of the auxiliary agent, which can be a conventional choice in the prior art, preferably at least one of a dispersant, a defoamer and a leveling agent. Among them, the dispersant is preferably at least one of BYK-9076, BYK-9010 and BYK-391. The defoamer is preferably at least one of BKY-054, BKY-057 and BYK-1794. The leveling agent is preferably at least one of BKY-300, BKY-302, BKY-310 and BYK-333.

[0049] In the present invention, the preparation method of the anti-corrosion bio-based epoxy coating may specifically include: firstly adding epoxy resin, curing agent and solvent into a dual planetary hybrid power reactor and vacuum stirring, then adding modified graphene oxide and optional auxiliary agent and continuing vacuum stirring, and obtaining the anti-corrosion bio-based epoxy coating after discharging. The vacuum condition is preferably a vacuum degree of <0.098MPa, and the stirring temperature may be 25℃±5℃

[0050] In the present invention, the anti-corrosion bio-based epoxy coating is obtained by coating the anti-corrosion bio-based epoxy coating on the surface of the substrate and curing it. The coating method can be: using at least one of a wire rod coater, a film coating machine, spraying or spin coating method to coat the bio-based epoxy coating on the surface of the metal substrate after sandblasting pretreatment. The curing method can be: heating the substrate coated with the coating at 70 to 90° C. for 24 to 30 hours until it is completely cured, thereby obtaining the bio-based epoxy anti-corrosion coating.

[0051] The present invention will be described in detail below through specific embodiments.

[0052] The parts of raw materials involved in the following examples and comparative examples are all parts by weight.

[0053] Preparation Example 1 Preparation of bio-based epoxy resin

[0054] (1) Dissolve diphenolic acid (20 parts, 50.0 g), 1,3-dimethoxy-2-propanol (11.84 parts, 29.6 g) and 4-(dimethylamino)pyridine (1 part, 2.5 g) in anhydrous dichloromethane (1000.0 g), cool to 0°C and heat using N 2 Purge; dissolve N,N-dicyclohexylcarbodiimide (22 parts, 55.0 g) in anhydrous dichloromethane (660.0 g) in a beaker, and add dropwise to the above solution within 2 hours, react at ambient temperature for 24 hours, collect the product and vacuum dry to obtain a brown solid, separate and purify the obtained brown solid by a column chromatography system to obtain a bio-based ester compound;

[0055] (2) The bio-based ester compound (5 parts, 10.0 g) obtained in step (1), epichlorohydrin (25 parts, 50.0 g) and anhydrous ethanol (190.0 g) were mixed and stirred at 80° C. for 10 min, and then a 50% by mass sodium hydroxide aqueous solution (64.0 g, 16 parts of sodium hydroxide) was added dropwise to the mixture, and the mixture was stirred at 80° C. for 30 min. After cooling to room temperature, the mixture was mixed with dichloromethane (320.0 g), and washed three times by centrifugation with deionized water (1000.0 g), and then mixed with anhydrous magnesium sulfate (40.0 g) to remove water, and then dichloromethane and ethanol were removed by rotary evaporation (80° C., 0.01 MPa), and then further purified by vacuum distillation (120° C.) to obtain bio-based epoxy resin A1.

[0056] The specific reaction process is as follows:

[0057]

[0058] Preparation Example 2 Preparation of Bio-based Epoxy Resin

[0059] (1) Salvianolic acid A (25 parts, 32.5 g), 1,3-dimethoxy-2-propanol (15 parts, 37.5 g) and 4-(dimethylamino)pyridine (1 part, 2.5 g) were dissolved in anhydrous dichloromethane (1000.0 g), cooled to 0°C and heated with N 2Purge; dissolve N,N-dicyclohexylcarbodiimide (22 parts, 55.0 g) in anhydrous dichloromethane (660.0 g) in a beaker, and add dropwise to the above solution within 2 hours, react at ambient temperature for 24 hours, collect the product and vacuum dry to obtain a brown solid, separate and purify the obtained brown solid by a column chromatography system to obtain a bio-based ester compound;

[0060] (2) The bio-based ester compound (7 parts, 14.0 g) obtained in step (1), epichlorohydrin (30 parts, 60.0 g) and anhydrous ethanol (190.0 g) were mixed and stirred at 80° C. for 10 min, and then a 50% by mass sodium hydroxide aqueous solution (64.0 g, 16 parts of sodium hydroxide) was added dropwise to the mixture, and stirred at 80° C. for 30 min. After cooling to room temperature, the mixture was mixed with dichloromethane (320.0 g), and washed three times by centrifugation with deionized water (1000.0 g), and then mixed with anhydrous magnesium sulfate (40.0 g) to remove water, and then dichloromethane and ethanol were removed by rotary evaporation (80° C., 0.01 MPa), and then further purified by vacuum distillation (120° C.) to obtain bio-based epoxy resin A2.

[0061] Preparation Example 3 Preparation of Bio-based Epoxy Resin

[0062] (1) Mycophenolic acid (15 parts, 37.5 g), 1,3-dimethoxy-2-propanol (10 parts, 25 g) and 4-(dimethylamino)pyridine (1 part, 2.5 g) were dissolved in anhydrous dichloromethane (1000.0 g), cooled to 0°C and heated with N 2 Purge; dissolve N,N-dicyclohexylcarbodiimide (22 parts, 55.0 g) in anhydrous dichloromethane (660.0 g) in a beaker, and add dropwise to the above solution within 2 hours, react at ambient temperature for 24 hours, collect the product and vacuum dry to obtain a brown solid, separate and purify the obtained brown solid by a column chromatography system to obtain a bio-based ester compound;

[0063] (2) The bio-based ester compound (10 parts, 20.0 g) obtained in step (1), epichlorohydrin (20 parts, 40.0 g) and anhydrous ethanol (190.0 g) were mixed and stirred at 80° C. for 10 min, and then a 50% by mass sodium hydroxide aqueous solution (64.0 g, 16 parts of sodium hydroxide) was added dropwise to the mixture, and stirred at 80° C. for 30 min. After cooling to room temperature, the mixture was mixed with dichloromethane (320.0 g), and washed three times by centrifugation with deionized water (1000.0 g), and then mixed with anhydrous magnesium sulfate (40.0 g) to remove water, and then dichloromethane and ethanol were removed by rotary evaporation (80° C., 0.01 MPa), and then further purified by vacuum distillation (120° C.) to obtain bio-based epoxy resin A3.

[0064] Preparation Example 4 Preparation of modified graphene oxide

[0065] 2.5 g of graphene oxide nanosheets (GO) were dispersed in 5 L of Tris buffer solution (pH = 8.5), stirred and ultrasonically dispersed for 30 min, and then 2.5 g of dopamine hydrochloride was added to the GO dispersion and stirred at 60 ° C for 36 h; after the reaction, the solid product was collected by 0.2 μm microporous membrane filtration, washed 3 times with deionized water, and the product was dried in a vacuum oven at 60 ° C for 12 h to obtain modified graphene oxide B.

[0066] Example 1 Preparation of bio-based epoxy coating

[0067] 20 parts of bisphenol F epoxy resin (EXA-835LV, viscosity of 2300 mPa·s at 25°C), 15 parts of bio-based epoxy resin A1, 17 parts of isophorone diamine, 7 parts of p-aminoazobenzene, and 40 parts of epichlorohydrin are added into a double planetary hybrid reactor in sequence, and vacuum stirred evenly; 0.6 parts of modified graphene oxide B, 0.1 parts of BKY-391, 0.2 parts of BKY-057, and 0.1 parts of BKY-333 are added into the reactor, and vacuum stirred evenly before discharging to obtain bio-based epoxy coating H1.

[0068] Example 2 Preparation of bio-based epoxy coating

[0069] 10 parts of bisphenol F epoxy resin (EP-4910E, viscosity at 25°C is 3500mPa·s), 20 parts of bio-based epoxy resin A1, 15 parts of hexamethylenediamine, 10 parts of p-aminoazobenzene, and 44.5 parts of xylene are added to a double planetary hybrid reactor in sequence, and vacuum stirred evenly; 0.2 parts of modified graphene oxide B, 0.1 parts of BKY-391, 0.1 parts of BKY-057, and 0.1 parts of BKY-333 are added to the reactor, and after vacuum stirring evenly, the material can be discharged to obtain bio-based epoxy coating H2.

[0070] Example 3 Preparation of bio-based epoxy coating

[0071] 15 parts of bisphenol F epoxy resin (EPALLOY 8220, with a viscosity of 1800-2800 mPa·s at 25°C), 10 parts of bio-based epoxy resin A1, 20 parts of isophorone diamine, 5 parts of p-aminoazobenzene, and 48.5 parts of dimethyl sulfoxide were added to a double planetary hybrid reactor in sequence, and vacuum stirred evenly; 1 part of modified graphene oxide B, 0.2 parts of BKY-391, 0.1 parts of BKY-057, and 0.2 parts of BKY-333 were added to the reactor, and vacuum stirred evenly before discharging to obtain bio-based epoxy coating H3.

[0072] Example 4 Preparation of Bio-based Epoxy Coating

[0073] The bio-based epoxy coating was prepared according to the method of Example 1, except that the same weight portion of bio-based epoxy resin A2 was used instead of bio-based epoxy resin A1, and the other conditions were the same as those of Example 1, so as to obtain bio-based epoxy coating H4.

[0074] Example 5 Preparation of Bio-based Epoxy Coating

[0075] The bio-based epoxy coating was prepared according to the method of Example 1, except that the same weight portion of bio-based epoxy resin A3 was used instead of bio-based epoxy resin A1, and the other conditions were the same as those of Example 1, so as to obtain bio-based epoxy coating H5.

[0076] Example 6 Preparation of Bio-based Epoxy Coating

[0077] The bio-based epoxy coating was prepared according to the method of Example 1, except that the same weight portion of bio-based epoxy resin A1 was used instead of bisphenol F epoxy resin (EXA-835LV, with a viscosity of 2300 mPa·s at 25°C), and the other conditions were the same as those in Example 1, thus obtaining bio-based epoxy coating H6.

[0078] Comparative Example 1 Preparation of Reference Bio-based Epoxy Coating

[0079] A reference bio-based epoxy coating was prepared according to the method of Example 2, except that the same weight portion of ethylenediamine was used instead of p-aminoazobenzene, and the other conditions were the same as in Example 2, so as to obtain a reference bio-based epoxy coating DH1.

[0080] Comparative Example 2 Preparation of Reference Bio-based Epoxy Coating

[0081] A reference bio-based epoxy coating was prepared according to the method of Example 3, except that modified graphene oxide was not added, and the other conditions were the same as those of Example 3, thus obtaining a reference bio-based epoxy coating DH2.

[0082] Comparative Example 3 Preparation of Reference Bio-based Epoxy Coating

[0083] A reference bio-based epoxy coating was prepared according to the method of Example 3, except that the same weight portion of isophoronediamine was used to replace p-aminoazobenzene and modified graphene oxide was not added, and the other conditions were the same as in Example 3, thus obtaining a reference bio-based epoxy coating DH3.

[0084] Test Case

[0085] The bio-based epoxy coatings prepared in the above examples and comparative examples were used to prepare a coating according to the following method: the bio-based epoxy coating was coated on a Q235 carbon steel sample (sample size was 150 mm×70 mm×5 mm), and the coating was obtained after curing at 90° C. for 24 hours, and the coating thickness was 100 μm. The prepared coating was tested for adhesion, impact resistance, acid resistance, alkali resistance, salt water resistance and salt spray resistance according to the following method, and the results are shown in Table 1.

[0086] (1) Coating appearance: Visually observe the coating surface.

[0087] (2) Adhesion: The test was conducted in accordance with the method in GB / T 9286-2021. A single-edged cutting tool was used to cut the surface of the sample 6 times in the horizontal and vertical directions with an interval of 2 mm. The surface condition of the cut area was observed and the adhesion level was determined (0: the cut edge was completely smooth and there was no shedding within the grid; 1: a small amount of coating shedding occurred at the intersection of the cuts, but the affected cross-cut area was no more than 5%).

[0088] (3) Impact resistance: The test was conducted in accordance with the method in GB / T 1732-2020. The impact tester was fixed on the surface of the sample to be tested and dropped from a certain height to observe whether cracks, wrinkles or peeling appeared on the coating surface. The highest height at which no cracks, wrinkles or peeling appeared on the coating surface was recorded for three tests.

[0089] (4) Acid resistance, alkali resistance, and salt water resistance: According to the method in GB / T 9274 standard, the sample to be tested is immersed in 5% H 2 SO 4 , 5% NaOH, 5% NaCl, when deformation, bubbling or shedding of the coating surface is observed, record the immersion time.

[0090] (5) Salt spray resistance: The sample to be tested is tested according to the method in GB / T 1771. When deformation, bubbling or shedding of the coating surface is observed, the salt spray resistance time is recorded.

[0091] Table 1

[0092]

[0093] From the results of Example 2 and Comparative Example 1, it can be seen that the modified graphene oxide provided by the present invention is not added, and the acid and alkali resistance time of the reference bio-based epoxy coating prepared thereby is reduced by about 0.47 times, the salt water resistance time is reduced by about 0.25 times, and the salt spray resistance time is reduced by about 0.25 times. From the results of Example 3 and Comparative Example 2, it can be seen that p-aminoazobenzene is not added, and the acid and alkali resistance time of the reference bio-based epoxy coating prepared thereby is reduced by about 0.42 times, the salt water resistance time is reduced by about 0.56 times, and the salt spray resistance time is reduced by about 0.53 times. From the results of Example 3 and Comparative Example 3, it can be seen that the modified graphene oxide and p-aminoazobenzene provided by the present invention are not added, and the acid and alkali resistance time of the reference bio-based epoxy coating prepared thereby is reduced by about 0.67 times, the salt water resistance time is reduced by about 0.65 times, and the salt spray resistance time is reduced by about 0.70 times. From the results of Example 6, it can be seen that when the added epoxy resin is all bio-based epoxy resin, the adhesion and impact resistance of the obtained bio-based epoxy coating are reduced, but can meet the actual application requirements. In summary, the bio-based epoxy coating provided by the present invention has good acid resistance, alkali resistance, salt water resistance and salt spray resistance.

[0094] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.

Claims

1. An anticorrosive bio-based epoxy coating, It is characterized in that The bio-based anti-corrosion coating comprises 20 to 40 parts by weight of epoxy resin, 15 to 35 parts by weight of curing agent, 0.2 to 1 part by weight of modified graphene oxide, 30 to 50 parts by weight of solvent and optional auxiliary agents; the epoxy resin comprises at least a bio-based epoxy resin; the bio-based epoxy resin is obtained by purifying a bio-based ester compound containing phenolic hydroxyl groups and a halogenated epoxy alkylene compound under alkaline medium conditions after substitution reaction; the curing agent comprises at least a first curing agent; the first curing agent is p-aminoazobenzene; the modified graphene oxide is obtained by modifying graphene oxide with dopamine hydrochloride.

2. The anticorrosive bio-based epoxy coating according to claim 1, It is characterized in that The epoxy resin includes bio-based epoxy resin and bisphenol F epoxy resin; Preferably, the mass ratio of the bio-based epoxy resin to the bisphenol F epoxy resin is 1:(0.5-2); Preferably, the viscosity of the bisphenol F epoxy resin at 25° C. is 1000 to 5000 mPa·s.

3. The anticorrosive bio-based epoxy coating according to claim 1, It is characterized in that The curing agent includes a first curing agent and a second curing agent; Preferably, the content of the first curing agent is 5 to 10 parts by weight; Preferably, the second curing agent is selected from at least one of isophoronediamine, hexamethylenediamine and polyetheramine.

4. The anticorrosive bio-based epoxy coating according to any one of claims 1 to 3, It is characterized in that In the preparation process of the bio-based epoxy resin, the amount of the bio-based ester compound containing phenolic hydroxyl groups is 5 to 10 parts by weight, the amount of the halogenated epoxy alkylene compound is 20 to 30 parts by weight, and the amount of the alkaline medium is 16 to 23 parts by weight; Preferably, the halogenated epoxyalkane compound is selected from epichlorohydrin and / or epichlorohydrin; Preferably, the alkaline medium is selected from at least one of sodium hydroxide, potassium hydroxide, magnesium hydroxide, calcium hydroxide, ammonia water, sodium carbonate and potassium carbonate.

5. The anticorrosive bio-based epoxy coating according to any one of claims 1 to 3, It is characterized in that The bio-based ester compounds containing phenolic hydroxyl groups are obtained by esterification of acid compounds containing phenolic hydroxyl groups with alcohol compounds containing hydroxyl groups and derivatives and then purified; Preferably, in the preparation process of the bio-based ester compound containing phenolic hydroxyl groups, the amount of the acid compound containing phenolic hydroxyl groups is 15 to 25 parts by weight, and the amount of the hydroxyl-containing alcohol compound and its derivatives is 10 to 15 parts by weight. Preferably, the acid compound containing phenolic hydroxyl group is selected from at least one of diphenolic acid, salvianolic acid A, mycophenolic acid and mycophenolic acid d3; Preferably, the hydroxyl-containing alcohol compound and its derivatives are selected from at least one of 1,3-dimethoxy-2-propanol, cinnamyl alcohol, phytol and coniferyl alcohol.

6. The anticorrosive bio-based epoxy coating according to claim 5, It is characterized in that The esterification reaction is carried out in the presence of a catalyst and / or a dehydrating agent; Preferably, in the preparation process of the bio-based ester compound containing phenolic hydroxyl groups, the amount of the catalyst is 0.5 to 1.5 parts by weight, and the amount of the dehydrating agent is 22 to 25 parts by weight; Preferably, the catalyst is selected from at least one of 4 (dimethylamino) pyridine, methanesulfonic acid, p-toluenesulfonic acid, concentrated sulfuric acid, tetrabutyl titanate and tin oxide; Preferably, the dehydrating agent is selected from at least one of N,N-dicyclohexylcarbodiimide, triethyl orthoformate, phosphorus pentoxide and p-toluenesulfonyl isocyanate.

7. The anticorrosive bio-based epoxy coating according to any one of claims 1 to 3, It is characterized in that The solvent is selected from at least one of methanol, ethanol, isopropanol, acetone, dimethyl sulfoxide, dimethylformamide, tetrahydrofuran, xylene, ether, dichloromethane, epichlorohydrin and carbon tetrachloride.

8. The method for preparing the anticorrosive bio-based epoxy coating according to any one of claims 1 to 7, It is characterized in that The method comprises: mixing epoxy resin, curing agent, modified graphene oxide, solvent and optional auxiliary agent and then discharging the mixture to obtain the anticorrosive bio-based epoxy coating.

9. An anti-corrosion bio-based epoxy coating, It is characterized in that The anti-corrosion bio-based epoxy coating is obtained by coating the anti-corrosion bio-based epoxy coating according to any one of claims 1 to 7 on the surface of a substrate and curing the coating.

10. Use of the anticorrosive bio-based epoxy paint according to any one of claims 1 to 7 or the anticorrosive bio-based epoxy coating according to claim 9 on the surface of a substrate with anticorrosion requirements.

Citation Information

Patent Citations

  • Bio-based thermosetting resin composite material and preparation method thereof

    CN110607077A

  • Chip-level epoxy underfill adhesive and preparation method thereof

    CN115820180A

  • Graphene oxide modified bio-based epoxy anticorrosive paint as well as preparation method and application thereof

    CN117844336A

  • Curing catalyst for epoxy resin and epoxy resin composition including the catalyst

    JP2006022342A

  • Method to characterize curing of epoxy with aromatic diamines

    US4717674A

Cited By

  • Bio-based epoxy resin and preparation method thereof

    CN120441510A