Novel coating for enhancing ice resistance of wind power blade
By incorporating self-healing microcapsules and super-hydrophobic nanoparticles into the coating of wind turbine blades, the problem that traditional coatings are difficult to repair when damaged is solved, the automatic repair and super-hydrophobic properties of the coating are achieved, and the anti-icing performance of wind turbine blades is improved. and reliability.
Patent Information
- Application Number
- CN202411026622.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-15
AI Technical Summary
Traditional anti-icing coatings on wind turbine blades are difficult to repair themselves when faced with tiny cracks or damage, resulting in reduced anti-icing performance, increased maintenance costs and downtime, and affecting power generation efficiency and reliability.
Self-healing microcapsules are prepared using an emulsion polymerization method and integrated into the coating, combined with super-hydrophobic nanoparticles, to achieve automatic repair and super-hydrophobic properties of the coating and enhance anti-icing properties.
It realizes the automatic repair function of the coating when it is damaged, reduces maintenance requirements, reduces the maintenance cost of wind turbine blades, improves power generation efficiency and reliability, and reduces the adhesion and accumulation of ice and snow.
Smart Images

Figure CN118772767A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coating preparation, in particular to a new type of coating for enhancing the ice resistance of wind turbine blades. Background Art
[0002] As the global demand for renewable energy continues to grow, wind power generation, as a clean and renewable form of energy, has become increasingly important. As the core component of the wind power generation system, the performance of wind turbine blades directly affects the power generation efficiency and reliability of the entire system. However, since wind turbine blades are exposed to complex and changeable natural environments for a long time, especially the ice and snow weather in cold areas, the operation of wind turbine blades has brought severe challenges. The adhesion of ice and snow not only increases the weight and load of the blades, but also easily causes ice to form on the blade surface, thereby affecting the normal operation of wind turbines and even causing safety accidents.
[0003] In response to the anti-icing problem faced by wind turbine blades, traditional technology has developed a variety of anti-icing coatings. These coatings mainly resist the adhesion and erosion of ice and snow by improving the hydrophobicity of the coating, lowering the freezing point and increasing the hardness of the coating. However, traditional technology is powerless when dealing with tiny cracks or damage on the blade surface. Once the coating is damaged, its anti-icing performance will be greatly reduced and it will be difficult to repair itself. This not only weakens the protective effect of the coating, but also increases the maintenance cost and downtime of the wind turbine blades, affecting the economy and reliability of wind power generation.
[0004] In view of the above problems, it is necessary to optimize the existing anti-icing coatings and retrograde coatings for wind turbine blades, and to realize the automatic repair function of the coating when damaged by integrating microcapsules with self-repairing function. Therefore, it is of great significance to develop a new type of coating that can comprehensively realize the above characteristics and enhance the anti-icing performance of wind turbine blades. Summary of the invention
[0005] The purpose of the present invention is to make up for the shortcomings of the prior art and provide a new type of coating for enhancing the anti-icing performance of wind turbine blades. It can realize the automatic repair function of the coating when damaged by integrating self-repairing microcapsules. At the same time, the addition of superhydrophobic nanoparticles gives the coating excellent superhydrophobic properties, making it difficult for water droplets to stay on the surface of the blades, effectively reducing the adhesion and accumulation of ice and snow.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: a new type of coating for enhancing the anti-icing performance of wind turbine blades, the preparation process of the coating includes:
[0007] S100, preparation of self-healing microcapsules: polyurethane prepolymer and catalyst are encapsulated in microcapsules by emulsion polymerization, and the size and distribution of microcapsules are controlled;
[0008] S200, mixing base resin and additives: uniformly mixing polyurethane resin, dispersant, defoamer and leveling agent in a certain proportion to form a base resin mixture;
[0009] S300, adding super-hydrophobic additives: adding super-hydrophobic nanoparticles into the matrix resin mixture, and uniformly dispersing the nanoparticles by high-speed dispersion or ultrasonic treatment;
[0010] S400, incorporating self-repairing microcapsules: adding the prepared self-repairing microcapsules into the mixture in a certain proportion, and continuing to stir and mix evenly to obtain an anti-icing coating with a self-repairing function;
[0011] S500, coating and curing: The coating is applied to the surface of the wind turbine blade by spraying, brushing and dipping, and after curing conditions, an anti-icing coating with self-repairing function is formed.
[0012] Further, the S100 includes:
[0013] S101, selecting a polyurethane prepolymer and a catalyst, and preparing a precursor of a microcapsule wall material, and selecting the wall material according to the desired performance of the microcapsule;
[0014] S102, using an emulsifier to mix the polyurethane prepolymer, the catalyst and the organic solvent to form a stable emulsion;
[0015] S103, using a layer-by-layer deposition method to make the wall material precursor form a uniform thin film on the surface of the droplet, and adjusting the thickness and uniformity of the wall material by controlling the concentration of the precursor, the dropping speed and the stirring intensity parameters;
[0016] S104, adjusting the pH value and temperature to promote the cross-linking reaction of the wall material precursor to form a strong microcapsule wall, separating the microcapsules from the suspension by centrifugation, filtration and spray drying, and washing and drying;
[0017] S105, inspecting the size, distribution and self-healing performance of the prepared microcapsules, screening out qualified microcapsules, and preparing for subsequent coating preparation.
[0018] Furthermore, in the S101, the polyurethane prepolymer is selected as isocyanate-based polyurethane prepolymer, the catalyst is selected as an organic tin catalyst, which is widely used in the synthesis of polyurethane prepolymer and the curing process of microcapsules, and the wall material precursor is selected as a mixture of gelatin and gum arabic, which can form a tough microcapsule wall with a certain elasticity when mixed.
[0019] Furthermore, the specific steps of using the layer-by-layer deposition method in S103 to form a uniform thin film of the wall material precursor on the surface of the droplet are:
[0020] (1) Slowly and evenly adding the wall material precursor solution into the emulsion or dispersion through a dropping device. The dropping speed needs to be precisely controlled so that the wall material is evenly deposited on the droplet surface;
[0021] (2) During the dropwise addition process, the speed of the stirrer is maintained to keep the droplets in suspension under the stirring action and to promote the uniform distribution of the wall material on the surface of the droplets;
[0022] (3) Repeatedly adding the wall material solution to form a multilayer wall material structure. After each addition, the next addition is performed after the wall material solidifies or cross-links on the surface of the droplet.
[0023] Furthermore, the S200 includes:
[0024] S201, using a weighing tool, weighing the raw materials of polyurethane resin, dispersant, defoamer and leveling agent, putting the weighed raw materials into a stirrer, and stirring at a low speed for preliminary mixing to prevent the raw materials from flying and agglomerating;
[0025] S202, increasing the stirring speed to fully mix all the raw materials to form a uniform matrix resin mixture;
[0026] S203, performing viscosity, dispersibility and stability performance tests on the mixed base resin.
[0027] Furthermore, the S300 includes:
[0028] S301, weighing super-hydrophobic nanoparticles, slowly adding the super-hydrophobic nanoparticles to the matrix resin mixture, and simultaneously starting a high-speed disperser, maintaining the dispersion time, so that the nanoparticles are evenly dispersed in the matrix resin to form a stable suspension;
[0029] S302, testing the particle size distribution and stability of the dispersed suspension to ensure that the super-hydrophobic nanoparticles are uniformly and stably dispersed in the matrix resin.
[0030] Furthermore, the specific steps of S302 for testing the particle size distribution of the dispersed suspension are:
[0031] (1) Take a portion of the sample from the dispersed suspension and dilute and process the sample according to the instrument requirements to avoid the influence of particle interactions on the measurement results;
[0032] (2) Place the processed sample in a particle size analyzer, which will automatically measure and record the particle size distribution data of the particles in the suspension;
[0033] (3) Analyze the measured data to understand the particle size distribution range, average particle size and particle size distribution curve information of the particles in the suspension, and evaluate whether the particle size distribution of the suspension meets the requirements based on the analysis results;
[0034] The specific steps of S302 for testing the stability of the dispersed suspension are:
[0035] (1) Place the dispersed suspension in a transparent container and let it stand for a period of time to observe whether the suspension is stratified or precipitated, and record the changes in the suspension during the standing period;
[0036] (2) centrifuging the suspension using a centrifuge, observing the state of the suspension after centrifugation, and recording the stratification of the suspension after centrifugation, the amount of sedimentation, and the clarity of the supernatant;
[0037] (3) Measure the particle size distribution of the suspension before and after the standing or centrifugation test, compare the results of the two measurements, and evaluate the change in the particle size distribution of the suspension during the standing or centrifugation process.
[0038] Furthermore, the S400 includes:
[0039] S401, slowly adding the prepared self-healing microcapsules into the matrix resin mixture containing super-hydrophobic nanoparticles, while starting the agitator and maintaining the stirring speed at a moderate level so that the microcapsules are evenly dispersed in the mixture;
[0040] S402, extending the stirring time to allow the microcapsules and the matrix resin to be fully and evenly mixed to form an anti-icing coating with a self-repairing function;
[0041] S403, test the viscosity, self-healing performance and anti-icing performance of the mixed coating to ensure that the coating meets the requirements.
[0042] Furthermore, the S500 includes:
[0043] S501, cleaning, rust removal and roughening the surface of the wind turbine blade, and evenly coating the prepared coating on the surface of the wind turbine blade by spraying, brushing and dipping, controlling the thickness and uniformity of the coating so that the coating can cover the entire blade surface and achieve the expected protective effect;
[0044] S502, placing the coated blade under curing conditions to allow the resin in the coating to undergo a cross-linking reaction and solidify into a film, and performing a self-repair test;
[0045] S503, conduct appearance inspection, thickness measurement and performance test on the coating after self-repair inspection, and the qualified blades can be put into use or carry out subsequent installation and commissioning work.
[0046] Furthermore, the specific steps of performing the self-repair inspection in S502 are:
[0047] (1) Use mechanical scratching, notching, impact and laser ablation methods to accurately simulate different types of micro cracks or damage on the coating surface;
[0048] (2) Subjecting damaged coating samples to preset environmental conditions, including specific temperature, humidity, light intensity, and cyclic temperature changes, to simulate the environmental factors encountered by the coating in actual use;
[0049] (3) Use a microscope, scanning electron microscope, and infrared spectrometer to regularly observe and record the self-healing process of the coating damage;
[0050] (4) Organize and analyze the observation records to evaluate the self-healing efficiency of the coating, the durability and stability of the repaired coating, and whether it meets the expected performance requirements.
[0051] Compared with the prior art, the new coating for enhancing the anti-icing performance of wind turbine blades has the following beneficial effects:
[0052] 1. The present invention integrates self-repairing microcapsules to achieve the automatic repair function of the coating when tiny cracks or damage occur. When the coating is damaged, the microcapsules will rupture to release the polyurethane prepolymer and catalyst inside. The catalyst promotes the polymerization reaction of the prepolymer, thereby filling the cracks and restoring the integrity of the coating, effectively extending the service life of the coating, reducing the frequent maintenance and replacement requirements caused by coating damage, and reducing the maintenance cost of wind turbine blades.
[0053] 2. The present invention adds super-hydrophobic nanoparticles to the coating, making it difficult for water droplets to adhere to the surface of the blades, and more likely to form spheres and slide down quickly, thereby effectively reducing the adhesion and accumulation of ice and snow on the surface of the blades. It not only reduces the weight burden of the blades, but also avoids the negative impact of ice and snow on the aerodynamic performance of the blades, thereby improving the power generation efficiency and reliability of wind turbine blades.
[0054] Other advantages, objectives and features of the present invention will be set forth in part in the following description and, in part, will be apparent to those skilled in the art based on an examination of the following or may be taught from the practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0056] Figure 1This is an operation diagram of a new coating process for enhancing the anti-icing performance of wind turbine blades.
[0057] Figure 2 A flow chart of a new coating for enhancing the ice resistance of wind turbine blades. DETAILED DESCRIPTION
[0058] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0059] Embodiment 1
[0060] This embodiment describes in detail a preparation process of a new coating for enhancing the anti-icing performance of wind turbine blades.
[0061] First, in the stage of preparing self-healing microcapsules (S100), polyurethane prepolymer, catalyst and appropriate amount of organic solvent are mixed in an emulsifier, and a stable emulsion is formed by high-speed shearing and stirring. The wall material precursor is formed into a uniform film on the surface of the droplet by a layer-by-layer deposition method. The thickness and uniformity of the wall material are adjusted by controlling the concentration, droplet addition speed and stirring intensity parameters of the precursor. Then, the pH value of the emulsion is adjusted to an appropriate range, and the temperature is increased to the cross-linking reaction temperature of the wall material precursor. Under this condition, the wall material precursor undergoes a cross-linking reaction to form a solid microcapsule wall. The microcapsules are separated from the suspension by a centrifuge, and the residual solvent and unreacted wall material precursor are removed by washing. Finally, the microcapsules are dried to a suitable moisture content using a spray dryer, and the size, distribution and self-healing performance of the prepared microcapsules are inspected using tools such as a microscope and a particle size analyzer, and microcapsules that meet the requirements are screened out for use.
[0062] Secondly, in the stage of preparing the matrix resin mixture (S200), use an electronic scale to accurately weigh each raw material, put it into the blender in a certain proportion, first stir it at a low speed to make the raw materials initially mixed evenly, increase the stirring speed to make all the raw materials fully mixed to form a uniform matrix resin mixture, and test the viscosity, dispersibility and stability of the mixed matrix resin to ensure that the quality of the mixture is qualified and there is no stratification, precipitation and the like.
[0063] Then, in the super-hydrophobic additive addition stage (S300), weigh an appropriate amount of super-hydrophobic nanoparticles, slowly add them to the matrix resin mixture, pay attention to avoid too much one-time addition to cause agglomeration, start a high-speed disperser or ultrasonic disperser, and disperse the mixture containing the nanoparticles, maintain appropriate dispersion time and intensity, so that the nanoparticles are evenly dispersed in the matrix resin, and the suspended liquid after dispersion is subjected to particle size distribution and stability test to ensure that the nanoparticles are evenly and stably dispersed in the matrix resin.
[0064] Next, in the stage of incorporating self-healing microcapsules (S400), the prepared self-healing microcapsules are slowly added to the matrix resin mixture containing super-hydrophobic nanoparticles in a certain proportion, the agitator is started, the stirring speed is maintained at a moderate level, the microcapsules are evenly dispersed in the mixture, the stirring time is appropriately extended to ensure that the microcapsules and the matrix resin are fully mixed, the viscosity, self-healing performance and anti-icing performance of the mixed coating are tested, and whether the self-healing effect and anti-icing performance of the coating meet the requirements are evaluated through simulated scratch experiments and low-temperature icing test methods.
[0065] Finally, in the coating and curing stage (S500), the surface of the wind turbine blade is thoroughly cleaned, rust-removed and roughened to improve the adhesion and durability of the coating. The prepared coating is evenly coated on the surface of the wind turbine blade by spraying, brushing or dipping. Attention is paid to controlling the thickness and uniformity of the coating to avoid problems caused by missing coating or excessive coating thickness. Appropriate curing conditions are selected according to the characteristics of the coating and the material of the wind turbine blade. The coated blade is placed under the set curing conditions for curing treatment, so that the resin in the coating undergoes a cross-linking reaction and solidifies into a film, forming an anti-icing coating with self-repairing function. The cured coating is subjected to appearance inspection, thickness measurement and performance testing (such as adhesion test, weather resistance test, etc.). Acceptable blades can be put into use or undergo subsequent installation and commissioning.
[0066] In summary, this embodiment prepares a new type of coating for enhancing the anti-icing performance of wind turbine blades. By integrating self-repairing microcapsules, the coating realizes the automatic repair function when damaged. At the same time, the addition of superhydrophobic nanoparticles gives the coating excellent superhydrophobic properties, making it difficult for water droplets to stay on the surface of the blades, effectively reducing the adhesion and accumulation of ice and snow.
[0067] Embodiment 2
[0068] This embodiment describes in detail a specific process for preparing self-repairing microcapsules of a new type of coating for enhancing the anti-icing performance of wind turbine blades.
[0069] For the selection and preparation of materials, the polyurethane prepolymer selects highly reactive isocyanate-based polyurethane prepolymer as the core material to ensure that it has good mechanical properties and self-healing potential after curing. The catalyst selects an organic tin catalyst, which is widely used in the synthesis of polyurethane prepolymers and the curing process of microcapsules to accelerate the cross-linking reaction of polyurethane. The wall material precursor selects a mixture of gelatin and gum arabic. The mixture of the two can form a tough microcapsule wall with a certain elasticity.
[0070] For the emulsification process, before emulsification, ensure that all equipment is clean and oil-free to avoid unnecessary pollution during the emulsification process. During emulsification, gradually add polyurethane prepolymer, catalyst and organic solvent, and adjust the speed of the emulsifier at the same time to obtain an emulsion with uniform particle size and stability. The stability of the emulsion can be judged by observing its fluidity and appearance.
[0071] For the generation of wall material thin film, the layer-by-layer deposition method is used to make the wall material precursor form a uniform thin film on the surface of the droplet. The thickness and uniformity of the wall material are adjusted by controlling the concentration of the precursor, the droplet acceleration and the stirring intensity parameters. The specific steps of the layer-by-layer deposition method are as follows:
[0072] (1) Slowly and evenly adding the wall material precursor solution into the emulsion or dispersion through a dropping device. The dropping speed needs to be precisely controlled so that the wall material is evenly deposited on the droplet surface;
[0073] (2) During the dropwise addition process, the stirrer is kept at an appropriate speed to keep the droplets suspended under stirring and promote the uniform distribution of the wall material on the droplet surface;
[0074] (3) Repeatedly adding the wall material solution to form a multilayer wall material structure. After each addition, wait for the wall material to solidify or cross-link on the surface of the droplet before adding the wall material again.
[0075] For the control of cross-linking reaction conditions, the pH value and temperature need to be precisely controlled to ensure that the wall material precursor undergoes a cross-linking reaction under appropriate conditions. Too high or too low a temperature may affect the speed and quality of the cross-linking reaction. During the reaction, samples can be taken regularly to observe the morphology and structural changes of the microcapsules in order to adjust the reaction conditions.
[0076] For separation and drying, during centrifugal separation, the appropriate centrifugal speed and time should be selected to completely separate the microcapsules and the suspension. During the washing process, deionized water or pure water should be used for multiple washings to completely remove the residual solvent and unreacted wall material precursors. During spray drying, the drying temperature, wind speed and spray speed need to be controlled to avoid deformation or rupture of the microcapsules.
[0077] In summary, this embodiment prepares a self-repairing microcapsule for a new type of coating for enhancing the anti-icing performance of wind turbine blades, thereby realizing the automatic repair function of the coating when damaged.
[0078] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A new type of coating for enhancing the anti-icing performance of wind turbine blades, characterized in that: The preparation method of the coating is: S100, preparation of self-healing microcapsules: polyurethane prepolymer and catalyst are encapsulated in microcapsules by emulsion polymerization, and the size and distribution of microcapsules are controlled; S200, mixing base resin and additives: uniformly mixing polyurethane resin, dispersant, defoamer and leveling agent in a certain proportion to form a base resin mixture; S300, adding super-hydrophobic additives: adding super-hydrophobic nanoparticles into the matrix resin mixture, and uniformly dispersing the nanoparticles by high-speed dispersion or ultrasonic treatment; S400, incorporating self-repairing microcapsules: adding the prepared self-repairing microcapsules into the mixture in a certain proportion, and continuing to stir and mix evenly to obtain an anti-icing coating with a self-repairing function; S500, coating and curing: The coating is applied to the surface of the wind turbine blade by spraying, brushing and dipping, and after curing conditions, an anti-icing coating with self-repairing function is formed.
2. The novel coating for enhancing the anti-icing performance of wind turbine blades according to claim 1 is characterized in that: The S100 includes: S101, selecting a polyurethane prepolymer and a catalyst, and preparing a precursor of a microcapsule wall material, and selecting the wall material according to the desired performance of the microcapsule; S102, using an emulsifier to mix the polyurethane prepolymer, the catalyst and the organic solvent to form a stable emulsion; S103, using a layer-by-layer deposition method to make the wall material precursor form a uniform thin film on the surface of the droplet, and adjusting the thickness and uniformity of the wall material by controlling the concentration of the precursor, the dropping speed and the stirring intensity parameters; S104, adjusting the pH value and temperature to promote the cross-linking reaction of the wall material precursor to form a strong microcapsule wall, separating the microcapsules from the suspension by centrifugation, filtration and spray drying, and washing and drying; S105, inspecting the size, distribution and self-healing performance of the prepared microcapsules, screening out qualified microcapsules, and preparing for subsequent coating preparation.
3. The novel coating for enhancing the anti-icing performance of wind turbine blades according to claim 2 is characterized in that: In the S101, the polyurethane prepolymer is an isocyanate-based polyurethane prepolymer, the catalyst is an organic tin catalyst, which is widely used in the synthesis of polyurethane prepolymers and the curing process of microcapsules, and the wall material precursor is a mixture of gelatin and gum arabic, which can form a tough microcapsule wall with a certain elasticity.
4. The novel coating for enhancing the anti-icing performance of wind turbine blades according to claim 2 is characterized in that: The specific steps of using the layer-by-layer deposition method in S103 to form a uniform thin film of the wall material precursor on the surface of the droplet are: (1) Slowly and evenly adding the wall material precursor solution into the emulsion or dispersion through a dropping device. The dropping speed needs to be precisely controlled so that the wall material is evenly deposited on the droplet surface; (2) During the dropwise addition process, the speed of the stirrer is maintained to keep the droplets in suspension under the stirring action and promote the uniform distribution of the wall material on the surface of the droplets; (3) Repeatedly adding the wall material solution to form a multilayer wall material structure. After each addition, the next addition is performed after the wall material solidifies or cross-links on the surface of the droplet.
5. The novel coating for enhancing the anti-icing performance of wind turbine blades according to claim 1 is characterized in that: The S200 includes: S201, using a weighing tool, weighing the raw materials of polyurethane resin, dispersant, defoamer and leveling agent, putting the weighed raw materials into a stirrer, and stirring at a low speed for preliminary mixing to prevent the raw materials from flying and agglomerating; S202, increasing the stirring speed to fully mix all the raw materials to form a uniform matrix resin mixture; S203, performing viscosity, dispersibility and stability performance tests on the mixed base resin.
6. The novel coating for enhancing the anti-icing performance of wind turbine blades according to claim 1 is characterized in that: The S300 includes: S301, weighing super-hydrophobic nanoparticles, slowly adding the super-hydrophobic nanoparticles to the matrix resin mixture, and simultaneously starting a high-speed disperser, maintaining the dispersion time, so that the nanoparticles are evenly dispersed in the matrix resin to form a stable suspension; S302, testing the particle size distribution and stability of the dispersed suspension to ensure that the super-hydrophobic nanoparticles are uniformly and stably dispersed in the matrix resin.
7. The novel coating for enhancing the anti-icing performance of wind turbine blades according to claim 6 is characterized in that: The specific steps of S302 for testing the particle size distribution of the dispersed suspension are: (1) Take a portion of the sample from the dispersed suspension and dilute and process the sample according to the instrument requirements to avoid the influence of particle interactions on the measurement results; (2) Place the processed sample in a particle size analyzer, which will automatically measure and record the particle size distribution data of the particles in the suspension; (3) Analyze the measured data to understand the particle size distribution range, average particle size and particle size distribution curve information of the particles in the suspension, and evaluate whether the particle size distribution of the suspension meets the requirements based on the analysis results; The specific steps of S302 for testing the stability of the dispersed suspension are: (1) Place the dispersed suspension in a transparent container and let it stand for a period of time to observe whether the suspension is stratified or precipitated, and record the changes in the suspension during the standing period; (2) centrifuging the suspension using a centrifuge, observing the state of the suspension after centrifugation, and recording the stratification of the suspension after centrifugation, the amount of sedimentation, and the clarity of the supernatant; (3) Measure the particle size distribution of the suspension before and after the standing or centrifugation test, compare the results of the two measurements, and evaluate the change in the particle size distribution of the suspension during the standing or centrifugation process.
8. A novel coating for enhancing the anti-icing performance of wind turbine blades according to claim 1, characterized in that: The S400 includes: S401, slowly adding the prepared self-healing microcapsules into the matrix resin mixture containing super-hydrophobic nanoparticles, while starting the agitator and maintaining the stirring speed at a moderate level so that the microcapsules are evenly dispersed in the mixture; S402, extending the stirring time to allow the microcapsules and the matrix resin to be fully and evenly mixed to form an anti-icing coating with a self-repairing function; S403, test the viscosity, self-healing performance and anti-icing performance of the mixed coating to ensure that the coating meets the requirements.
9. The novel coating for enhancing the anti-icing performance of wind turbine blades according to claim 1 is characterized in that: The S500 includes: S501, cleaning, rust removal and roughening the surface of the wind turbine blade, and evenly coating the prepared coating on the surface of the wind turbine blade by spraying, brushing and dipping, controlling the thickness and uniformity of the coating so that the coating can cover the entire blade surface and achieve the expected protective effect; S502, placing the coated blade under curing conditions to allow the resin in the coating to undergo a cross-linking reaction and solidify into a film, and performing a self-repair test; S503, conduct appearance inspection, thickness measurement and performance test on the coating after self-repair inspection, and the qualified blades can be put into use or carry out subsequent installation and commissioning work.
10. The novel coating for enhancing the anti-icing performance of wind turbine blades according to claim 9, characterized in that: The specific steps of performing the self-repair test in S502 are: (1) Use mechanical scratching, notching, impact and laser ablation methods to accurately simulate different types of micro cracks or damage on the coating surface; (2) Subjecting damaged coating samples to preset environmental conditions, including specific temperature, humidity, light intensity, and cyclic temperature changes, to simulate the environmental factors encountered by the coating in actual use; (3) Use a microscope, scanning electron microscope, and infrared spectrometer to regularly observe and record the self-healing process of the coating damage; (4) Organize and analyze the observation records to evaluate the self-healing efficiency of the coating, the durability and stability of the repaired coating, and whether it meets the expected performance requirements.
Citation Information
Patent Citations
Self-repairing water-based super-hydrophobic coating based on microcapsule type and preparing method thereof
CN105885679A
Self-healing polyurethane nano-micro capsules for automotive painting
CN108329743A
Self-repairing anticorrosive outdoor building graphene coating and preparation method thereof
CN108912870A
Natural water-based antifouling coating and preparation method thereof as well as antifouling agent microcapsule and preparation method thereof
CN113426387A