A method for preparing anti-ultraviolet polymer self-adhesive waterproof coiled material

By using phosphorus-containing bisphenylketone vinyl triazine as an ultraviolet-resistant monomer and flame retardant monomer in the waterproof coil, modifying polyethylene and combining it with other materials, the aging of the waterproof coil under ultraviolet radiation is solved. Problem, significantly improving UV resistance and flame retardant properties and extending service life.

CN118772792BActive Publication Date: 2024-11-19BEIXIN YUWANG WATERPROOF TECH (ANHUI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411263734.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-19
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

The existing waterproof coils prepared by polyolefins age under ultraviolet radiation, resulting in a shortened service life. The traditional benzophenone ultraviolet absorbers are easy to volatilize and precipitate, making it difficult to improve their UV resistance.

Method used

The phosphorus-containing bisphenyl ketone vinyl triazine is used as the anti-ultraviolet monomer and flame retardant monomer, and the polyethylene is modified through grafting reaction, and combined with polyethylene, antioxidants, stearic acid, titanium dioxide, etc. Prepare anti-ultraviolet polymer self-adhesive waterproof coils.

Benefits of technology

It significantly improves the UV resistance and flame retardant properties of the waterproof coil, extends the service life, and reduces the precipitation of monomers during processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_5
    Figure SMS_5
  • Figure SMS_6
    Figure SMS_6
  • Figure QLYQS_1
    Figure QLYQS_1
Patent Text Reader

Abstract

The invention relates to the technical field of waterproof coiled materials, and discloses a method for preparing an anti-ultraviolet polymer self-adhesive waterproof coiled material. The invention uses 2,4-dihydroxybenzophenone and 2-bromo-N-(bromoethyl)ethylamine to react to obtain an intermediate 1. The invention uses cyanuric chloride as an intermediate reactant to react with the intermediate 1, pentaerythritol phosphate and 3-butene-1-amine in sequence to obtain phosphorus-containing bis-diphenyl ketone vinyl triazine, and the phosphorus-containing bis-diphenyl ketone vinyl triazine is grafted with maleic anhydride and polyethylene under the initiation of diisopropylbenzene peroxide to obtain modified polyethylene. Finally, the polyethylene, the modified polyethylene, an antioxidant and the like are uniformly mixed, molded, and a layer of SIS hot-melt pressure-sensitive adhesive is coated on the surface to obtain an anti-ultraviolet polymer self-adhesive waterproof coiled material. The invention prepares the modified polyethylene, which has good compatibility with polyethylene, reduces the precipitation phenomenon of benzophenone and pentaerythritol phosphate, and increases the anti-ultraviolet ability and flame retardant effect of the waterproof coiled material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterproof coiled materials, in particular to a method for preparing an anti-ultraviolet polymer self-adhesive waterproof coiled material. Background Art

[0002] Self-adhesive waterproofing membranes generally include self-adhesive polymer modified asphalt waterproofing membranes and waterproofing membranes with self-adhesive layers. They have the advantages of pressure sensitivity, waterproofness, environmental protection and safety, and are widely used in my country's civil engineering, subway tunnels, bridge deck waterproofing and other fields. Polyolefin plastics such as polyethylene, polypropylene, and thermoplastic polyolefins have good physical and mechanical properties and are often used as the base material of self-adhesive waterproofing membranes. However, waterproofing membranes prepared from polyolefins will produce free radicals under the action of ultraviolet radiation, which will lead to aging of the waterproofing membranes and shorten their service life. Therefore, how to improve the UV resistance of waterproofing membranes is a hot topic in current research.

[0003] Among common UV absorbers, benzophenone UV absorbers are widely used due to their low price and good UV absorption performance. However, traditional benzophenone has the characteristics of small molecular weight, easy volatility and easy precipitation, which is not conducive to the improvement of UV resistance. Therefore, it is necessary to improve the precipitation resistance of benzophenone. Phosphate flame retardants are the main types of organophosphorus flame retardants. Pentaerythritol phosphate (PEPA) is a phosphate flame retardant with good flame retardant performance, which is widely used in various flame retardant and fireproof fields.

[0004] For example, the patent application publication number CN111117057A discloses an antistatic, anti-UV polymer self-adhesive film waterproofing membrane. The invention uses polyethylene, antioxidants, etc. as raw materials to prepare a waterproofing membrane with good antistatic properties, but does not improve the flame retardant properties of the waterproofing membrane. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing an anti-ultraviolet polymer self-adhesive waterproof roll. The phosphorus-containing bis(diphenyl ketone) vinyl triazine of the present invention contains an anti-ultraviolet monomer and a flame retardant monomer. The prepared polymer self-adhesive waterproof roll has good anti-ultraviolet performance and flame retardant performance.

[0006] The present invention is implemented by the following technical solutions:

[0007] The present invention discloses a method for preparing an anti-ultraviolet polymer self-adhesive waterproof coiled material, and the specific operations are as follows:

[0008] (1) Add maleic anhydride, phosphorus-containing bis(diphenyl ketone) vinyl triazine and diisopropylbenzene peroxide into polyethylene, stir and mix evenly, and carry out grafting reaction in a torque rheometer at 190-210°C, with a rotation speed of 40-60 r / min and a grafting time of 10-20 min to obtain modified polyethylene.

[0009] (2) Add polyethylene, modified polyethylene, antioxidant, stearic acid and titanium dioxide into the rheometer, mix them evenly at 160-180°C, and then place them on a molding machine for compression molding. The molding temperature is controlled at 210°C. After molding, apply a layer of SIS hot melt pressure sensitive adhesive on the surface. The coating temperature is 140°C and the coating thickness is 0.4mm to obtain an anti-UV polymer self-adhesive waterproof membrane.

[0010] More preferably, the mass ratio of maleic anhydride, phosphorus-containing bis(diphenyl ketone) vinyl triazine, dicumyl peroxide and polyethylene is 2-4:1-3:0.5-2:100.

[0011] Further preferably, the mass ratio of polyethylene, modified polyethylene, antioxidant, stearic acid and titanium dioxide is 100:80-120:0.2-0.5:0.5-1:1.5-3.

[0012] Preferably, the preparation method of phosphorus-containing bis(diphenyl ketone) vinyl triazine is:

[0013] S1: Under nitrogen conditions, 2,4-dihydroxybenzophenone was added to a 1-2 mol / L sodium hydroxide aqueous solution, stirred to dissolve, and then 2-bromo-N-(bromoethyl)ethylamine was added thereto, and the reaction was carried out at 80-95°C for 3-6 hours. After the reaction was completed, the mixture was washed with deionized water and dried to obtain intermediate 1, whose reaction formula is .

[0014] S2: Add cyanuric chloride to acetone solvent, stir to dissolve, then add intermediate 1 and 10% sodium hydroxide aqueous solution, react at 0-5°C for 4-8h, distill under reduced pressure, wash with deionized water, and dry to obtain intermediate 2, whose reaction formula is: .

[0015] S3: Add intermediate 2 and pentaerythritol phosphate to acetone solvent, stir and disperse, then add triethylamine, react at 20-35°C for 2-4h, and after the reaction, distill under reduced pressure, wash with deionized water, and dry to obtain intermediate 3, whose reaction formula is: .

[0016] S4: Add intermediate 3 to acetone solvent, stir and disperse, add 3-butene-1-amine at 0-5°C, adjust the pH to 7-8 with saturated sodium carbonate, react for 1-3h, heat to 40-55°C, adjust the pH to 8-9 with saturated sodium carbonate, continue to react for 5-10h, filter, distill under reduced pressure, wash with deionized water, and dry to obtain phosphorus-containing bis(diphenyl ketone) vinyl triazine, whose reaction formula is: .

[0017] More preferably, the molar ratio of 2,4-dihydroxybenzophenone to 2-bromo-N-(bromoethyl)ethylamine is 0.8-1.4:1.

[0018] More preferably, the molar ratio of cyanuric chloride to intermediate 1 is 1:1.

[0019] More preferably, the molar ratio of intermediate 2, pentaerythritol phosphate and triethylamine is 1:1:1-1.5.

[0020] More preferably, the molar ratio of the intermediate 3 to 3-butene-1-amine is 1:1-1.5.

[0021] Compared with the prior art, the present invention has the following advantages:

[0022] (1) The phosphorus-containing bis(diphenyl ketone) vinyl triazine prepared by a series of reactions of the present invention has a novel structure and a simple preparation method. The bis(diphenyl ketone) anti-ultraviolet structure and the pentaerythritol phosphate flame retardant structure contained therein are used as raw materials to prepare a waterproof roll material having good flame retardant and anti-ultraviolet properties. In addition, the anti-ultraviolet effect of the bis(diphenyl ketone) anti-ultraviolet structure contained therein is better than that of a single anti-ultraviolet structure.

[0023] (2) The present invention grafts phosphorus-containing bis(diphenyl ketone) vinyl triazine and maleic anhydride into polyethylene, blends them with polyethylene, and evenly distributes them in the waterproof membrane, thereby increasing the compatibility of the monomer structure with polyethylene, reducing the precipitation of the monomer structure during use or processing, increasing the durability of the waterproof membrane, and further improving the anti-ultraviolet effect and flame retardant effect of the waterproof membrane. DETAILED DESCRIPTION

[0024] The following is a further description of the anti-ultraviolet polymer self-adhesive waterproofing membrane of the present invention in conjunction with some specific embodiments. The specific embodiments are for further illustrating the present invention in detail, but do not limit the protection scope of the present invention.

[0025] Antioxidant: 1010 antioxidant. Embodiment 1

[0026] (1) Under nitrogen conditions, 28 mmol of 2,4-dihydroxybenzophenone was added to 20 mL of 1 mol / L sodium hydroxide aqueous solution and stirred to dissolve. Then, 20 mmol of 2-bromo-N-(bromoethyl)ethylamine was added thereto and reacted at 95°C for 5 h. After the reaction was completed, the mixture was washed with deionized water and dried to obtain intermediate 1.

[0027] (2) Add 20 mmol of cyanuric chloride to 50 mL of acetone solvent and stir to dissolve. Then add 20 mmol of intermediate 1 and 10 mL of 10% sodium hydroxide aqueous solution. React at 5 °C for 6 h. Distill under reduced pressure, wash with deionized water and dry to obtain intermediate 2.

[0028] (3) 50 mmol of intermediate 2 and 50 mmol of pentaerythritol phosphate were added to 100 mL of acetone solvent, stirred and dispersed, and then 50 mmol of triethylamine was added thereto. The mixture was reacted at 35°C for 3 h. After the reaction was completed, it was distilled under reduced pressure, washed with deionized water, and dried to obtain intermediate 3.

[0029] (4) Add 40 mmol of intermediate 3 to 100 mL of acetone solvent and stir to disperse. Then add 40 mmol of 3-butene-1-amine at 0°C, adjust the pH to 7 with saturated sodium carbonate, react for 3 h, heat to 40°C, adjust the pH to 8 with saturated sodium carbonate, and continue to react for 5 h. After the reaction is completed, filter, evaporate under reduced pressure, wash with deionized water, and dry to obtain phosphorus-containing bis(diphenyl ketone) vinyl triazine.

[0030] (5) Add 1.2 g of maleic anhydride, 1.8 g of phosphorus-containing bis(diphenyl ketone) vinyl triazine, and 1.2 g of diisopropylbenzene peroxide into 60 g of polyethylene, stir and mix well, and carry out grafting reaction in a torque rheometer at 200°C, with a rotation speed of 50 r / min and a grafting time of 15 min to obtain modified polyethylene.

[0031] (6) Add 50 g of polyethylene, 40 g of modified polyethylene, 0.1 g of antioxidant, 0.5 g of stearic acid, and 1.2 g of titanium dioxide into a rheometer, mix them evenly at 170 °C, and then place them on a molding machine for compression molding. Control the molding temperature to be 210 °C. After molding, apply a layer of SIS hot melt pressure sensitive adhesive on its surface. The coating temperature is 140 °C and the coating thickness is 0.4 mm to obtain an anti-UV polymer self-adhesive waterproof membrane. Embodiment 2

[0032] (1) Under nitrogen conditions, 20 mmol of 2,4-dihydroxybenzophenone was added to 20 mL of 1.5 mol / L sodium hydroxide aqueous solution and stirred to dissolve. Then, 20 mmol of 2-bromo-N-(bromoethyl)ethylamine was added thereto and reacted at 85°C for 6 h. After the reaction was completed, the mixture was washed with deionized water and dried to obtain intermediate 1.

[0033] (2) Add 20 mmol of cyanuric chloride to 50 mL of acetone solvent and stir to dissolve. Then add 20 mmol of intermediate 1 and 10 mL of 10% sodium hydroxide aqueous solution. React at 5 °C for 6 h. Distill under reduced pressure, wash with deionized water and dry to obtain intermediate 2.

[0034] (3) 50 mmol of intermediate 2 and 50 mmol of pentaerythritol phosphate were added to 100 mL of acetone solvent, stirred and dispersed, and then 65 mmol of triethylamine was added thereto. The reaction was carried out at 25°C for 4 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with deionized water, and dried to obtain intermediate 3.

[0035] (4) Add 40 mmol of intermediate 3 to 100 mL of acetone solvent and stir to disperse. Then add 60 mmol of 3-butene-1-amine at 5°C, adjust the pH to 8 with saturated sodium carbonate, react for 2 h, heat to 40°C, adjust the pH to 9 with saturated sodium carbonate, and continue to react for 10 h. After the reaction is completed, filter, evaporate under reduced pressure, wash with deionized water, and dry to obtain phosphorus-containing bis(diphenyl ketone) vinyl triazine.

[0036] (5) Add 2 g of maleic anhydride, 1 g of phosphorus-containing bis(diphenyl ketone) vinyl triazine, and 0.3 g of diisopropylbenzene peroxide into 60 g of polyethylene, stir and mix well, and carry out grafting reaction in a torque rheometer at 210°C, with a rotation speed of 60 r / min and a grafting time of 10 min to obtain modified polyethylene.

[0037] (6) Add 50 g of polyethylene, 45 g of modified polyethylene, 0.25 g of antioxidant, 0.4 g of stearic acid, and 1.5 g of titanium dioxide into a rheometer, mix them evenly at 180 °C, and then place them on a molding machine for compression molding. Control the molding temperature to be 210 °C. After molding, apply a layer of SIS hot melt pressure sensitive adhesive on its surface. The coating temperature is 140 °C and the coating thickness is 0.4 mm to obtain an anti-UV polymer self-adhesive waterproof membrane. Embodiment 3

[0038] (1) Under nitrogen conditions, 16 mmol of 2,4-dihydroxybenzophenone was added to 20 mL of 2 mol / L sodium hydroxide aqueous solution and stirred to dissolve. Then, 20 mmol of 2-bromo-N-(bromoethyl)ethylamine was added thereto and reacted at 80°C for 3 h. After the reaction was completed, the mixture was washed with deionized water and dried to obtain intermediate 1.

[0039] (2) Add 20 mmol of cyanuric chloride to 50 mL of acetone solvent and stir to dissolve. Then add 20 mmol of intermediate 1 and 10 mL of 10% sodium hydroxide aqueous solution. React at 5 °C for 4 h. Distill under reduced pressure, wash with deionized water and dry to obtain intermediate 2.

[0040] (3) 50 mmol of intermediate 2 and 50 mmol of pentaerythritol phosphate were added to 100 mL of acetone solvent, stirred and dispersed, and then 50 mmol of triethylamine was added thereto. The reaction was carried out at 35° C. for 4 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with deionized water, and dried to obtain intermediate 3.

[0041] (4) Add 40 mmol of intermediate 3 to 100 mL of acetone solvent and stir to disperse. Then add 50 mmol of 3-butene-1-amine at 0°C and adjust the pH to 7 with saturated sodium carbonate. The reaction is carried out for 1 h. The temperature is raised to 45°C and the pH is adjusted to 9 with saturated sodium carbonate. The reaction is continued for 6 h. After the reaction is completed, the mixture is filtered, evaporated under reduced pressure, washed with deionized water and dried to obtain phosphorus-containing bis(diphenyl ketone) vinyl triazine.

[0042] (5) Add 2.4 g of maleic anhydride, 0.6 g of phosphorus-containing bis(diphenyl ketone) vinyl triazine, and 1 g of diisopropylbenzene peroxide to 60 g of polyethylene, stir and mix well, and carry out grafting reaction in a torque rheometer at 190°C, with a rotation speed of 40 r / min and a grafting time of 20 min to obtain modified polyethylene.

[0043] (6) Add 50 g of polyethylene, 50 g of modified polyethylene, 0.2 g of antioxidant, 0.25 g of stearic acid and 0.75 g of titanium dioxide into a rheometer, mix them evenly at 160 °C, and then place them on a molding machine for compression molding. Control the molding temperature to be 210 °C. After molding, apply a layer of SIS hot melt pressure sensitive adhesive on its surface. The coating temperature is 140 °C and the coating thickness is 0.4 mm to obtain an anti-UV polymer self-adhesive waterproof membrane. Embodiment 4

[0044] (1) Under nitrogen conditions, 25 mmol of 2,4-dihydroxybenzophenone was added to 20 mL of 1.5 mol / L sodium hydroxide aqueous solution and stirred to dissolve. Then, 20 mmol of 2-bromo-N-(bromoethyl)ethylamine was added thereto and reacted at 85°C for 5 h. After the reaction was completed, the mixture was washed with deionized water and dried to obtain intermediate 1.

[0045] (2) Add 20 mmol of cyanuric chloride to 50 mL of acetone solvent and stir to dissolve. Then add 20 mmol of intermediate 1 and 10 mL of 10% sodium hydroxide aqueous solution. React at 0°C for 8 h. Distill under reduced pressure, wash with deionized water and dry to obtain intermediate 2.

[0046] (3) 50 mmol of intermediate 2 and 50 mmol of pentaerythritol phosphate were added to 100 mL of acetone solvent, stirred and dispersed, and then 60 mmol of triethylamine was added thereto. The mixture was reacted at 20°C for 2 h. After the reaction was completed, it was evaporated under reduced pressure, washed with deionized water, and dried to obtain intermediate 3.

[0047] (4) Add 40 mmol of intermediate 3 to 100 mL of acetone solvent and stir to disperse. Then add 50 mmol of 3-butene-1-amine at 5°C and adjust the pH to 7 with saturated sodium carbonate. The reaction is carried out for 2 h. The temperature is raised to 45°C and the pH is adjusted to 8 with saturated sodium carbonate. The reaction is continued for 6 h. After the reaction is completed, the mixture is filtered, evaporated under reduced pressure, washed with deionized water and dried to obtain phosphorus-containing bis(diphenyl ketone) vinyl triazine.

[0048] (5) Add 2.4 g of maleic anhydride, 0.6 g of phosphorus-containing bis(diphenyl ketone) vinyl triazine, and 1.2 g of diisopropylbenzene peroxide to 60 g of polyethylene, stir and mix well, and carry out grafting reaction in a torque rheometer at 210°C, with a rotation speed of 50 r / min and a grafting time of 10 min to obtain modified polyethylene.

[0049] (6) Add 50 g of polyethylene, 55 g of modified polyethylene, 0.15 g of antioxidant, 0.3 g of stearic acid, and 1.5 g of titanium dioxide into a rheometer, mix them evenly at 170 °C, and then place them on a molding machine for compression molding. Control the molding temperature to be 210 °C. After molding, apply a layer of SIS hot melt pressure sensitive adhesive on its surface. The coating temperature is 140 °C and the coating thickness is 0.4 mm to obtain an anti-UV polymer self-adhesive waterproof membrane. Embodiment 5

[0050] (1) Under nitrogen conditions, 20 mmol of 2,4-dihydroxybenzophenone was added to 20 mL of 2 mol / L sodium hydroxide aqueous solution and stirred to dissolve. Then, 20 mmol of 2-bromo-N-(bromoethyl)ethylamine was added thereto and reacted at 85°C for 4 h. After the reaction was completed, the mixture was washed with deionized water and dried to obtain intermediate 1.

[0051] (2) Add 20 mmol of cyanuric chloride to 50 mL of acetone solvent and stir to dissolve. Then add 20 mmol of intermediate 1 and 10 mL of 10% sodium hydroxide aqueous solution. React at 5 °C for 5 h. Distill under reduced pressure, wash with deionized water and dry to obtain intermediate 2.

[0052] (3) 50 mmol of intermediate 2 and 50 mmol of pentaerythritol phosphate were added to 100 mL of acetone solvent, stirred and dispersed, and then 75 mmol of triethylamine was added thereto. The reaction was carried out at 25°C for 4 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with deionized water, and dried to obtain intermediate 3.

[0053] (4) 40 mmol of intermediate 3 was added to 100 mL of acetone solvent and stirred for dispersion. At 0°C, 60 mmol of 3-butene-1-amine was added thereto. The pH was adjusted to 8 using saturated sodium carbonate. The reaction was carried out for 2 h. The temperature was raised to 45°C. The pH was adjusted to 9 using saturated sodium carbonate. The reaction was continued for 6 h. After the reaction was completed, the mixture was filtered, evaporated under reduced pressure, washed with deionized water, and dried to obtain phosphorus-containing bis(diphenyl ketone) vinyl triazine.

[0054] (5) Add 2.2 g of maleic anhydride, 1.5 g of phosphorus-containing bis(diphenyl ketone) vinyl triazine, and 1 g of diisopropylbenzene peroxide to 60 g of polyethylene, stir and mix well, and carry out grafting reaction in a torque rheometer at 200°C, with a rotation speed of 60 r / min and a grafting time of 10 min to obtain modified polyethylene.

[0055] (6) Add 50 g of polyethylene, 60 g of modified polyethylene, 0.1 g of antioxidant, 0.5 g of stearic acid, and 1.2 g of titanium dioxide into a rheometer, mix them evenly at 170 °C, and then place them on a molding machine for compression molding. Control the molding temperature to be 210 °C. After molding, apply a layer of SIS hot melt pressure sensitive adhesive on its surface. The coating temperature is 140 °C and the coating thickness is 0.4 mm to obtain an anti-UV polymer self-adhesive waterproof membrane.

[0056] Comparative Example 1

[0057] (1) Add 2 g of maleic anhydride and 0.3 g of diisopropylbenzene peroxide to 60 g of polyethylene, stir and mix well, and carry out grafting reaction in a torque rheometer at 210°C, with a rotation speed of 60 r / min and a grafting time of 10 min to obtain modified polyethylene.

[0058] (2) Add 50 g of polyethylene, 45 g of modified polyethylene, 0.25 g of antioxidant, 0.4 g of stearic acid, and 1.5 g of titanium dioxide into a rheometer, mix them evenly at 180 °C, and then place them on a molding machine for compression molding. The molding temperature is controlled at 210 °C. After molding, apply a layer of SIS hot melt pressure sensitive adhesive on its surface. The coating temperature is 140 °C and the coating thickness is 0.4 mm to obtain an anti-UV polymer self-adhesive waterproof membrane.

[0059] Refer to GB / T2406.2-2009 and use an oxygen index tester to test the flame retardant properties of waterproof membranes.

[0060] Table 1:

[0061]

[0062] As can be seen from the table, the flame retardant effect of Examples 1-5 is better than that of Comparative Example 1. This is because Examples 1-5 contain a large amount of phosphorus and nitrogen. When heated, phosphorus produces strong dehydrating substances such as phosphoric acid and metaphosphoric acid, which can promote the dehydration of the material into carbon, forming a dense carbon layer on the surface of the material to hinder combustion; when heated, nitrogen produces refractory gas, which dilutes the content of flammable gas in the air. The two work together to improve the flame retardant performance of the material. However, there is no such element in Comparative Example 1, so its flame retardant effect is poor.

[0063] Refer to GB23441-2009 to test the UV resistance of waterproof membranes. Place the waterproof membrane in a UV box at 45°C for 10 days, and refer to GB / T328.20-2007 to test the peel strength.

[0064] Table 2:

[0065]

[0066] It can be seen from the table that the anti-ultraviolet ability of Examples 1-5 is better than that of Comparative Example 1. This is because Examples 1-5 contain benzophenone anti-ultraviolet absorbers, which can absorb free radicals generated by the waterproof membrane, increase the viscosity of the membrane surface, and thus increase the peel strength. Therefore, the waterproof membrane prepared by the present invention has good anti-ultraviolet ability.

[0067] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing an anti-ultraviolet polymer self-adhesive waterproof coiled material, characterized in that: The preparation method is: (1) Preparation method of modified polyethylene Add maleic anhydride, phosphorus-containing bis(diphenyl ketone) vinyl triazine and diisopropylbenzene peroxide into polyethylene, stir and mix evenly, and carry out grafting reaction in a torque rheometer at 190-210° C., with a rotation speed of 40-60 r / min and a grafting time of 10-20 min to obtain modified polyethylene; The structural formula of the phosphorus-containing bis(diphenyl ketone) vinyl triazine is as follows ; (2) Preparation method of anti-ultraviolet polymer self-adhesive waterproof membrane Add polyethylene, modified polyethylene, antioxidant, stearic acid and titanium dioxide into the rheometer, mix evenly at 160-180°C, and then place them on a molding machine for compression molding. The molding temperature is controlled at 210°C. After molding, apply a layer of SIS hot melt pressure-sensitive adhesive on the surface. The coating temperature is 140°C and the coating thickness is 0.4mm to obtain an anti-UV polymer self-adhesive waterproof membrane.

2. The method for preparing the anti-ultraviolet polymer self-adhesive waterproof coiled material according to claim 1, characterized in that: In the above (1), the mass ratio of maleic anhydride, phosphorus-containing bis(diphenyl ketone) vinyl triazine, diisopropylbenzene peroxide and polyethylene is 2-4:1-3:0.5-2:

100.

3. The method for preparing the anti-ultraviolet polymer self-adhesive waterproof coiled material according to claim 1, characterized in that: In the above (2), the mass ratio of polyethylene, modified polyethylene, antioxidant, stearic acid and titanium dioxide is 100:80-120:0.2-0.5:0.5-1:1.5-3.

4. The method for preparing the anti-ultraviolet polymer self-adhesive waterproof coiled material according to claim 1, characterized in that: In the above (1), the preparation method of phosphorus-containing bis(diphenyl ketone) vinyl triazine is as follows: S1: Under nitrogen conditions, 2,4-dihydroxybenzophenone was added to a 1-2 mol / L sodium hydroxide aqueous solution, stirred to dissolve, and then 2-bromo-N-(bromoethyl)ethylamine was added thereto, and the reaction was carried out at 80-95° C. for 3-6 hours. After the reaction was completed, the mixture was washed with deionized water and dried to obtain intermediate 1; S2: Add cyanuric chloride to acetone solvent, stir to dissolve, then add intermediate 1 and 10% sodium hydroxide aqueous solution, react at 0-5°C for 4-8h, distill under reduced pressure, wash with deionized water, and dry to obtain intermediate 2; S3: adding intermediate 2 and pentaerythritol phosphate to acetone solvent, stirring and dispersing, then adding triethylamine thereto, reacting at 20-35° C. for 2-4 hours, and after the reaction is completed, distilling under reduced pressure, washing with deionized water, and drying to obtain intermediate 3; S4: Add intermediate 3 to acetone solvent, stir and disperse, add 3-butene-1-amine at 0-5°C, adjust the pH to 7-8 with saturated sodium carbonate, react for 1-3h, heat to 40-55°C, adjust the pH to 8-9 with saturated sodium carbonate, continue to react for 5-10h, filter after the reaction, distill under reduced pressure, wash with deionized water, and dry to obtain phosphorus-containing bis(diphenyl ketone) vinyl triazine.

5. The method for preparing the anti-ultraviolet polymer self-adhesive waterproof coiled material according to claim 4, characterized in that: In the S1, the molar ratio of 2,4-dihydroxybenzophenone to 2-bromo-N-(bromoethyl)ethylamine is 0.8-1.4:

1.

6. The method for preparing the anti-ultraviolet polymer self-adhesive waterproof coiled material according to claim 4, characterized in that: In S2, the molar ratio of cyanuric chloride to intermediate 1 is 1:

1.

7. The method for preparing the anti-ultraviolet polymer self-adhesive waterproof coiled material according to claim 4, characterized in that: In the S3, the molar ratio of the intermediate 2, pentaerythritol phosphate and triethylamine is 1:1:1-1.