Waterproof shoe material and preparation method thereof
By using a combination of ethylene-vinyl acetate copolymer, modified silicone oil and aliphatic isocyanate in shoe materials, a stable cross-linked structure is formed, which solves the problem of insufficient waterproof performance of hot melt adhesive in high and low temperature environments and improves the quality of shoe materials. Excellent bonding strength and waterproof performance, extending service life.
Patent Information
- Application Number
- CN202411117291.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-10-15
AI Technical Summary
Existing hot-melt adhesives have insufficient waterproof performance in high or low temperature environments, resulting in insufficient adhesion to shoe materials and prone to glue opening problems, affecting the quality and service life of shoes.
Using ethylene-vinyl acetate copolymer as the matrix resin, combined with modified silicone oil and aliphatic isocyanate as modifiers, the bonding strength and waterproof performance are improved through tackifiers and cross-linking agents to form a stable cross-linked structure and enhance thermal stability. and water resistance.
It effectively improves the waterproof performance and bonding strength of the shoe material, reduces the occurrence of glue opening, and ensures that the shoe material still maintains good waterproof performance and bonding strength after long-term use.
Smart Images

Figure BDA0004993994970000061 
Figure BDA0004993994970000071
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of shoe materials, and in particular to a waterproof shoe material and a preparation method thereof. Background Art
[0002] In the process of making shoes, the upper is connected to the sock inside the shoe by sewing. However, the sewing method requires a lot of manpower, and the production process takes a long time, resulting in reduced work efficiency. Therefore, in order to simplify the construction time of the sewing part, reduce the labor of the sewing machine, and effectively improve the manufacturing efficiency, the upper is usually connected to the shoe lining by gluing. Therefore, hot melt adhesive is widely used for gluing shoe materials, and the performance of hot melt adhesive directly affects the final quality of the shoes.
[0003] At present, the raw material commonly used for hot melt adhesive is ethylene-vinyl acetate copolymer. Although hot melt adhesive based on ethylene-vinyl acetate copolymer is economical and low-priced, it can meet the needs of most products with low bonding strength requirements. However, due to the different use environments of shoes, the waterproof performance of ethylene-vinyl acetate copolymer will be affected in some high or low temperature environments, resulting in insufficient bonding strength of hot melt adhesive and causing the product to debond, thus affecting the quality of shoes. Summary of the invention
[0004] In order to improve the problem of easy debonding of waterproof shoe materials in the related art, the present application provides a waterproof shoe material and a preparation method thereof.
[0005] In the first aspect, the present application provides a waterproof shoe material, which adopts the following technical solution: A waterproof shoe material, comprising the following raw materials by weight: Ethylene-vinyl acetate copolymer 70-80 parts, modified silicone oil 18-20 parts, aliphatic isocyanate 3-5 parts, tackifier 10-12 parts, antioxidant 1.2-1.4 parts, crosslinking agent 2-3 parts, filler 4-6 parts, wax 5-7 parts; The modified silicone oil comprises vinyl-terminated polydimethylsiloxane and fluorine-containing acrylate, and the weight ratio of the vinyl-terminated polydimethylsiloxane to the fluorine-containing acrylate is 10:(7.5-8.5).
[0006] By adopting the above technical scheme, the waterproof shoe material uses ethylene-vinyl acetate copolymer as the matrix resin, and uses modified silicone oil and aliphatic isocyanate as the modifier of ethylene-vinyl acetate copolymer, and the bonding strength of the waterproof shoe material is improved by a tackifier to reduce the occurrence of debonding. Wherein, the joint action of modified silicone oil and aliphatic isocyanate can effectively improve the stability of ethylene-vinyl acetate copolymer, so that the waterproof performance of the colloid is not affected by temperature changes, and the shoe material is still not easy to debond after long-term use. At the same time, the unsaturated double bond in the terminal vinyl polydimethylsiloxane is combined with the unsaturated double bond in the fluorinated acrylate, which is conducive to improving the hydrophobicity of the colloid. In addition, aliphatic isocyanate can form a cross-linked structure with ethylene-vinyl acetate copolymer and terminal vinyl polydimethylsiloxane under the action of a cross-linking agent, improve the thermal stability and water resistance of the colloid, and is conducive to improving the bonding strength of the colloid.
[0007] Preferably, the fluorine-containing acrylate includes at least one of heptafluoroisobutyl methacrylate and dodecafluoroheptyl methacrylate.
[0008] By adopting the above technical solution, the surface free energy of the fluorocarbon group in the fluorinated acrylate is low, and the fluorocarbon group has the special property of migrating to the surface and enriching, so it can be used to hydrophobically modify the polymer matrix to improve the hydrophobic properties of the material. The siloxy group in the vinyl-terminated polydimethylsiloxane also has a low surface free energy. The combination of fluorinated acrylate and vinyl-terminated polydimethylsiloxane can significantly improve the waterproof performance of the colloid without affecting the bonding strength of the colloid.
[0009] Preferably, the aliphatic isocyanate includes at least one of 4,4'-dicyclohexylmethane diisocyanate and isophorone diisocyanate.
[0010] By adopting the above technical solution, the isocyanate group in the aliphatic isocyanate is combined with the hydroxyl group in the fluorinated acrylate, thereby improving the aging, yellowing and debonding problems of the colloid during use and maintaining the transparency or original color of the hot melt adhesive.
[0011] Preferably, the tackifier includes at least one of rosin resin and petroleum resin.
[0012] By adopting the above technical solution, the surface of the upper and the sock is a rough interface. When the colloid contacts the upper, it will fill and penetrate into the gaps and grooves of the upper to form many mosaic structures. After the colloid cools, the mosaic structure tends to be stable, thereby producing a good bonding effect. The main function of the tackifying resin is to reduce the melt viscosity of the hot melt adhesive, improve its wettability and initial adhesion to the bonded surface, so as to achieve improved bonding strength. In addition, the tackifying resin can also adjust the heat resistance temperature and air-drying time of the adhesive.
[0013] Preferably, the antioxidant includes at least one of antioxidant 1010 and antioxidant 264 .
[0014] By adopting the above technical solution, the antioxidant is mainly used to reduce the degradation problem of hot melt adhesive in a hot oxygen environment and improve the stability of the ethylene-vinyl acetate copolymer matrix resin. The antioxidant can reduce the breakage of carbon-hydrogen bonds in the molecular structure, prevent the oxidation reaction from proceeding, and reduce the molecular weight, thereby achieving an antioxidant effect, helping to maintain the bonding strength and bonding performance of the hot melt adhesive and reducing the performance degradation caused by the oxidation reaction.
[0015] Preferably, the crosslinking agent includes at least one of γ-aminopropyltriethoxysilane and γ-glycidyloxypropyltrimethoxysilane.
[0016] By adopting the above technical solution, the cross-linking agent can react with moisture in the air, solidify and cross-link to form a stable chemical structure. Since the bridge is irreversible, it will not creep or become brittle due to changes in ambient temperature, and has high toughness and strong initial adhesion.
[0017] Preferably, the filler includes at least one of nano calcium carbonate and nano silicon dioxide.
[0018] By adopting the above technical solution, the filler migrates to the coating surface during the colloid film formation process, forms a micro-nano structure on the coating surface, increases the surface roughness, and thus improves the hydrophobicity and oleophobicity of the coating. In addition, the filler is also used to reduce the shrinkage of the colloid, reduce the transitional penetration of the adhesive surface, and prolong the operability time.
[0019] Preferably, the wax is a microcrystalline wax with a molecular weight of 4000-5000.
[0020] By adopting the above technical solution, microcrystalline wax is used to reduce the melting point and melt viscosity of hot melt adhesive, improve the fluidity and wettability of the colloid, increase the bonding strength, and reduce the agglomeration of the colloid.
[0021] In a second aspect, the present application provides a method for preparing a waterproof shoe material, which adopts the following technical solution: A method for preparing a waterproof shoe material comprises the following steps: S1. Ethylene-vinyl acetate copolymer, modified silicone oil, aliphatic isocyanate, and tackifier are heated to 120-130°C to form a molten colloid, antioxidant, crosslinking agent, filler, and wax are added to maintain the temperature and mixed evenly, and then cooled and discharged to obtain a hot melt adhesive; S2. Heat the hot melt adhesive to 145-155°C to make it melt, use the hot melt adhesive to fit the shoe upper and the sock cover together, and then press and cool to obtain the shoe material.
[0022] Preferably, the preparation method of the modified silicone oil is: Dissolve terminal vinyl polydimethylsiloxane in methyl ether to obtain a modified liquid, heat the modified liquid to 50-60°C, add fluorinated acrylate to the modified liquid, stir to make the fluorinated acrylate evenly dispersed in the modified liquid, remove the solvent by distillation, cool to room temperature after the reaction is complete, and obtain modified silicone oil.
[0023] By adopting the above technical solution, the construction process of using hot melt adhesive to fit the sock cover to the shoe upper can effectively simplify the construction time of the sewing machine part, greatly reduce the labor of the sewing machine, and effectively improve the manufacturing efficiency. At the same time, the hot melt adhesive part can effectively be waterproof.
[0024] This application has the following beneficial effects: 1. In the present application, the waterproof shoe material uses ethylene-vinyl acetate copolymer as the matrix resin, and uses modified silicone oil and aliphatic isocyanate as the modifier of ethylene-vinyl acetate copolymer, and the bonding strength of the waterproof shoe material is improved by a tackifier to reduce the occurrence of debonding. Among them, the joint action of modified silicone oil and aliphatic isocyanate can effectively improve the stability of ethylene-vinyl acetate copolymer, so that the waterproof performance of the colloid is not affected by temperature changes, so that the shoe material is still not easy to debond after long-term use. At the same time, the unsaturated double bonds in the terminal vinyl polydimethylsiloxane are combined with the unsaturated double bonds in the fluorinated acrylate, which is conducive to improving the hydrophobicity of the colloid. In addition, aliphatic isocyanate can form a cross-linked structure with ethylene-vinyl acetate copolymer and terminal vinyl polydimethylsiloxane under the action of a cross-linking agent, improve the thermal stability and water resistance of the colloid, and is conducive to improving the bonding strength of the colloid.
[0025] 2. In this application, the surface of the upper and the sock is a rough interface. When the colloid contacts the upper, it will fill and penetrate into the gaps and grooves of the upper to form many mosaic structures. After the colloid cools, the mosaic structure tends to be stable, thus producing a good bonding effect. The main function of the tackifying resin is to reduce the melt viscosity of the hot melt adhesive, improve its wettability and initial adhesion to the bonded surface, so as to achieve improved bonding strength. In addition, the tackifying resin can also adjust the heat resistance temperature and air-drying time of the adhesive. DETAILED DESCRIPTION
[0026] Preparation Example Preparation Example 1 Preparation of modified silicone oil: Dissolve 10 kg of vinyl-terminated polydimethylsiloxane in 100 kg of methyl ether to obtain a modified liquid, heat the modified liquid to 50°C, add 7.5 kg of heptafluoroisobutyl methacrylate to the modified liquid, stir for 1 hour to evenly disperse the heptafluoroisobutyl methacrylate in the modified liquid, remove the methyl ether by distillation, and cool to room temperature after the reaction is complete to obtain modified silicone oil.
[0027] Preparation Example 2 Preparation of modified silicone oil: Dissolve 10 kg of vinyl-terminated polydimethylsiloxane in 100 kg of methyl ether to obtain a modified liquid, heat the modified liquid to 55°C, add 8.0 kg of dodecafluoroheptyl methacrylate to the modified liquid, stir for 1 hour to evenly disperse the dodecafluoroheptyl methacrylate in the modified liquid, remove the methyl ether by distillation, and cool to room temperature after the reaction is complete to obtain modified silicone oil.
[0028] Preparation Example 3 Preparation of modified silicone oil: Dissolve 10 kg of vinyl-terminated polydimethylsiloxane in 100 kg of methyl ether to obtain a modified liquid, heat the modified liquid to 60°C, add 8.5 kg of heptafluoroisobutyl methacrylate to the modified liquid, stir for 1 hour to evenly disperse the heptafluoroisobutyl methacrylate in the modified liquid, remove the methyl ether by distillation, and cool to room temperature after the reaction is complete to obtain modified silicone oil. Example
[0029] Example 1 A waterproof shoe material, comprising the following raw materials: 70kg ethylene-vinyl acetate copolymer (Formosa Plastics 7470M), 18kg modified silicone oil (modified silicone oil prepared by Preparation 1), 3kg 4,4'-dicyclohexylmethane-diisocyanate, 10kg rosin resin, 1.2kg antioxidant 1010, 2kg γ-aminopropyltriethoxysilane, 4kg nano calcium carbonate, 5kg microcrystalline wax (molecular weight 4000).
[0030] The method for preparing the waterproof shoe material in this embodiment comprises the following steps: S1. Ethylene-vinyl acetate copolymer, modified silicone oil, 4,4'-dicyclohexylmethane-diisocyanate, and rosin resin are heated to 120°C to form a molten colloid, antioxidant 1010, γ-aminopropyl triethoxysilane, nano-calcium carbonate, and microcrystalline wax are added to maintain the temperature and mixed evenly, and then cooled and discharged to obtain a hot melt adhesive; S2. Heat the hot melt adhesive to 145°C to make it molten, use the hot melt adhesive to fit the shoe upper and the sock cover together, and then press and cool to obtain the shoe material.
[0031] Example 2 A waterproof shoe material, comprising the following raw materials: 75kg ethylene-vinyl acetate copolymer (Formosa Plastics 7470M), 19kg modified silicone oil (modified silicone oil prepared by Preparation 2), 4kg isophorone diisocyanate, 11kg petroleum resin, 1.3kg antioxidant 264, 2.5kg γ-glycidyloxypropyltrimethoxysilane, 5kg nano-silica, 6kg microcrystalline wax (molecular weight 5000).
[0032] The method for preparing the waterproof shoe material in this embodiment comprises the following steps: S1. Ethylene-vinyl acetate copolymer, modified silicone oil, isophorone diisocyanate, and petroleum resin are heated to 125°C to form a molten colloid, antioxidant 264, γ-glycidyloxypropyl trimethoxysilane, nano-silica, and microcrystalline wax are added to maintain the temperature and mixed evenly, and then cooled and discharged to obtain a hot melt adhesive; S2. Heat the hot melt adhesive to 150°C to melt it, use the hot melt adhesive to fit the shoe upper and the sock cover together, and then press and cool them to obtain the shoe material.
[0033] Example 3 A waterproof shoe material, comprising the following raw materials: 80kg ethylene-vinyl acetate copolymer (Formosa Plastics 7470M), 20kg modified silicone oil (modified silicone oil prepared by Preparation 3), 5kg isophorone diisocyanate, 12kg petroleum resin, 1.4kg antioxidant 264, 3.0kg γ-glycidyloxypropyltrimethoxysilane, 5kg nano-silica, 6kg microcrystalline wax (molecular weight 5000).
[0034] The method for preparing the waterproof shoe material in this embodiment comprises the following steps: S1. Ethylene-vinyl acetate copolymer, modified silicone oil, isophorone diisocyanate, and petroleum resin are heated to 125°C to form a molten colloid, antioxidant 264, γ-glycidyloxypropyl trimethoxysilane, nano-silica, and microcrystalline wax are added to maintain the temperature and mixed evenly, and then cooled and discharged to obtain a hot melt adhesive; S2. Heat the hot melt adhesive to 150°C to melt it, use the hot melt adhesive to fit the shoe upper and the sock cover together, and then press and cool them to obtain the shoe material.
[0035] Comparative Example Comparative Example 1 A waterproof shoe material, which is different from Example 1 in that: The modified silicone oil is replaced by an equal amount of ethylene-vinyl acetate copolymer.
[0036] Comparative Example 2 A waterproof shoe material, which is different from Example 1 in that: The modified silicone oil is replaced by an equal amount of vinyl-terminated polydimethylsiloxane.
[0037] Comparative Example 3 A waterproof shoe material, which is different from Example 1 in that: The modified silicone oil was replaced by an equal amount of 4,4'-dicyclohexylmethane-diisocyanate.
[0038] Comparative Example 4 A waterproof shoe material, which is different from Example 1 in that: 4,4'-Dicyclohexylmethane diisocyanate was replaced by an equal amount of heptafluoroisobutyl methacrylate.
[0039] Comparative Example 5 A waterproof shoe material, which is different from Example 1 in that: 4,4'-Dicyclohexylmethane diisocyanate was replaced by an equal amount of 4,4'-diphenylmethane diisocyanate.
[0040] Performance testing 1. Rainproof performance test: Test according to GB / T 14577-1993 standard. Sample size 14cm*14cm, test water temperature (20±2)℃. Fix the sample to be tested on the rain rack, use a beaker to measure 250ml of water, pour it into the funnel for spraying test. After the spraying is completed, remove the sample, tap it three times on the table, and compare the rating. Visual rating: Level 5-small water droplets dripping quickly; Level 4-large water droplets formed; Level 3-part of the sample is stained with water droplets; Level 2-partial wetting; Level 1-the entire surface is wetted.
[0041] 2. Water repellency test: GB / T 4744-2013 "Hydrostatic pressure test for testing and evaluation of waterproof performance of textiles" standard. The sample is φ165mm, and the test water temperature is (27±2)℃. Place the sample on the tester, turn on the switch, start the water pump to fill it with water and then turn it off, then fix the sample, reset it, set the value to zero, adjust the gear, start the water pump until three water drops appear on the surface of the sample, turn off the water pump, and record the value at this time as the hydrostatic pressure of the test.
[0042] 3. Peel strength test: Test the effect of different pressing temperatures on the peel strength of shoe materials according to GB / T 2791-1995. Test the peel strength between the bonded upper and the socks, and use a material testing machine to test 200mm×25mm samples. Cut 5 pieces of each bonded sample and peel the sample 50mm in the length direction. Adjust the upper and lower clamps of the material testing machine to 50mm, set the clamp rising speed to 100±10mm / min, start the instrument for testing, stop after peeling 100mm, record the load change during the peeling process, and use the 12 peak method to calculate the peel strength value, which is the peel strength value of each sample.
[0043] Table 1 According to the comparison between Example 1 and Comparative Example 1 and the data in Table 1, it can be seen that when the waterproof shoe material is made without adding modified silicone oil to the raw materials, the peel strength between the shoe material fabrics is small, the bonding performance of the hot melt adhesive is poor, and the shoe material is prone to debonding. In addition, the stability of ethylene-vinyl acetate copolymer is poor, which has a significant impact on the waterproof performance of the shoe material.
[0044] According to the comparison between Example 1 and Comparative Example 2 and the data in Table 1, it can be seen that when the vinyl-terminated polydimethylsiloxane is directly added to the raw materials to make shoe materials without modification, the waterproof performance of the shoe materials is poor. After modification, the vinyl-terminated polydimethylsiloxane is combined with the fluorinated acrylate, so that the hydrophobic group is added to the molecular structure, which can significantly improve the waterproof performance of the colloid without affecting the bonding strength of the colloid.
[0045] According to the comparison between Example 1 and Comparative Example 3 and the data in Table 1, it can be seen that the addition of 4,4'-dicyclohexylmethane-diisocyanate alone as a modifier for ethylene-vinyl acetate copolymer will affect the bonding strength and waterproof performance of the shoe material, making the shoe material prone to debonding and water seepage.
[0046] According to the comparison between Example 1 and Comparative Example 4 and the data in Table 1, it can be seen that the use of 4,4'-dicyclohexylmethane-diisocyanate is more conducive to improving the peel strength between the shoe material fabrics and the bonding performance of the shoe material. The isocyanate group is combined with the hydroxyl group, which is not prone to the problem of debonding and aging, and the service life of the shoe material is extended. At the same time, it has no effect on the waterproof performance of the shoe material.
[0047] According to the comparison between Example 1 and Comparative Example 5 and the data in Table 1, it can be seen that aliphatic isocyanate is better than aromatic isocyanate in improving the waterproof performance and bonding strength of shoe materials.
[0048] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A waterproof shoe material, characterized in that: By weight, it contains the following raw materials: Ethylene-vinyl acetate copolymer 70-80 parts, modified silicone oil 18-20 parts, aliphatic isocyanate 3-5 parts, tackifier 10-12 parts, antioxidant 1.2-1.4 parts, crosslinking agent 2-3 parts, filler 4-6 parts, wax 5-7 parts; The modified silicone oil comprises vinyl-terminated polydimethylsiloxane and fluorine-containing acrylate, and the weight ratio of the vinyl-terminated polydimethylsiloxane to the fluorine-containing acrylate is 10:(7.5-8.5).
2. A waterproof shoe material according to claim 1, characterized in that: The fluorine-containing acrylate includes at least one of heptafluoroisobutyl methacrylate and dodecafluoroheptyl methacrylate.
3. A waterproof shoe material according to claim 1, characterized in that: The aliphatic isocyanate includes at least one of 4,4'-dicyclohexylmethane diisocyanate and isophorone diisocyanate.
4. The waterproof shoe material according to claim 1, characterized in that: The tackifier includes at least one of rosin resin and petroleum resin.
5. The waterproof shoe material according to claim 1, characterized in that: The antioxidant includes at least one of the antioxidant 1010 and the antioxidant 264 .
6. The waterproof shoe material according to claim 1, characterized in that: The crosslinking agent includes at least one of γ-aminopropyltriethoxysilane and γ-glycidyloxypropyltrimethoxysilane.
7. The waterproof shoe material according to claim 1, characterized in that: The filler includes at least one of nano calcium carbonate and nano silicon dioxide.
8. The waterproof shoe material according to claim 1, characterized in that: The wax is a microcrystalline wax with a molecular weight of 4000-5000.
9. A method for preparing a waterproof shoe material according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1. Ethylene-vinyl acetate copolymer, modified silicone oil, aliphatic isocyanate, and tackifier are heated to 120-130°C to form a molten colloid, antioxidant, crosslinking agent, filler, and wax are added to maintain the temperature and mixed evenly, and then cooled and discharged to obtain a hot melt adhesive; S2. Heat the hot melt adhesive to 145-155°C to melt it, use the hot melt adhesive to fit the shoe upper and the sock cover together, and then press and cool them to obtain the shoe material.
10. The method for preparing a waterproof shoe material according to claim 9, characterized in that: The preparation method of the modified silicone oil is: Dissolve terminal vinyl polydimethylsiloxane in methyl ether to obtain a modified liquid, heat the modified liquid to 50-60°C, add fluorinated acrylate to the modified liquid, stir to make the fluorinated acrylate evenly dispersed in the modified liquid, remove the solvent by distillation, cool to room temperature after the reaction is complete, and obtain modified silicone oil.