Pre-crosslinked packaging adhesive film and preparation method and application thereof
By using pre-crosslinked encapsulating adhesive film in busbarless photovoltaic modules and increasing the cross-linking degree of the adhesive film, the problem of local shrinkage and streaks after lamination is solved, and the stability and power performance of the module are improved.
Patent Information
- Application Number
- CN202411130449.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-10-15
AI Technical Summary
The encapsulation film of busbarless photovoltaic modules is prone to local shrinkage holes or streaks after lamination, which affects module stability and power attenuation.
Pre-crosslinked encapsulating adhesive film is used. Its raw materials include main thermoplastic particles, cross-linking monomers, thermal initiators, coupling agents, light stabilizers and photoinitiators. Through ultraviolet light irradiation, a cross-linking degree of 5%-50% is achieved. Reduce film shrinkage.
It improves the stability of components, suppresses power attenuation, and improves appearance abnormalities after film lamination.
Smart Images

Figure CN118772801A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar photovoltaic module packaging, and in particular to a pre-crosslinked packaging adhesive film and a preparation method and application thereof. Background Art
[0002] The busbarless module adopts 0BB technology, which is an innovative photovoltaic cell module technology. This technology eliminates the main grid of the traditional cell and uses welding strips to derive current in the module link. Specifically, the busbarless cell uses welding strips to collect the fine grid current and realize the interconnection of cells. The width of the welding strip is smaller than the width of the traditional busbar. In addition, the busbarless cell usually uses copper welding strips, and the original silver electrode busbar is completely replaced, realizing the function of base metal replacing the traditional silver busbar. The application of busbarless module encapsulation film in solar panels can not only improve the conversion efficiency of the battery, but also reduce the manufacturing cost. Due to its superior performance, the busbarless module encapsulation film has become the mainstream choice of solar panel encapsulation materials.
[0003] Conventional busbar-free encapsulation films are thin and have a large shrinkage rate. After the components are laminarized, local shrinkage holes or stripes are prone to occur, which affects the appearance of the components and causes hot spot effects, which in turn leads to reduced stability of solar cells and excessive power attenuation.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a pre-crosslinked encapsulation adhesive film and a preparation method and application thereof, which are beneficial to improving the stability of solar cells and inhibiting power attenuation.
[0006] The present invention is achieved in that: In a first aspect, the present invention provides a pre-crosslinked encapsulation film, wherein the degree of crosslinking of the pre-crosslinked encapsulation film is 5%-50%; the raw materials of the pre-crosslinked encapsulation film include: main thermoplastic particles, crosslinking monomers, thermal initiators, coupling agents, light stabilizers and photoinitiators.
[0007] In an optional embodiment, the mass fraction of the main thermoplastic particles in the raw material is 85wt%-97wt%; and / or the main thermoplastic particles are selected from at least one of EPE particles, POE particles, EVA particles and PVB particles.
[0008] In an optional embodiment, the mass fraction of the cross-linking monomer in the raw material is 1.0wt%-10wt%; and / or the cross-linking monomer is selected from at least one of 2-phenoxyethyl acrylate, triallyl cyanurate, trimethylolpropane trimethacrylate, 2-hydroxyethyl methacrylate phosphate and triallyl isocyanurate.
[0009] In an optional embodiment, the mass fraction of the thermal initiator in the raw material is 0.6wt%-3.0wt%; and / or the thermal initiator is selected from at least one of tert-butyl hydroperoxide, di-tert-butyl peroxide, di-tert-amyl peroxide and tert-butyl peroxypivalate.
[0010] In an optional embodiment, the mass fraction of the coupling agent in the raw material is 0.5wt%-1.5wt%; and / or, the coupling agent is selected from at least one of coupling agent KH-550, coupling agent KH-560, coupling agent KH-570, coupling agent PM-1 and coupling agent PM-2.
[0011] In an optional embodiment, the mass fraction of the light stabilizer in the raw material is 0.2wt%-1.0wt%; and / or, the light stabilizer is selected from at least one of light stabilizer 622, light stabilizer B75, light stabilizer 770, and light stabilizer HA-10.
[0012] In an optional embodiment, the mass fraction of the photoinitiator in the raw material is 0.1wt%-3.0wt%; and / or, the photoinitiator is selected from at least one of photoinitiator 754, photoinitiator 907, photoinitiator 184, photoinitiator 369, photoinitiator 1173, photoinitiator TPO, photoinitiator BP, photoinitiator 819, photoinitiator PBZ and photoinitiator MBF.
[0013] In an optional embodiment, the pre-crosslinked packaging film has a thickness of 50 μm-100 μm.
[0014] In a second aspect, the present invention provides a method for preparing the pre-cross-linked packaging film described in any one of the aforementioned embodiments, comprising: mixing the raw materials evenly and then coating the substrate, and then irradiating the substrate with ultraviolet light until the pre-cross-linking degree of the film layer reaches 5%-50%, thereby obtaining the pre-cross-linked packaging film.
[0015] In a third aspect, the present invention provides a use of the pre-crosslinked encapsulation film described in any one of the aforementioned embodiments in a busbar-free solar cell module.
[0016] The present invention has the following beneficial effects: The present invention adds a photoinitiator to the raw materials of the encapsulation film, which is beneficial to improving the pre-crosslinking degree of the encapsulation film, and obtaining a pre-crosslinked encapsulation film with a crosslinking degree of 5%-50%. The improvement of the pre-crosslinking degree is beneficial to reducing the shrinkage rate of the film, and further helps to improve the abnormal conditions that affect the appearance such as shrinkage holes and stripes after the film is laminarized, thereby helping to improve the stability of the component and inhibit power attenuation. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0018] Figure 1 This is a local image of electroluminescent defect detection (EL) of the packaging film prepared in Example 1.
[0019] Figure 2 This is a local image of electroluminescent defect detection (EL) of the packaging film prepared in Example 2.
[0020] Figure 3 This is a local image of electroluminescent defect detection (EL) of the packaging film prepared in Example 3.
[0021] Figure 4 This is a local image of electroluminescent defect detection (EL) of the packaging film prepared in Comparative Example 1. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0023] The embodiment of the present invention provides a pre-crosslinked packaging film, wherein the degree of crosslinking of the pre-crosslinked packaging film is 5%-50%; The raw materials of the pre-crosslinked packaging film include: main thermoplastic particles, crosslinking monomers, thermal initiators, coupling agents, light stabilizers and photoinitiators.
[0024] In the embodiment of the present invention, the crosslinking degree of the pre-crosslinked packaging film is 5%-50%, specifically 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or any value between 5% and 50%. Adding a photoinitiator to the raw material of the packaging film is beneficial to improving the pre-crosslinking degree of the packaging film, reducing the shrinkage rate of the film, and further improving the abnormal conditions that affect the appearance such as shrinkage cavities and stripes after the film is laminated, thereby improving the stability of the component and suppressing the attenuation of power.
[0025] In an optional embodiment, the mass fraction of the main thermoplastic particles in the raw material is 85wt%-97wt%; and / or the main thermoplastic particles are selected from at least one of EPE particles, POE particles, EVA particles and PVB particles.
[0026] In an optional embodiment, the mass fraction of the cross-linking monomer in the raw material is 1.0wt%-10wt%; and / or the cross-linking monomer is selected from at least one of 2-phenoxyethyl acrylate, triallyl cyanurate, trimethylolpropane trimethacrylate, 2-hydroxyethyl methacrylate phosphate and triallyl isocyanurate.
[0027] In an optional embodiment, the mass fraction of the thermal initiator in the raw material is 0.6wt%-3.0wt%; and / or the thermal initiator is selected from at least one of tert-butyl hydroperoxide, di-tert-butyl peroxide, di-tert-amyl peroxide and tert-butyl peroxypivalate.
[0028] In an optional embodiment, the mass fraction of the coupling agent in the raw material is 0.5wt%-1.5wt%; and / or, the coupling agent is selected from at least one of coupling agent KH-550 (3-aminopropyltriethoxysilane), coupling agent KH-560 (γ-(2,3-epoxypropoxy)propyltrimethoxysilane), coupling agent KH-570 (γ-(methacryloyloxy)propyltrimethoxysilane), coupling agent PM-1 and coupling agent PM-2 (2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate).
[0029] In an optional embodiment, the mass fraction of the light stabilizer in the raw material is 0.2wt%-1.0wt%; and / or, the light stabilizer is selected from at least one of light stabilizer 622 (hindered amine light stabilizer 622), light stabilizer B75 (BASF light stabilizer B75), light stabilizer 770 (HALS770), and light stabilizer HA-10 (bis-2,2,6,6-tetramethylpiperidinol sebacate).
[0030] In an optional embodiment, the mass fraction of the photoinitiator in the raw material is 0.1wt%-3.0wt%; and / or, the photoinitiator is selected from photoinitiator 754 (2-[(2-oxo-2-phenylacetoxy)ethoxy]ethyl 2-oxo-2-phenylacetate), photoinitiator 907 (Caccure907, molecular formula is C13H17NO2S), photoinitiator 184 (1-hydroxycyclohexyl phenyl ketone), photoinitiator 369 (2-benzyl-2-dimethyl At least one of photoinitiator 1173 (2-hydroxy-2-methyl-1-phenyl-1-propanone), photoinitiator TPO (diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide), photoinitiator BP (C13H10O), photoinitiator 819 (phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide), photoinitiator PBZ (4-Benzoylbiphenyl) and photoinitiator MBF (methyl benzoylformate).
[0031] In an optional embodiment, the thickness of the pre-crosslinked packaging film is 50 μm-100 μm, specifically 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm or any value between 50 μm and 100 μm. Increasing the pre-crosslinking degree of the packaging film is conducive to reducing the thickness of the packaging film, thereby helping to save costs.
[0032] An embodiment of the present invention also provides a method for preparing the pre-crosslinked packaging film described in any one of the aforementioned embodiments, comprising: mixing the raw materials evenly and then coating the substrate, and then irradiating the substrate with ultraviolet light until the pre-crosslinking degree of the film layer reaches 5%-50%, thereby obtaining the pre-crosslinked packaging film.
[0033] The embodiment of the present invention further provides a use of the pre-crosslinked packaging film described in any one of the aforementioned embodiments in a busbar-free solar cell module.
[0034] After the pre-packaging adhesive film in the present application is prepared, the crystalline silicon cell sheets are packaged and laminated, and further cross-linking is completed during the lamination process to obtain a solar cell module.
[0035] The features and performance of the present invention are further described in detail below in conjunction with the examples, wherein the commercially available encapsulation film can be selected from existing commercially available products, and the commercially available encapsulation film model used in the following examples and comparative examples is P507T2 of Haiyouwei. The commercially available encapsulation film is used in conjunction with the encapsulation film in the examples or comparative examples to enhance the bonding strength and suppress the phenomenon of cold solder joints.
[0036] Example 1 This embodiment provides a method for preparing a pre-crosslinked packaging film, which specifically includes the following steps: A. Prepare the materials. The mass fractions of the components in the raw materials are as follows: 1. EVA particles: 95%; 2. 2-Phenoxyethyl acrylate: 2%; 3. Tert-butyl hydroperoxide: 1%; 4. Coupling agent KH570: 1%; 5. Light stabilizer 770: 0.5%; 6. Photoinitiator 907: 0.5%; B. Preparation: The above materials are mixed evenly, hot-melt coated, and the coated film is irradiated with ultraviolet light at room temperature, and the energy and irradiation time of the ultraviolet lamp are adjusted to obtain a pre-crosslinked packaging film with a crosslinking degree as shown in Table 1. The thickness is 50 μm. The local electroluminescence defect detection (EL) image is as follows Figure 1 .
[0037] C. Test: A solar cell is obtained by laminating a seven-layer structure of glass / commercially available encapsulation film / encapsulation film prepared in this embodiment / crystalline silicon cell / encapsulation film prepared in this embodiment / commercially available encapsulation film / backplane, and a TC200 test is performed on the solar cell. The process and technical parameters of the TC200 test are: 200 thermal cycle tests, conditions: -40°C to +85°C. The power attenuation of the solar cell module before and after the test is shown in Table 1.
[0038] Table 1
[0039] Example 2 This embodiment provides a method for preparing a pre-crosslinked packaging film, which specifically includes the following steps: A. Prepare the materials. The mass fractions of the components in the raw materials are as follows: 1. POE particles: 90%; 2. 2-Hydroxyethyl methacrylate phosphate: 6.5%; 3. Di-tert-butyl peroxide: 1.5%; 4. Coupling agent KH560: 1%; 5. Light stabilizer 622: 0.5%; 6. Photoinitiator 754: 0.5%; B. Preparation: The above materials are mixed evenly, hot-melt coated, and the coated film is irradiated with ultraviolet light at room temperature, and the energy and irradiation time of the ultraviolet lamp are adjusted to obtain a pre-crosslinked packaging film with a crosslinking degree as shown in Table 2, and a thickness of 50 μm. The local electroluminescence defect detection (EL) image is as follows Figure 2 .
[0040] C. Test: A solar cell is obtained by laminating a seven-layer structure of glass / commercially available encapsulation film / encapsulation film prepared in this embodiment / crystalline silicon cell / encapsulation film prepared in this embodiment / commercially available encapsulation film / backplane, and a TC200 test is performed on the solar cell. The process and technical parameters of the TC200 test are: 200 thermal cycle tests, conditions: -40°C to +85°C. The power attenuation of the solar cell module before and after the test is shown in Table 2.
[0041] Table 2
[0042] Example 3 This embodiment provides a method for preparing a pre-crosslinked packaging film, which specifically includes the following steps: A. Prepare the materials. The mass fractions of the components in the raw materials are as follows: 1. EPE particles: 85%; 2. Triallyl isocyanurate: 10%; 3. Tert-butyl peroxypivalate: 1.5%; 4. Coupling agent PM-2: 1%; 5. Light stabilizer B75: 1.0%; 6. Photoinitiator 819: 1.5%; B. Preparation: The above materials are mixed evenly, hot-melt coated, and the coated film is irradiated with ultraviolet light at room temperature, and the energy and irradiation time of the ultraviolet lamp are adjusted to obtain a pre-crosslinked packaging film with a crosslinking degree as shown in Table 3, and a thickness of 50 μm. The local electroluminescence defect detection (EL) image is as follows Figure 3 .
[0043] C. Test: A solar cell is obtained by laminating a seven-layer structure of glass / commercially available encapsulation film / encapsulation film prepared in this embodiment / crystalline silicon cell / encapsulation film prepared in this embodiment / commercially available encapsulation film / backplane, and a TC200 test is performed on the solar cell. The process and technical parameters of the TC200 test are: 200 thermal cycle tests, conditions: -40°C to +85°C. The power attenuation of the solar cell module before and after the test is shown in Table 3.
[0044] Table 3
[0045] Comparative Example 1 This comparative example provides a method for preparing a packaging film, which specifically includes the following steps: A. Preparation of materials: The raw material composition is different from that of Example 1 only in that photoinitiator 907 is not added; B. Preparation: The above materials are mixed evenly, hot-melt coated, and the coated film is irradiated with ultraviolet light at room temperature, and the energy and irradiation time of the ultraviolet lamp are adjusted to obtain a packaging film with a cross-linking degree as shown in Table 4 and a thickness of 50 μm. The local electroluminescence defect detection (EL) image is as follows Figure 4 , local cold solder joints and stripes appear.
[0046] C. Test: A solar cell is obtained by laminating the seven-layer structure of / commercially available encapsulation film / encapsulation film prepared in this comparative example / crystalline silicon cell / encapsulation film prepared in this comparative example / commercially available encapsulation film / backplane, and a TC200 test is performed on the solar cell. The process and technical parameters of the TC200 test are: 200 thermal cycle tests, conditions: -40℃~+85℃. The power attenuation of the solar cell module before and after the test is shown in Table 4.
[0047]
[0048] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A pre-crosslinked packaging film, characterized in that: The crosslinking degree of the pre-crosslinked packaging film is 5%-50%; the raw materials of the pre-crosslinked packaging film include: main thermoplastic particles, crosslinking monomers, thermal initiators, coupling agents, light stabilizers and photoinitiators.
2. The pre-crosslinked packaging film according to claim 1, characterized in that: The mass fraction of the main thermoplastic particles in the raw material is 85wt%-97wt%; and / or the main thermoplastic particles are selected from at least one of EPE particles, POE particles, EVA particles and PVB particles.
3. The pre-crosslinked packaging film according to claim 1, characterized in that: The mass fraction of the crosslinking monomer in the raw material is 1.0wt%-10wt%; and / or the crosslinking monomer is selected from at least one of 2-phenoxyethyl acrylate, triallyl cyanurate, trimethylolpropane trimethacrylate, 2-hydroxyethyl methacrylate phosphate and triallyl isocyanurate.
4. The pre-crosslinked packaging film according to claim 1, characterized in that: The mass fraction of the thermal initiator in the raw material is 0.6wt%-3.0wt%; and / or, the thermal initiator is selected from at least one of tert-butyl hydroperoxide, di-tert-butyl peroxide, di-tert-amyl peroxide and tert-butyl peroxypivalate.
5. The pre-crosslinked packaging film according to claim 1, characterized in that: The mass fraction of the coupling agent in the raw material is 0.5wt%-1.5wt%; and / or, the coupling agent is selected from at least one of coupling agent KH-550, coupling agent KH-560, coupling agent KH-570, coupling agent PM-1 and coupling agent PM-2.
6. The pre-crosslinked packaging film according to claim 1, characterized in that: The mass fraction of the light stabilizer in the raw material is 0.2wt%-1.0wt%; and / or, the light stabilizer is selected from at least one of light stabilizer 622, light stabilizer B75, light stabilizer 770, and light stabilizer HA-10.
7. The pre-crosslinked packaging film according to claim 1, characterized in that: The mass fraction of the photoinitiator in the raw material is 0.1wt%-3.0wt%; and / or, the photoinitiator is selected from at least one of photoinitiator 754, photoinitiator 907, photoinitiator 184, photoinitiator 369, photoinitiator 1173, photoinitiator TPO, photoinitiator BP, photoinitiator 819, photoinitiator PBZ and photoinitiator MBF.
8. The pre-crosslinked packaging film according to claim 1, characterized in that: The thickness of the pre-crosslinked packaging film is 50 μm-100 μm.
9. A method for preparing the pre-crosslinked packaging film according to any one of claims 1 to 8, characterized in that: include: The raw materials are mixed evenly and then coated on a substrate, and then irradiated with ultraviolet light until the pre-crosslinking degree of the film layer reaches 5%-50%, thereby obtaining the pre-crosslinked packaging film.
10. Use of the pre-crosslinked encapsulation film according to any one of claims 1 to 8 in a busbar-free solar cell module.