Antistatic glue and preparation method thereof

Through the combination of modified carbon black and nanoscale carbon nanotubes, the problems of poor dispersion and high cost of conductive fillers in antistatic adhesives are solved, and efficient antistatic properties and industrially suitable preparation of antistatic adhesives are achieved.

CN118772807APending Publication Date: 2024-10-15TAIHU JINZHANG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410968318.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

During the processing and use of existing antistatic adhesives, conductive fillers are difficult to disperse and have poor compatibility with polymers. Moreover, the cost of materials such as nanosilver wires and nanocopper wires is high, resulting in poor antistatic performance and difficulty in widespread application.

Method used

Using a method of combining modified carbon black and nanoscale carbon nanotubes, the carbon black is coated with polypyrrole to improve its dispersion properties, and the cost is reduced by blending nanoscale and micron scale fillers to form an efficient antistatic glue.

Benefits of technology

Excellent antistatic effect and peeling strength are obtained, and the preparation method is simple, suitable for industrial production, reducing costs, and at the same time improving the heat resistance and aging resistance of the antistatic adhesive.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004952370350000071
    Figure BDA0004952370350000071
  • Figure BDA0004952370350000081
    Figure BDA0004952370350000081
Patent Text Reader

Abstract

The invention discloses an antistatic adhesive and a preparation method thereof, and belongs to the technical field of antistatic adhesives, the antistatic adhesive comprises the following raw materials by weight: 30-50 parts of a non-functional acrylate monomer, 10-20 parts of a functional acrylate monomer, 0.1-0.5 part of an initiator, 0.1-1 part of a cross-linking agent, 5-10 parts of carbon nanotubes, 3-6 parts of modified carbon black, and 60-80 parts of a solvent. The preparation method comprises the following steps: adding the non-functional acrylate monomer, the functional acrylate monomer and the initiator into the solvent in parts by weight, heating to 65-85 DEG C, stirring and mixing, then adding the cross-linking agent, the carbon nanotubes and the modified carbon black, and continuously mixing and cooling to obtain the antistatic adhesive. The antistatic adhesive obtained in the invention has excellent antistatic effect and peel strength, and has good heat resistance, aging resistance and other properties. Meanwhile, the preparation method is simple, convenient to operate and suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of antistatic adhesives, and in particular relates to an antistatic adhesive and a preparation method thereof. Background Art

[0002] With the rapid development of electronic technologies such as mobile phones, computers and touch displays, the integration of electronic materials is getting higher and higher, microelectronics are becoming more and more sophisticated, and the sensitivity to static electricity is increasing. For example, field effect transistors, chips, large-scale integrated circuits and touch screens are becoming more and more sensitive to the harm caused by static electricity. These electronic materials are required to be selected in low humidity environments with a surface resistivity of 10 10 The antistatic protective film has a resistance of less than Ω·m and a long-lasting antistatic effect.

[0003] In the prior art, the method of adding inorganic fillers with conductive ability to the glue is often used to improve the antistatic performance, such as adding conductive carbon black, nano gold powder, nano silver powder, nano copper powder, nano gold wire, nano silver wire, nano copper wire and other materials. However, these fillers are difficult to disperse and have poor compatibility with polymers. In addition, materials such as nano silver wire and nano copper wire are expensive and costly, and are not suitable for widespread promotion and application. Therefore, it is necessary to develop an antistatic glue with good antistatic effect and low economic cost, and then prepare an antistatic protective film to guide the static electricity generated during the processing of electronic materials, so as to avoid the accumulation of static electricity during the processing process. Harm to electronic materials is the focus of current attention. Summary of the invention

[0004] The object of the present invention is to provide an antistatic adhesive and a preparation method thereof, so as to improve the antistatic performance of the antistatic adhesive.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] An antistatic adhesive comprises the following raw materials in parts by weight:

[0007] 30-50 parts of non-functional acrylate monomer, 10-20 parts of functional acrylate monomer, 0.1-0.5 parts of initiator, 0.1-1 parts of crosslinking agent, 5-10 parts of carbon nanotubes, 3-6 parts of modified carbon black, 60-80 parts of solvent;

[0008] The modified carbon black is prepared by the following steps:

[0009] Add carbon black and hexadecyltrimethylammonium bromide (CTAB) into deionized water, stir ultrasonically, add concentrated hydrochloric acid, pyrrole and ammonium persulfate, continue stirring, dilute and stand, filter and wash, and freeze-dry to obtain modified carbon black. The modified carbon black is obtained by coating the surface with polypyrrole, which improves the dispersion performance of carbon black and avoids aggregation in the material, thereby hindering the transmission channel of electrons.

[0010] Furthermore, the usage ratio of carbon black, hexadecyltrimethylammonium bromide, deionized water, concentrated hydrochloric acid and pyrrole is 0.01-0.012 g: 0.41-0.42 g: 120 mL: 1 mL: 0.23-0.235 g.

[0011] Furthermore, the particle size of the carbon black is 100-150 μm.

[0012] Furthermore, the non-functional acrylic acid ester monomer is at least one of methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate and butyl methacrylate.

[0013] Furthermore, the functional acrylate monomer is at least one of acrylic acid, hydroxyethyl acrylate, methacrylic acid, hydroxyethyl methacrylate and hydroxypropyl methacrylate.

[0014] Furthermore, the initiator is at least one of benzoyl peroxide, cumene hydroperoxide and azobisisobutyronitrile.

[0015] Furthermore, the cross-linking agent is N,N-methylenebisacrylamide.

[0016] Furthermore, the solvent is at least one of toluene, ethyl acetate, butyl acetate, acetone and methanol.

[0017] Furthermore, the particle size of the carbon nanotubes is 200-400 nm.

[0018] The present invention also provides a method for preparing an antistatic adhesive, comprising the following steps:

[0019] According to weight, non-functional acrylate monomer, functional acrylate monomer and initiator are added to the solvent, heated to 65-85° C., stirred and mixed, and then a crosslinking agent, carbon nanotubes and modified carbon black are added, and the mixture is continuously mixed and cooled to obtain an antistatic adhesive.

[0020] Beneficial effects of the present invention:

[0021] In the present invention, when preparing the antistatic adhesive, firstly, non-functional acrylate monomer, functional acrylate monomer and initiator are added to a solvent to carry out polymerization reaction, and then a crosslinking agent, carbon nanotubes and modified carbon black are added to react to obtain the antistatic adhesive, and the obtained antistatic adhesive has excellent antistatic effect and peel strength, and has good heat resistance and aging resistance. At the same time, the preparation method is simple, easy to operate, and suitable for industrial production.

[0022] Furthermore, the addition of modified carbon black effectively fills the gaps between carbon nanotubes, promotes the formation of conductive paths, and effectively improves the antistatic effect of the antistatic adhesive. At the same time, the present invention also uses nano-scale carbon nanotubes and micron-scale modified carbon black for mixing. Since nano-scale fillers are expensive, blending nano-scale fillers with micron-scale fillers can reduce costs. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1

[0025] This embodiment provides a modified carbon black, and the preparation steps are as follows:

[0026] 0.01 g of carbon black (particle size of 120 μm) and 0.41 g of CTAB were added to 120 mL of deionized water, and ultrasonically stirred for 10 min. 1 mL of concentrated hydrochloric acid was added, and stirred for 10 min in an ice-water bath. 0.23 g of pyrrole was added, and the reaction was stirred for 15 min. 0.82 g of ammonium persulfate was added, and the stirring was continued for 24 h. The mixture was diluted with deionized water and ethanol, and allowed to stand for 5 h. The mixture was filtered with deionized water and anhydrous ethanol in turn, washed, and freeze-dried to obtain modified carbon black.

[0027] Example 2

[0028] This embodiment provides a modified carbon black, and the preparation steps are as follows:

[0029] 0.012 g of carbon black (particle size of 120 μm) and 0.42 g of CTAB were added to 120 mL of deionized water, and ultrasonically stirred for 10 min. 1 mL of concentrated hydrochloric acid was added, and stirred for 10 min under ice-water bath conditions. 0.24 g of pyrrole was added, and the reaction was stirred for 15 min. 0.82 g of ammonium persulfate was added, and stirring was continued for 24 h. The mixture was diluted with deionized water and ethanol, and allowed to stand for 5 h. The mixture was filtered with deionized water and anhydrous ethanol in turn, washed, and freeze-dried to obtain modified carbon black.

[0030] Comparative Example 1

[0031] This embodiment provides a modified carbon black, and the preparation steps are as follows:

[0032] 0.012 g of carbon black (particle size of 120 μm) was added to 120 mL of deionized water, ultrasonically stirred for 10 min, filtered, washed, and freeze-dried to obtain modified carbon black.

[0033] Example 3

[0034] This embodiment provides an antistatic adhesive, comprising the following raw materials in parts by weight:

[0035] 35 parts of methyl acrylate, 15 parts of acrylic acid, 0.1 parts of benzoyl peroxide, 0.2 parts of N,N-methylenebisacrylamide, 5 parts of carbon nanotubes (particle size is 200nm), 3 parts of modified carbon black in Example 1, and 60 parts of toluene.

[0036] The preparation steps are as follows:

[0037] Methyl acrylate, acrylic acid and benzoyl peroxide were added to the solvent by weight, the temperature was raised to 65° C., and the mixture was stirred and mixed. N,N-methylenebisacrylamide, carbon nanotubes and the modified carbon black in Example 1 were then added, the mixture was further mixed, and the mixture was cooled to obtain an antistatic adhesive.

[0038] Example 4

[0039] This embodiment provides an antistatic adhesive, comprising the following raw materials in parts by weight:

[0040] 35 parts of methyl acrylate, 15 parts of acrylic acid, 0.1 parts of benzoyl peroxide, 0.2 parts of N,N-methylenebisacrylamide, 5 parts of carbon nanotubes (particle size is 200nm), 3 parts of modified carbon black in Example 2, and 60 parts of toluene.

[0041] The preparation steps are as follows:

[0042] Methyl acrylate, acrylic acid and benzoyl peroxide were added to the solvent by weight, the temperature was raised to 65° C., and the mixture was stirred and mixed. N,N-methylenebisacrylamide, carbon nanotubes and the modified carbon black in Example 2 were then added, the mixture was continued to be mixed, and the mixture was cooled to obtain an antistatic adhesive.

[0043] Example 5

[0044] The only difference from Example 3 is that:

[0045] 3 parts of the modified carbon black in Example 1 were replaced with 6 parts of the modified carbon black in Example 1, and the remaining raw materials and steps were the same as those in Example 3.

[0046] Example 6

[0047] This embodiment provides an antistatic adhesive, comprising the following raw materials in parts by weight:

[0048] 45 parts of methyl methacrylate, 10 parts of hydroxyethyl acrylate, 0.3 parts of azobisisobutyronitrile, 0.5 parts of N,N-methylenebisacrylamide, 8 parts of carbon nanotubes (particle size of 300nm), 5 parts of modified carbon black in Example 1, and 70 parts of ethyl acetate.

[0049] The preparation steps are as follows:

[0050] Methyl methacrylate, hydroxyethyl acrylate and azobisisobutyronitrile were added to ethyl acetate by weight, the temperature was raised to 75° C., and the mixture was stirred and mixed. N,N-methylenebisacrylamide, carbon nanotubes and the modified carbon black in Example 1 were then added, the mixture was continued to be mixed, and the mixture was cooled to obtain an antistatic adhesive.

[0051] Example 7

[0052] This embodiment provides an antistatic adhesive, comprising the following raw materials in parts by weight:

[0053] 25 parts of methyl acrylate, 25 parts of butyl acrylate, 10 parts of acrylic acid, 10 parts of hydroxypropyl methacrylate, 0.3 parts of azobisisobutyronitrile, 0.5 parts of N,N-methylenebisacrylamide, 6 parts of carbon nanotubes (particle size 400nm), 6 parts of modified carbon black in Example 1, and 75 parts of ethyl acetate.

[0054] The preparation steps are as follows:

[0055] Methyl acrylate, butyl acrylate, acrylic acid, hydroxypropyl methacrylate and azobisisobutyronitrile were added to ethyl acetate by weight, the temperature was raised to 85° C., and the mixture was stirred and mixed. N,N-methylenebisacrylamide, carbon nanotubes and the modified carbon black in Example 1 were then added, the mixture was continued to be mixed, and the mixture was cooled to obtain an antistatic adhesive.

[0056] Comparative Example 2

[0057] The only difference from Example 3 is that:

[0058] Three parts of the modified carbon black in Example 1 were replaced by three parts of the modified carbon black in Comparative Example 1, and the remaining raw materials and steps were the same as those in Example 3.

[0059] Comparative Example 3

[0060] This comparative example provides an antistatic adhesive, comprising the following raw materials in parts by weight:

[0061] 35 parts of methyl acrylate, 15 parts of acrylic acid, 0.1 parts of benzoyl peroxide, 0.2 parts of N,N-methylenebisacrylamide, 5 parts of carbon nanotubes (particle size: 200 nm), and 60 parts of toluene.

[0062] The preparation steps are as follows:

[0063] Methyl acrylate, acrylic acid and benzoyl peroxide are added to a solvent by weight, the temperature is raised to 65° C., and the mixture is stirred and mixed. N,N-methylenebisacrylamide and carbon nanotubes are then added, the mixture is further mixed, and the mixture is cooled to obtain an antistatic adhesive.

[0064] Comparative Example 4

[0065] The only difference from Example 3 is that:

[0066] 3 parts of the modified carbon black in Example 1 were replaced with 1.5 parts of the modified carbon black in Example 1, and the remaining raw materials and steps were the same as those in Example 3.

[0067] Comparative Example 5

[0068] The only difference from Example 5 is that:

[0069] 6 parts of the modified carbon black in Example 1 were replaced with 7.5 parts of the modified carbon black in Example 1, and the remaining raw materials and steps were the same as those in Example 5.

[0070] Comparative Example 6

[0071] This comparative example provides an antistatic adhesive, comprising the following raw materials in parts by weight:

[0072] 60 parts of methyl acrylate, 5 parts of acrylic acid, 0.1 parts of benzoyl peroxide, 0.2 parts of N,N-methylenebisacrylamide, 5 parts of carbon nanotubes (particle size is 200nm), 3 parts of modified carbon black in Example 1, and 60 parts of toluene.

[0073] The preparation steps are as follows:

[0074] Methyl acrylate, acrylic acid and benzoyl peroxide were added to the solvent by weight, the temperature was raised to 65° C., and the mixture was stirred and mixed. N,N-methylenebisacrylamide, carbon nanotubes and the modified carbon black in Example 1 were then added, the mixture was further mixed, and the mixture was cooled to obtain an antistatic adhesive.

[0075] The performance test of the antistatic adhesive obtained in Example 3 to Example 7 and Comparative Example 2 to Comparative Example 6 was carried out:

[0076] The obtained antistatic adhesive was coated on the surface of a 25 μm thick high-transparent PET film. After the adhesive was coated, a 25 μm transparent PET release film was covered on the surface of the adhesive layer. The film was irradiated under a 365 nm UVLED surface light source for 15 min at a light intensity of 400 mW / cm 2 , take it out, place it at room temperature for 72 hours, and then perform the following performance tests:

[0077] 1) Film surface resistivity: tested using FT-303 surface resistivity tester from Zhejiang Ningbo Ruike Weiye Instrument Co., Ltd., with a test voltage of 100V.

[0078] 2) 180° peel strength: KJ-1065 series computerized material tensile testing machine produced by Dongguan Kejian Testing Instrument Co., Ltd. was used, with a tensile speed of 300 mm / min.

[0079] The above test results are shown in Table 1:

[0080] Table 1

[0081]

[0082]

[0083] As can be seen from Table 1, compared with Comparative Examples 2-6, the antistatic adhesive prepared in Examples 3-7 has a lower surface resistivity and a higher peel strength. By comparing Examples 3-4 with Comparative Examples 2-3 and in combination with Table 1, it can be seen that the modified carbon black in Examples 1 and 2 is added to Examples 3 and 4, respectively, and the modified carbon black in Comparative Example 1 is added to Comparative Example 2, and no modified carbon black is added to Comparative Example 3. It can be seen from Comparative Example 2 and Example 3 that the carbon black modified by the polypyrrole coating surface has excellent dispersion performance, and polypyrrole also has certain conductivity, which will not affect the original anti-electrical performance, and can be beneficial to the dispersion of carbon black, thereby enhancing the antistatic performance of the antistatic adhesive. It can be seen from Comparative Example 3 and Example 3 that the addition of modified carbon black effectively fills the gaps between carbon nanotubes, promotes the formation of conductive paths, and effectively improves the antistatic effect in the antistatic adhesive. It can be seen from Comparative Example 4 and Example 3, Comparative Example 5 and Example 5 in combination with Table 1 that 1.5 parts of the modified carbon black in Example 1 are added in Comparative Example 4, and 7.5 parts of the modified carbon black in Example 1 are added in Comparative Example 5. It can be seen that the amount of modified carbon black also affects the antistatic performance and bonding performance of the antistatic adhesive. In summary, it can be seen that the antistatic adhesive obtained in the present invention has excellent antistatic performance and peel strength.

[0084] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0085] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An antistatic adhesive, characterized in that: It includes the following raw materials in parts by weight: 30-50 parts of non-functional acrylate monomer, 10-20 parts of functional acrylate monomer, 0.1-0.5 parts of initiator, 0.1-1 parts of crosslinking agent, 5-10 parts of carbon nanotubes, 3-6 parts of modified carbon black, 60-80 parts of solvent; The modified carbon black is prepared by the following steps: Add carbon black and hexadecyltrimethylammonium bromide into deionized water, stir ultrasonically, add concentrated hydrochloric acid, pyrrole and ammonium persulfate, continue stirring, dilute and let stand, filter and wash, and freeze-dry to obtain modified carbon black.

2. The antistatic adhesive according to claim 1, characterized in that: The usage ratio of carbon black, hexadecyltrimethylammonium bromide, deionized water, concentrated hydrochloric acid and pyrrole is 0.01-0.012 g: 0.41-0.42 g: 120 mL: 1 mL: 0.23-0.235 g.

3. The antistatic adhesive according to claim 1, characterized in that: The particle size of the carbon black is 100-150 μm.

4. The antistatic adhesive according to claim 1, characterized in that: The non-functional acrylic acid ester monomer is at least one of methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate and butyl methacrylate.

5. The antistatic adhesive according to claim 1, characterized in that: The functional acrylate monomer is at least one of acrylic acid, hydroxyethyl acrylate, methacrylic acid, hydroxyethyl methacrylate and hydroxypropyl methacrylate.

6. The antistatic adhesive according to claim 1, characterized in that: The initiator is at least one of benzoyl peroxide, cumene hydroperoxide and azobisisobutyronitrile.

7. The antistatic adhesive according to claim 1, characterized in that: The cross-linking agent is N,N-methylenebisacrylamide.

8. The antistatic adhesive according to claim 1, characterized in that: The solvent is at least one of toluene, ethyl acetate, butyl acetate, acetone and methanol.

9. The antistatic adhesive according to claim 1, characterized in that: The particle size of the carbon nanotubes is 200-400nm.

10. The method for preparing an antistatic adhesive according to claim 1, characterized in that: The following steps are involved: According to weight, non-functional acrylate monomer, functional acrylate monomer and initiator are added to the solvent, heated to 65-85° C., stirred and mixed, and then a crosslinking agent, carbon nanotubes and modified carbon black are added, and the mixture is continuously mixed and cooled to obtain an antistatic adhesive.