Low-modulus and high-viscosity adhesive, preparation method thereof and adhesive tape
By adjusting the components and molecular weight of the acrylate copolymer and acrylate oligomer, and combining cross-linking and coupling agents, the problem of balancing the adhesion and cohesion of low-modulus adhesives and the problem of small molecule migration in the existing technology was solved, and a High-tack adhesives and tapes that achieve good aging resistance and tack properties.
Patent Information
- Application Number
- CN202411007175.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-15
AI Technical Summary
It is difficult for existing folded OCA to balance adhesion and cohesion under low modulus conditions, and there is also the risk of small molecule migration and rework that easily leaves adhesive residue.
By designing the components and molecular weight of acrylate copolymers and acrylate oligomers, combined with the use of cross-linking and coupling agents, the wetting characteristics of the adhesive are adjusted to prepare low-modulus, high-viscosity adhesives, and use specific The preparation method of the adhesive tape ensures the compatibility and low migration of the adhesive.
It achieves the requirements of adhesion and no residual glue under low modulus conditions, and improves the aging resistance and viscosity performance of the product.
Smart Images

Figure BDA0004963302740000071 
Figure BDA0004963302740000091 
Figure BDA0004963302740000092
Abstract
Description
Technical Field
[0001] The invention relates to the field of adhesive materials, and in particular to a low-modulus, high-viscosity adhesive, a preparation method thereof and an adhesive tape. Background Art
[0002] In recent years, with the continuous advancement of technology, thinner and lighter, foldable electronic devices have gradually become popular. As electronic devices become thinner and lighter, the film materials used in corresponding display devices also need to be developed to be thinner and lighter. With the diversification and thinness of foldable products, the number of portable bag-type foldable electronic products has gradually increased. In order to better protect foldable electronic products, attaching folding protective films on their folding display screens has gradually become a demand of more and more people.
[0003] The main problems of the existing technology are: the existing folding OCA is mainly synthesized by solvent method and UV method. The solvent method has the disadvantage that it cannot take into account both adhesion and cohesion under the conditions of low temperature and low modulus. The folding glue obtained by the UV method has the risk of small molecule migration and residual glue in later rework. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a low modulus, high viscosity adhesive, a preparation method thereof and an adhesive tape in view of the above-mentioned deficiencies in the prior art. The present invention adjusts the wetting properties of the adhesive by controlling the cross-linking method and the method of adding oligomers while ensuring the low modulus of the main body, thereby taking into account the requirements of adhesion, low modulus and no residual adhesive.
[0005] To achieve the above object, the technical solution adopted by the present invention is: in the first aspect of the present invention, a low modulus, high viscosity adhesive is provided, comprising the following raw material components in parts by weight: 100 parts of acrylate copolymer, 0.2-10 parts of acrylate oligomer, 0.005-0.5 parts of crosslinking agent, and 0-0.5 parts of coupling agent;
[0006] The acrylate copolymer and acrylate oligomer are both obtained by polymerizing soft monomers, functional monomers and crosslinking monomers under the action of an initiator.
[0007] Preferably, the soft monomer is selected from at least one of isooctyl (meth)acrylate, n-butyl acrylate, and methoxy polyethylene glycol acrylate.
[0008] Preferably, the functional monomer is selected from at least one of dimethyl acrylamide, diethyl acrylamide, tetrahydrofuran (meth) acrylate, phenoxyethyl (meth) acrylate, N-vinyl pyrrolidone, glycerol formal (meth) acrylate, isobornyl acrylate, cyclotrimethylolpropane formal acrylate, (2-ethyl-2-methyl-1,3-dioxolan-4-yl) acrylate, and 3-ethyl-3-epoxypropyl methyl acrylate.
[0009] Preferably, the crosslinking monomer is a hydroxyl-containing monomer selected from at least one of hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyoctyl (meth)acrylate.
[0010] Preferably, the raw materials for preparing the acrylic ester copolymer include, by weight:
[0011] Soft monomer 75-98 parts, functional monomer 0.1-20% parts, cross-linking monomer 0.1-10% parts, initiator 0.02-0.4 parts, solvent 50-200 parts;
[0012] Among them, the mass ratio of functional monomer: cross-linking monomer does not exceed 1.5.
[0013] Preferably, the preparation method of the acrylate copolymer is:
[0014] Dissolve the soft monomer, functional monomer and crosslinking monomer in a solvent, introduce nitrogen for 0.5-2h, heat to 50-70°C, add part of the initiator, react for 3-12h, then add the remaining initiator, heat to 72-80°C, react for 1-4h, cool to room temperature after the reaction, dilute the product to a solid content of 15-40%, and obtain an acrylate copolymer;
[0015] The weight average molecular weight of the acrylic ester copolymer is 100-200W, and the PDI is 1.5-10.
[0016] Preferably, the soft monomer in the raw materials for preparing the acrylic ester copolymer is isooctyl acrylate, the functional monomer is dimethyl acryloyl, and the cross-linking monomer is hydroxyethyl acrylate.
[0017] Preferably, the raw materials for preparing the acrylate oligomer include, by weight:
[0018] 75-98 parts of soft monomer, 0.1-20% of functional monomer, 0.1-10% of cross-linking monomer, 0.5-1 part of initiator, and 50-200 parts of solvent.
[0019] Preferably, the preparation method of the acrylate oligomer is:
[0020] The soft monomer, the functional monomer and the cross-linking monomer are dissolved in a solvent, nitrogen is introduced for 0.5-2 hours, the mixture is heated to 50-80° C., an initiator is added, the mixture is reacted for 4-8 hours, after the reaction is completed, the mixture is cooled to room temperature, and the product is diluted to a solid content of 15-40% to obtain an acrylate oligomer;
[0021] The weight average molecular weight of the acrylic ester oligomer is 0.5-30W, and the PDI is 1-5.
[0022] Preferably, the soft monomer in the raw materials for preparing the acrylic ester oligomer is a mixture of isooctyl acrylate and n-butyl acrylate, the functional monomer is diethylacrylamide, and the crosslinking monomer is hydroxyethyl acrylate.
[0023] A second aspect of the present invention provides a method for preparing the low modulus, high viscosity adhesive as described above, comprising the following steps:
[0024] By weight, 100 parts of acrylate copolymer, 0.2-10 parts of acrylate oligomer, 0.005-0.5 parts of crosslinking agent and 0-0.5 parts of coupling agent are mixed and stirred evenly to obtain the low modulus and high viscosity adhesive.
[0025] The third aspect of the present invention provides a low modulus, high viscosity tape, which is prepared by the following method: the low modulus, high viscosity adhesive as described above is evenly coated on the base film, the dry adhesive thickness is controlled to be 10-40 μm, and dried at 80-120°C for 2-5 min. A release film is attached to the adhesive surface, and the adhesive surface is aged at 50-70°C for 1-4 days to obtain the low modulus, high viscosity tape.
[0026] The beneficial effects of the present invention are:
[0027] The present invention provides a low modulus, high viscosity adhesive and an adhesive tape product based on the adhesive. The present invention designs the components and molecular weight of an acrylate oligomer so that the acrylate oligomer and the acrylate copolymer have good compatibility and low migration, and can ensure that the product performance is met while making the product have good aging resistance. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.
[0029] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0030] The test methods used in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are all commercially available unless otherwise specified. In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0031] The present invention provides a low modulus, high viscosity adhesive, comprising the following raw material components in parts by weight: 100 parts of an acrylate copolymer, 0.2-10 parts of an acrylate oligomer, 0.005-0.5 parts of a crosslinking agent, and 0-0.5 parts of a coupling agent;
[0032] Both acrylate copolymers and acrylate oligomers are obtained by polymerizing soft monomers, functional monomers and crosslinking monomers under the action of an initiator.
[0033] In a preferred embodiment, the soft monomer is at least one of alkyl acrylate monomers (including ethyl, propyl, butyl, pentyl, heptyl, octyl, nonyl, decyl, polyalkyl and isomers thereof), preferably with an average carbon atom of 3-12, and preferably isomers with more than 8 carbon atoms. In a further preferred embodiment, the soft monomer is selected from at least one of isooctyl (meth)acrylate, n-butyl acrylate, and methoxy polyethylene glycol acrylate. Wherein, isooctyl (meth)acrylate is represented as isooctyl acrylate or isooctyl methacrylate, and this method is also used in other places throughout the text for the convenience of simple description.
[0034] In a preferred embodiment, the functional monomer is preferably a low Tg amide-containing monomer, for example, the functional monomer is selected from at least one of tetrahydrofuran (meth)acrylate, phenoxyethyl (meth)acrylate, N-vinyl pyrrolidone, glycerol formal (meth)acrylate, isobornyl acrylate, cyclotrimethylolpropane formal acrylate, (2-ethyl-2-methyl-1,3-dioxolane-4-yl)acrylate, 3-ethyl-3-epoxypropyl methyl acrylate, dimethylacrylamide, diethylacrylamide (oxygen-containing heterocycle, ether bond, nitrogen-containing heterocycle, amide group), etc.
[0035] In a preferred embodiment, the crosslinking monomer is a hydroxyl-containing monomer selected from at least one of hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyoctyl (meth)acrylate, more preferably at least one of hydroxyethyl (meth)acrylate and hydroxybutyl (meth)acrylate.
[0036] In a preferred embodiment, the initiator is at least one of an azo initiator (such as azobisisobutyronitrile) and a peroxide initiator (benzoyl peroxide).
[0037] In a preferred embodiment, the raw materials for preparing the acrylic ester copolymer include, by weight:
[0038] Soft monomer 75-98 parts, functional monomer 0.1-20% parts, cross-linking monomer 0.1-10% parts, initiator 0.02-0.4 parts, solvent 50-200 parts;
[0039] In order to ensure that the modulus is within the design range, the mass ratio of functional monomer: cross-linking monomer shall not exceed 1.5.
[0040] In a preferred embodiment, the preparation method of the acrylate copolymer is:
[0041] Dissolve the soft monomer, functional monomer and crosslinking monomer in a solvent, introduce nitrogen for 0.5-2h, heat to 50-70°C, add part of the initiator, react for 3-12h, then add the remaining initiator, heat to 72-80°C, react for 1-4h, cool to room temperature after the reaction, dilute the product to a solid content of 15-40%, and obtain an acrylate copolymer;
[0042] The weight average molecular weight of the acrylic ester copolymer is 100-200W, and the PDI is 1.5-10.
[0043] In a preferred embodiment, the raw materials for preparing the acrylic ester copolymer include the soft monomer is isooctyl acrylate, the functional monomer is dimethyl acryloyl, and the cross-linking monomer is hydroxyethyl acrylate.
[0044] In a preferred embodiment, the raw materials for preparing the acrylate oligomer include, by weight:
[0045] 75-98 parts of soft monomer, 0.1-20% of functional monomer, 0.1-10% of cross-linking monomer, 0.5-1 part of initiator, and 50-200 parts of solvent.
[0046] In a preferred embodiment, the preparation method of the acrylate oligomer is:
[0047] The soft monomer, the functional monomer and the cross-linking monomer are dissolved in a solvent, nitrogen is introduced for 0.5-2 hours, the mixture is heated to 50-80° C., an initiator is added, the mixture is reacted for 4-8 hours, after the reaction is completed, the mixture is cooled to room temperature, and the product is diluted to a solid content of 15-40% to obtain an acrylate oligomer;
[0048] The weight average molecular weight of the acrylate oligomer is 0.5-30W, and the PDI is 1-5.
[0049] In a preferred embodiment, the soft monomer in the raw material for preparing the acrylate oligomer is a mixture of isooctyl acrylate and n-butyl acrylate, the functional monomer is diethylacrylamide, and the crosslinking monomer is hydroxyethyl acrylate.
[0050] In a preferred embodiment, the crosslinking agent is selected from at least one of isocyanate crosslinking agents (preferably aliphatic polyisocyanates), epoxy adhesives, imide adhesives, multifunctional metal chelates, and polyurethane crosslinking agents.
[0051] In a preferred embodiment, the coupling agent is selected from at least one of 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltrihexyloxysilane, 3-methacryloxypropyltrimethoxysilane, KH570, etc. Adding the coupling agent can improve durability.
[0052] The present invention also provides a method for preparing the above low modulus, high viscosity adhesive, comprising the following steps:
[0053] By weight, 100 parts of acrylate copolymer, 0.2-10 parts of acrylate oligomer, 0.005-0.5 parts of crosslinking agent and 0-0.5 parts of coupling agent are mixed and stirred evenly to obtain a low modulus and high viscosity adhesive.
[0054] The present invention also provides a low modulus, high viscosity tape, which is prepared by the following method: uniformly coating the low modulus, high viscosity adhesive according to any one of claims 1 to 10 on a base film, controlling the dry adhesive thickness to be 10-40 μm, drying at 80-120° C. for 2-5 min, attaching a release film to the adhesive surface, and aging at 50-70° C. for 1-4 days to obtain a low modulus, high viscosity tape.
[0055] The above is the overall concept of the present invention, and detailed embodiments and comparative examples are provided below on the basis of the overall concept of the present invention to further illustrate the present invention.
[0056] Acrylate polymer A and several different acrylate oligomers, denoted as acrylate oligomers a, b, c, and d, were prepared in advance according to the following method.
[0057] 1. Acrylate polymer A
[0058] 100g of ethyl acetate, 80g of isooctyl acrylate (soft monomer), 5g of dimethyl acrylamide (functional monomer), and 10g of hydroxyethyl acrylate (cross-linking monomer) were put into a flask, and nitrogen was introduced for 1 hour. After the temperature was raised to 60°C, 0.05g of BPO was added. After the reaction was continued for 6 hours, 0.03g of BPO was added, and the temperature was raised to 78°C and the reaction was continued for 2 hours. After the reaction was completed, the temperature was cooled to room temperature and diluted with ethyl acetate to a solid content of 35%, to obtain an acrylate copolymer A.
[0059] 2-1. Acrylate oligomer a
[0060] 100g of ethyl acetate, 55g of n-butyl acrylate (soft monomer), 20g of isooctyl acrylate (soft monomer), 20g of diethyl acrylamide (functional monomer), and 5g of hydroxyethyl acrylate (cross-linking monomer) are put into a flask, and nitrogen is introduced for 1 hour. After the temperature is raised to 78°C, 2g of BPO is added and the reaction is carried out for 4 hours. After the reaction is completed, the temperature is cooled to room temperature and diluted with ethyl acetate to a solid content of 35% to obtain acrylate oligomer a.
[0061] 2-2, Acrylate oligomer b
[0062] 100g of ethyl acetate, 55g of n-butyl acrylate, 20g of isooctyl acrylate, 20g of diethylacrylamide, and 5g of hydroxyethyl acrylate are put into a flask, and nitrogen is introduced for 1h. After the temperature is raised to 78°C, 1g of BPO is added and the reaction is carried out for 4h. After the reaction is completed, the temperature is cooled to room temperature and diluted with ethyl acetate to a solid content of 35% to obtain acrylate oligomer b.
[0063] 2-3. Acrylate oligomer c
[0064] 100g of ethyl acetate, 55g of n-butyl acrylate, 20g of isooctyl acrylate, 20g of diethylacrylamide, and 5g of hydroxyethyl acrylate are put into a flask, and nitrogen is introduced for 1h. After the temperature is raised to 78°C, 0.2g of BPO is added and the reaction is carried out for 4h. After the reaction is completed, the temperature is cooled to room temperature and diluted with ethyl acetate to a solid content of 35% to obtain acrylate oligomer c.
[0065] 2-4, Acrylate oligomer d
[0066] 100 g of ethyl acetate, 65 g of n-butyl acrylate, 20 g of isooctyl acrylate, 10 g of acrylic acid, and 5 g of hydroxyethyl acrylate were placed in a flask, and nitrogen was introduced for 1 hour. After the temperature was raised to 78°C, 0.2 g of BPO was added and the reaction was carried out for 4 hours. After the reaction was completed, the temperature was cooled to room temperature and diluted with ethyl acetate to a solid content of 35% to obtain acrylate oligomer d.
[0067] The performance indicators of the above polymers are shown in Table 1 below:
[0068] Table 1
[0069]
[0070] The molecular weight test was performed using gel chromatography (GPC) using a gel chromatograph Waters GPC1515.
[0071] Example 1
[0072] A low modulus, high viscosity tape is prepared by the following method:
[0073] By weight, 100 parts of acrylate copolymer A, 5 parts of acrylate oligomer a, 0.2 parts of toluene diisocyanate, and 0.02 parts of 3-(2,3-epoxypropoxy)propyltrimethoxysilane were mixed and stirred to obtain a low modulus, high viscosity adhesive;
[0074] The adhesive was evenly coated on a 50 μm PET film, the dry adhesive thickness was controlled to be 25 μm, and dried at 120° C. for 3 min. A release film was attached to the adhesive surface, and aged at 70° C. for 2 days to obtain the low modulus, high viscosity tape, which was recorded as sample Ab.
[0075] Example 2
[0076] A low modulus, high viscosity tape is prepared by the following method:
[0077] By weight, 100 parts of acrylate copolymer A, 5 parts of acrylate oligomer b, 0.2 parts of toluene diisocyanate, and 0.02 parts of 3-(2,3-epoxypropoxy)propyltrimethoxysilane were mixed and stirred to obtain a low modulus, high viscosity adhesive;
[0078] The adhesive was evenly coated on a 50 μm PET film, the dry adhesive thickness was controlled to be 25 μm, and dried at 120° C. for 3 min. A release film was attached to the adhesive surface and aged at 70° C. for 2 days to obtain the low modulus, high viscosity tape, which was recorded as sample Ac.
[0079] Comparative Example 1
[0080] A low modulus, high viscosity tape is prepared by the following method:
[0081] By weight, 100 parts of acrylate copolymer A, 5 parts of acrylate oligomer a, 0.2 parts of toluene diisocyanate, and 0.02 parts of 3-(2,3-epoxypropoxy)propyltrimethoxysilane were mixed and stirred to obtain a low modulus, high viscosity adhesive;
[0082] The adhesive was evenly coated on a 50 μm PET film, the dry adhesive thickness was controlled to be 25 μm, and dried at 120° C. for 3 min. A release film was attached to the adhesive surface and aged at 70° C. for 2 days to obtain the low modulus, high viscosity tape, which was recorded as sample Aa.
[0083] Comparative Example 2
[0084] A low modulus, high viscosity tape is prepared by the following method:
[0085] By weight, 100 parts of acrylate copolymer A, 0.2 parts of toluene diisocyanate, and 0.02 parts of 3-(2,3-epoxypropoxy)propyltrimethoxysilane were mixed and stirred evenly to obtain a low modulus, high viscosity adhesive;
[0086] The adhesive was evenly coated on a 50 μm PET film, the dry adhesive thickness was controlled to be 25 μm, and dried at 120° C. for 3 min. A release film was attached to the adhesive surface and aged at 70° C. for 2 days to obtain the low modulus, high viscosity tape, which was recorded as sample A.
[0087] Comparative Example 3
[0088] A low modulus, high viscosity tape is prepared by the following method:
[0089] By weight, 100 parts of acrylate copolymer A, 5 parts of acrylate oligomer d, 0.2 parts of toluene diisocyanate, and 0.02 parts of 3-(2,3-epoxypropoxy)propyltrimethoxysilane were mixed and stirred to obtain a low modulus, high viscosity adhesive;
[0090] The adhesive was evenly coated on a 50 μm PET film, the dry adhesive thickness was controlled to be 25 μm, and dried at 120° C. for 3 min. A release film was attached to the adhesive surface, and aged at 70° C. for 2 days to obtain the low modulus, high viscosity tape, which was recorded as sample Ad.
[0091] The peeling force, haze and aging performance tests were performed on the tape samples of Examples 1-2 and Comparative Examples 1-3. The test results are shown in Tables 2 and 3 below:
[0092] Table 2 Peel force and haze before aging
[0093]
[0094] Table 3 Peel strength and haze after aging at 85℃ / 85% for 7 days
[0095]
[0096] Among them, the peel force is tested according to ASTM D 3330, the transmittance and haze test standard is ASTM D1003, and the test instrument is WGT-S transmittance and haze tester;
[0097] The aging performance test method is to place the sample under 85°C temperature / 85% humidity conditions for 7 days and then re-test each item to compare the stability of the performance before and after aging.
[0098] According to the test results in Table 2 and Table 3:
[0099] In Comparative Example 2, no acrylate oligomer was added, and the viscosity after curing was not high, indicating that the acrylate oligomer can greatly improve the viscosity of the adhesive;
[0100] When glue is matched with different oligomers, when the type of oligomer is incompatible with the polymer, the glue will become foggy, as shown in Comparative Example 3;
[0101] When the molecular weight of the glue is too small, residual glue is easy to form and the performance is unstable after aging, such as Comparative Example 1; when the molecular weight is too large, the polymer is not easy to disperse and a good viscosity-increasing effect cannot be achieved, such as Comparative Example 3.
[0102] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A low modulus, high viscosity adhesive, It is characterized in that The invention comprises the following raw material components in parts by weight: 100 parts of acrylate copolymer, 0.2-10 parts of acrylate oligomer, 0.005-0.5 parts of crosslinking agent and 0-0.5 parts of coupling agent; The acrylate copolymer and acrylate oligomer are both obtained by polymerizing soft monomers, functional monomers and crosslinking monomers under the action of an initiator.
2. The low modulus, high viscosity adhesive according to claim 1, It is characterized in that The soft monomer is selected from at least one of isooctyl (meth)acrylate, n-butyl acrylate, and methoxy polyethylene glycol acrylate.
3. The low modulus, high viscosity adhesive according to claim 1, It is characterized in that The functional monomer is selected from at least one of dimethyl acrylamide, diethyl acrylamide, tetrahydrofuran (meth) acrylate, phenoxyethyl (meth) acrylate, N-vinyl pyrrolidone, glycerol formal (meth) acrylate, isobornyl acrylate, cyclotrimethylolpropane formal acrylate, (2-ethyl-2-methyl-1,3-dioxolan-4-yl) acrylate, and 3-ethyl-3-epoxypropyl methyl acrylate.
4. The low modulus, high viscosity adhesive according to claim 1, It is characterized in that The crosslinking monomer is a hydroxyl-containing monomer selected from at least one of hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyoctyl (meth)acrylate.
5. The low modulus, high viscosity adhesive according to claim 1, It is characterized in that The raw materials for preparing the acrylic ester copolymer include, by weight: Soft monomer 75-98 parts, functional monomer 0.1-20% parts, cross-linking monomer 0.1-10% parts, initiator 0.02-0.4 parts, solvent 50-200 parts; Among them, the mass ratio of functional monomer: cross-linking monomer does not exceed 1.
5.
6. The low modulus, high viscosity adhesive according to claim 5, It is characterized in that The preparation method of the acrylic acid ester copolymer is as follows: Dissolve the soft monomer, functional monomer and crosslinking monomer in a solvent, introduce nitrogen for 0.5-2h, heat to 50-70°C, add part of the initiator, react for 3-12h, then add the remaining initiator, heat to 72-80°C, react for 1-4h, cool to room temperature after the reaction, dilute the product to a solid content of 15-40%, and obtain an acrylate copolymer; The weight average molecular weight of the acrylic ester copolymer is 100-200W, and the PDI is 1.5-10.
7. The low modulus, high viscosity adhesive according to claim 6, It is characterized in that The raw materials for preparing the acrylic ester copolymer include isooctyl acrylate as the soft monomer, dimethyl acryloyl as the functional monomer, and hydroxyethyl acrylate as the cross-linking monomer.
8. The low modulus, high viscosity adhesive according to claim 1, It is characterized in that The raw materials for preparing the acrylic ester oligomer include, by weight: 75-98 parts of soft monomer, 0.1-20% of functional monomer, 0.1-10% of cross-linking monomer, 0.5-1 part of initiator, and 50-200 parts of solvent.
9. The low modulus, high viscosity adhesive according to claim 8, It is characterized in that The preparation method of the acrylate oligomer is: The soft monomer, the functional monomer and the cross-linking monomer are dissolved in a solvent, nitrogen is introduced for 0.5-2 hours, the mixture is heated to 50-80° C., an initiator is added, the mixture is reacted for 4-8 hours, after the reaction is completed, the mixture is cooled to room temperature, and the product is diluted to a solid content of 15-40% to obtain an acrylate oligomer; The weight average molecular weight of the acrylic ester oligomer is 0.5-30W, and the PDI is 1-5.
10. The low modulus, high viscosity adhesive according to claim 9, It is characterized in that The soft monomer in the raw materials for preparing the acrylic ester oligomer is a mixture of isooctyl acrylate and n-butyl acrylate, the functional monomer is diethyl acrylamide, and the crosslinking monomer is hydroxyethyl acrylate.
11. A method for preparing a low modulus, high viscosity adhesive as claimed in any one of claims 1 to 10, It is characterized in that The following steps are involved: By weight, 100 parts of acrylate copolymer, 0.2-10 parts of acrylate oligomer, 0.005-0.5 parts of crosslinking agent and 0-0.5 parts of coupling agent are mixed and stirred evenly to obtain the low modulus and high viscosity adhesive.
12. A low modulus, high viscosity tape, It is characterized in that The low modulus, high viscosity adhesive tape is prepared by the following method: the low modulus, high viscosity adhesive as described in any one of claims 1 to 10 is evenly coated on the base film, the dry adhesive thickness is controlled to be 10-40 μm, and the adhesive is dried at 80-120° C. for 2-5 min. A release film is attached to the adhesive surface, and the adhesive is aged at 50-70° C. for 1-4 days to obtain the low modulus, high viscosity adhesive tape.
Citation Information
Patent Citations
Low-modulus flexible acrylate adhesive and preparation method thereof
CN111073525A
Adhesive film suitable for plastic image display device
CN115895494A
Acrylate chip adhesive and application thereof
CN115960576A
UV visbreaking adhesive and preparation method thereof
CN116042140A
Normal-temperature high-modulus ultraviolet imprinting adhesive and preparation method thereof
CN116478650A
Cited By
Photocuring high-temperature-resistant optical fiber coating and preparation method thereof
CN119264813A