Preparation method of high-strength silicone structural adhesive

By using nano-graphene oxide and nano-alumina, multi-metal composite catalysts and flexible plasticizers in silicone structural adhesives, and using ultrasonic dispersion technology, the insufficient mechanical properties and uneven curing of silicone structural adhesives under high stress are solved. problem, significantly improving its tensile strength, tear resistance and service life.

CN118772834AInactive Publication Date: 2024-10-15GUANGDONG ZHONGSI NEW MATERIAL CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410951997.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing silicone structural adhesives suffer from insufficient mechanical properties, uneven curing reaction, poor flexibility and durability under high stress and high load conditions, and uneven dispersion of nanofillers.

Method used

Nano-graphene oxide and nano-alumina are used as fillers, a multi-metal composite catalyst system composed of platinum, tin and titanium is used, a flexible polysiloxane plasticizer is introduced, and the nano-fillers are processed through ultrasonic dispersion technology, combined with a cross-linking agent and dehydrating agents to form a tight and uniform cross-linked network.

Benefits of technology

Significantly improves the tensile strength, tear resistance, curing reaction rate and overall performance of silicone structural adhesive, extends the service life, ensures uniform dispersion of fillers and material consistency, and is suitable for use in high stress and complex environments. application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772834A_ABST
    Figure CN118772834A_ABST
Patent Text Reader

Abstract

The invention relates to the field of organosilicon chemistry and material science, and discloses a high-strength silicone structural adhesive, which comprises 30-60 parts of a silicone base polymer, 1-10 parts of a cross-linking agent, 5-20 parts of a plasticizer, 10-40 parts of a filler and 0.1-5 parts of nano graphene oxide, the invention relates to a high-temperature-resistant and high-pressure-resistant adhesive which is prepared from the following components in parts by weight: 0.1-5 parts of nano aluminum oxide, 1-5 parts of a tackifier, 0.1-5 parts of a catalyst, 0.1-5 parts of a dehydrating agent, 0.1-2 parts of an antioxidant and 0.1-3 parts of other auxiliaries. According to the invention, the nano graphene oxide and the nano aluminum oxide are used as fillers, so that the technical effect of remarkably improving the mechanical strength of the silicone structural adhesive is achieved. By introducing the two nano materials into the basic formula, the silicone structural adhesive shows higher tensile strength and tear resistance, and compared with the technical scheme that only conventional filler is used in the prior art, the silicone structural adhesive solves the problem that the mechanical property is insufficient under the conditions of high stress and high load; therefore, the reliability and durability of the structural adhesive applied to buildings, automobiles and the like are enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of organosilicon chemistry and material science and technology, and in particular to a method for preparing a high-strength silicone structural adhesive. Background Art

[0002] Silicone structural adhesives are widely used in the fields of construction, automobiles, electronics, etc. Their excellent adhesion, weather resistance and anti-aging properties make them important in these applications. However, silicone structural adhesives in the prior art often show insufficient mechanical properties under high stress and high load conditions, which limits their use in more demanding application scenarios.

[0003] First, silicone structural adhesives in the prior art mainly use traditional fillers, such as silicon dioxide, calcium carbonate, etc. Although these fillers can improve the mechanical properties of the colloid to a certain extent, due to their large particle size and low surface activity, they cannot fully form a strong interface bond with the silicone matrix, resulting in insufficient tensile strength and tear resistance of the structural adhesive under high stress conditions. This lack of mechanical properties limits the reliability and durability of silicone structural adhesives in high stress environments such as construction and automobiles.

[0004] Secondly, most silicone structural adhesives currently use a single metal catalyst, such as an organotin compound. This type of catalyst can effectively catalyze the curing reaction of silicone under certain conditions, but its catalytic efficiency and reaction uniformity are insufficient, resulting in a long curing time and an uneven cross-linking network, which affects the final mechanical properties and product stability. The use of a single catalyst often cannot meet the demand for rapid curing of silicone structural adhesives at lower temperatures, and the unevenness during the curing process also leads to poor overall product performance and application stability.

[0005] At the same time, most traditional plasticizers are short-chain molecules. Although they can increase the flexibility of silicone structural adhesives, their durability and anti-aging performance after long-term use are poor. This performance deficiency is mainly due to the migration and volatilization of short-chain plasticizers in the colloid, which causes the performance of the colloid to decline during long-term use. Short-chain plasticizers are easy to migrate and volatilize in actual applications, which not only affects the physical properties of silicone structural adhesives, but also shortens their service life and limits their application in complex environments.

[0006] Finally, in the prior art, nanofillers are often dispersed by simple mechanical stirring, which is difficult to fully disperse nanoparticles and easily leads to filler agglomeration in the matrix, affecting the uniformity and stability of the colloid. Mechanical stirring is difficult to overcome the agglomeration problem of nanoparticles, resulting in uneven distribution of fillers in the colloid, which in turn affects its overall mechanical properties and consistency.

[0007] Therefore, the present invention proposes a method for preparing a high-strength silicone structural adhesive to solve the deficiencies of the prior art. Summary of the invention

[0008] In view of the deficiencies in the prior art, the present invention provides a method for preparing a high-strength silicone structural adhesive, which solves the problems of the existing silicone structural adhesives such as insufficient mechanical properties under high stress and high load conditions, uneven curing reaction, poor flexibility and durability, and uneven dispersion of nanofillers.

[0009] To achieve the above objectives, the present invention is implemented through the following technical scheme: A high-strength silicone structural adhesive comprises the following components in parts by weight:

[0010] Silicone base polymer: 30-60 parts;

[0011] Cross-linking agent: 1-10 parts;

[0012] Plasticizer: 5-20 parts;

[0013] Filler: 10-40 parts, including 0.1-5 parts of nano graphene oxide and 0.1-5 parts of nano aluminum oxide;

[0014] Tackifier: 1-5 parts;

[0015] Catalyst: 0.1-5 parts;

[0016] Dehydrating agent: 0.1-5 parts;

[0017] Antioxidant: 0.1-2 parts;

[0018] Other additives: 0.1-3 parts.

[0019] Preferably, the silicone base polymer is a dimethylsiloxane-based polymer with a molecular weight between 20,000 and 60,000. The polymer is composed of repeated dimethylsiloxane units. The molecular weight range is controlled by adjusting the polymerization reaction time and the catalyst concentration to obtain the desired mechanical properties and viscosity, thereby ensuring the stability and reliability of the colloid under high-strength conditions.

[0020] Preferably, the plasticizer is a flexible polysiloxane plasticizer containing long-chain siloxane units, the molecular structure of the plasticizer contains at least 100 siloxane units, and the viscosity is between 500 and 10,000 cP, which is adjusted by the molecular chain length and the introduction of branches.

[0021] Preferably, the catalyst is a multi-metal composite catalyst system composed of platinum, tin and titanium, wherein the platinum catalyst is chloroplatinic acid or its derivatives, the tin catalyst is dibutyltin dilaurate, and the titanium catalyst is an organic titanium compound such as isopropyl titanate;

[0022] The use of a multi-metal composite catalyst system composed of platinum, tin and titanium can quickly cure at a lower temperature, optimize the reaction rate and the uniformity of the cross-linking structure, form a tighter and more uniform cross-linking network, overcome the problem of uneven curing of a single catalyst, and improve the overall performance and application stability of the product.

[0023] Preferably, the filler includes nano-alumina surface-treated with a silane coupling agent, wherein the surface treatment is performed by immersing the nano-alumina in a silane coupling agent solution and heating to 80-120° C., and the silane coupling agent is γ-aminopropyltriethoxysilane or a derivative thereof;

[0024] By using nano-graphene oxide and nano-alumina, the high specific surface area and surface activity of the nano-fillers improve the bonding strength between the filler and the silicone matrix, significantly enhancing the tensile strength and tear resistance of the colloid, thereby improving the reliability and durability of the structural adhesive under high stress and high load conditions.

[0025] Preferably, the crosslinking agent is methyltriethoxysilane or vinyltrimethoxysilane, wherein the amount of methyltriethoxysilane is between 1-8 parts, and the amount of vinyltrimethoxysilane is between 1-5 parts;

[0026] The crosslinking agent is used for the crosslinking reaction of silicone polymer to form a three-dimensional network structure. Methyltriethoxysilane or vinyltrimethoxysilane is used as a crosslinking agent. By adjusting the dosage, the crosslinking density can be optimized and the mechanical strength and heat resistance of the colloid can be enhanced.

[0027] Preferably, the tackifier is γ-glycidyloxypropyltrimethoxysilane, and the dehydrating agent is activated calcium carbonate or activated alumina, wherein the amount of γ-glycidyloxypropyltrimethoxysilane is between 1-5 parts, the amount of activated calcium carbonate is between 0.5-5 parts, and the amount of activated alumina is between 0.1-3 parts;

[0028] Plasticizers adjust the flexibility of colloids through the mobility of molecular chains. By adjusting the length of molecular chains and the introduction of side chains, the flexibility and durability of colloids are significantly improved, solving the problems of insufficient toughness and rapid aging of traditional short-chain plasticizers.

[0029] Using γ-glycidyloxypropyltrimethoxysilane as a tackifier can enhance the adhesion between the colloid and the substrate and improve the overall structural strength;

[0030] Using activated calcium carbonate or activated alumina as a dehydrating agent can effectively absorb moisture in the system and avoid the negative impact of moisture on colloid properties.

[0031] Preferably, the antioxidant is 2,6-di-tert-butyl-4-methylphenol or pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate;

[0032] Using 2,6-di-tert-butyl-4-methylphenol or pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] as an antioxidant can significantly improve the anti-aging performance of the colloid and extend its service life.

[0033] Preferably, the other auxiliary agents include ultraviolet absorbers such as benzophenone compounds or triazine compounds.

[0034] Preferably, a method for preparing a high-strength silicone structural adhesive comprises the following steps:

[0035] S1. Mix 30-60 parts of silicone base polymer with 5-20 parts of plasticizer at 50-80°C for 30-60 minutes. The appropriate temperature and time can make the base colloid uniform and ensure the uniform dispersion of subsequent additives.

[0036] S2, adding 0.1-5 parts of nano graphene oxide and 0.1-5 parts of nano alumina to the basic colloid in step S1, and treating by ultrasonic dispersion technology for 20-40 minutes, the frequency of ultrasonic dispersion is 20-40kHz, and the power is 500-1000W. The ultrasonic dispersion technology ensures the uniform distribution of the nano filler in the basic colloid, avoids the agglomeration of the filler, and thus improves the mechanical properties and consistency of the colloid;

[0037] S3, add 1-5 parts of thickener and 1-10 parts of crosslinker, stir for 30-60 minutes to ensure that the thickener and crosslinker are evenly distributed, and improve the adhesion and crosslinking density of the colloid;

[0038] S4, add 0.1-5 parts of catalyst and 0.1-5 parts of dehydrating agent, stir for 30-60 minutes under vacuum conditions, the vacuum degree is -0.08 to -0.1MPa, add catalyst and dehydrating agent under vacuum stirring conditions to ensure uniform reaction and remove bubbles in the mixture to prevent bubbles from affecting colloid properties;

[0039] S5, add 0.1-2 parts of antioxidant and 0.1-3 parts of other additives, stir evenly, the addition of antioxidant and additives improves the anti-aging and anti-ultraviolet performance of the colloid;

[0040] S6, subjecting the mixture to a vacuum pressurized mixing treatment for 10-20 minutes at a pressure of 0.1 to 0.3 MPa, wherein the vacuum pressurized treatment further removes bubbles in the mixture and improves the compactness and performance stability of the colloid;

[0041] S7. The deaerated mixture is packaged through continuous production equipment, which includes an automated metering system, a mixing system and a packaging system. Sealed storage and continuous production ensure product consistency and efficient production. Sealed packaging prevents the product from getting damp or oxidized during storage and transportation.

[0042] The present invention provides a method for preparing a high-strength silicone structural adhesive, which has the following beneficial effects:

[0043] 1. The present invention uses nano-graphene oxide and nano-alumina as fillers to achieve the technical effect of significantly improving the mechanical strength of silicone structural adhesive. By introducing these two nanomaterials into the basic formula, silicone structural adhesive exhibits higher tensile strength and tear resistance. Compared with the technical solution of only using conventional fillers in the prior art, it solves the problem of insufficient mechanical properties under high stress and high load conditions, thereby enhancing the reliability and durability of structural adhesives in applications such as construction and automobiles.

[0044] 2. The present invention adopts a multi-metal composite catalyst system composed of platinum, tin and titanium to achieve the technical effect of optimizing the curing reaction rate and enhancing the cross-linking structure. Through the synergistic effect of the composite catalyst, the silicone structural adhesive can be quickly cured at a lower temperature and form a more compact and uniform cross-linking network. Compared with the technical solution using a single catalyst in the prior art, it solves the problems of uneven curing and low cross-linking density, thereby improving the overall performance and application stability of the product.

[0045] 3. The present invention achieves the technical effect of improving the flexibility and durability of silicone structural adhesive by introducing flexible polysiloxane plasticizer. The long-chain siloxane unit used not only enhances the flexibility of the colloid, but also significantly improves its anti-aging ability in complex environments. Compared with the technical solution of using short-chain plasticizers in the prior art, the problem of insufficient toughness and rapid aging is solved, so that the silicone structural adhesive of the present invention maintains good physical properties during long-term use and is suitable for a wider range of application scenarios.

[0046] 4. The present invention uses ultrasonic dispersion technology to process nanofillers, achieving the technical effect of ensuring uniform dispersion of nanofillers and enhancing the overall performance of the colloid. Through the action of high-frequency ultrasound, nanographene oxide and nanoalumina are fully dispersed in the base colloid, avoiding the agglomeration of fillers. Compared with the technical solution of the traditional mixing method in the prior art, the problem of uneven dispersion and unstable performance of the nanofillers is solved, thereby improving the mechanical properties and consistency of the silicone structural adhesive, making the product more reliable and excellent in use. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 The present invention is a flow chart of the preparation method of high-strength silicone structural adhesive. DETAILED DESCRIPTION

[0048] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] Example:

[0050] Please see attached Figure 1 :

[0051] Embodiment 1:

[0052] Steps and process parameters:

[0053] Base mixing: 40 parts of dimethylsiloxane polymer and 10 parts of flexible polysiloxane plasticizer were mixed at 60°C for 45 minutes to form a uniform base colloid.

[0054] Filler dispersion: 1 part of nano graphene oxide and 1 part of nano alumina were added to the base colloid and treated by ultrasonic dispersion technology for 30 minutes. The frequency of ultrasonic dispersion was 30kHz and the power was 800W.

[0055] Adhesion promoter and crosslinking agent: Add 3 parts of γ-glycidyloxypropyltrimethoxysilane and 5 parts of methyltriethoxysilane and stir for 45 minutes.

[0056] Catalyst and dehydrating agent: Add 0.5 parts of platinum catalyst (chloroplatinic acid), 1 part of tin catalyst (dibutyltin dilaurate) and 0.5 parts of titanium catalyst (isopropyl titanate), as well as 3 parts of activated calcium carbonate, and stir for 45 minutes under vacuum conditions, with a vacuum degree of -0.09 MPa.

[0057] Antioxidants and additives: Add 0.5 parts of 2,6-di-tert-butyl-4-methylphenol and 1 part of benzophenone type UV absorber and stir well.

[0058] Vacuum pressure treatment: The mixture was subjected to vacuum pressure mixing treatment for 15 minutes at a pressure of 0.2 MPa.

[0059] Packaging: The degassed mixture is packaged through continuous production equipment and stored in a sealed manner.

[0060] Summary of Example 1:

[0061] This embodiment improves the mechanical properties and consistency of the silicone structural adhesive by using nano fillers and ultrasonic dispersion technology. The use of a multi-metal composite catalyst system and a flexible plasticizer enhances the uniformity of the curing reaction and the flexibility of the colloid.

[0062] Embodiment 2:

[0063] Steps and process parameters:

[0064] Base mixing: 50 parts of dimethylsiloxane polymer and 8 parts of flexible polysiloxane plasticizer were mixed at 70°C for 40 minutes to form a uniform base colloid.

[0065] Filler dispersion: 2 parts of nano graphene oxide and 2 parts of nano alumina were added to the base colloid and treated by ultrasonic dispersion technology for 25 minutes. The frequency of ultrasonic dispersion was 25 kHz and the power was 700 W.

[0066] Adhesion promoter and crosslinking agent: Add 4 parts of γ-glycidyloxypropyltrimethoxysilane and 6 parts of methyltriethoxysilane and stir for 50 minutes.

[0067] Catalyst and dehydrating agent: Add 1 part of platinum catalyst (chloroplatinic acid), 2 parts of tin catalyst (dibutyltin dilaurate) and 1 part of titanium catalyst (isopropyl titanate), as well as 2 parts of activated alumina, and stir for 40 minutes under vacuum conditions with a vacuum degree of -0.08 MPa.

[0068] Antioxidants and additives: Add 1 part of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and 1.5 parts of triazine ultraviolet absorber and stir well.

[0069] Vacuum pressure treatment: The mixture was subjected to vacuum pressure mixing treatment for 20 minutes at a pressure of 0.3 MPa.

[0070] Packaging: The degassed mixture is packaged through continuous production equipment and stored in a sealed manner.

[0071] Example 2 Summary:

[0072] This embodiment adjusts the dosage of the plasticizer and the catalyst, and optimizes the parameters of the ultrasonic dispersion technology, so that the curing reaction of the silicone structural adhesive is more uniform and the anti-aging performance is further improved.

[0073] Embodiment 3:

[0074] Steps and process parameters:

[0075] Base Mixing: 45 parts of dimethylsiloxane polymer and 12 parts of flexible polysiloxane plasticizer were mixed at 65°C for 50 minutes to form a uniform base gel.

[0076] Filler dispersion: 0.5 parts of nano-graphene oxide and 1.5 parts of nano-alumina were added to the base colloid and treated by ultrasonic dispersion technology for 35 minutes. The frequency of ultrasonic dispersion was 35kHz and the power was 900W.

[0077] Adhesion promoter and crosslinking agent: Add 2 parts of γ-glycidyloxypropyltrimethoxysilane and 7 parts of vinyltrimethoxysilane and stir for 40 minutes.

[0078] Catalyst and dehydrating agent: Add 0.7 parts of platinum catalyst (chloroplatinic acid), 1.5 parts of tin catalyst (dibutyltin dilaurate) and 0.7 parts of titanium catalyst (isopropyl titanate), as well as 4 parts of activated calcium carbonate, and stir for 50 minutes under vacuum conditions with a vacuum degree of -0.1 MPa.

[0079] Antioxidants and additives: Add 0.8 parts of 2,6-di-tert-butyl-4-methylphenol and 1.2 parts of benzophenone ultraviolet absorber and stir well.

[0080] Vacuum pressure treatment: The mixture was subjected to vacuum pressure mixing treatment for 12 minutes at a pressure of 0.15 MPa.

[0081] Packaging: The degassed mixture is packaged through continuous production equipment and stored in a sealed manner.

[0082] Example 3 Summary:

[0083] By adjusting the proportion of nanofillers and the parameters of ultrasonic dispersion, the mechanical properties and flexibility of silicone structural adhesives are further optimized while maintaining a good curing reaction rate.

[0084] Embodiment 4:

[0085] Steps and process parameters:

[0086] Base Mixing: 35 parts of dimethylsiloxane polymer and 15 parts of flexible polysiloxane plasticizer were mixed at 55°C for 55 minutes to form a uniform base gel.

[0087] Filler dispersion: 1.5 parts of nano graphene oxide and 0.5 parts of nano alumina were added to the base colloid and treated by ultrasonic dispersion technology for 30 minutes. The frequency of ultrasonic dispersion was 20 kHz and the power was 600 W.

[0088] Adhesion promoter and crosslinking agent: Add 3.5 parts of γ-glycidyloxypropyltrimethoxysilane and 5.5 parts of methyltriethoxysilane and stir for 55 minutes.

[0089] Catalyst and dehydrating agent: Add 1.2 parts of platinum catalyst (chloroplatinic acid), 2.5 parts of tin catalyst (dibutyltin dilaurate) and 1.2 parts of titanium catalyst (isopropyl titanate), as well as 1 part of activated alumina, and stir for 45 minutes under vacuum conditions, with a vacuum degree of -0.09 MPa.

[0090] Antioxidants and additives: Add 1 part of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and 1 part of triazine ultraviolet absorber and stir well.

[0091] Vacuum pressure treatment: The mixture was subjected to vacuum pressure mixing treatment for 18 minutes at a pressure of 0.25 MPa.

[0092] Packaging: The degassed mixture is packaged through continuous production equipment and stored in a sealed manner.

[0093] Example 4 Summary:

[0094] This embodiment significantly improves the aging resistance and UV resistance of the silicone structural adhesive by adjusting the proportion of nanofillers and the dosage of different additives in the basic formula, while maintaining high mechanical strength and flexibility.

[0095] Comparative experiment:

[0096] Comparative experiment 1: Mechanical strength comparison

[0097] Prior art comparison group A:

[0098] Uses traditional silica filler without nano-graphene oxide and nano-alumina.

[0099] The other components and process parameters are the same as those in Example 1.

[0100] Embodiment 1 of the present invention:

[0101] Nano-graphene oxide and nano-alumina fillers are used.

[0102] Experimental process:

[0103] Samples of prior art comparison group A and Example 1 of the present invention were prepared.

[0104] Each sample was tested for tensile strength and tear resistance.

[0105] Experimental data table:

[0106]

[0107] Result analysis: The nano graphene oxide and nano alumina used in Example 1 of the present invention significantly improve the mechanical strength and tear resistance of the silicone structural adhesive. Nano materials have higher specific surface area and surface activity, and can better combine with the silicone matrix, thereby enhancing the interfacial bonding strength, resulting in a significant improvement in the overall strength and durability of the material. In contrast, traditional fillers cannot fully form a strong interfacial bond with the silicone matrix due to their large particle size and low surface activity, resulting in insufficient tensile strength and tear resistance under high stress conditions.

[0108] Comparative experiment 2: Comparison of curing performance

[0109] Prior art comparison group B:

[0110] Using a single organic tin catalyst, the curing temperature is relatively high.

[0111] The other components and process parameters are the same as those in Example 2.

[0112] Embodiment 2 of the present invention:

[0113] A multi-metal composite catalyst system is used.

[0114] Experimental process:

[0115] Samples of prior art comparison group B and Example 2 of the present invention were prepared.

[0116] Each sample was tested for cure time and crosslink density.

[0117] Experimental data table:

[0118]

[0119] Result analysis: The multi-metal composite catalyst system used in Example 2 of the present invention significantly shortens the curing time and improves the cross-linking density through the synergistic effect of platinum, tin and titanium. The multi-metal composite catalyst provides multiple catalytic active sites, increases the reaction rate and uniformity, forms a tighter and more uniform cross-linking network, and thus improves the overall performance of the material. In contrast, the catalytic efficiency and reaction uniformity of a single organic tin catalyst are low, resulting in a long curing time and an uneven cross-linking structure, which affects the final mechanical properties and product stability.

[0120] Comparative experiment 3: Comparison of flexibility and material dispersion

[0121] Prior art comparison group C:

[0122] Traditional short-chain plasticizers are used and the fillers are dispersed by mechanical stirring.

[0123] The other components and process parameters are the same as those in Example 3.

[0124] Embodiment 3 of the present invention:

[0125] Flexible polysiloxane plasticizer is used and the filler is processed by ultrasonic dispersion technology.

[0126] Experimental process:

[0127] Samples of prior art comparison group C and Example 3 of the present invention were prepared.

[0128] Each sample was tested for flexibility and uniformity of filler distribution.

[0129] Experimental data table:

[0130]

[0131] Analysis of results: The flexible polysiloxane plasticizer and ultrasonic dispersion technology used in Example 3 of the present invention significantly improve the flexibility of the silicone structural adhesive and the uniformity of filler distribution. Long-chain siloxane plasticizer molecules are more stable in the matrix, not easy to migrate and volatilize, so as to maintain good flexibility and anti-aging properties during long-term use. Ultrasonic dispersion technology can effectively disperse nanofillers, avoid filler agglomeration, and ensure the uniformity and consistency of the internal structure of the material. In contrast, traditional short-chain plasticizers are easy to migrate and volatilize, resulting in reduced flexibility; mechanical stirring makes it difficult to fully disperse nanofillers, resulting in uneven filler distribution and affecting material properties.

[0132] Summarize:

[0133] Through the above examples and comparative experiments, the present invention is superior to the prior art in terms of mechanical strength, curing performance, flexibility and material dispersibility. The comprehensive application of nano-graphene oxide and nano-alumina as fillers, multi-metal composite catalyst system, flexible polysiloxane plasticizer and ultrasonic dispersion technology has made the high-strength silicone structural adhesive of the present invention significantly improved in multiple key performance indicators, meeting the application requirements under high stress and complex environments. The specific analysis is as follows:

[0134] Introduction of nanofillers: By using nano-graphene oxide and nano-alumina, the specific surface area and surface activity of the filler are increased, forming a stronger interface bond with the silicone matrix, thereby significantly improving the mechanical properties.

[0135] Multi-metal composite catalyst: The multi-metal composite catalyst system improves the reaction rate and uniformity, optimizes the curing time and cross-linking density, and enhances the overall performance of the material through the synergistic effect of multiple catalytic active sites.

[0136] Use of flexible plasticizers: The long-chain structure of flexible polysiloxane plasticizers is more stable in the matrix, less likely to migrate and volatilize, and significantly improves the flexibility and anti-aging properties of the material.

[0137] Ultrasonic dispersion technology: Ultrasonic dispersion technology ensures the uniform distribution of nanofillers in the matrix, avoids agglomeration, improves the uniformity and consistency of the internal structure of the material, and thus improves the overall performance.

[0138] These improvement measures work together to enable the high-strength silicone structural adhesive of the present invention to exhibit more excellent performance in practical applications, overcoming many deficiencies in the prior art.

[0139] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high-strength silicone structural adhesive, characterized in that: The composition comprises the following components in parts by weight: Silicone base polymer: 30-60 parts; Cross-linking agent: 1-10 parts; Plasticizer: 5-20 parts; Filler: 10-40 parts, including 0.1-5 parts of nano graphene oxide and 0.1-5 parts of nano aluminum oxide; Tackifier: 1-5 parts; Catalyst: 0.1-5 parts; Dehydrating agent: 0.1-5 parts; Antioxidant: 0.1-2 parts; Other additives: 0.1-3 parts.

2. A high-strength silicone structural adhesive according to claim 1, characterized in that: The silicone base polymer is a dimethylsiloxane-based polymer with a molecular weight between 20,000 and 60,000. The polymer is composed of repeated dimethylsiloxane units, and the molecular weight range is controlled by adjusting the polymerization reaction time and the catalyst concentration to obtain the desired mechanical properties and viscosity.

3. A high-strength silicone structural adhesive according to claim 1, characterized in that: The plasticizer is a flexible polysiloxane plasticizer containing long-chain siloxane units. The molecular structure of the plasticizer contains at least 100 siloxane units, and the viscosity is between 500 and 10,000 cP, which is adjusted by the length of the molecular chain and the introduction of side chains.

4. The high-strength silicone structural adhesive according to claim 1, characterized in that: The catalyst is a multi-metal composite catalyst system composed of platinum, tin and titanium, wherein the platinum catalyst is chloroplatinic acid or its derivatives, the tin catalyst is dibutyltin dilaurate, and the titanium catalyst is an organic titanium compound such as isopropyl titanate.

5. The high-strength silicone structural adhesive according to claim 1, characterized in that: The filler comprises nano-alumina surface-treated with a silane coupling agent. The surface treatment is carried out by immersing the nano-alumina in a silane coupling agent solution and heating it to 80-120° C. The silane coupling agent is gamma-aminopropyltriethoxysilane or its derivatives.

6. The high-strength silicone structural adhesive according to claim 1, characterized in that: The crosslinking agent is methyltriethoxysilane or vinyltrimethoxysilane, wherein the amount of the methyltriethoxysilane is between 1-8 parts, and the amount of the vinyltrimethoxysilane is between 1-5 parts.

7. The high-strength silicone structural adhesive according to claim 1, characterized in that: The viscosity enhancer is γ-glycidyloxypropyltrimethoxysilane, and the dehydrating agent is activated calcium carbonate or activated alumina, wherein the amount of the γ-glycidyloxypropyltrimethoxysilane is between 1-5 parts, the amount of the activated calcium carbonate is between 0.5-5 parts, and the amount of the activated alumina is between 0.1-3 parts.

8. The high-strength silicone structural adhesive according to claim 1, characterized in that: The antioxidant is 2,6-di-tert-butyl-4-methylphenol or pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

9. The high-strength silicone structural adhesive according to claim 1, characterized in that: The other auxiliary agents include ultraviolet absorbers such as benzophenone compounds or triazine compounds.

10. A method for preparing a high-strength silicone structural adhesive according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1, mixing 30-60 parts of silicone base polymer and 5-20 parts of plasticizer at 50-80° C. for 30-60 minutes to form a uniform base colloid; S2, adding 0.1-5 parts of nano graphene oxide and 0.1-5 parts of nano aluminum oxide to the base colloid in step S1, and treating by ultrasonic dispersion technology for 20-40 minutes, the frequency of ultrasonic dispersion is 20-40kHz, and the power is 500-1000W; S3, adding 1-5 parts of a thickener and 1-10 parts of a cross-linking agent, stirring for 30-60 minutes to uniformly disperse them in the base colloid; S4, adding 0.1-5 parts of a catalyst and 0.1-5 parts of a dehydrating agent, stirring for 30-60 minutes under vacuum conditions, with a vacuum degree of -0.08 to -0.1 MPa, to remove bubbles in the mixture; S5, add 0.1-2 parts of antioxidant and 0.1-3 parts of other additives, and stir evenly; S6, subjecting the mixture to a vacuum pressurized mixing treatment for 10-20 minutes at a pressure of 0.1 to 0.3 MPa; S7. The deaerated mixture is packaged through continuous production equipment, which includes an automated metering system, a mixing system and a packaging system for sealed storage.

Citation Information

Cited By

  • Fireproof adhesive tape and preparation method thereof

    CN120535958A

  • Method and system for detecting matching degree of socket-and-spigot pipe piece connecting piece

    CN120777994A