Silicone sealant and preparation method thereof
By adding calcium sulfate whiskers and SAP resin to the silicone sealant, and utilizing the bonding between the silane coupling agent and the whisker filler, combined with the antifungal agent loaded with nanosilver, the problem of silicone sealant in concrete sealing is solved. The problem of insufficient tensile bond strength has significantly improved its bond strength and mildew resistance.
Patent Information
- Application Number
- CN202410952434.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Silicone sealant has the problem of insufficient tensile bond strength when sealing concrete, which limits its application scope.
By adding calcium sulfate whiskers and SAP resin to the formula of the silicone sealant, and using the silane coupling agent to bond with the whisker filler, the dispersion effect and cross-linking reaction of the whisker filler are improved, thereby improving the tensile bonding strength. At the same time, halloysite nanotubes loaded with nanosilver are used as antifungal agents to enhance the tensile bonding strength of the silicone sealant.
Significantly improves the tensile bonding strength of silicone sealant, overcomes the defects in the original technology, and maintains good anti-mildew properties.
Smart Images

Figure BDA0004947594370000091 
Figure BDA0004947594370000101
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of sealants, and more specifically, to a silicone sealant and a preparation method thereof. Background Art
[0002] Silicone sealant is a high-quality adhesive sealing material made of polydimethylsiloxane as the base material, on which appropriate fillers, plasticizers, coupling agents and other additives are added. It has excellent weather resistance, heat resistance, aging resistance and electrical insulation properties, and has been widely used in many fields such as construction, electronics, and automobiles. The curing principle of silicone sealant is to react with water in the air at room temperature to form a cross-linked network structure, and then form a cured product with a certain strength. In silicone sealant, the role of plasticizer is to increase flexibility and extrudability, and it will also have a certain impact on the bonding strength of silicone sealant.
[0003] In the related art, there is a silicone sealant, which is prepared according to the following steps: 100 parts by weight of a base polymer, 20 parts by weight of a plasticizer, 20 parts by weight of an imidazoline-containing polyorganosiloxane, and 60 parts by weight of nano calcium carbonate are added to a high-speed mixer, dehydrated and blended for 4 hours at a temperature of 120°C, a vacuum degree of 0.09MP, and a rotation speed of 40rpm, and then cooled to obtain a base material; the base material is ground by three rollers, and then the base material is mixed with 10 parts by weight of fumed silica, 5 parts by weight of a fluorescent additive, 2 parts by weight of KathonTM910SB mildew inhibitor, 8 parts by weight of methyltrimethoxysilane, 3 parts by weight of tert-butyl titanate, and 2 parts by weight of a silane coupling agent KH-550, and vacuum stirred for 2 hours at a rotation speed of 40rpm to obtain a silicone sealant. In the above scheme, the plasticizer is dimethyl silicone oil, and the base polymer is hydroxyl-terminated polydimethylsiloxane.
[0004] With respect to the above-mentioned related technologies, the inventors believe that although the silicone sealant in the related technologies has certain flexibility and extrudability by adding plasticizers, it has the defect of insufficient tensile bonding strength when sealing concrete, which limits the application scope of silicone sealant. Summary of the invention
[0005] In the related art, silicone sealant has the defect of insufficient tensile bonding strength when sealing concrete. In order to improve this defect, the present application provides a silicone sealant and a preparation method thereof.
[0006] In a first aspect, the present application provides a silicone sealant, which adopts the following technical solution: A silicone sealant comprises the following components in parts by weight: 100-120 parts of a base polymer, 60-65 parts of nano calcium carbonate, 8-20 parts of a whisker filler, 1.5-3.5 parts of a SAP resin, 10-15 parts of fumed silica, 12-16 parts of a silane coupling agent, 20-25 parts of a plasticizer, 2-5 parts of a mildewproof agent, and 0.5-0.7 parts of a catalyst; the base polymer comprises hydroxyl-terminated polydimethylsiloxane, and the whisker filler comprises calcium sulfate whiskers.
[0007] By adopting the above technical scheme, the present application adds a whisker filler represented by calcium sulfate whisker in the formula of silicone sealant, and adds SAP resin. In the silicone sealant of the present application, the silane coupling agent can bond with the hydroxyl group on the surface of the whisker filler in addition to being a cross-linking agent and a tackifier and undergoing cross-linking copolymerization reaction with the base polymer. The SAP resin can improve the water absorption and water retention of the silicone sealant, increase the moisture content in the silicone sealant, thereby promoting the cross-linking copolymerization between the silane coupling agent and the base polymer and the bonding between the silane coupling agent and the whisker filler. The bonding between the silane coupling agent and the whisker filler reduces the agglomeration of the whisker filler on the one hand, improves the dispersion effect of the whisker filler, and indirectly realizes the cross-linking of the whisker filler and the base polymer on the other hand, thereby improving the tensile bonding strength of the silicone sealant using the high tensile strength of the whisker filler, overcoming the defects in the related art.
[0008] Preferably, the calcium sulfate whiskers are prepared according to the following method: The hydrochloric acid and gypsum are mixed, the mixture is heated, and the mixture is subjected to microwave irradiation. After irradiation for a period of time, the heating and irradiation are stopped, the mixture is filtered while hot, the filtrate is cooled, and then the filtrate is allowed to age and crystallize. After the aging is completed, the filtrate is filtered again, and then the filter residue is dried to obtain calcium sulfate whiskers.
[0009] By adopting the above technical scheme, the present application preferably obtains a method for preparing calcium sulfate whiskers, wherein gypsum is first dissolved using hydrochloric acid with the assistance of microwaves, and then the insoluble matter in the gypsum is filtered out, and then calcium sulfate crystals are allowed to grow freely through aging and crystallization to obtain calcium sulfate whiskers.
[0010] Preferably, the microwave irradiation time is 25-35 min.
[0011] By adopting the above technical solution, the present application optimizes the time range of microwave irradiation, promotes the growth of calcium sulfate whiskers, and improves the microscopic morphology of calcium sulfate whiskers. The calcium sulfate whiskers prepared under the above conditions have a better cross-linking effect with the silane coupling agent, which helps to enhance the tensile bonding strength of the silicone sealant.
[0012] Preferably, the whisker filler further comprises silica sol modified whiskers, and the silica sol modified whiskers are prepared according to the following method: The calcium sulfate whiskers and silica sol are mixed, stirred and centrifuged, and the obtained precipitates are dried to obtain silica sol modified whiskers.
[0013] By adopting the above technical solution, the present application further optimizes the calcium sulfate whisker, uses silica sol to treat the calcium sulfate whisker, and covers the surface of the calcium sulfate whisker with a layer of silicon dioxide by drying and dehydrating the silica sol. The bonding effect between silicon dioxide and the silane coupling agent is better than that between calcium sulfate, so when the whisker filler includes silica sol-modified whiskers, the bonding effect between the whisker filler and the silane coupling agent is better, which can more fully improve the tensile bonding strength of the silicone sealant.
[0014] Preferably, the silica sol is prepared according to the following method: Anhydrous ethanol, TEOS and deionized water are mixed, stirred and heated to obtain a mixture, the mixture is cooled, hydrochloric acid is added to the mixture, and stirring is continued at room temperature for a period of time to obtain silica sol.
[0015] By adopting the above technical solution, the present application uses hydrochloric acid to promote the hydrolysis of TEOS in a solvent system composed of anhydrous ethanol and water to obtain silica sol. The silica sol prepared according to the above method can form a silicon dioxide layer on the surface of the calcium sulfate whisker and obtain silica sol-modified whiskers with better bonding effect with the silane coupling agent.
[0016] Preferably, the weight ratio of the silica sol modified whiskers to the calcium sulfate whiskers is (1.4-1.8):1.
[0017] By adopting the above technical solution, the present application optimizes the weight ratio of silica sol-modified whiskers and calcium sulfate whiskers, which helps to fully improve the tensile bonding strength of silicone sealant.
[0018] Preferably, the mildew inhibitor is prepared according to the following method: (1) dissolving chitosan in an acetic acid aqueous solution, adding succinic anhydride to the obtained solution, diluting it with methanol and stirring it to obtain a chitosan modified solution; (2) adding halloysite nanotubes to the chitosan modified solution, adjusting the pH with hydrochloric acid after stirring, continuing to stir the reaction and then centrifuging, washing and drying the precipitate to obtain chitosan modified nanotubes; (3) mixing silver nitrate, modified nanotubes and methanol, stirring and then shaking, centrifuging the product, washing the precipitate with methanol, and vacuum drying to obtain silver ion modified nanotubes; (4) Mixing the silver ion-modified nanotubes, sodium borohydride and sodium hydroxide solution, adding water to dilute, stirring and centrifuging, washing and vacuum drying the precipitate to obtain a mildew inhibitor.
[0019] By adopting the above technical scheme, the present application first uses succinic anhydride to modify chitosan, and introduces a carboxyl group into the chitosan molecule. After chitosan reacts with the silanol group on the surface of the halloysite nanotube by the carboxyl group, the chitosan molecule can be grafted to the surface of the halloysite nanotube. Afterwards, the silver ions are complexed by chitosan, and then the silver ions are reduced to silver elemental substance by sodium borohydride, so that the surface-loaded halloysite nanotubes with nano silver, i.e., a mildew inhibitor, can be obtained. In addition to playing a mildew-proof effect, this mildew inhibitor can also be bonded with a silane coupling agent through the silanol group remaining on the surface, and has a certain reinforcing effect on silicone sealant, which helps to improve the tensile bonding strength of silicone sealant.
[0020] Preferably, the halloysite nanotubes are activated before use, and the activation treatment method is: soaking the halloysite nanotubes in hydrochloric acid for 4-8 days, shaking them at certain time intervals during the treatment, and then centrifuging them, and washing and drying the obtained precipitate to complete the activation treatment of the halloysite nanotubes.
[0021] By adopting the above technical solution, the present application uses hydrochloric acid to immerse the halloysite nanotubes, which helps to increase the total amount of silanol groups on the surface of the halloysite nanotubes, improves the bonding effect of the mildew inhibitor and the silane coupling agent, and helps to improve the tensile bonding strength of the silicone sealant.
[0022] Preferably, the halloysite nanotubes are immersed in hydrochloric acid for 5-7 days.
[0023] By adopting the above technical solution, the present application optimizes the immersion time of the halloysite nanotubes in hydrochloric acid, which helps to improve the tensile bonding strength of the silicone sealant.
[0024] In a second aspect, the present application provides a method for preparing silicone sealant, which adopts the following technical solution.
[0025] A method for preparing a silicone sealant comprises the following steps: (1) mixing a base polymer, nano calcium carbonate, a whisker filler, and a plasticizer under heating conditions to obtain a base material, and grinding the base material for later use; (2) The base material, fumed silica, silane coupling agent, mildew inhibitor and catalyst are mixed and then stirred in vacuum to obtain silicone sealant.
[0026] By adopting the above technical scheme, the present application first uses a base polymer, nano-calcium carbonate, a whisker filler, and a plasticizer to prepare a base material, and then mixes the base material with fumed silica, a silane coupling agent, a mildew inhibitor, and a catalyst, and then stirs to prepare a silicone sealant.
[0027] In summary, this application has the following beneficial effects: 1. The present application adds whisker fillers represented by calcium sulfate whiskers and SAP resin to the formula of silicone sealant. The bonding of the silane coupling agent and the whisker filler reduces the agglomeration of the whisker filler and improves the dispersion effect of the whisker filler. On the other hand, it also indirectly realizes the cross-linking of the whisker filler and the base polymer, while the SAP resin promotes the bonding of the silane coupling agent and the whisker filler, thereby improving the tensile bonding strength of the silicone sealant by utilizing the high tensile strength of the whisker filler, and overcoming the defects in the related art.
[0028] 2. In the present application, the preferred whisker filler also includes silica sol-modified whiskers. Silica sol is used to form a silicon dioxide layer on the surface of the calcium sulfate whiskers, thereby improving the bonding effect between the whisker filler and the silane coupling agent, thereby being able to more fully improve the tensile bonding strength of the silicone sealant.
[0029] 3. The present application uses halloysite nanotubes loaded with nanosilver as a mildew preventer, which can bond with the silane coupling agent through the residual silanol groups on the surface, has a certain reinforcing effect on the silicone sealant, and helps to improve the tensile bonding strength of the silicone sealant. DETAILED DESCRIPTION
[0030] The present application is further described in detail below in conjunction with embodiments, preparation examples and comparative examples. The raw materials involved in the present application can all be obtained commercially.
[0031] Preparation Example of Calcium Sulfate Whiskers The following is an explanation using Preparation Example 1.
[0032] Preparation Example 1 In this preparation example, calcium sulfate whiskers were prepared according to the following method: According to the dosage of 0.22g calcium sulfate per milliliter of hydrochloric acid, 2.8mol / L hydrochloric acid and gypsum are mixed, the mixture is heated at 70°C, and the mixture is irradiated with microwaves at a power of 400W. The heating and irradiation are stopped after 15 minutes, the mixture is filtered while hot, the filtrate is cooled, and then the filtrate is waited for aging and crystallization at room temperature. After aging for 4 hours, it is filtered again, and then the filter residue is dried at 60°C for 12 hours to obtain calcium sulfate whiskers.
[0033] As shown in Table 1, the difference between Preparation Examples 1-5 is that the microwave irradiation time is different.
[0034] Table 1 Microwave irradiation time sample Microwave irradiation time / min Preparation Example 1 15 Preparation Example 2 20 Preparation Example 3 25 Preparation Example 4 30 Preparation Example 5 35 Preparation Example of Silica Sol Modified Whiskers The following is an explanation using Preparation Example 6 as an example.
[0035] Preparation Example 6 This preparation example provides a silica sol, which is prepared according to the following method: Anhydrous ethanol, TEOS and deionized water were mixed in a volume ratio of 28:22:6.2, and heated at 60°C with magnetic stirring for 2 h to obtain a mixture. The mixture was cooled to 20°C, and hydrochloric acid was added to the mixture (the amount added was equivalent to 1 / 4 of the volume of deionized water), and stirring was continued at 20°C for 24 h to obtain a silica sol.
[0036] In this preparation example, calcium sulfate whiskers were prepared according to the following method: The calcium sulfate whiskers of Preparation Example 5 were mixed with silica sol at a ratio of 1 g:50 mL, stirred for 10 minutes, and then centrifuged. The obtained precipitate was dried at 100° C. to obtain silica sol-modified whiskers.
[0037] Preparation Example of Antifungal Agent The following is an explanation of Preparation Example 7.
[0038] Preparation Example 7 This preparation example provides a mildew inhibitor, which is prepared according to the following method: (1) dissolving chitosan in a 2 wt % acetic acid aqueous solution at a weight ratio of 1:49, adding succinic anhydride equivalent to 5 wt % of chitosan to the obtained solution, diluting it to 1.5 times the volume with methanol and stirring to obtain a chitosan modified solution; (2) adding 20% by weight of halloysite nanotubes to the chitosan modified solution, adjusting the pH to 3.0 with hydrochloric acid after stirring, continuing the stirring reaction for 2 hours, and then centrifuging, washing and drying the precipitate to obtain chitosan modified nanotubes; (3) silver nitrate, modified nanotubes and methanol are mixed in a weight ratio of 1:10:50, and after stirring, the mixture is shaken, the product is centrifuged, the precipitate is washed with methanol, and the silver ion modified nanotubes are obtained after vacuum drying; (4) silver ion modified nanotubes, sodium borohydride and sodium hydroxide solution are mixed in a 250 mL conical flask, diluted with water to pH = 8, stirred and centrifuged, the precipitate is washed with water and vacuum dried to obtain a mildew inhibitor; in this step, the molar ratio of sodium borohydride to silver nitrate in step (3) is 1:1, and the concentration of the sodium hydroxide solution is 0.01 mol / L.
[0039] Preparation Example 8 The difference between this preparation example and preparation example 7 is that the halloysite nanotubes are further activated before use, and the activation method is: The halloysite nanotubes are immersed in 4 mol / L hydrochloric acid at a ratio of 1 g:20 mL for 4 days, and oscillated every 12 hours during the treatment. The resulting precipitate is then centrifuged and washed and dried to complete the activation of the halloysite nanotubes.
[0040] As shown in Table 2, the difference between Preparation Examples 8-12 is that the activation treatment time (referred to as activation time) of the halloysite nanotubes in hydrochloric acid is different.
[0041] Table 2 Activation time sample Activation time / day Preparation Example 8 4 Preparation Example 9 5 Preparation Example 10 6 Preparation Example 11 7 Preparation Example 12 8 Example
[0042] Examples 1-5 The following description is given by taking Example 1 as an example.
[0043] Example 1 This embodiment provides a silicone sealant, including the following heavy components: 100 kg of base polymer, 60 kg of nano calcium carbonate (CAS: 471-34-1), 8 kg of whisker filler, 1.5 kg of SAP resin, and fumed silica. 10kg, silane coupling agent 12kg, plasticizer 20kg, mildew inhibitor 2kg, catalyst 0.5kg; the base polymer is α, ω-dihydroxy polydimethylsiloxane (107 glue), the SAP resin is sodium polyacrylate (CAS:9003-04-7), the whisker filler is the calcium sulfate whisker of Preparation Example 1, the silane coupling agent is prepared by mixing methyltrimethoxysilane and KH550 in a weight ratio of 4:1, the plasticizer is dimethyl silicone oil (viscosity 0.35Pa·s), the mildew inhibitor is KathonTM910SB mildew inhibitor, and the catalyst is tert-butyl titanate.
[0044] This embodiment provides a method for preparing a silicone sealant, comprising the following steps: (1) dehydrating and blending the base polymer, nano calcium carbonate, whisker filler and plasticizer at 120° C., at a vacuum degree of 0.09 MPa and a rotation speed of 40 rpm for 4 h to obtain a base material, and grinding the base material with three rollers for later use; (2) The base material, fumed silica, silane coupling agent, mildew inhibitor, and catalyst are mixed and stirred in a vacuum at a rotation speed of 40 rpm for 2 hours to obtain a silicone sealant.
[0045] As shown in Table 3, the differences between Examples 1-5 are mainly due to the different raw material ratios of the silicone sealant.
[0046] Table 3 Raw material ratio of silicone sealant sample Example 1 Example 2 Example 3 Example 4 Example 5 Base polymer / kg 100 105 110 115 120 Nano calcium carbonate / kg 60 61 62 64 65 Whisker filler / kg 8 11 14 17 20 SAP resin / kg 1.5 2 2.5 3 3.5 Fumed silica / kg 10 11 12 14 15 Silane coupling agent / kg 12 13 14 15 16 Plasticizer / kg 20 21 22 24 25 Antifungal agent / kg 2 3 3.5 4 5 Catalyst / kg 0.5 0.5 0.6 0.7 0.7 Embodiment 5-9 As shown in Table 4, the difference between Examples 5-9 is that the preparation examples of calcium sulfate whiskers are different.
[0047] Table 4 Preparation example of calcium sulfate whisker sample Preparation Example Example 5 Preparation Example 1 Example 6 Preparation Example 2 Example 7 Preparation Example 3 Example 8 Preparation Example 4 Example 9 Preparation Example 5 Example 10 The difference between this embodiment and embodiment 8 is that the whisker filler is prepared by mixing the calcium sulfate whiskers of preparation example 5 and the silica sol-modified whiskers of preparation example 6 in a weight ratio of 1:1.
[0048] As shown in Table 5, the difference between Examples 10-14 is that the weight ratio of calcium sulfate whiskers to silica sol-modified whiskers (referred to as whisker ratio) is different.
[0049] Table 5 Whisker ratio sample Whisker ratio Example 10 1:1 Embodiment 11 1.2:1 Example 12 1.4:1 Example 13 1.6:1 Embodiment 14 1.8:1 Embodiment 15 The difference between this embodiment and embodiment 14 is that the mildew inhibitor is prepared according to the method of preparation example 7.
[0050] As shown in Table 6, the difference between Examples 15-20 is that the preparation examples of the mildew inhibitors are different.
[0051] Table 6 Preparation example of antifungal agent sample Preparation Example Embodiment 15 Preparation Example 7 Example 16 Preparation Example 8 Embodiment 17 Preparation Example 9 Embodiment 18 Preparation Example 10 Embodiment 19 Preparation Example 11 Embodiment 20 Preparation Example 12 Comparative Example Comparative Example 1 A silicone sealant is prepared according to the following steps: 100 parts by weight of a base polymer, 20 parts by weight of a plasticizer, 20 parts by weight of an imidazoline-containing polyorganosiloxane, and 60 parts by weight of nano calcium carbonate are added to a high-speed mixer, dehydrated and blended for 4 hours at a temperature of 120°C, a vacuum degree of 0.09MP, and a rotation speed of 40rpm, and then cooled to obtain a base material; the base material is ground by three rollers, and then the base material is mixed with 10 parts by weight of fumed silica, 5 parts by weight of a fluorescent additive, 2 parts by weight of KathonTM910SB mildew inhibitor, 8 parts by weight of methyltrimethoxysilane, 3 parts by weight of tert-butyl titanate, and 2 parts by weight of a silane coupling agent KH-550, and vacuum stirred for 2 hours at a rotation speed of 40rpm to obtain a silicone sealant. In the above scheme, the plasticizer is dimethyl silicone oil, and the base polymer is hydroxyl-terminated polydimethylsiloxane. The structure of polyorganosiloxane containing imidazoline group can be expressed as: HO[Me2SiO] 241.5 [Me(C3H6lmC 17 H 31)SiO5]H, wherein lm refers to an imidazole ring.
[0052] Comparative Example 2 The difference between this comparative example and Example 1 is that the components of the silicone sealant do not include whisker fillers.
[0053] Comparative Example 3 The difference between this comparative example and Example 1 is that the components of the silicone sealant do not include SAP resin.
[0054] Performance testing methods 1. Tensile bond strength With reference to GB 16776-2005 "Silicone structural sealants for construction" and GB / T 13477.8-2002 "Test methods for building sealing materials Part 8: Determination of tensile adhesion", the tensile bond strength of the silicone sealant was tested using a cement mortar board, and the tensile bond strength measured in Comparative Example 1 was used as a benchmark to calculate the ratio of the tensile bond strength of each embodiment and comparative example to the tensile bond strength of Comparative Example 1, and the ratio was recorded as the relative bonding rate. The results are shown in Table 7.
[0055] 2. Anti-mildew effect With reference to JC / T885-2001 "Anti-mildew sealants for construction" and GB / T1741-2007 "Determination of mildew resistance of paint films", the mildew resistance level of silicone sealants was measured. The results are shown in Table 7.
[0056] Table 7 Test results Combining Examples 1-5 and Comparative Example 1 and Table 7, it can be seen that the relative bonding rates measured in Examples 1-5 are relatively high, indicating that with the combination of whisker filler and SAP resin, the silicone sealant of the present application has good tensile bonding strength.
[0057] Combining Example 1 and Comparative Examples 2-3 and Table 7, it can be seen that the relative bonding rates measured in Comparative Examples 2-3 are all lower than those in Example 1. This is because when the whisker filler is used alone, the bonding effect between the silane coupling agent and the whisker filler is poor, so the contribution of the whisker filler to the tensile bonding strength is limited. When the SAP resin is used alone, the tensile bonding strength of the silicone sealant is difficult to be fully improved due to the absence of the whisker filler.
[0058] It can be seen from Examples 5-9 and Table 7 that in the method for preparing calcium sulfate whiskers, controlling the microwave irradiation time to 25-35 min helps to enhance the tensile bonding strength of the silicone sealant.
[0059] It can be seen from Example 8, Examples 10-14 and Table 7 that the addition of silica sol-modified whiskers helps to improve the tensile bonding strength of silicone sealants. This is because the bonding effect between silicon dioxide and the silane coupling agent is better than that between calcium sulfate. Therefore, when the whisker filler includes silica sol-modified whiskers, the bonding effect between the whisker filler and the silane coupling agent is better.
[0060] It can be seen from Example 14, Examples 15-20 and Table 7 that the addition of the mildew inhibitor improves the tensile bonding strength of the silicone sealant. This is because the mildew inhibitor prepared in the present application bonds with the silane coupling agent through the residual silanol groups on the surface, and has a certain reinforcing effect on the silicone sealant. When the halloysite nanotubes are activated with hydrochloric acid before use, especially when the treatment time is 4-8 days, the mildew inhibitor has a more obvious effect on improving the tensile bonding strength of the silicone sealant.
[0061] It can be seen from Examples 1-20 and Table 7 that the silicone sealant of the present application has good anti-mildew performance.
[0062] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A silicone sealant, characterized in that: The invention comprises the following components in parts by weight: 100-120 parts of a base polymer, 60-65 parts of nano calcium carbonate, 8-20 parts of a whisker filler, 1.5-3.5 parts of a SAP resin, 10-15 parts of fumed silica, 12-16 parts of a silane coupling agent, 20-25 parts of a plasticizer, 2-5 parts of a mildewproof agent, and 0.5-0.7 parts of a catalyst; the base polymer comprises hydroxyl-terminated polydimethylsiloxane, and the whisker filler comprises calcium sulfate whiskers.
2. The silicone sealant according to claim 1, characterized in that: The calcium sulfate whiskers are prepared as follows: The hydrochloric acid and gypsum are mixed, the mixture is heated, and the mixture is subjected to microwave irradiation. After irradiation for a period of time, the heating and irradiation are stopped, the mixture is filtered while hot, the filtrate is cooled, and then the filtrate is allowed to age and crystallize. After the aging is completed, the filtrate is filtered again, and then the filter residue is dried to obtain calcium sulfate whiskers.
3. The silicone sealant according to claim 2, characterized in that: The microwave irradiation time is 25-35 minutes.
4. The silicone sealant according to claim 2, characterized in that: The whisker filler also includes silica sol modified whiskers, and the silica sol modified whiskers are prepared according to the following method: The calcium sulfate whiskers and silica sol are mixed, stirred and centrifuged, and the obtained precipitates are dried to obtain silica sol modified whiskers.
5. The silicone sealant according to claim 4, characterized in that: The silica sol is prepared according to the following method: Anhydrous ethanol, TEOS and deionized water are mixed, stirred and heated to obtain a mixture, the mixture is cooled, hydrochloric acid is added to the mixture, and stirring is continued at room temperature for a period of time to obtain silica sol.
6. The silicone sealant according to claim 4, characterized in that: The weight ratio of the silica sol modified whiskers to the calcium sulfate whiskers is (1.4-1.8):
1.
7. The silicone sealant according to claim 1, characterized in that: The mildew inhibitor is prepared according to the following method: (1) dissolving chitosan in an acetic acid aqueous solution, adding succinic anhydride to the obtained solution, diluting it with methanol and stirring it to obtain a chitosan modified solution; (2) adding halloysite nanotubes to the chitosan modified solution, adjusting the pH with hydrochloric acid after stirring, continuing to stir the reaction and then centrifuging, washing and drying the precipitate to obtain chitosan modified nanotubes; (3) mixing silver nitrate, modified nanotubes and methanol, stirring and then oscillating, centrifuging the product, washing the precipitate with methanol, and vacuum drying to obtain silver ion modified nanotubes; (4) Mixing the silver ion-modified nanotubes, sodium borohydride and sodium hydroxide solution, diluting with water, stirring and centrifuging, and washing and vacuum drying the precipitate to obtain a mildew inhibitor.
8. The silicone sealant according to claim 7, characterized in that: The halloysite nanotubes are also activated before use, and the activation method is as follows: The activation treatment of the halloysite nanotubes can be completed by soaking the halloysite nanotubes in hydrochloric acid for 4-8 days, shaking them at certain time intervals during the treatment, and then centrifuging them. The obtained precipitate can be washed and dried.
9. The silicone sealant according to claim 8, characterized in that: The halloysite nanotubes are immersed in hydrochloric acid for 5-7 days.
10. The method for preparing the silicone sealant according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) mixing a base polymer, nano calcium carbonate, a whisker filler and a plasticizer under heating conditions to obtain a base material, and grinding the base material for later use; (2) The base material, fumed silica, silane coupling agent, mildew inhibitor and catalyst are mixed and then stirred in vacuum to obtain silicone sealant.