Phase change composite material and preparation method thereof

By forming a double-layer porous skeleton in the phase change material and encapsulating the phase change material, the problems of low thermal conductivity and easy material leakage in the existing technology are solved, efficient thermal management and heat storage capabilities are achieved, and thermal insulation is provided. , a solution integrating heat conduction and heat storage, which improves thermal management efficiency and safety.

CN118772848APending Publication Date: 2024-10-15UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410909253.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing phase change materials have problems such as low thermal conductivity, easy leakage of liquid phase materials, high rigidity of solid phase materials, and supercooling in the cooling process. In addition, traditional refrigeration and heating methods consume a lot of energy, are highly destructive to the environment, and lack centralized isolation. A material that integrates heat, heat conduction and heat storage.

Method used

By adding dispersant and thermally conductive filler to water to form a thermally conductive layer precursor suspension solution, immersing it in the thermal insulation material to form a double-layer porous skeleton, and encapsulating the phase change material in it through the vacuum impregnation method, a thermally conductive layer precursor with thermal insulation, thermal conductivity and thermal storage properties is prepared. Functional phase change composites.

Benefits of technology

It achieves efficient thermal management, has good anti-seepage performance, shape stability, thermal conductivity and heat storage capacity. It has high heat storage density, high stability, fast thermal response to light, low preparation cost, high enthalpy value, and can It absorbs heat slowly during the day and releases it slowly at night, improving thermal management efficiency and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772848A_ABST
    Figure CN118772848A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of phase change energy storage and heat conduction, and particularly relates to a phase change composite material and a preparation method of the phase change composite material. The phase change composite material prepared by the invention has the advantages of large heat storage density, high stability, rapid thermal response to illumination, low preparation cost, high enthalpy value and simple preparation process. Through the combination of the thermal insulation material and the high-thermal-conductivity material, the phase-change composite material can slowly absorb heat in the daytime, and after energy is slowly released at night, the energy is transmitted and used through the high-thermal-conductivity material, so that the temperature of a thermal management object can be regulated and controlled, and the thermal management efficiency and safety are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of phase change energy storage and heat conduction, and specifically relates to a phase change composite material and a preparation method thereof. Background Art

[0002] Phase change heat storage technology is one of the main directions of energy storage technology. Its main purpose is to utilize the phase change thermal effect to store the heat lost in the external environment in the form of latent heat, and autonomously release and utilize the energy under appropriate conditions to improve energy utilization. The use of phase change energy storage technology to collect and store thermal energy in sunlight instead of traditional fossil fuel combustion can provide a new source of energy for daily production and life. Although phase change materials have great advantages, there are still some challenges, including low thermal conductivity, easy leakage of liquid phase materials, high rigidity of solid phase materials, and a certain degree of supercooling in the cooling process. Therefore, practical solutions are needed before they can be widely used.

[0003] At the same time, with the continuous improvement of people's living standards, when faced with high or low temperature weather, people will take various measures to cool or heat to achieve the purpose of regulating temperature, but traditional methods (such as air conditioning, electric fans, etc.) consume a lot of energy and cause damage to the environment. With the development of materials science, researchers are also deeply developing functional materials to achieve efficient use of thermal energy and improve the problems caused by the above situation. This requires the material to have special photothermal, electrothermal, magnetic thermal and other properties, absorb and release heat when stimulated by external stimuli, without any energy input, and has the potential to replace traditional high-energy consumption technologies. Summary of the invention

[0004] The present invention provides a phase change composite material and a preparation method thereof, so as to solve the problem in the prior art of lacking a special material integrating heat insulation, heat conduction and heat storage.

[0005] To achieve the above object, the present invention proposes the following technical solutions:

[0006] A method for preparing a phase change composite material comprises the following steps:

[0007] Step 1, adding a dispersant and a thermal conductive filler into water to obtain a thermal conductive layer precursor suspension solution;

[0008] Step 2, immersing the heat insulating material into the heat conductive layer precursor suspension solution to obtain a double-layer porous skeleton, wherein the double-layer porous skeleton includes a heat insulating layer formed by the heat insulating material and a heat conductive layer formed by the heat conductive material;

[0009] Step 3, shaping and encapsulating the phase change material in a double-layer porous skeleton to obtain a phase change composite material.

[0010] Preferably, step 1 is specifically:

[0011] A dispersant and a thermal conductive filler are added to water, and magnetic stirring is performed to obtain a thermal conductive layer precursor suspension solution.

[0012] Preferably, in step 1, the ratio of the added amount of the dispersant to the thermal conductive filler is 10:50-150.

[0013] Preferably, step 2 is specifically:

[0014] The heat insulating material is immersed in the heat conducting layer precursor suspension solution, directionally frozen, and then placed in a freeze dryer to obtain a double-layer porous skeleton after being dried.

[0015] Preferably, step 3 is specifically:

[0016] The phase change material is shaped and encapsulated in a double-layer porous skeleton by a vacuum impregnation method to obtain a phase change composite material.

[0017] Preferably, the dispersant in step 1 is any one of carboxymethyl cellulose, nanocellulose, polyvinyl alcohol, and aramid nanofiber.

[0018] Preferably, the thermally conductive filler in step 1 is any one of graphene, reduced graphene oxide, carbon nanotubes, boron nitride, MXene, aluminum nitride, and silicon carbide.

[0019] Preferably, the thermal insulation material is polyimide foam.

[0020] Preferably, the phase change material is any one of polyethylene glycol, paraffin, fatty acid, and inorganic hydrated salt.

[0021] A phase change composite material is prepared by the preparation method of the phase change composite material.

[0022] The present invention is beneficial in that:

[0023] The present invention proposes a method for preparing a phase change composite material. The thermal insulation material can achieve good thermal insulation in the PI layer, the addition of thermal conductive filler can improve the thermal conductivity of the aerogel layer, and the high loading rate of the phase change material can make it have excellent heat storage capacity, so that a phase change material with good anti-seepage performance and shape stability, strong thermal conductivity and heat storage capacity, high melting enthalpy value and high energy storage efficiency can be obtained.

[0024] The phase change composite material prepared by the present invention has the advantages of high heat storage density, high stability, rapid thermal response to light, low preparation cost, high enthalpy value and simple preparation process. By combining thermal insulation materials and high thermal conductivity materials, the phase change composite material can slowly absorb heat during the day and release the energy slowly at night. After being transmitted and used through the high thermal conductivity material, the temperature of the thermal management object can be regulated, thereby improving the efficiency and safety of thermal management. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:

[0026] Figure 1 It is a schematic diagram of a process for preparing a phase change composite material;

[0027] Figure 2 The physical diagrams of embodiments 1 to 3 provided by the present invention;

[0028] Figure 3 In Examples 1 to 3, abcd are SEM images of the graphene composite aerogel and polyimide foam prepared in Example 1, Example 2, and Example 3 before loading PEG6000;

[0029] Figure 4 In Examples 1 to 3, abcd are SEM images of the graphene composite aerogel and polyimide foam loaded with PEG6000 prepared in Example 1, Example 2, and Example 3, respectively;

[0030] Figure 5 The DSC heating curves and cooling curves of the graphene nanosheet aerogel and polyimide foam loaded with PEG6000 and PEG6000 in Examples 1 to 3 provided by the present invention;

[0031] Figure 6 A physical diagram of Example 4 provided by the present invention;

[0032] Figure 7 is the SEM image of the aerogel in Example 4, abcde are the SEM images of PAS / CMC, C-PI / CNTs-0.5, C-PI / CNTs-1\, C-PI / CNTs-2, and C-PI / CNTs-3 before loading PEG6000, respectively;

[0033] Figure 8 are the SEM images of the composite phase change materials in Example 4, and abcde are the SEM images of PEG / PAS / CMC, PEG / C-PI / CNTs-0.5, PEG / C-PI / CNTs-1, PEG / C-PI / CNTs-2, and PEG / C-PI / CNTs-3 after loading PEG6000, respectively. DETAILED DESCRIPTION

[0034] The present invention will be described in detail below with reference to the accompanying drawings and in combination with embodiments. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other without conflict.

[0035] The following detailed description is an exemplary description, which is intended to provide further detailed description of the present invention. Unless otherwise specified, all technical terms used in the present invention have the same meaning as those generally understood by those skilled in the art to which the present invention belongs. The terms used in the present invention are only for describing specific embodiments, and are not intended to limit the exemplary embodiments according to the present invention.

[0036] See also Figure 1 As shown, the present invention provides a method for preparing a phase change composite material, comprising the following steps:

[0037] Step 1, adding a dispersant and a thermal conductive filler into water, and performing magnetic stirring to obtain a thermal conductive layer precursor suspension solution;

[0038] Step 2, immersing the heat insulating material into the heat conductive layer precursor suspension solution, performing directional freezing, placing the material into a freeze dryer after freezing, and obtaining a double-layer porous skeleton after drying;

[0039] The double-layer porous skeleton comprises a heat-insulating layer and a heat-conducting layer, wherein the heat-insulating layer is formed of a heat-insulating material, and the heat-conducting layer is formed of a heat-conducting material.

[0040] Step 3, the phase change material is shaped and encapsulated in a double-layer porous skeleton by a vacuum impregnation method to obtain a phase change composite material.

[0041] In a specific embodiment, the dispersant is any one of carboxymethyl cellulose, nanocellulose, polyvinyl alcohol, aramid nanofiber, etc.

[0042] In a specific embodiment, the thermally conductive filler is any one of graphene, reduced graphene oxide, carbon nanotubes, boron nitride, MXene, aluminum nitride, and silicon carbide.

[0043] In a specific embodiment, the thermal insulation material comprises polyimide foam.

[0044] In a specific embodiment, the double skeleton material of the double-layer porous skeleton is polyimide foam and carbon nanotube aerogel, or polyimide foam, carboxymethyl cellulose and graphene nanosheet aerogel, or polyurethane and carbon nanotube aerogel, or polyethylene carbon nanotube aerogel and the like.

[0045] In a specific embodiment, in the phase change composite material, polyimide foam, polyimide aerogel, polyimide film, polyurethane sponge, melamine sponge, carboxymethyl cellulose aerogel, etc. are thermal insulation layers, and graphene aerogel, carbon nanotube aerogel, MXene aerogel, boron nitride aerogel, carbonized biomass, etc. are thermal conductive layers.

[0046] In a specific embodiment, the phase change material is any one of polyethylene glycol, paraffin, fatty acid, and inorganic hydrated salt.

[0047] In a specific embodiment, in the phase change composite material of step 1, the ratio of the added amount of the dispersant and the thermal conductive filler in the aerogel is 10:50-150.

[0048] The present invention also provides a phase change composite material, which is made by the phase change composite material preparation method.

[0049] Example 1

[0050] Step 1: Add 0.1 g of carboxymethyl cellulose (CMC) to a beaker containing 10 mL of deionized water, and stir the mixture magnetically for 1 hour until it is completely mixed. Then add 0.05 g of graphene nanosheets to the above solution and stir magnetically for 8 hours to obtain a uniformly dispersed CMC / GNP suspension. Place the polyimide foam on the suspension and slightly immerse it, use liquid nitrogen for directionally freezing, and then put it into a freeze dryer for drying.

[0051] Step 2, apply 80°C heat to PEG6000 until it is completely melted into liquid, immerse the constructed double-layer skeleton into the molten PEG, and vacuum impregnate it in a vacuum drying oven at 80°C for 8 hours; then, use an oven to heat the sample and use filter paper to leak the sample to obtain a phase change composite material.

[0052] Example 2

[0053] Step 1: Add 0.1 g of carboxymethyl cellulose (CMC) to a beaker containing 10 mL of deionized water, and stir the mixture magnetically for 1 hour until it is completely mixed. Then add 0.1 g of graphene nanosheets to the above solution and stir magnetically for 8 hours to obtain a uniformly dispersed CMC / GNP suspension. Place the polyimide foam on the suspension and slightly immerse it, use liquid nitrogen for directionally freezing, and then put it into a freeze dryer for drying.

[0054] Step 2, apply 80°C heat to PEG6000 until it is completely melted into liquid, immerse the constructed double-layer skeleton into the molten PEG, and vacuum impregnate it in a vacuum drying oven at 80°C for 8 hours; then, use an oven to heat the sample and use filter paper to leak the sample to obtain a phase change composite material.

[0055] Example 3

[0056] Step 1: Add 0.1 g of carboxymethyl cellulose (CMC) to a beaker containing 10 mL of deionized water, and stir the mixture magnetically for 1 hour until it is completely mixed. Then add 0.15 g of graphene nanosheets to the above solution and stir magnetically for 8 hours to obtain a uniformly dispersed CMC / GNP suspension. Place the polyimide foam on the suspension and slightly immerse it, use liquid nitrogen for directionally freezing, and then put it into a freeze dryer for drying.

[0057] Step 2, apply 80°C heat to PEG6000 until it is completely melted into liquid, immerse the constructed double-layer skeleton into the molten PEG, and vacuum impregnate it in a vacuum drying oven at 80°C for 8 hours; then, use an oven to heat the sample and use filter paper to leak the sample to obtain a phase change composite material.

[0058] Examples 1-3 are shown in the figure Figure 2 shown.

[0059] In Examples 1-3, the loading rate of graphene aerogel (GA-1) on polyethylene glycol is 95.66%, the loading rate of graphene aerogel (GA-2) on polyethylene glycol is 94.94%, and the loading rate of graphene aerogel (GA-3) on polyethylene glycol is 94.36%.

[0060] In Examples 1-3, in the DSC test, the melting enthalpy (Hm) and crystallization enthalpy (Hc) of PCM (PEG / GA-1) were 137.66 J / g and 133.30 J / g, respectively, and the melting temperature (Tm) and crystallization temperature (Tc) were 63.15°C and 36.03°C, respectively. The melting enthalpy (Hm) and crystallization enthalpy (Hc) of PCM (PEG / GA-2) were 123.07 J / g and 124.67 J / g, respectively, and the melting temperature (Tm) and crystallization temperature (Tc) were 61.68°C and 40.76°C, respectively. The melting enthalpy (Hm) and crystallization enthalpy (Hc) of PCM (PEG / GA-3) were 123.52 J / g and 117.82 J / g, respectively, and the melting temperature (Tm) and crystallization temperature (Tc) were 61.19°C and 40.90°C, respectively.

[0061] In Examples 1 to 3, the polyimide foam (PI) loading rate is 98.37%; in the DSC test, the melting enthalpy (Hm) and crystallization enthalpy (Hc) of PCM (PEG / PI) are 143.20 J / g and 133.53 J / g, respectively, and the melting temperature (Tm) and crystallization temperature (Tc) are 72.43°C and 42.50°C, respectively.

[0062] Meanwhile, in Examples 1 to 3, the melting enthalpy (Hm) and crystallization enthalpy (Hc) of the PEG6000 used in the DSC test were 158.21 J / g and 145.86 J / g, respectively, and the melting temperature (Tm) and crystallization temperature (Tc) were 63.33° C. and 42.08° C., respectively.

[0063] In Examples 1 to 3, the SEM images of the graphene composite aerogel and polyimide foam prepared in Example 1, Example 2, and Example 3 before loading PEG6000 are shown in FIG. Figure 3 a, b, c, and d are shown respectively.

[0064] In Examples 1 to 3, the SEM images of the graphene composite aerogel and polyimide foam loaded with PEG6000 prepared in Examples 1, 2 and 3 are as follows: Figure 4 a, b, c, and d are shown respectively.

[0065] In Examples 1 to 3, the DSC heating curves and cooling curves of the graphene nanosheet aerogel and the polyimide foam loaded with PEG6000 and PEG6000 are as follows: Figure 5 shown.

[0066] Example 4

[0067] Step 1, 2g 4,4'-diaminodiphenyl ether (ODA) and 24g N,N-dimethylacetamide (DMAc) are mixed, and then 2.21g of pyromellitic anhydride (PMDA) is added to the above solution, and the mixture is placed in an ice-water bath, and continuously mixed by magnetic stirring for 2 hours until a uniform state is reached. Subsequently, 1.01g of triethylamine is added to the resulting mixed solution, and mechanical stirring is performed for 5 hours to obtain a polyamic acid (PAA) precursor solution. Freeze-drying is performed to obtain a water-soluble polyamic acid solid. 3g PAA, 0.84g TEA and 200g deionized water are added to a beaker, and stirred until the PAA particles are completely dissolved to obtain a polyamic acid salt (PAS) solution.

[0068] Step 2, add 0.5, 1, 2, 3wt% CNTs to 5g PAS solution respectively and stir magnetically until mixed evenly. Add 100mg CMC to 5g PAS solution and stir until mixed evenly. Then pour the mixed solution into a freezing mold with a bottom of thermally conductive brass, an edge of thermally insulating plastic, and a diameter of 25mm for freezing. The frozen sample is placed in a low temperature environment of -60°C for freeze drying to sublime ice crystals to obtain PAS / CNTs and PAS / CMC aerogels. Then, the solvent is evaporated at 200°C and thermal imidization is performed at 300°C to obtain a polyimide series sample PI / CNTs-x. The carbon nanotube aerogel is carbonized at 800°C to obtain C-PI / CNTs-x. After the preparation of C-PI / CNTs-x aerogel is completed, it is placed above the PAS / CMC solution to freeze and combine to obtain an integrated aerogel. Subsequently, the above aerogel is completely immersed in molten PEG6000 for 8 hours by vacuum impregnation. After removing the excess PEG, the PEG / PAS / CMC@PEG / C-PI / CNTs integrated composite phase change material was obtained, such as Figure 6 shown.

[0069] In Example 4, the loading rate of PEG / PAS / CMC on polyethylene glycol is 87.03%, the loading rate of PEG / C-PI / CNTs-0.5 on polyethylene glycol is 92.14%, the loading rate of PEG / C-PI / CNTs-1 on polyethylene glycol is 91.75%, the loading rate of PEG / C-PI / CNTs-2 on polyethylene glycol is 95.56, and the loading rate of PEG / C-PI / CNTs-3 on polyethylene glycol is 95.54%.

[0070] In Example 4, in the DSC test, the melting enthalpy (Hm) and crystallization enthalpy (Hc) of PEG / PAS / CMC are 139.50 J / g and 133.96 J / g, respectively, and the melting temperature (Tm) and crystallization temperature (Tc) are 58.12°C and 44.35°C, respectively. The melting enthalpy (Hm) and crystallization enthalpy (Hc) of PEG / C-PI / CNTs-0.5 are 145.12 J / g and 138.40 J / g, respectively, and the melting temperature (Tm) and crystallization temperature (Tc) are 60.83°C and 41.86°C, respectively. The melting enthalpy (Hm) and crystallization enthalpy (Hc) of PEG / C-PI / CNTs-1 are 147.63 J / g and 142.50 J / g, respectively, and the melting temperature (Tm) and crystallization temperature (Tc) are 59.81°C and 41.97°C, respectively. The melting enthalpy (Hm) and crystallization enthalpy (Hc) of PEG / C-PI / CNTs-2 were 160.30 J / g and 152.99 J / g, respectively, and the melting temperature (Tm) and crystallization temperature (Tc) were 59.06°C and 40.66°C, respectively. The melting enthalpy (Hm) and crystallization enthalpy (Hc) of PEG / C-PI / CNTs-3 were 153.80 J / g and 140.43 J / g, respectively, and the melting temperature (Tm) and crystallization temperature (Tc) were 59.20°C and 40.82°C, respectively.

[0071] The SEM images of PAS / CMC, C-PI / CNTs-0.5, C-PI / CNTs-1\, C-PI / CNTs-2, and C-PI / CNTs-3 in Example 4 before loading PEG6000 are shown in Figure 2. Figure 7 As shown in a, b, c, d, and e.

[0072] The SEM images of PEG / PAS / CMC, PEG / C-PI / CNTs-0.5, PEG / C-PI / CNTs-1, PEG / C-PI / CNTs-2, and PEG / C-PI / CNTs-3 loaded with PEG6000 in Example 4 are shown in Figure 2. Figure 8 As shown in a, b, c, d, and e.

[0073] The phase change composite material provided by the present invention has good anti-seepage performance and shape stability, strong thermal conductivity and heat storage capacity, high melting enthalpy value and high energy storage efficiency.

[0074] Secondly, the aerogel and polyimide foam used in the present invention both have rich porous structures and large specific surface areas, which can absorb phase change materials to solve their leakage problems, and show a higher loading rate after loading phase change core materials. At the same time, the special structure of polyimide foam material makes it have good flame retardancy, long life, high and low temperature resistance, and environmental friendliness. Both show good thermal reliability and thermal stability, as well as good phase change behavior.

[0075] Third, the phase change composite material provided by the present invention integrates thermal insulation, thermal conductivity and heat storage: polyimide foam has extremely strong thermal insulation performance and can achieve good thermal insulation in the thermal insulation layer; the addition of thermal conductive filler can improve the thermal conductivity of the aerogel layer; the high loading rate of the phase change material can make it have excellent heat storage capacity.

[0076] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention.

[0077] The phase change composite material provided by the present invention has the advantages of high heat storage density, high stability, rapid thermal response to light and voltage, low preparation cost, high enthalpy value, and simple preparation process. Through structural design, it can be used as a thermal management material and building material. By combining thermal insulation materials and high thermal conductivity materials, heat is slowly absorbed during the day, and energy is slowly released at night. After being transmitted and used through high thermal conductivity materials, the temperature of the thermal management object can be regulated, thereby improving thermal management efficiency and safety.

[0078] It is known from common technical knowledge that the present invention can be implemented by other embodiments that do not deviate from its spirit or essential features. Therefore, the above disclosed embodiments are only illustrative in all respects and are not exclusive. All changes within the scope of the present invention or within the scope equivalent to the present invention are included in the present invention.

[0079] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a phase change composite material, characterized in that: The steps include: Step 1: adding a dispersant and a thermal conductive filler to water to obtain a thermal conductive layer precursor suspension solution; Step 2: Immersing a heat-insulating material into the heat-conducting layer precursor suspension solution to obtain a double-layer porous skeleton, wherein the double-layer porous skeleton includes a heat-insulating layer formed by the heat-insulating material and a heat-conducting layer formed by the heat-conducting material; Step 3: Shape and encapsulate the phase change material in the double-layer porous skeleton to obtain a phase change composite material.

2. The method for preparing a phase change composite material according to claim 1, wherein: Step 1 is as follows: A dispersant and a thermal conductive filler are added to water and magnetic stirring is performed to obtain a thermal conductive layer precursor suspension solution.

3. The method for preparing a phase change composite material according to claim 1, wherein: In step 1, the ratio of the added amount of the dispersant to the thermal conductive filler is 10:50-150.

4. The method for preparing a phase change composite material according to claim 1, wherein: Step 2 is as follows: The heat insulating material is immersed in the heat conducting layer precursor suspension solution, directionally frozen, and then placed in a freeze dryer to obtain a double-layer porous skeleton after being frozen.

5. The method for preparing a phase change composite material according to claim 1, wherein: Step 3 is as follows: The phase change material is shaped and encapsulated in a double-layer porous skeleton by a vacuum impregnation method to obtain a phase change composite material.

6. The method for preparing a phase change composite material according to claim 1, wherein: The dispersant in step 1 is any one of carboxymethyl cellulose, nanocellulose, polyvinyl alcohol, and aramid nanofiber.

7. The method for preparing a phase change composite material according to claim 1, wherein: The thermally conductive filler in step 1 is any one of graphene, reduced graphene oxide, carbon nanotubes, boron nitride, MXene, aluminum nitride, and silicon carbide.

8. The method for preparing a phase change composite material according to claim 1, wherein: The heat insulating material is polyimide foam.

9. The method for preparing a phase change composite material according to claim 1, wherein: The phase change material is any one of polyethylene glycol, paraffin, fatty acid, and inorganic hydrated salt.

10. A phase change composite material, characterized in that: The phase change composite material is made by the preparation method of a phase change composite material according to any one of claims 1-9.

Citation Information

Cited By

  • Heat insulation-heat conduction integrated phase change composite material and preparation method thereof

    CN119978538A

  • Thermal insulation-thermal conduction integrated phase change composite material and preparation method thereof

    CN119978538B

  • MXene synergistic composite phase change heat storage material and preparation method thereof

    CN120484785A