Blue-blue light aluminate fluorescent powder and composite fluorescent glass thereof

By developing blue cyan aluminate phosphors and composite fluorescent glass, and using near-ultraviolet excitation technology, the problems of blue light overflow and cyan light loss in white LED lighting have been solved, and the quantum efficiency and thermal stability of the phosphors have been improved to meet the needs Meet the needs of indoor lighting and wide color gamut display.

CN118772882AActive Publication Date: 2024-10-15DONGHUA UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410769422.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

Existing white LED lighting suffers from problems such as blue light overflow and lack of cyan light, such as high color temperature, low color rendering index, and aging of phosphors in heat and light radiation environments, making it difficult to meet the requirements of indoor lighting and wide color gamut display.

Method used

Develop a blue cyan aluminate phosphor and its composite fluorescent glass. It emits blue cyan light with a peak wavelength of 450-500nm through near-ultraviolet excitation. It is combined with mesoporous silica molecular sieve sintering to improve the thermal stability of the phosphor. and spectral uniformity.

Benefits of technology

It achieves high quantum efficiency and thermal quenching resistance, the luminous intensity of the phosphor remains stable at 150°C, and the thermal stability of the composite fluorescent glass is significantly improved, making it suitable for full-spectrum lighting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772882A_ABST
    Figure CN118772882A_ABST
Patent Text Reader

Abstract

The invention relates to blue-blue light aluminate fluorescent powder and composite fluorescent glass thereof. The fluorescent powder has the following general formula: A < x > B < y > Eu < k > Al < h > C < g > O < 34 + delta >, wherein A is one or more of Na, K, Rb and Cs; b is one or more of Ba, Sr, Ca and Mg; c is one or more of Ga, B and In; x, y, k, h, g and delta are molar coefficients, 0 < = x < = 2.6, 0 < = y < = 2.6, 0 < = k < = 0.6, 0 < = h < = 22, 0 < = g < = 22, and delta changes according to an electroneutrality rule. Uniformly mixing fluorescent powder with the mesoporous silica molecular sieve, and sintering in a discharge plasma sintering furnace to obtain the fluorescent glass. The fluorescent powder and the fluorescent glass can be effectively excited by (near) ultraviolet light (360-420 nm), and are suitable for being used as blue and cyan fluorescent materials in full-spectrum illumination excited by the near ultraviolet light.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of fluorescent materials, and particularly relates to a blue-cyan aluminate fluorescent powder and a composite fluorescent glass thereof. Background Art

[0002] As a new type of solid-state light source, white light emitting diodes (WLEDs) have the advantages of small size, long life, fast response speed, and green environmental protection compared with traditional incandescent tungsten filament bulbs and fluorescent lamps. White light LEDs can be flat packaged and easily developed into thin and portable products. They have gradually replaced traditional lighting sources and are known as the fourth generation of lighting sources. As a composite light, white light can be obtained from the three primary colors of red, green, and blue or from a combination of other colors. At present, the main ways to obtain white light are: a combination of three primary color LED chips, a blue light LED chip combined with Y 3 Al 5 O 12 :Ce 3+ (YAG) yellow phosphor, near-ultraviolet LED chip combined with red, green and blue phosphor. Among them, the three-primary color LED chip combination has complex control circuits, high requirements for packaging technology, and easy light color drift with extended use time, which is not suitable for indoor lighting. Blue LED chip combined with YAG yellow phosphor is the current mainstream commercial white light realization method. This combination has the advantages of high light conversion efficiency, good thermal stability, and simple packaging process. However, due to the lack of red light components in this combination, its color temperature is high and the color rendering index is low. Long-term use will affect human sleep and various physiological activities, and it is difficult to meet the requirements of indoor lighting or wide color gamut display. In contrast, near-ultraviolet LED chips combined with red, green and blue phosphors can obtain white light with good color rendering effect and adjustable color temperature, which better solves the problem of blue light overflow in blue LED chips combined with YAG yellow phosphors. It is suitable for indoor lighting and lighting environments with high color reproduction requirements, so research in recent years has been on the rise. Among the phosphors of many systems, the lack of luminescence in the cyan region (480-520nm) is becoming increasingly obvious. In white solid-state lighting, the lack of cyan often results in reduced uniformity of white light, which is not conducive to improving the color rendering index. This phenomenon is commonly known as the cyan gap. Therefore, in order to obtain full-spectrum white light LEDs close to the solar spectrum, it is crucial to develop near-ultraviolet excited cyan fluorescent materials.

[0003] At present, traditional LED lighting mainly uses a mixture of phosphor and silicone / epoxy resin as a photoconversion material. Although this process has been industrialized, it has the problem of low luminescence threshold under high power: silicone / epoxy resin is severely aged when exposed to heat and light radiation for a long time, affecting product performance. In order to solve this problem, phosphors are often encapsulated in glass or ceramic matrices with better physical and chemical stability. Among them, the glass matrix has the advantages of high transmittance, simple preparation process and adjustable components, making composite fluorescent glass a research hotspot for solid-state lighting photoconversion materials. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a blue-cyan aluminate phosphor and a composite fluorescent glass thereof, which can be effectively excited by (near) ultraviolet light (360-420nm) and is suitable as a blue and cyan fluorescent material for full-spectrum lighting excited by near-ultraviolet light.

[0005] The present invention provides a blue cyan aluminate phosphor, which has the following general formula: x B y Eu k Al h C g O 34+δ ; A is one or more of Na, K, Rb, Cs; B is one or more of Ba, Sr, Ca, Mg; C is one or more of Ga, B, In; x, y, k, h, g, δ are molar coefficients, 0≤x≤2.6, 0≤y≤2.6, 0≤k≤0.6, 0≤h≤22, 0≤g≤22, δ changes according to the law of electrical neutrality.

[0006] Furthermore, the phosphor emits blue-cyan light with a peak wavelength of 450nm-500nm.

[0007] The present invention also provides a method for preparing a blue-cyan aluminate phosphor, comprising the following steps:

[0008] (1) Weighing the corresponding proportions of reactant raw materials according to the stoichiometric ratio;

[0009] (2) Grinding the above-mentioned reactant raw materials uniformly to obtain a mixed powder, and transferring the mixed powder into a crucible;

[0010] (3) placing the crucible in a horizontal tube furnace and keeping it at 1300-1400° C. for 4-6 hours in a reducing atmosphere. After the reaction is completed, the crucible is crushed and ground to obtain a blue-cyan aluminate phosphor.

[0011] Furthermore, the reducing atmosphere in step (3) is composed of 10% to 20% H 2and 80%-90% N 2 composition.

[0012] The invention also provides a blue-cyan aluminate composite fluorescent glass, which is obtained by mixing and sintering the blue-cyan aluminate fluorescent powder and the mesoporous silicon oxide molecular sieve.

[0013] Furthermore, the mesoporous silica molecular sieve is one or more of FDU-12, SBA-15, MCM-41, MSN and ZSM-5.

[0014] Furthermore, the composite fluorescent glass emits blue light with a peak wavelength of 443 nm.

[0015] The present invention also provides a method for preparing a blue-cyan aluminate composite fluorescent glass, comprising the following steps:

[0016] (1) grinding blue-cyan aluminate phosphor and mesoporous silica molecular sieve to obtain a mixed powder, and placing the powder into a mold;

[0017] (2) placing the mold in a spark plasma sintering furnace for sintering, wherein the sintering process parameters are: sintering temperature of 910-1000°C, heating rate of 100-600°C / min, pressure of 50-60MPa, holding time of 1-3min, and vacuum sintering; (3) double-sided grinding and polishing of the fluorescent glass block obtained in step (2) to obtain blue-cyan aluminate composite fluorescent glass.

[0018] Furthermore, the mass ratio of the blue-cyan aluminate phosphor to the mesoporous silica molecular sieve is 0.01-0.25:1.

[0019] Furthermore, the blue-cyan aluminate phosphor or the blue-cyan aluminate composite fluorescent glass is effectively excited by near-ultraviolet light of 360-420 nm.

[0020] The invention also provides the use of blue-cyan aluminate fluorescent powder or blue-cyan aluminate composite fluorescent glass in full-spectrum lighting excited by near-ultraviolet light.

[0021] Beneficial Effects

[0022] The phosphor and composite fluorescent glass provided by the present invention can be effectively excited by (near) ultraviolet light of 360-420nm. Among them, the aluminate phosphor can emit blue-green light with a peak wavelength of 450-500nm; at room temperature, its fluorescence quantum efficiency can reach up to 98.26%; at 150°C, its luminous intensity can be maintained at a maximum of 86.90% at room temperature, which has the advantages of high quantum efficiency and good resistance to thermal quenching compared with the existing near-ultraviolet excited cyan fluorescent materials; the composite fluorescent glass can emit blue light with a peak wavelength of 443nm; at room temperature, its fluorescence quantum efficiency is 79.51%; at 150°C, its luminous intensity can be maintained at a maximum of 105.6% at room temperature, showing anti-thermal quenching performance. After the above-mentioned phosphor is compounded with the mesoporous silica molecular sieve, its thermal stability is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 K prepared in Example 1 1.8 Eu 0.4 Al 17.83 Ga 4 O 33.9 X-ray diffraction spectrum of phosphor;

[0024] Figure 2 K prepared in Example 1 1.8 Eu 0.4 Al 17.83 Ga 4 O 33.9 Excitation spectrum (a), emission spectrum (b), fluorescence quantum efficiency diagram (c) and variable temperature fluorescence spectrum (d) of the phosphor;

[0025] Figure 3 K prepared in Example 2 1.4 Ba 0.4 Eu 0.4 Al 17.83 Ga 4 O 33.9 X-ray diffraction spectrum of phosphor;

[0026] Figure 4 K prepared in Example 2 1.4 Ba 0.4 Eu 0.4 Al 17.83 Ga 4 O 33.9 Excitation spectrum (a), emission spectrum (b), fluorescence quantum efficiency diagram (c) and variable temperature fluorescence spectrum (d) of the phosphor;

[0027] Figure 5 K prepared in Example 3 1.0 Ba 0.8 Eu 0.4 Al17.83 Ga 4 O 33.9 X-ray diffraction spectrum of phosphor;

[0028] Figure 6 K prepared in Example 3 1.0 Ba 0.8 Eu 0.4 Al 17.83 Ga 4 O 33.9 Excitation spectrum (a), emission spectrum (b), fluorescence quantum efficiency diagram (c) and variable temperature fluorescence spectrum (d) of the phosphor;

[0029] Figure 7 K prepared in Example 4 1.8 Eu 0.4 Al 17.83 Ga 4 O 33.9 X-ray diffraction spectrum of composite fluorescent glass;

[0030] Figure 8 K prepared in Example 4 1.8 Eu 0.4 Al 17.83 Ga 4 O 33.9 Excitation spectrum (a), emission spectrum (b), fluorescence quantum efficiency diagram (c) and variable temperature fluorescence spectrum (d) of the composite fluorescent glass;

[0031] Fig. 9 K prepared in Comparative Example 1 1.8 Eu 0.4 Al 21.83 O 33.9 X-ray diffraction spectrum of phosphor;

[0032] Fig.10 K prepared in Comparative Example 1 1.8 Eu 0.4 Al 21.83 O 33.9 Excitation spectrum (a), emission spectrum (b), fluorescence quantum efficiency diagram (c) and variable temperature fluorescence spectrum (d) of the phosphor;

[0033] Fig.11 This is a performance diagram of the blue-cyan aluminate phosphor of the present invention. DETAILED DESCRIPTION

[0034] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0035] In the following examples and comparative examples, the instruments used for testing the relevant properties of the prepared samples are:

[0036] 1. The crystal structure and phase analysis of the samples were conducted using a Japanese Rigaku D / max-2500 X-ray diffractometer, with the radiation source being a Cu target Ka1 radiation line.

[0037] 2. The excitation spectrum and emission spectrum of the sample were tested using the F-4600 fluorescence spectrometer produced by Hitachi, Japan;

[0038] 3. The temperature spectrum of the sample was tested using the FLS1000 fluorescence spectrometer from Edinburgh, UK;

[0039] 4. The internal quantum efficiency of the sample was tested by a Hamamatsu Quantaurus-QY plus fluorescence spectrometer with an integrating sphere.

[0040] Example 1

[0041] Weigh K 2 CO 3 (0.157 g), Al(OH) 3 (1.000 g), Ga 2 O 3 (0.267 g), Eu 2 O 3 (0.050 g), H 3 BO 3 The above raw materials were mixed and ground to make the raw materials uniform, and then the mixed powder was placed in an alumina crucible and placed in a reducing atmosphere (10% by volume of H 2 and 90% of N 2 The composition of the reducing atmosphere in the following embodiments is the same as that of the reducing atmosphere in this embodiment) and the mixture is heated to 1300°C at a heating rate of 5°C / min, kept warm for 4 hours, and naturally cooled to below 200°C with the furnace, taken out, and the product is fully ground to obtain sample S1.

[0042] The prepared sample S1 was subjected to crystal structure and phase analysis. Figure 1 As shown by Figure 1 It can be seen that the main crystalline phase of sample S1 prepared in this embodiment is K1.8 Eu 0.4 Al 17.83 Ga 4 O 33.9 , no mixed phases were seen.

[0043] The prepared sample S1 was tested for fluorescence performance, and the test results are as follows: Figure 2 As shown. Figure 2 (a) It can be seen that the sample S1 prepared in this embodiment can be effectively excited by (near) ultraviolet light of about 360-420nm; Figure 2 (b) It can be seen that the sample S1 prepared in this embodiment can emit blue light with a peak wavelength of 450nm after being excited by 400nm near-ultraviolet light; Figure 2 (c) It can be seen that the fluorescence quantum yield of sample S1 prepared in this embodiment is 98.26% under 400nm near-ultraviolet light excitation at 25°C; Figure 2 (d) It can be seen that the sample S1 prepared in this embodiment has excellent resistance to thermal quenching. At 150°C, its fluorescence intensity can be maintained at 84.84% of that at room temperature.

[0044] Example 2

[0045] Weigh K 2 CO 3 (0.138 g), Ba 2 CO 3 (0.056 g), Al(OH) 3 (1.000 g), Ga 2 O 3 (0.267 g), Eu 2 O 3 (0.050 g), H 3 BO 3 (0.075g), mix the above raw materials and grind them to make the raw materials mixed evenly, then put the mixed powder into an alumina crucible, and then put it into a horizontal tube furnace with a reducing atmosphere, heat it to 1300°C at a heating rate of 5°C / min, keep it warm for 4h, cool it naturally to below 200°C with the furnace, take it out, and grind the product thoroughly to obtain sample S2.

[0046] The prepared sample S2 was subjected to crystal structure and phase analysis. Figure 3 As shown by Figure 3 It can be seen that the main crystalline phase of sample S2 prepared in this embodiment is K 1.4 Ba 0.4 Eu 0.4 Al 17.83 Ga 4 O 33.9 No obvious impurities were observed.

[0047] The prepared sample S2 was tested for fluorescence performance, and the test results are as follows: Figure 4 As shown. Figure 4 (a) It can be seen that the sample S2 prepared in this embodiment can be effectively excited by 360-420nm (near) ultraviolet light; Figure 4 (b) It can be seen that the sample S2 prepared in this embodiment can emit cyan light with a peak wavelength of 476nm after being excited by 400nm near-ultraviolet light; Figure 4 (c) It can be seen that the fluorescence quantum yield of sample S2 prepared in this embodiment is 97.97% under 400nm near-ultraviolet light excitation at 25°C; Figure 4 (d) It can be seen that the sample S2 prepared in this embodiment has excellent resistance to thermal quenching. At 150°C, its fluorescence intensity can be maintained at 85.20% of that at room temperature.

[0048] Example 3

[0049] Weigh K 2 CO 3 (0.118 g), Ba 2 CO 3 (0.112 g), Al(OH) 3 (1.000 g), Ga 2 O 3 (0.267 g), Eu 2 O 3 (0.050 g), H 3 BO 3 (0.075g), mix the above raw materials and grind them to make the raw materials mixed evenly, then put the mixed powder into an alumina crucible, and then put it into a horizontal tube furnace with a reducing atmosphere, heat it to 1300℃ at a heating rate of 5℃ / min, keep it warm for 4h, cool it naturally to below 200℃, take it out, grind the product thoroughly to obtain sample S3.

[0050] The prepared sample S3 was subjected to crystal structure and phase analysis. Figure 5 As shown by Figure 5 It can be seen that the main crystalline phase of sample S3 prepared in this embodiment is K 1.0 Ba 0.8 Eu 0.4 Al 17.83 Ga 4 O 33.9 No obvious impurities were observed.

[0051] The prepared sample S3 was tested for fluorescence performance, and the test results are as follows: Figure 6 As shown. Figure 6(a) It can be seen that the sample S3 prepared in this embodiment can be effectively excited by 360-420nm (near) ultraviolet light; Figure 6 (b) It can be seen that the sample S3 prepared in this embodiment can emit cyan light with a peak wavelength of 500nm after being excited by 400nm near-ultraviolet light; Figure 6 (c) It can be seen that the fluorescence quantum yield of sample S3 prepared in this embodiment is 84.43% under 400nm near-ultraviolet light excitation at 25°C; Figure 6 (d) It can be seen that the sample S3 prepared in this embodiment has excellent resistance to thermal quenching. At 150°C, its fluorescence intensity can be maintained at 86.90% of that at room temperature.

[0052] Example 4

[0053] The blue aluminate phosphor and mesoporous silica molecular sieve were uniformly mixed in a mass ratio of 0.1:10 and loaded into a graphite mold, and then placed in a spark plasma sintering (SPS) device for sintering. SPS was carried out under vacuum conditions and the sintering pressure was 50MPa. The heating rate during the sintering process was 100-600℃ / min; the sintering temperature was 910-1000℃; and the insulation time was 1min. After sintering, the instrument power was turned off and cooled to room temperature with the furnace. After the sample was taken out and subjected to grinding, polishing and other processes, the composite fluorescent glass S4 was obtained.

[0054] The prepared composite fluorescent glass was subjected to crystal structure and phase analysis. Figure 7 As shown by Figure 7 It can be seen that the composite fluorescent glass is composed of amorphous phase and K 1.8 Eu 0.4 Al 17.83 Ga 4 O 33.9 Phase composition. XRD results show that K 1.8 Eu 0.4 Al 17.83 Ga 4 O 33.9 The phase remains stable after high-temperature sintering.

[0055] The prepared composite fluorescent glass was tested for fluorescence performance. The test results are as follows: Figure 8 As shown. Figure 8 (a) It can be seen that the composite fluorescent glass prepared in this embodiment can be effectively excited by 360-380nm (near) ultraviolet light; Figure 8 (b) It can be seen that the composite fluorescent glass prepared in this embodiment can emit blue light with a peak wavelength of 443nm after being excited by 360nm ultraviolet light; Figure 8(c) It can be seen that the fluorescence quantum yield of sample S4 prepared in this embodiment is 79.51% under 360nm ultraviolet light excitation at 25°C; Figure 8 (d) It can be seen that the composite fluorescent glass prepared in this embodiment has anti-thermal quenching performance. At 150° C., its fluorescence intensity can be maintained at 105.6% of that at room temperature, and its thermal stability is significantly improved.

[0056] Comparative Example 1

[0057] Weigh K 2 CO 3 (0.129 g), Al(OH) 3 (1.000 g), Eu 2 O 3 (0.041 g), H 3 BO 3 (0.058g), mix the above raw materials evenly and then grind them to make the raw materials evenly mixed, then put the mixed powder into an alumina crucible, and then put it into a horizontal tube furnace with a reducing atmosphere, heat it to 1300°C at a heating rate of 5°C / min, keep it warm for 4h, cool it naturally to below 200°C with the furnace, take it out, and grind the product thoroughly to obtain a comparison sample S5.

[0058] The prepared comparative sample S5 was subjected to crystal structure and phase analysis. Fig. 9 As shown by Fig. 9 It can be seen that the main crystalline phase of sample S5 prepared in this comparative example is K 1.8 Eu 0.4 Al 21.83 O 33.9 , with a small amount of Al 2 O 3 Mixed phase.

[0059] The prepared comparative sample S5 was tested for fluorescence performance, and the test results are as follows: Fig.10 As shown. Fig.10 (a) It can be seen that the absorption of the comparative sample S5 prepared in this comparative example at 400nm is weaker than that of the samples S1-S3, and the optimal excitation is located at 360nm, indicating that the component regulation of the present invention can significantly improve the absorption of the aluminate phosphor in the near-ultraviolet band. Fig.10 (b) It can be seen that the comparative sample S5 prepared in this comparative example can emit blue light with a peak wavelength of 450nm after being excited by near-ultraviolet light of 400nm; Fig.10 (c) It can be seen that the fluorescence quantum yield of the comparative sample S5 prepared in this comparative example is 74.29% under 400nm near-ultraviolet light excitation at 25°C, which is significantly lower than that of the samples S1-S3; Fig.10(d) It can be seen that at 150°C, the fluorescence intensity of the comparative sample S5 is 81.80% of that at room temperature, which is lower than that of the S1-S4 samples in Examples 1-4.

[0060] In summary, the present invention can significantly improve the absorption efficiency of aluminate phosphor in the near-ultraviolet region, and improve its fluorescence quantum yield and thermal stability by controlling the components. In addition, by encapsulating the phosphor in a glass matrix, the thermal stability of the fluorescent material can be effectively improved, and the composite fluorescent glass even exhibits an anti-thermal quenching effect, which has good application prospects.

Claims

1. A blue-cyan aluminate phosphor, Features: The phosphor has the following general formula: x B y Eu k Al h C g O 34+δ ; A is one or more of Na, K, Rb, Cs; B is one or more of Ba, Sr, Ca, Mg; C is one or more of Ga, B, In; x, y, k, h, g, δ are molar coefficients, 0≤x≤2.6, 0≤y≤2.6, 0≤k≤0.6, 0≤h≤22, 0≤g≤22, δ changes according to the law of electrical neutrality.

2. The phosphor according to claim 1, Features: The phosphor emits blue-cyan light with a peak wavelength of 450nm-500nm.

3. A method for preparing the blue-cyan aluminate phosphor according to any one of claims 1 to 2, comprising the following steps: (1) Weighing the reactant raw materials in corresponding proportions according to the stoichiometric ratio; (2) Grinding the above-mentioned reactant raw materials uniformly to obtain a mixed powder, and transferring the mixed powder into a crucible; (3) placing the crucible in a horizontal tube furnace and keeping it at 1300-1400° C. for 4-6 hours in a reducing atmosphere. After the reaction is completed, the crucible is crushed and ground to obtain a blue-cyan aluminate phosphor.

4. The preparation method according to claim 3, Features: The reducing atmosphere in step (3) is composed of 10% to 20% H 2 and 80%-90% N 2 composition.

5. A blue-green aluminate composite fluorescent glass, Features: The blue-cyan aluminate phosphor is obtained by mixing and sintering the blue-cyan aluminate phosphor as claimed in claim 1 and a mesoporous silicon oxide molecular sieve.

6. The composite fluorescent glass according to claim 5, Features: The mesoporous silica molecular sieve is one or more of FDU-12, SBA-15, MCM-41, MSN and ZSM-5.

7. The composite fluorescent glass according to claim 5, Features: The composite fluorescent glass emits blue light with a peak wavelength of 443 nm.

8. A method for preparing a blue-cyan aluminate composite fluorescent glass as described in any one of claims 5 to 7, comprising the following steps: (1) grinding blue-cyan aluminate phosphor and mesoporous silica molecular sieve to obtain a mixed powder, and loading the powder into a mold; (2) placing the mold in a discharge plasma sintering furnace for sintering, wherein the sintering process parameters are: sintering temperature of 910-1000°C, heating rate of 100-600°C / min, pressure of 50-60MPa, holding time of 1-3min, and vacuum sintering; (3) double-sided grinding and polishing the fluorescent glass block obtained in step (2) to obtain a blue-cyan aluminate composite fluorescent glass.

9. The blue-cyan aluminate phosphor according to claim 1 or the blue-cyan aluminate composite fluorescent glass according to claim 5, Features: Efficiently excited by near-UV light at 360-420nm.

10. Use of the blue-cyan aluminate phosphor according to claim 1 or the blue-cyan aluminate composite fluorescent glass according to claim 5 in full-spectrum lighting excited by near-ultraviolet light.

Citation Information

Patent Citations

  • Fluorescent glass ceramic and preparation method thereof

    CN111847883A

  • Aluminosilicate fluorescent material capable of emitting green light

    CN112126433A

  • Eu &lt; 2 + &gt;-doped cyan fluorescent powder with high quantum efficiency and preparation method thereof