Preventing hydrogen sulfide emissions in production of hot asphalt or bitumen

By adding calcium nitrate aqueous solution or powder to hot asphalt or asphalt, hydrogen sulfide is oxidized into sulfate, which solves the safety hazards and environmental problems caused by hydrogen sulfide emission, achieves harmless hydrogen sulfide treatment, and reduces health risks.

CN118772918APending Publication Date: 2024-10-15YARA INTERNATIONAL ASA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411008975.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2017-07-17
Filing Date
2018-07-17
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

During the production of hot asphalt or bitumen, hydrogen sulfide emissions pose safety concerns and existing compounds are difficult or harmful to handle, leading to health risks and environmental concerns.

Method used

At a temperature of 150 to 200°C, calcium nitrate aqueous solution or calcium nitrate powder is added to asphalt or asphalt mixture to oxidize hydrogen sulfide into sulfate to form soluble sulfate to avoid the generation of waste materials.

Benefits of technology

It effectively reduces the gas phase migration of hydrogen sulfide, reduces health risks to workers, and solves the problem of hydrogen sulfide emissions by forming gypsum as a harmless reaction product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004963760680000053
    Figure BDA0004963760680000053
  • Figure BDA0004963760680000061
    Figure BDA0004963760680000061
Patent Text Reader

Abstract

The present application relates to a method for preventing hydrogen sulfide emissions in the production of hot asphalt or bitumen at a temperature of 150 to 200 DEG C wherein the method comprises the steps of providing an asphalt or bitumen mixture, heating the mixture to a temperature of 150 to 200 DEG C, and adding an aqueous calcium nitrate solution or calcium nitrate powder while mixing the asphalt or asphalt mixture. The present application also relates to the use of an aqueous calcium nitrate solution or calcium nitrate powder for preventing hydrogen sulfide emissions during the mixing of asphalt or asphalt mixtures in the production of hot asphalt or asphalt at a temperature of 150 to 200 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an application with the PCT international application date of July 17, 2018, PCT international application number PCT / EP2018 / 069363, and Chinese national application number 201880033194.1, whose invention name is “Preventing the emission of hydrogen sulfide in the production of hot asphalt or bitumen”. Technical Field

[0002] The present application relates to preventing the emission of hydrogen sulfide (H2S) in the production of hot asphalt or bitumen, more particularly hot asphalt or bitumen at a temperature of 150 to 200°C. Background Art

[0003] Hydrogen sulfide (H2S) is a naturally occurring gas present in a variety of crude oils. It is also formed by the degradation of sulfur compounds in the oil when exposed to high temperatures or catalysts during the refining process of the oil. The main blending component for asphalt production, vacuum tower bottoms (VTB), has a particularly high H2S concentration because they do not undergo additional treatment for removing H2S by distillation, stripping and desulfurization processes. VTB belongs to the heaviest products from the refining tower and is generally a product in which sulfur compounds are concentrated. Due to the high viscosity of asphalt, it is stored at high temperatures (i.e., 149 to 204°C), which is high enough to promote further thermal cracking of sulfur-containing compounds and the formation of additional H2S. The amount of cracking and generation of H2S depends on the structure of the sulfur compounds present in the oil and on the temperatures involved during processing. H2S has a tendency to migrate from the liquid phase to the gas phase above the oil. Certain tank conditions such as increased liquid volume, agitation and high temperatures may make this existing harmful situation worse by changing the partition coefficient of H2S (i.e. the ratio of H2S in the liquid and gas phases of crude oil) in favor of the vapor space. Asphalt has a large amount of H2S partitioning into the gas phase. Typically, 1 ppm of H2S in the liquid phase of asphalt is associated with 400 ppm in the gas phase. Asphalt can therefore contain extremely high levels of H2S in the gas phase, even exceeding 3% (30,000 ppm), which may cause a variety of problems and risks, such as the safety of people involved in its storage, handling and transportation (such as workers in refineries and road operations) and to some extent people living in the area of ​​such installations and construction sites. Exposure to already very low levels of H2S may cause significant health effects, and long-term exposure produces diseases. H2S is particularly harmful because it reduces the sense of smell at concentrations as low as 30 ppm, and at concentrations of 700 ppm death may occur within a few breaths.

[0004] Today, a variety of chemicals are used to prevent hydrogen sulfide emissions from hot asphalt or asphalt mixes, such as caustic, peroxides, formaldehyde, nitrites, and amines.

[0005] WO2005065177 discloses a method for reducing hydrogen sulfide emissions from asphalt, which comprises adding an inorganic or organic metal salt H2S scavenger to the asphalt, wherein the metal in the metal salt H2S scavenger is selected from the group consisting of zinc, cadmium, mercury, copper, silver, nickel, platinum, iron, magnesium and mixtures thereof, in particular selected from the group consisting of zinc oxide, cadmium oxide, copper oxide, magnesium oxide and mixtures thereof.

[0006] US20060116450 discloses the use of an additive to reduce sulfur emissions in crude oil fractions such as bitumen, wherein the additive to reduce emissions comprises a dispersion of a metal oxide, specifically selected from zinc oxide, iron oxide, aluminum oxide and combinations thereof.

[0007] EP0421683 discloses a method for reducing H2S release in bitumen, which comprises introducing an oil-soluble metal carboxylate into hot bitumen, wherein in particular the metal in the carboxylate is zinc, iron, copper or zirconium.

[0008] However, a problem with these compounds is that they are hazardous or difficult to handle.

[0009] It is therefore an object of the present application to provide a solution for preventing the formation of hydrogen sulfide in the production of hot asphalt or bitumen. Summary of the invention

[0010] According to a first aspect of the present application, there is provided a method for preventing hydrogen sulfide emissions in the production of hot asphalt or bitumen at a temperature of 150 to 200° C., wherein the method comprises the following steps:

[0011] - Provide asphalt or bitumen mixtures;

[0012] - heating the mixture to a temperature of 150 to 200° C.;

[0013] - Adding calcium nitrate aqueous solution or calcium nitrate powder while mixing the asphalt or bitumen mixture.

[0014] When the bitumen or asphalt mixture is heated to a temperature of 150 to 200°C to maintain its workability, there is sufficient heat to oxidize the hydrogen sulfide to sulfate by the calcium nitrate added during the mixing process. The hydrogen sulfide formed dissolves in the water present in the asphalt or asphalt mixture. Therefore, the material subsequently treated with calcium nitrate is S 2- . S 2- It is oxidized in an organic matrix, since calcium nitrate is also soluble in organic matrices. The reaction product formed is CaSO4 (gypsum) mixed in hot asphalt or bitumen, thus generating no waste.

[0015] Calcium nitrate powder refers to calcium nitrate particles with a particle size less than 0.5 mm.

[0016] In one embodiment of the method according to the present application, calcium nitrate is added in an amount of 0.5 to 2.0 mg per mg of sulfide present in the bitumen or asphalt mixture. More specifically, calcium nitrate is added in an amount of about 1 mg per mg of sulfide present in the bitumen or asphalt mixture.

[0017] In one embodiment of the method according to the present application, the water content of the calcium nitrate powder is 1 wt % to 33 wt %.

[0018] In one embodiment of the method according to the present application, the concentration of the aqueous calcium nitrate solution is 45% to 55% by weight of calcium nitrate and 45% to 55% by weight of water.

[0019] According to a second aspect of the application, the use of an aqueous calcium nitrate solution or calcium nitrate powder for reducing hydrogen sulfide emissions during mixing of an asphalt or bitumen mixture in the production of hot asphalt or bitumen at a temperature of 150 to 200°C is described.

[0020] In a specific use according to the present application, calcium nitrate is used in an amount of 0.5 to 2.0 mg per mg of sulphide present in the bitumen or asphalt mixture.

[0021] In a more specific use according to the present application, calcium nitrate is used in an amount of about 1 mg per mg of sulphide present in the bitumen or asphalt mixture.

[0022] In one possible use according to the present application, calcium nitrate powder is used having a water content of 1% to 33% by weight.

[0023] In another possible use according to the present application, an aqueous calcium nitrate solution having a concentration of 45% to 55% by weight of calcium nitrate and 45% to 55% by weight of water is used. DETAILED DESCRIPTION

[0024] A method for preventing the emission of hydrogen sulfide (H2S) in the production of hot asphalt or bitumen according to the present application is described herein. More specifically, the main purpose of the method according to the present application is to counteract the emission of H2S from hot asphalt or bitumen mixtures, rather than to eliminate the emission. The method comprises the following steps:

[0025] - prepare or provide asphalt or bituminous mixtures,

[0026] - heating the asphalt or bitumen mixture to a temperature of 150 to 200°C, and

[0027] - Adding calcium nitrate aqueous solution or calcium nitrate powder while mixing the asphalt or bitumen mixture.

[0028] More specifically, calcium nitrate is added in an amount of 0.5 to 2.0 mg and most specifically in an amount of about 1 mg per mg of sulphide present in the asphalt or bitumen mixture.

[0029] In the context of the present invention, the term "asphalt or bitumen mixture" is the residual and heaviest fraction obtained during the refining of crude oil. It contains very long chain hydrocarbon compounds that do not evaporate during the refining process and, in addition, contains mineral impurities and sulfur compounds. It is understood that asphalt or bitumen mixtures do not consist of homogeneous single hydrocarbon compounds.

[0030] Suitable assays and ASTM standard methods for determining the sulfide content of petroleum products are known. For bitumen and asphalt, the so-called and well-known "can test" method is usually used, in which a sample, such as a bitumen or asphalt sample, is placed in a metal container and, after heating the container, the H2S emission of the sample is determined by measuring the H2S content of the head space in the metal container. For example, the measurement of hydrogen sulfide in the gas phase can be carried out according to ASTM D5705-15.

[0031] More specifically, the concentration of hydrogen sulfide in bitumen or asphalt can be determined by the so-called Baker Hughes field can test method (see, e.g., Draper and Stark, 2012, which is incorporated herein by reference, http: / / www.digitalrefining.com / article / 1000336#.WWxveYSGPRY) which allows a more reproducible means of establishing a gas phase in a sample container. In this method, a quart-sized metal can is used which is half-filled with bitumen which is most appropriately sampled in the field, fresh asphalt directly from the unit into the sampling container. The metal can is then sealed and shaken using a specially designed container which enables the sample to be thoroughly stirred while protecting the operator from accidental releases of hot bitumen. The sample is tested using a gas detection tube immediately after storage at the relevant temperature and time period.

[0032] When calcium nitrate powder is used, the water content of the calcium nitrate powder is preferably from 1% to 33% by weight. The particle size of the calcium nitrate powder is not critical.

[0033] When an aqueous calcium nitrate solution is used, the concentration of calcium nitrate therein is preferably 45 to 55% by weight, and the remainder is 45 to 55% by weight of water.

[0034] The application also relates to the use of an aqueous calcium nitrate solution of calcium nitrate powder in the production of hot asphalt or bitumen mixes during mixing of the asphalt or bitumen mixes, wherein the temperature of the hot asphalt or bitumen mix is ​​between 150 and 200° C. to prevent the emission of hydrogen sulfide.

[0035] In particular, calcium nitrate is used in an amount of 0.5 to 2.0 mg and more particularly in an amount of about 1 mg per mg of sulphide present in the asphalt or bitumen mixture.

[0036] When calcium nitrate powder is used, the water content of the calcium nitrate powder is 1 wt % to 33 wt %. When an aqueous calcium nitrate solution is used as an alternative, the concentration of the solution is 45 wt % to 55 wt % calcium nitrate and 45 wt % to 55 wt % water.

[0037] Example

[0038] Using an asphalt emulsion called Elastopaz, aqueous calcium nitrate and sulfide solutions, and Experiments were performed. Elastopaz is a single component asphalt polymer liquid membrane commercialized by the Israeli company Pazkar Ltd. It is an American company Commercial gas detection tubes.

[0039] Add approximately 100 ml of Elastopaz to a 600 ml beaker. Place a watch glass over the beaker and place the beaker on a hot plate with a magnetic stirrer. Heat the Elastopaz to a boiling point of approximately 100°C and add a 1 g / l calcium nitrate aqueous solution and a 1 g / l sodium sulfide nonahydrate aqueous solution to the hot Elastopaz. To ensure proper mixing, add the calcium nitrate aqueous solution and the sodium sulfide nonahydrate aqueous solution in a vortex created by the magnetic stirrer. Use an extension hose to Placed in the head space above the beaker under a watch glass to measure the amount of hydrogen sulfide produced. The amount of hydrogen sulfide was measured three times in succession in each sample. The time between each measurement was 8 to 10 minutes. The samples were kept at boiling point during all measurements.

[0040] A total of 12 samples were analyzed. Four different calcium nitrate additions, 0 ml, 2.5 ml, 5 ml and 10 ml, were equivalent to 0, 25, 50 and 100 mg calcium nitrate / liter Elastopaz, respectively, and three replicates were analyzed for each. 2 - / L Elastopaz 5 ml of sodium sulfide nonahydrate aqueous solution was added to each sample.

[0041]

[0042]

[0043] Table 1

[0044] As the results shown in Table 1, it is shown that adding calcium nitrate to hot asphalt or bitumen during the mixing process prevents the emission of hydrogen sulfide. When 2.5 and 5.0 ml of calcium nitrate aqueous solution were added, hydrogen sulfide was reduced. Adding 10.0 ml of calcium nitrate aqueous solution appeared to be overdosing.

Claims

1. A method for reducing hydrogen sulfide emissions in the production of hot asphalt or bitumen, wherein the method The following steps are involved: - Provide asphalt or bitumen mixtures; - heating the mixture to a temperature of 150 to 200° C.; - Adding an aqueous solution of calcium nitrate or calcium nitrate powder while mixing the asphalt or bitumen mixture.

2. The method according to claim 1, wherein calcium nitrate is added in an amount of 0.5 to 2.0 mg per mg of sulphide present in the asphalt or bitumen mixture.

3. A method according to claim 2, wherein calcium nitrate is added in an amount of about 1 mg per mg of sulphide present in the asphalt or bitumen mixture.

4. The method according to any one of claims 1 to 3, wherein the water content of the calcium nitrate powder is from 1% to 33% by weight.

5. The method according to any one of claims 1 to 3, wherein the concentration of the aqueous calcium nitrate solution is 45% to 55% by weight of calcium nitrate and 45% to 55% by weight of water.

6. Use of an aqueous solution of calcium nitrate or calcium nitrate powder added during mixing of an asphalt or bitumen mixture in the production of hot asphalt or bitumen at a temperature of 150 to 200° C. for preventing the emission of hydrogen sulphide.

7. Use according to claim 6, wherein calcium nitrate is used in an amount of 0.5 to 2.0 mg per mg of sulphide present in the asphalt or bituminous mixture.

8. Use according to claim 7, wherein calcium nitrate is used in an amount of about 1 mg per mg of sulphide present in the asphalt or bitumen mixture.

9. The method according to claim 6, wherein calcium nitrate powder is used having a water content of 1% to 33% by weight.

10. The method according to claim 6, wherein an aqueous calcium nitrate solution having a concentration of 45% to 55% by weight of calcium nitrate and 45% to 55% by weight of water is used.

Citation Information

Patent Citations

  • Process for preparing bitumen compositions with reduced hydrogen sulfide emission

    CN101076558A

  • Method for reducing hydrogen sulfide evolution from asphalt

    CN101945934A

  • Hydrogen sulfide treating agent for oil fields and method for treating hydrogen sulfide