Graphite self-lubricating powder metallurgy material and preparation method thereof

Through the preparation of graphite self-lubricating powder metallurgy materials, the lubrication problem of compressor guide vane bearings under high temperature and high radiation conditions is solved, the wear resistance and self-lubricating properties of the material are achieved, and the normal operation and safety of the gas turbine are ensured.

CN118773473APending Publication Date: 2024-10-15DONGFANG TURBINE CO LTD

Patent Information

Application Number
CN202410807658.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The lubricating material of the existing compressor guide vane bearings does not have sustainability and stability under high temperature and high radiation conditions, resulting in frictional sticking and serious wear, which threatens the safe operation of the gas turbine.

Method used

Graphite self-lubricating powder metallurgy material is used, including copper powder, tin powder, graphite particles, aluminum powder, cobalt powder and molybdenum disulfide. It is prepared through mechanical stirring and hot-pressing sintering processes to form a material with excellent wear resistance and self-lubricating properties. Material used to replace traditional lubricating grease and avoid regular maintenance.

Benefits of technology

It provides efficient self-lubrication, wear resistance and thermal stability, ensuring the normal operation of the gas turbine, avoiding the disadvantages of traditional materials requiring regular maintenance, and improving the mechanical performance and safety of the guide vane bearings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773473A_ABST
    Figure CN118773473A_ABST
Patent Text Reader

Abstract

The invention discloses a graphite self-lubricating powder metallurgy material and a preparation method thereof, and relates to the technical field of powder metallurgy, and the graphite self-lubricating powder metallurgy material comprises the following components in parts by weight: 60-80 parts of copper powder, 6-15 parts of tin powder, 6-18 parts of graphite particles, 1-3 parts of aluminum powder, 2-5 parts of cobalt powder, 1-6 parts of molybdenum disulfide and 0.5-3 parts of a binder. The prepared material has excellent wear resistance, self-lubricating property, dual protection property, thermal stability, good machining property and mechanical property, can be applied to manufacturing of the guide vane bearing of the gas compressor, effectively avoids the adverse factor that regular maintenance is needed in the prior art, and can ensure normal service of the gas turbine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of powder metallurgy, and more specifically to the technical field of graphite self-lubricating powder metallurgy materials and preparation methods thereof. Background Art

[0002] A gas turbine is a rotary power machine that uses a continuously flowing gas as a working fluid and converts heat energy into mechanical work. The compressor, combustion chamber and gas turbine are the three major components of a gas turbine. The flow rate, power and pressure ratio of the compressor directly affect the overall performance of the gas turbine. The guide vanes of the compressor usually need to be adaptively adjusted according to the bleed air pressure, bleed air conversion flow rate, gas turbine operating conditions, etc. to ensure that the compressor works stably under different loads. It is an important component for adjusting the characteristics of the compressor. The guide vane bearing of the compressor is one of the most critical parts to ensure the rotation of the guide vanes to adjust the blade angle. If it has friction, jamming, or severe wear, it will cause the gas turbine unit to "surge" at the least, and even stop or blades fall off at the worst, and even cause serious consequences of power grid accidents. Existing patents disclose the following technologies:

[0003] The patent with publication number CN115839400A and patent name "A copper-based high-temperature and high-irradiation self-lubricating gear and its preparation method" discloses the following content: A copper-based high-temperature and high-irradiation self-lubricating gear and its preparation method. The preparation materials of the copper-based high-temperature and high-irradiation self-lubricating gear include the following components: graphite powder, tungsten disulfide powder, low-melting point soft metal powder and high-melting point soft metal powder, the low-melting point soft metal powder includes one or more of lead powder, bismuth powder and tin powder, and the high-melting point soft metal powder includes copper powder. Copper-based alloys can act as a skeleton at high temperatures and are not damaged when subjected to transmission impact loads and thermal shocks. The graphite powder and tungsten disulfide powder in the self-lubricating gear form a solid lubricating film under friction conditions, and the low-melting point soft metal can melt at high temperatures to form a liquid lubricating film. Through the synergistic effect of low-melting-point soft metal with graphite powder and tungsten disulfide powder, a lubrication effect similar to that of "lubricating grease" is achieved. The copper-based self-lubricating gears of this application have high load-bearing capacity, low shear strength, low friction coefficient, high temperature resistance, radiation resistance, and can achieve long-term lubrication without human intervention.

[0004] The patent with publication number CN110791676A and patent name "A self-lubricating copper-based composite material for guide rails and its preparation method" discloses the following content: A self-lubricating copper-based composite material for guide rails and its preparation method, firstly preparing the base copper alloy in a vacuum electromagnetic induction melting furnace, and then adding nickel-plated graphite, SiC, W, graphene and other micro-nano particles to the base alloy to improve the tensile strength, conductivity, wear resistance and ablation resistance of the copper-based composite material. The matrix alloy raw materials used in the present invention are high-purity Cu, Cr, Zr, Ag, and Nb, and the reinforcing phase particles are nickel-plated graphite with a density of 2.25 g / cm3, SiC with a density of 3.2 g / cm3, W with a density of 8.75 g / cm3, and a flaky graphene thin material with a thickness of 100 nm. The novel high-strength, high-conductivity, ablation-resistant, and highly wear-resistant nickel-plated graphite, SiC, W, and graphene micro-nano particle-reinforced self-lubricating copper-based composite material prepared by the method of the present invention overcomes the problem that the existing copper alloys' ultra-high conductivity and high strength, high wear resistance, and high ablation resistance are not compatible with each other at the same time.

[0005] In addition, the guide vane bearings of the compressor are currently mainly made of ordinary structural steel materials. A lubricating coating is applied to the surface of the bearing material before service. Lubricating grease is continuously added during service and regular maintenance and inspection are performed. The above solution has also had a lot of disadvantages during the long-term operation of the power plant: it is difficult to form effective solid lubrication during service or the solid lubricating film formed does not have the characteristics of continuity and stability, resulting in problems such as difficulty in rotating the guide vanes and severe wear, which directly threatens the safe operation of the unit. Summary of the invention

[0006] The purpose of the present invention is to solve the above technical problems and provide a graphite self-lubricating powder metallurgy material and a preparation method thereof.

[0007] In order to achieve the above-mentioned purpose, the present invention specifically adopts the following technical solutions:

[0008] One aspect of the present invention provides a graphite self-lubricating powder metallurgy material, characterized in that it includes the following components by weight: 60-80 parts of copper powder, 6-15 parts of tin powder, 6-18 parts of graphite particles, 1-3 parts of aluminum powder, 2-5 parts of cobalt powder, 1-6 parts of molybdenum disulfide and 0.5-3 parts of binder.

[0009] In one embodiment, the copper powder is one or more of atomized copper powder, electrolytic copper powder, reduced copper powder, and plasma copper powder.

[0010] In one embodiment, the tin powder has a diameter between 5 and 80 μm.

[0011] In one embodiment, the graphite particles have a size between 500-2000 μm.

[0012] In one embodiment, the aluminum powder has a size between 10 and 30 μm.

[0013] In one embodiment, the cobalt powder has a size between 5 μm and 45 μm.

[0014] In one embodiment, the molybdenum disulfide has a size between 4 μm and 16 μm.

[0015] In one embodiment, the binder is one of stearic acid or ethylene glycol.

[0016] Another aspect of the present invention provides a method for preparing a graphite self-lubricating powder metallurgy material, which is used to prepare the above-mentioned graphite self-lubricating powder metallurgy material.

[0017] The steps include:

[0018] S1. Mix copper powder, tin powder, graphite particles, aluminum powder, cobalt powder and molybdenum disulfide according to a proportion, and add a binder in a percentage of the sum of the mass of the components after mixing;

[0019] S2. Mechanically stir in a powder mixer at a stirring rate of 100 to 900 r / min, and mix the powder thoroughly for 4 to 10 hours;

[0020] S3, after vacuum, hot pressing sintering is carried out in a nitrogen protective atmosphere, heating to 600-650°C under normal pressure, and keeping the temperature for 50-80 minutes;

[0021] S4, then raise the temperature to 900-980°C under a pressure of 3.0-5.0MPa and keep the temperature for 150-240min. After sintering, cool the furnace to 50°C and then take it out of the furnace to obtain a graphite self-lubricating powder metallurgy material.

[0022] The beneficial effects of the present invention are as follows:

[0023] The present invention is reasonably designed and provides a graphite self-lubricating powder metallurgy material and a preparation method thereof. The prepared material has excellent wear resistance, self-lubricating property, dual protection, thermal stability, good machining performance and mechanical properties, and can be applied to the manufacture of guide blade bearings of the above-mentioned compressor, and effectively avoids the disadvantageous factor of the prior art requiring regular maintenance, thereby ensuring the normal service of the gas turbine. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 It is the corresponding metallographic picture in Example 1.

[0026] Figure 2 It is the metallographic picture corresponding to the comparative example 1 of the prior art. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.

[0028] Therefore, the following detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] The present embodiment provides a graphite self-lubricating powder metallurgy material, which includes the following components by weight: 60 parts of copper powder, 15 parts of tin powder, 9 parts of graphite particles with a particle size of 800-2000 μm, 3 parts of aluminum powder, 5 parts of cobalt powder, 6 parts of molybdenum disulfide, and 2 parts of stearic acid.

[0031] The preparation method is as follows:

[0032] S1, mixing copper powder, tin powder, graphite particles, aluminum powder, cobalt powder and molybdenum disulfide according to a proportion;

[0033] S2, after adding the binder in a percentage of the sum of the mass of the components after mixing, mechanically stir in a powder mixer at a stirring rate of 100r / min, and mix the powder thoroughly for 10h;

[0034] S3, after vacuum, hot pressing sintering is carried out in a nitrogen protective atmosphere, heating to 650°C at normal pressure and keeping the temperature for 50 minutes;

[0035] S4, then raise the temperature to 900°C under a pressure of 5.0MPa and keep it at this temperature for 240min. After sintering, cool it to 50°C and then take it out of the furnace.

[0036] Example 2

[0037] The present embodiment provides a graphite self-lubricating powder metallurgy material, which includes the following components by weight: 72 parts of copper powder, 8 parts of tin powder, 12 parts of graphite particles with a particle size of 500-2000 μm, 2 parts of aluminum powder, 2.5 parts of cobalt powder, 2.5 parts of molybdenum disulfide, and 1 part of ethylene glycol.

[0038] The preparation method is as follows:

[0039] S1, mixing copper powder, tin powder, graphite particles, aluminum powder, cobalt powder and molybdenum disulfide according to a proportion;

[0040] S2, after adding the binder in a percentage of the sum of the mass of the components after mixing, mechanically stir in a powder mixer at a stirring rate of 900r / min, and mix the powder thoroughly for 4h;

[0041] S3, after vacuum, hot pressing sintering is carried out in a nitrogen protective atmosphere, heating to 600°C under normal pressure and keeping the temperature for 80 minutes;

[0042] S4, then raise the temperature to 980℃ under the pressure of 2.2MPa and keep it at this temperature for 150min. After sintering, cool it to 50℃ and then take it out of the furnace.

[0043] Example 3

[0044] The present embodiment provides a graphite self-lubricating powder metallurgy material, which includes the following components by weight: 72 parts of copper powder, 6 parts of tin powder, 157 parts of graphite particles, 1 part of aluminum powder, 2 parts of cobalt powder, 1.5 parts of molybdenum disulfide, and 1.8 parts of ethylene glycol.

[0045] The preparation method is as follows:

[0046] S1. Mix copper powder, tin powder, graphite particles with a particle size of 1000-1800 μm, aluminum powder, cobalt powder and molybdenum disulfide according to a proportion;

[0047] S2, after adding the binder in a percentage of the sum of the mass of the components after mixing, mechanically stir in a powder mixer at a stirring rate of 500r / min, and mix thoroughly for 7h;

[0048] S3, after vacuum, hot pressing sintering is carried out in a nitrogen protective atmosphere, heating to 630°C at normal pressure and keeping the temperature for 65 minutes;

[0049] S4, then raise the temperature to 960°C at a pressure of 4.0 MPa and keep it at this temperature for 200 minutes. After sintering, cool it to 50°C and then take it out of the furnace.

[0050] The corresponding material properties of the above embodiments are shown in Table 1.

[0051] Table 1 Corresponding test data of the embodiment

[0052] Yield strength / MPa Compressive strength / MPa Average friction coefficient Wear rate / mm3 / (Nm) Example 1 120 387 0.11 2.4×10-5 Example 2 125 392 0.15 2.6×10-5 Example 3 132 406 0.18 3.2×10-5 Comparative Example 102 326 0.29 3.7×10-4

[0053] Comparative Example 1:

[0054] Attached Figure 1 Attached is the corresponding metallographic picture in Example 1. Figure 2 It is the metallographic picture corresponding to the comparative example 1 of the prior art.

[0055] Comparison of the corresponding metallographic images in Example 1 and the comparative example shows that the metal matrix in Comparative Example 1 is continuous and dense, and the added large-particle graphite is dimensionally stable after final molding. The graphite particles in Comparative Example 1 of the prior art are relatively small and dispersed in the metal matrix. The data in Table 1 of the corresponding test data of the embodiment show that the yield strength and compressive strength of Example 1 are significantly higher than those of Comparative Example 1. This is because the dispersed distribution of the low-strength lubricating material in Comparative Example 1 reduces the continuity of the matrix material, thereby reducing the overall strength of the material; at the same time, the average friction coefficient and wear rate of Example 1 are also better than those of the comparative example. This is because the large-particle graphite with stable size after final molding in Example 1 can continuously provide lubricating medium for the relatively high-strength matrix during the friction process, maintaining a low average friction coefficient and wear rate. Therefore, the present invention has better performance than the prior art.

Claims

1. A graphite self-lubricating powder metallurgy material, characterized in that: The invention comprises the following components by weight: 60-80 parts of copper powder, 6-15 parts of tin powder, 6-18 parts of graphite particles, 1-3 parts of aluminum powder, 2-5 parts of cobalt powder, 1-6 parts of molybdenum disulfide and 0.5-3 parts of binder.

2. The graphite self-lubricating powder metallurgy material according to claim 1, characterized in that: The copper powder is one or more of atomized copper powder, electrolytic copper powder, reduced copper powder and plasma copper powder.

3. The graphite self-lubricating powder metallurgy material according to claim 1, characterized in that: The tin powder has a diameter between 5 and 80 μm.

4. The graphite self-lubricating powder metallurgy material according to claim 1, characterized in that: The graphite particles have a size between 500 and 2000 μm.

5. The graphite self-lubricating powder metallurgy material according to claim 1, characterized in that: The aluminum powder has a size between 10 and 30 μm.

6. The graphite self-lubricating powder metallurgy material according to claim 1, characterized in that: The cobalt powder has a size between 5 and 45 μm.

7. The graphite self-lubricating powder metallurgy material according to claim 1, characterized in that: The molybdenum disulfide has a size between 4 and 16 μm.

8. The graphite self-lubricating powder metallurgy material according to claim 1, characterized in that: The binder is one of stearic acid or ethylene glycol.

9. A method for preparing a graphite self-lubricating powder metallurgy material, characterized in that: Used to prepare a graphite self-lubricating powder metallurgy material as claimed in any one of claims 1 to 8.

10. The method for preparing a graphite self-lubricating powder metallurgy material according to claim 9, characterized in that: The steps include: S1. Mix copper powder, tin powder, graphite particles, aluminum powder, cobalt powder and molybdenum disulfide according to a proportion, and add a binder in a percentage of the sum of the mass of the components after mixing; S2. Mechanically stir in a powder mixer at a stirring rate of 100 to 900 r / min, and mix the powder thoroughly for 4 to 10 hours; S3, after vacuum, hot pressing sintering is carried out in a nitrogen protective atmosphere, heating to 600-650°C under normal pressure, and keeping the temperature for 50-80 minutes; S4, then raise the temperature to 900-980°C under a pressure of 3.0-5.0MPa and keep the temperature for 150-240min. After sintering, cool the furnace to 50°C and then take it out of the furnace to obtain a graphite self-lubricating powder metallurgy material.

Citation Information

Patent Citations

  • Self-lubricating copper-based composite material for guide rails and preparation method thereof

    CN110791676A

  • Copper-based high-temperature high-irradiation self-lubricating gear, preparation method and transmission device

    CN115839400A

Cited By

  • Powder metallurgy friction material and preparation method thereof, brake pad and hydro-generator

    CN120961911A