Cu-Al-Ni phase change heat dissipation material and preparation method thereof

Through the preparation of Cu-Al-Ni phase change heat dissipation materials, the low thermal conductivity and packaging problems of traditional solid-solid phase change materials are solved, and efficient and environmentally friendly heat dissipation management of electronic devices is achieved. It has ultra-high thermal conductivity and stability and is suitable for for high power electronic devices.

CN118773476APending Publication Date: 2024-10-15HARBIN UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410809466.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively solve the heat dissipation problems of high operating temperature, high heat flux density and high-power electronic devices, especially traditional solid-solid phase change materials with low thermal conductivity, complex composite process and high cost, and need to be packaged to prevent liquid phase leakage problem.

Method used

Cu-Al-Ni phase change heat dissipation material is used, which is composed of 83.4% ~ 83.7% Cu, 12.9% ~ 13.2% Al and 3.4% Ni. It is prepared through arc melting and argon protection processes to form a highly thermally conductive shape memory alloy. The ingot is cast and quenched at high temperature to obtain a Cu-Al-Ni phase change heat dissipation material that does not require packaging.

Benefits of technology

It has realized a Cu-Al-Ni phase change heat dissipation material that does not require packaging, is environmentally friendly, has ultra-high thermal conductivity and high energy storage density. It can quickly absorb the heat generated by electronic devices and has excellent thermal cycle stability and comprehensive heat dissipation indicators. FOM The value is as high as 5856×106J2K-1s-1m-4.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773476A_ABST
    Figure CN118773476A_ABST
Patent Text Reader

Abstract

The invention discloses a Cu-Al-Ni phase change heat dissipation material and a preparation method thereof, belongs to the field of phase change heat dissipation materials, and particularly relates to the Cu-Al-Ni phase change heat dissipation material and the preparation method thereof. The invention aims to solve the problem of heat management of electronic devices with high working temperature, high heat flux and high power. The material is composed of, by mass, 83.4%-83.7% of Cu, 12.9%-13.2% of Al and 3.4% of Ni. The method comprises arc melting; and the smelted cast ingot is subjected to solution treatment and then subjected to water quenching, and the alloy with uniform components is obtained. The obtained material has ultrahigh thermal conductivity which is up to 98-101 Wm <-1 > K <-1 > in a high-temperature austenite state. In addition, the FOM value of the alloy is 5856 * 10 < 6 > J2K <-1 > s <-1 > m <-4 > and is 9 times that of a commercial phase change material. After thermal training, the alloy is excellent in thermal cycling stability and can be applied to application scenes such as thermal management of high-power electronic devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of phase-change heat dissipation materials, and in particular relates to a Cu-Al-Ni phase-change heat dissipation material and a preparation method thereof. Background Art

[0002] With the development of the emerging high-power electronic industry, electronic devices are developing towards miniaturization, integration and high power. These electronic devices will generate a lot of heat when working. If the heat cannot be effectively dissipated, it will reduce work efficiency, shorten service life and even cause safety hazards. Therefore, timely and efficient heat dissipation is extremely important for electronic devices. Using phase change materials to absorb heat is a new heat dissipation method. Its advantage is that its own temperature remains basically unchanged during phase change and it can absorb the heat of electronic devices to prevent overheating and failure. Currently, commonly used phase change heat dissipation materials are divided into solid-liquid phase change materials and solid-solid phase change materials. Solid-liquid phase change materials have attracted widespread attention due to their low cost and latent heat, but there is a serious problem that the liquid phase is easy to leak when the solid and liquid melt. Special devices are required for packaging, which will increase the weight of the heat storage device and sacrifice the heat storage capacity. Solid-solid phase change materials have the advantages of no packaging, environmental protection, small volume change, and high energy storage density. They have been widely studied in recent years, but traditional solid-solid phase change materials have limitations, mainly low thermal conductivity, and often need to be compounded with other high thermal conductivity materials. The compounding process is complex, costly, and difficult to prepare. Many current electronic devices have high operating temperatures, high heat flux density, and high power density. Their development is hindered by integration and performance issues. Therefore, there is an urgent need to develop solid-solid phase change materials that do not require compounding and have high thermal conductivity to solve the heat dissipation problem of high-power electronic devices. Summary of the invention

[0003] The present invention aims to solve the problem of heat management of electronic devices with high operating temperature, high heat flux density and high power, and provides a Cu-Al-Ni phase change heat dissipation material and a preparation method thereof.

[0004] The invention provides a Cu-Al-Ni phase-change heat dissipation material, which consists of 83.4% to 83.7% Cu, 12.9% to 13.2% Al and 3.4% Ni in terms of mass percentage.

[0005] The preparation method of the above Cu-Al-Ni phase change heat dissipation material is completed according to the following steps:

[0006] 1. According to the mass percentage of 83.4% to 83.7% Cu, 12.9% to 13.2% Al and 3.4% Ni, Cu metal, Al metal and Ni metal are weighed as raw materials respectively, and the surface oxide scale of the metal elements is removed;

[0007] 2. Place Al metal, Cu metal and Ni metal in the arc melting furnace from bottom to top, evacuate to below 10Pa and then fill with 0.07Mpa argon gas for gas washing, repeat the gas washing for more than 4 times; evacuate to 5×10 -3 Pa, and then fill with 0.5Mpa argon as protective gas; adjust the melting current to 550A in the argon atmosphere to melt the Cu-Al-Ni alloy by arc, and repeat the melting for more than 6 times, ensure the uniform composition of the alloy ingot by electromagnetic stirring, slowly close the arc and wait for cooling, and mechanically polish to remove surface impurities to obtain a Cu-Al-Ni shape memory alloy ingot;

[0008] 3. The Cu-Al-Ni shape memory alloy ingot is sealed in a quartz tube filled with argon, placed in a box-type resistance furnace, kept warm for 25 to 35 minutes at a temperature of 850 to 950°C, and finally quickly quenched in water to obtain a Cu-Al-Ni phase change heat dissipation material.

[0009] Beneficial effects of the present invention:

[0010] Compared with traditional solid-liquid phase change materials, the Cu-Al-Ni phase change heat dissipation material with excellent comprehensive performance described in the present invention has the advantages of no need for packaging, environmental protection, high energy storage density, etc.

[0011] The phase change heat dissipation material prepared by the present invention has an ultra-high thermal conductivity (101Wm -1 K -1 ), can absorb the heat generated by electronic devices more quickly and prevent them from overheating and failure.

[0012] The alloy prepared by the invention has excellent thermal cycle stability and can be used repeatedly in the operation of electronic devices.

[0013] The phase change heat dissipation material also has an ultra-high comprehensive heat dissipation index FOM (5856×10 6 J 2 K -1 s -1 m -4 ), which is 9 times that of commercial phase change materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 Cu 83.4 Al 13.2 Ni 3.4 DSC curve of phase change heat dissipation material;

[0015] Figure 2 Cu 83.5 Al 13.1 Ni 3.4 DSC curve of phase change heat dissipation material;

[0016] Figure 3 Cu 83.6 Al 13.0 Ni 3.4 DSC curve of phase change heat dissipation material;

[0017] Figure 4 Cu 83.7 Al 12.9 Ni 3.4 DSC curve of phase change heat dissipation material;

[0018] Figure 5 Cu 83.4 Al 13.2 Ni 3.4 DSC curve of the phase change heat dissipation material for 30 thermal cycles;

[0019] Figure 6 Cu 83.4 Al 13.2 Ni 3.4 A graph showing the change in specific heat capacity of phase change heat dissipation materials with temperature;

[0020] Figure 7 Cu 83.4 Al 13.2 Ni 3.4 A graph showing the thermal conductivity of a phase change heat dissipation material changing with temperature;

[0021] Figure 8 A comparison chart of FOM values ​​of different phase change materials. DETAILED DESCRIPTION

[0022] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.

[0023] Specific implementation method 1: In this implementation method, a Cu-Al-Ni phase change heat dissipation material is composed of 83.4% to 83.7% Cu, 12.9% to 13.2% Al and 3.4% Ni by mass percentage.

[0024] Specific implementation method 2: In this implementation method, a preparation method of a Cu-Al-Ni phase change heat dissipation material is completed by the following steps:

[0025] 1. According to the mass percentage of 83.4% to 83.7% Cu, 12.9% to 13.2% Al and 3.4% Ni, Cu metal, Al metal and Ni metal are weighed as raw materials respectively, and the surface oxide scale of the metal elements is removed;

[0026] 2. Place Al metal, Cu metal and Ni metal in the arc melting furnace from bottom to top, evacuate to below 10Pa and then fill with 0.07Mpa argon gas for gas washing, repeat the gas washing for more than 4 times; evacuate to 5×10 -3 Pa, and then fill with 0.5Mpa argon as protective gas; adjust the melting current to 550A in the argon atmosphere to melt the Cu-Al-Ni alloy by arc, and repeat the melting for more than 6 times, ensure the uniform composition of the alloy ingot by electromagnetic stirring, slowly close the arc and wait for cooling, and mechanically polish to remove surface impurities to obtain a Cu-Al-Ni shape memory alloy ingot;

[0027] 3. The Cu-Al-Ni shape memory alloy ingot is sealed in a quartz tube filled with argon, placed in a box-type resistance furnace, kept warm for 25 to 35 minutes at a temperature of 850 to 950°C, and finally quickly quenched in water to obtain a Cu-Al-Ni phase change heat dissipation material.

[0028] The Cu-Al-Ni phase change heat dissipation material prepared in this embodiment is transferred to the Cu-Al-Ni phase change heat dissipation material through the heat flow generated by the high-power electronic device, causing it to undergo a reverse martensitic phase transformation, absorbing the heat generated by the device, thereby achieving a temperature control effect.

[0029] Specific embodiment 3: This embodiment differs from specific embodiment 2 in that in step 1, 83.6% Cu, 13.0% Al and 3.4% Ni by mass percentage are respectively weighed as raw materials, and the rest is the same as specific embodiment 2.

[0030] Specific embodiment 4: This embodiment differs from specific embodiment 2 in that in step 1, 83.5% Cu, 13.1% Al and 3.4% Ni by mass percentage are respectively weighed as raw materials, and the rest is the same as specific embodiment 2.

[0031] Specific embodiment 5: This embodiment differs from specific embodiment 2 in that the heating and cooling rate of the Cu-Al-Ni phase change heat dissipation material obtained in step 3 is 40K / min, and the adjustable phase change temperature range is 100-200° C. The rest is the same as specific embodiment 2.

[0032] Specific implementation example 6: This implementation example is different from specific implementation example 2 in that when Cu-Al-Ni phase change heat dissipation material is used as a practical material that can be recycled, the phase change temperature and heat storage capacity remain unchanged after multiple thermal cycle stability tests. Other aspects are the same as specific implementation example 2.

[0033] Specific embodiment 7: This embodiment is different from the specific embodiment 2 in that the thermal conductivity of the Cu-Al-Ni phase change heat dissipation material obtained in step 3 is 101Wm -1 K -1 The rest is the same as the second specific implementation method.

[0034] Can absorb the heat generated by electronic devices more quickly and effectively.

[0035] Specific embodiment 8: This embodiment is different from the specific embodiment 2 in that the heat dissipation comprehensive performance index FOM value of the Cu-Al-Ni phase change heat dissipation material obtained in step 3 is as high as 5856×10 6 J 2 K -1 s -1 m -4 The rest is the same as the second specific implementation method.

[0036] Specific embodiment 9: This embodiment differs from specific embodiment 2 in that: in step 3, the temperature is kept at 900° C. for 30 minutes, and then the material is rapidly quenched in water. The rest is the same as specific embodiment 2.

[0037] The following examples are used to verify the beneficial effects of the present invention:

[0038] Embodiment 1: The preparation method of Cu-Al-Ni phase change heat dissipation material is completed according to the following steps:

[0039] 1. According to the mass percentage of 83.4% Cu, 13.2% Al and 3.4% Ni, weigh Cu metal, Al metal and Ni metal as raw materials respectively, and remove the oxide scale on the surface of the metal elements; weigh the ingredients using a balance with an accuracy of 0.0001g, and ensure that the error between the actual mass of all elements in the weighing and the calculated value is within ±0.0002g;

[0040] 2. Place Al metal, Cu metal and Ni metal in the arc melting furnace from bottom to top, evacuate to below 10Pa and then fill with 0.07Mpa argon gas for gas washing, repeat the gas washing for more than 4 times; evacuate to 5×10 -3 Pa, and then fill with 0.5Mpa argon as protective gas; adjust the melting current to 550A in the argon atmosphere to melt the Cu-Al-Ni alloy by arc, and repeat the melting for more than 6 times, ensure the uniform composition of the alloy ingot by electromagnetic stirring, slowly close the arc and wait for cooling, and mechanically polish to remove surface impurities to obtain a Cu-Al-Ni shape memory alloy ingot;

[0041] 3. The Cu-Al-Ni shape memory alloy ingot was sealed in a quartz tube filled with argon, placed in a box-type resistance furnace, kept warm for 30 minutes at 900°C, and finally quickly quenched in water to obtain a Cu-Al-Ni phase change heat dissipation material; the Cu-Al-Ni phase change heat dissipation material was cut into Φ3×1mm by wire cutting. -3 of small discs.

[0042] Embodiment 2: This embodiment differs from Embodiment 1 in that: in step 1, 83.5% Cu, 13.1% Al and 3.4% Ni are weighed as raw materials, respectively. The rest is the same as Embodiment 1.

[0043] Embodiment 3: This embodiment differs from Embodiment 1 in that: in step 1, 83.6% Cu, 13.1% Al and 3.4% Ni are weighed as raw materials, respectively. The rest is the same as Embodiment 1.

[0044] Embodiment 4: This embodiment differs from Embodiment 1 in that: in step 1, 83.7% Cu, 12.9% Al and 3.4% Ni are weighed as raw materials, respectively. The rest is the same as Embodiment 1.

[0045] The DSC curves of the alloys with different compositions in Examples 1 to 4 are as follows: Figures 1 to 4 As shown, under the condition of heating / cooling rate of 40K / min, its performance parameters are:

[0046] (1)Cu 83.4 Al 13.2 Ni 3.4 : Phase transition temperature A f =142.1℃, latent heat of phase change ΔH=8.47J / g, and its DSC curve is as follows Figure 1 shown.

[0047] (2)Cu 83.5 Al 13.1 Ni 3.4 : Phase transition temperature A f =160.1℃, latent heat of phase change ΔH=8.52J / g, and its DSC curve is as follows Figure 2 shown.

[0048] (3)Cu 83.6 Al 13.0 Ni 3.4 : Phase transition temperature A f =179.4℃, latent heat of phase change ΔH=8.82J / g, and its DSC curve is as follows Figure 3shown.

[0049] (4)Cu 83.7 Al 12.9 Ni 3.4 : Phase transition temperature A f =193.4℃, latent heat of phase change ΔH=9.13J / g, and its DSC curve is as follows Figure 4 shown.

[0050] It should be noted that the phase transition temperature of the alloy is increased by reducing the Al content and increasing the Cu content.

[0051] Figure 5 Cu 83.4 Al 13.2 Ni 3.4 DSC curve of the phase change heat dissipation material after 30 thermal cycle stability after multiple training. Under the condition of heating / cooling rate of 40K / min, after 30 martensitic phase transformations, the phase transformation temperature (M s , M f , A s , A f ) did not shift, and the endothermic and exothermic peak areas did not change (the latent heat of phase change remained unchanged). 83.4 Al 13.2 Ni 3.4 Phase change heat dissipation materials have excellent thermal cycle stability and can be recycled in the heat dissipation of electronic devices.

[0052] Figure 6 Cu 83.4 Al 13.2 Ni 3.4 The curve of the specific heat capacity of phase change heat dissipation material changing with temperature. In the low-temperature martensitic state, the specific heat capacity remains unchanged as the temperature rises. Then, during the transformation process, a large peak appears. This is the result of the alloy absorbing a large amount of latent heat during the reverse martensitic phase transformation, which cannot represent the true specific heat capacity value. After the phase transformation, the specific heat capacity in the austenitic state returns to the level before the transformation. This shows that Cu 83.4 Al 13.2 Ni 3.4 The specific heat capacity of the phase change heat dissipation material in the low-temperature martensite state and the high-temperature austenite state does not change with the transformation of the alloy phase.

[0053] Figure 7 Cu 83.4 Al 13.2 Ni 3.4 The graph of the thermal conductivity of phase change heat dissipation material changing with temperature. As can be seen from the figure, Cu 83.4 Al 13.2 Ni 3.4The thermal conductivity of phase change heat dissipation materials gradually increases with the increase of temperature. After heating, the thermal conductivity increases from 70Wm at 80℃ to -1 K -1 Increase to 81Wm at 115℃ -1 K -1 The alloy then undergoes a reverse martensitic phase transformation, and the thermal conductivity rises sharply. This is due to the abnormal specific heat capacity and increased electronic thermal conductivity caused by the change in carrier mobility during the phase transformation. After the phase transformation, the thermal conductivity in the austenite state is as high as 101Wm -1 K -1 The thermal conductivity of this phase change heat dissipation material is much higher than that of traditional solid-liquid and solid-solid phase change materials (usually 0.21~1.0Wm -1 K -1 ) This fully illustrates that Cu 83.4 Al 13.2 Ni 3.4 Phase change heat dissipation materials have ultra-high thermal conductivity and can absorb the heat generated by electronic devices more quickly.

[0054] Figure 8 The figure is a comparison chart of the comprehensive heat dissipation index FOM of different phase change materials. FOM is defined as the ability of phase change materials to quickly absorb / release a large amount of latent heat in a small volume. FOM = k·ρ·L, where ρ·L represents the volume heat storage capacity of PCM, and k represents the heat flux rate from the heat source to the PCM. Therefore, FOM is an important and reliable indicator for evaluating the thermal management performance of phase change materials. We calculated and compared the FOM values ​​of different types of phase change materials. As can be seen from the figure, within the operating temperature range of high-power electronic devices (100-200°C), the FOM values ​​of traditional solid-liquid and solid-solid phase change materials are less than 2366×10 6 J 2 K -1 s - 1 m -4 . And our Cu 83.4 Al 13.2 Ni 3.4 The FOM value of the alloy is as high as 5856×10 6 J 2 K -1 s -1 m -4 , which is the highest value in this temperature range. This is because the Cu-Al-Ni phase change heat dissipation material has ultra-high thermal conductivity and density compared to other phase change materials. The ultra-high FOM value of the Cu-Al-Ni phase change heat dissipation material indicates that it has great potential in the thermal management of high-power electronic devices.

[0055] From the above description, it can be seen that the Cu-Al-Ni phase change heat dissipation material with ultra-high comprehensive performance proposed by the present invention absorbs the heat generated by electronic devices by virtue of its reversible martensitic phase transformation characteristics, and due to its ultra-high thermal conductivity (101Wm -1 K -1 ), huge comprehensive heat dissipation index FOM (5856×10 6 J 2 K -1 s -1 m -4 ) and excellent stability, which makes it have broad application prospects in the field of thermal management of high-power electronic devices.

Claims

1. A Cu-Al-Ni phase change heat dissipation material, characterized in that The composition of the Cu-Al-Ni phase-change heat dissipation material is composed of 83.4% to 83.7% Cu, 12.9% to 13.2% Al and 3.4% Ni in terms of mass percentage.

2. The method for preparing a Cu-Al-Ni phase change heat dissipation material according to claim 1, characterized in that The preparation method of Cu-Al-Ni phase change heat dissipation material is completed according to the following steps:

1. According to the mass percentage of 83.4% to 83.7% Cu, 12.9% to 13.2% Al and 3.4% Ni, Cu metal, Al metal and Ni metal are weighed as raw materials respectively, and the surface oxide scale of the metal elements is removed; 2. Place Al metal, Cu metal and Ni metal in the arc melting furnace from bottom to top, evacuate to below 10Pa and then fill with 0.07Mpa argon gas for gas washing, repeat the gas washing for more than 4 times; evacuate to 5×10 - 3 Pa, and then fill with 0.5Mpa argon as protective gas; adjust the melting current to 550A in the argon atmosphere to melt the Cu-Al-Ni alloy by arc, and repeat the melting for more than 6 times, ensure the uniform composition of the alloy ingot by electromagnetic stirring, slowly close the arc and wait for cooling, and mechanically polish to remove surface impurities to obtain a Cu-Al-Ni shape memory alloy ingot; 3. The Cu-Al-Ni shape memory alloy ingot is sealed in a quartz tube filled with argon, placed in a box-type resistance furnace, kept warm for 25 to 35 minutes at a temperature of 850 to 950°C, and finally quickly quenched in water to obtain a Cu-Al-Ni phase change heat dissipation material.

3. The method for preparing a Cu-Al-Ni phase change heat dissipation material according to claim 2, characterized in that In step 1, Cu metal element, Al metal element and Ni metal element are weighed as raw materials according to the mass percentage of 83.6% Cu, 13.0% Al and 3.4% Ni respectively.

4. The method for preparing a Cu-Al-Ni phase change heat dissipation material according to claim 2, characterized in that In step 1, Cu metal element, Al metal element and Ni metal element are weighed as raw materials according to the mass percentage of 83.5% Cu, 13.1% Al and 3.4% Ni respectively.

5. The method for preparing a Cu-Al-Ni phase change heat dissipation material according to claim 2, characterized in that The heating / cooling rate of the Cu-Al-Ni phase change heat dissipation material obtained in step 3 is 40K / min, and the adjustable phase change temperature range is 100-200°C.

6. The method for preparing a Cu-Al-Ni phase change heat dissipation material according to claim 2, characterized in that When Cu-Al-Ni phase change heat dissipation material is used as a practical recyclable material, the phase change temperature and heat storage capacity remain unchanged after multiple thermal cycle stability tests.

7. The method for preparing a Cu-Al-Ni phase change heat dissipation material according to claim 2, characterized in that The thermal conductivity of the Cu-Al-Ni phase change heat dissipation material obtained in step 3 is 101Wm -1 K -1 .

8. The method for preparing a Cu-Al-Ni phase change heat dissipation material according to claim 2, characterized in that The heat dissipation comprehensive performance index FOM value of the Cu-Al-Ni phase change heat dissipation material obtained in step 3 is as high as 5856×10 6 J 2 K -1 s -1 m -4 .

9. The method for preparing a Cu-Al-Ni phase change heat dissipation material according to claim 2, characterized in that In step 3, the temperature is kept at 900° C. for 30 minutes, and finally, it is quickly quenched in water.

Citation Information

Patent Citations

  • Ultra-elastic memory heat treatment method for copper-base shape memory alloy obtained by thermal continuous casting

    CN101148745A

  • Optimization method of CuAlNi memory alloy 4D printing process

    CN114535600A

  • Manufacturing method of Cu-Ni-Al series sintered alloy

    CN114729420A

  • Polycrystal Co-V-Ga-Ti memory alloy with large elastic heat effect and preparation method thereof

    CN117535560A

  • SOLID STATE MARTENSITIC TRANSFORMATION PHASE CHANGE MATERIAL CO'qMPONENTS FOR THERMAL ENERGY STORAGE AND TRANSIENT HEAT TRANSFER SYSTEMS

    US20200407615A1