Ti-Zr-V series light refractory multi-principal-element eutectic alloy as well as preparation method and application of Ti-Zr-V series light refractory multi-principal-element eutectic alloy
By designing a Ti-Zr-V series lightweight refractory multi-principal eutectic alloy and combining the BCC1 and BCC2 phase structures, the problems of high density and poor casting formability of refractory high-entropy alloys were solved, achieving low density and excellent casting performance. , suitable for aerospace parts applications.
Patent Information
- Application Number
- CN202410864917.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-01
AI Technical Summary
The high density and poor casting formability of refractory high-entropy alloys limit their application in the field of aviation parts. In particular, there are few studies on eutectic refractory high-entropy alloys composed of BCC1+BCC2 phase structures.
A Ti-Zr-V series lightweight refractory multi-principal eutectic alloy was designed. By regulating the proportions of Ti, Zr, and V, and combining the BCC1 and BCC2 phase structures, it achieved low density and good casting fluidity, using vacuum The alloy is prepared using an arc melting process.
It achieves low density (5.5-6.1g/cm3) and excellent casting performance, improves the corrosion resistance, wear resistance and high temperature stability of the alloy, and is suitable for casting of complex precision components and aerospace parts.
Smart Images

Figure CN118773479A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technology of high-entropy alloys, and particularly to a Ti-Zr-V series lightweight refractory multi-principal element eutectic alloy, a preparation method thereof, and uses thereof. Background Art
[0002] Aero-engines are national key equipment and an important manifestation of a country's scientific and technological strength. The service environment of aero-components is extremely harsh, posing higher requirements for the currently under-research metallic materials. Since 2010, refractory high-entropy alloys have received extensive attention due to their excellent mechanical properties and high-temperature stability, and are expected to become candidate materials for the next-generation aerospace components. Refractory high-entropy alloys generally consist mainly of elements with melting points above 1500 °C, which greatly limits the casting conditions of refractory high-entropy alloys. Since the concept of eutectic high-entropy alloys was proposed by Professor Lu Yiping of Dalian University of Technology in 2014, the eutectic high-entropy alloy system has developed rapidly. For the currently reported eutectic high-entropy alloys, they mainly consist of FCC + B2 phase structures or FCC + BCC phase structures, while less research has been carried out on eutectic refractory high-entropy alloys composed of BCC1 + BCC2 phase structures. In addition, high density is another huge challenge currently faced by refractory high-entropy alloys. Summary of the Invention
[0003] An object of the present invention is to propose a Ti-Zr-V series lightweight refractory multi-principal element eutectic alloy in view of the problems of high density and poor castability of the above-mentioned refractory high-entropy alloys. This alloy combines the design concepts of refractory high-entropy alloys and eutectic alloys, combines the BCC1 solid solution enriched with Ti and V elements and the BCC2 solid solution enriched with Ti and Zr elements, and exhibits a lower density and excellent casting fluidity. The lightweight refractory multi-principal element eutectic alloy provided by the present invention has both excellent castability and a lower density, and is expected to realize the engineering application of multi-principal element refractory alloys.
[0004] To achieve the above object, the technical solution adopted by the present invention is: a Ti-Zr-V series lightweight refractory multi-principal element eutectic alloy, whose general formula is Ti a Zr b V c , where 14% < a < 25%, 48% < b < 55%, 26% < c < 31%, and a + b + c = 100, and a, b, and c respectively correspond to the molar percentages of the elements.
[0005] Further, the general formula Ti a Zr b V c satisfies: 14.5% < a < 25%, 48.5% < b < 55%, 27% < c < 30.5%.
[0006] Furthermore, the Ti-Zr-V series lightweight refractory multi-principal eutectic alloy has a BCC1 and BCC2 dual-phase structure.
[0007] Furthermore, the Ti-Zr-V series lightweight refractory multi-principal eutectic alloy has a density of 6.1 g / cm 3 and below.
[0008] Furthermore, the Ti-Zr-V series lightweight refractory multi-principal eutectic alloy has a density of 5.5-6.1 g / cm 3 .
[0009] Another object of the present invention is to disclose a method for preparing a Ti-Zr-V series lightweight refractory multi-principal eutectic alloy, comprising the following steps:
[0010] Step 1, grinding: grinding the surface of the metal element raw materials Ti, Zr, V to remove the oxide scale and impurities on the surface;
[0011] Step 2, cleaning: put the polished metal single substance raw materials Ti, Zr, and V into separate containers, pour ethanol, use an ultrasonic cleaner to clean them, and after fully drying, put them into sealed bags for standby use;
[0012] Step 3, ingredients: weigh each component according to the general formula;
[0013] Step 4, smelting: put the metal single substance raw materials Ti, Zr, and V into the copper crucible of the vacuum arc melting furnace, and place the Ti ingot prepared in advance in another copper crucible; close the furnace door, evacuate, and fill with high-purity argon; after high-frequency arc initiation, first melt the Ti ingot, and then melt the metal single substance raw materials in the copper crucible, turn off the current after they are completely melted, and then cool the furnace; repeat this step for the smelted alloy raw materials; after the smelting is completed, open the furnace door and take out the sample after the alloy ingot is completely cooled, and obtain a Ti-Zr-V series lightweight refractory multi-principal eutectic alloy.
[0014] Furthermore, when selecting single-element raw materials, the purity of the metal single-element raw materials Ti, Zr, and V is greater than or equal to 99.95wt.%.
[0015] Furthermore, during the ultrasonic cleaning in step 2, the metal element raw material is cleaned at least 3 to 4 times, and each cleaning time is at least 6 to 10 minutes.
[0016] Furthermore, when the single substance raw material is weighed, the weighing error is ±0.001g.
[0017] Furthermore, in step 4, the vacuum degree of the arc furnace is evacuated to 5×10 -3 Pa, and high-purity argon gas is filled in the range of -0.05 to -0.03Pa.
[0018] Furthermore, when melting the Ti ingot, the ingot is melted for 3 to 6 times, each time for 60 to 70 seconds, so as to remove excess oxygen as much as possible; when melting the alloy raw material, the ingot is repeatedly turned over and melted for 8 to 10 times, each time for 100 to 120 seconds, so as to obtain a uniform organizational structure.
[0019] Furthermore, when melting the alloy ingot, the current is 350-600A, and the molten state is maintained for 1-2 minutes.
[0020] Another object of the present invention is to disclose a Ti-Zr-V series lightweight refractory multi-principal eutectic alloy for use in the field of aerospace parts.
[0021] The Ti-Zr-V series lightweight refractory multi-principal eutectic alloy, the preparation method and use thereof of the present invention have the following advantages compared with the prior art:
[0022] 1) The present invention realizes a eutectic structure design of a Ti-Zr-V series lightweight refractory multi-main eutectic element alloy, and obtains a refractory multi-main element alloy with a eutectic structure by adjusting the ratio of the main components Ti, Zr, and V;
[0023] 2) The Ti-Zr-V series lightweight refractory multi-principal eutectic alloy of the present invention not only exhibits low density (5.5-6.1g / cm 3 ), and the selected Ti, Zr, and V elements are beneficial to the improvement of the corrosion resistance, wear resistance, and high temperature stability of the alloy, so it has potential application prospects in the field of engineering structures;
[0024] 3) The Ti-Zr-V series lightweight refractory multi-principal eutectic alloy of the present invention is composed of BCC1 (enriched in Ti and V elements) and BCC2 (enriched in Ti and Zr elements) phases;
[0025] 4) Compared with traditional refractory multi-principal element alloys, the Ti-Zr-V series lightweight refractory multi-principal element eutectic alloy of the present invention has the advantages of low melting point and good fluidity, and can be used to cast various large-sized complex precision components and can achieve one-piece molding.
[0026] In summary, the lightweight refractory multi-principal eutectic alloy in the present invention exhibits lower density and excellent casting fluidity through the combination of BCC1 solid solution enriched in Ti and V elements and BCC2 solid solution enriched in Ti and Zr elements, and also exhibits excellent comprehensive mechanical properties. Therefore, it has potential application prospects in aerospace components. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 For Example 1Ti 14.5 Zr 55 V 30.5 Microstructure of lightweight refractory multi-principal eutectic alloy in cast state;
[0028] Figure 2 For Example 1Ti 14.5 Zr 55 V 30.5 XRD pattern of lightweight refractory multi-principal eutectic alloy in cast state;
[0029] Figure 3 For Example 1Ti 14.5 Zr 55 V 30.5 Room temperature compressive engineering stress-strain curves of lightweight refractory multi-principal eutectic alloys in cast state;
[0030] Figure 4 For Example 2Ti 24.4 Zr 48.6 V 27 XRD pattern of lightweight refractory multi-principal element hypereutectic alloy in cast state;
[0031] Figure 5 For Example 2Ti 24.4 Zr 48.6 V 27 Room temperature tensile engineering stress-strain curves of a lightweight refractory multi-principal element hypereutectic alloy in the as-cast state. DETAILED DESCRIPTION
[0032] The present invention is further described below with reference to the examples. The description of the technical features described below is based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples. It should be noted that:
[0033] Unless otherwise stated, the units used in this specification are all international standard units, and the numerical values and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.
[0034] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values A and B.
[0035] In the present specification, a numerical range expressed using "above" or "below" means a numerical range including the number.
[0036] In this specification, the word "may" means both performing a certain process and not performing a certain process.
[0037] In this specification, the use of "optional" or "optional" indicates that certain substances, components, execution steps, application conditions and other factors are used or not used.
[0038] In this specification, when "normal temperature" or "room temperature" is used, the temperature may be 15-25°C.
[0039] In this manual, the reagents or instruments used without indicating the manufacturer are all conventional products that can be obtained through commercial purchase.
[0040] Example 1
[0041] This embodiment discloses a lightweight refractory multi-principal eutectic alloy, the general formula of which is Ti 14.5 Zr 55 V 30.5 The specific preparation method is as follows:
[0042] Step 1, grinding: Use different types (80#, 240# and 600#) of SiC sandpaper to grind the surface of metal element raw materials Ti, Zr, V (purity is 99.95wt.%) to remove surface oxide scale and impurities.
[0043] Step 2, cleaning: Put the polished metal single substance raw materials Ti, Zr, and V into separate beakers, pour alcohol into them, and perform ultrasonic cleaning. During ultrasonic cleaning, clean the metal single substance raw materials 3 times, and each cleaning time is 8 minutes. After being fully dried, put them into sealed bags for later use.
[0044] Step 3, ingredients: convert the mass percentage according to the molar percentage of the light refractory multi-principal eutectic alloy. Based on the total mass of each alloy ingot being 50g, weigh each single element raw material using an electronic balance. The weighed masses of the single element raw materials Ti, Zr, and V are 7.206g, 27.460g, and 15.334g, respectively, with a weighing error of ±0.001g.
[0045] Step 4: Melting: Place the prepared raw materials into a copper crucible in a vacuum arc furnace, and place the prepared Ti ingot in another copper crucible. Close the furnace door and evacuate to 4.5×10 -3 After the arc reaches -0.05 Pa, high-purity argon is reversed to -0.05 Pa. After the arc is struck, the Ti ingot is first melted three times, each time for 60 seconds, to remove as much excess oxygen as possible. Then the mixed raw materials are melted and repeatedly turned over and melted for 9 times, each time for 120 seconds, to obtain a uniform organizational structure, and finally Ti is obtained. 14.5 Zr 55 V 30.5 Lightweight refractory multi-principal eutectic alloy.
[0046] Figure 1 For Example 1Ti 14.5 Zr 55 V 30.5 The microstructure of the lightweight refractory multi-principal eutectic alloy in the cast state shows that the prepared alloy has typical eutectic microstructural characteristics;
[0047] Figure 2For Example 1Ti 14.5 Zr 55 V 30.5 The XRD spectrum of the lightweight refractory multi-principal eutectic alloy in the cast state shows that the Ti 14.5 Zr 55 V 30.5 Lightweight refractory multi-principal eutectic alloys consist of BCC1+BCC2 phase structures;
[0048] Figure 3 For Example 1Ti 14.5 Zr 55 V 30.5 The room temperature compressive engineering stress-strain curve of the lightweight refractory multi-principal eutectic alloy in the cast state shows that the Ti 14.5 Zr 55 V 30.5 The compressive strength and fracture plasticity of the lightweight refractory multi-principal element eutectic alloy are 1400MPa and 8.2% respectively, showing relatively excellent mechanical properties.
[0049] Example 2
[0050] This embodiment discloses a lightweight refractory multi-principal hypoeutectic alloy, the general formula of which is Ti 24.4 Zr 48.6 V 27 The specific preparation method is as follows:
[0051] Step 1, grinding: Use different types (80#, 240# and 600#) of SiC sandpaper to grind the surface of metal element raw materials Ti, Zr, V (purity is 99.95wt.%) to remove surface oxide scale and impurities.
[0052] Step 2, cleaning: Put the polished metal single substance raw materials Ti, Zr, and V into separate beakers, pour alcohol into them, and perform ultrasonic cleaning. During ultrasonic cleaning, clean the metal single substance raw materials 3 times, and each cleaning time is 8 minutes. After being fully dried, put them into sealed bags for later use.
[0053] Step 3, batching: convert the mass percentage according to the molar percentage of the light refractory multi-principal eutectic alloy. Based on the total mass of each alloy ingot being 50g, weigh each single element raw material using an electronic balance 7, and the weighed masses of the single element raw materials Ti, Zr, and V are 12.597g, 24.001g, and 13.402g, respectively, with a weighing error of ±0.001g.
[0054] Step 4: Melting: Place the prepared raw materials into a copper crucible in a vacuum arc furnace, and place the prepared Ti ingot in another copper crucible. Close the furnace door and evacuate to 4.5×10 -3After the arc reaches -0.05 Pa, high-purity argon is reversed to -0.05 Pa. After the arc is struck, the Ti ingot is first melted three times, each time for 60 seconds, to remove as much excess oxygen as possible. Then the mixed raw materials are melted and repeatedly turned over and melted for 9 times, each time for 120 seconds, to obtain a uniform organizational structure, and finally Ti is obtained. 24.4 Zr 48.6 V 27 Lightweight refractory multi-principal eutectic alloy.
[0055] Figure 4 For Example 2Ti 24.4 Zr 48.6 V 27 The XRD spectrum of the lightweight refractory multi-principal hypereutectic alloy in the cast state shows that the Ti 24.4 Zr 48.6 V 27 Lightweight refractory multi-principal hypereutectic alloy consists of BCC1+BCC2 phase structure;
[0056] Figure 5 For Example 2Ti 24.4 Zr 48.6 V 27 The room temperature tensile engineering stress-strain curve of the lightweight refractory multi-principal element hypereutectic alloy in the cast state shows that the Ti 24.4 Zr 48.6 V 27 The tensile strength and fracture plasticity of the lightweight refractory multi-principal element hypereutectic alloy are 885MPa and 9.5% respectively, showing relatively excellent mechanical properties.
[0057] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A Ti-Zr-V series lightweight refractory multi-principal eutectic alloy, characterized in that: Its general formula is Ti a Zr b V c , where 14% < a < 25%, 48% < b < 55%, 26% < c < 31%, and a + b + c = 100, and a, b, and c respectively correspond to the molar percentages of the elements.
2. The Ti-Zr-V series lightweight refractory multi-principal eutectic alloy according to claim 1, characterized in that: The Ti-Zr-V series lightweight refractory multi-principal eutectic alloy has a BCC1 and BCC2 dual-phase structure.
3. The Ti-Zr-V series lightweight refractory multi-principal eutectic alloy according to claim 1, characterized in that: The Ti-Zr-V series lightweight refractory multi-principal eutectic alloy has a density of 6.1 g / cm 3 and below.
4. A method for preparing the Ti-Zr-V series lightweight refractory multi-principal element eutectic alloy according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step 1, grinding: grinding the surface of the metal element raw materials Ti, Zr, V to remove the oxide scale and impurities on the surface; Step 2, cleaning: put the polished metal single substance raw materials Ti, Zr, and V into separate containers, pour ethanol, use an ultrasonic cleaner to clean them, and after fully drying, put them into sealed bags for standby use; Step 3, ingredients: weigh each component according to the general formula; Step 4, smelting: put the metal single substance raw materials Ti, Zr, and V into the copper crucible of the vacuum arc melting furnace, and place the Ti ingot prepared in advance in another copper crucible; close the furnace door, evacuate, and fill with high-purity argon; after high-frequency arc initiation, first melt the Ti ingot, and then melt the metal single substance raw materials in the copper crucible, turn off the current after they are completely melted, and then cool the furnace; repeat this step for the smelted alloy raw materials; after the smelting is completed, open the furnace door and take out the sample after the alloy ingot is completely cooled, and obtain a Ti-Zr-V series lightweight refractory multi-principal eutectic alloy.
5. The method for preparing the Ti-Zr-V series lightweight refractory multi-principal element eutectic alloy according to claim 4, characterized in that: The purity of the metal single substance raw materials Ti, Zr and V is greater than or equal to 99.95wt.%.
6. The method for preparing the Ti-Zr-V series lightweight refractory multi-principal element eutectic alloy according to claim 4, characterized in that: During ultrasonic cleaning in step 2, the metal element raw material is cleaned at least 3 to 4 times, and each cleaning time is at least 6 to 10 minutes.
7. The method for preparing the Ti-Zr-V series lightweight refractory multi-principal element eutectic alloy according to claim 4, characterized in that: Step 4: The vacuum degree of the arc furnace is reduced to 5×10 -3 Pa, filled with high-purity argon gas at -0.05~-0.03Pa.
8. The method for preparing the Ti-Zr-V series lightweight refractory multi-principal element eutectic alloy according to claim 4, characterized in that: When melting Ti ingots, melt them 3 to 6 times, each time for 60 to 70 seconds; when melting alloy raw materials, turn them over and melt them 8 to 10 times, each time for 100 to 120 seconds.
9. The method for preparing the Ti-Zr-V series lightweight refractory multi-principal element eutectic alloy according to claim 4, characterized in that: When melting alloy ingots, the current is 350-600A and the molten state is maintained for 1-2 minutes.
10. Use of the Ti-Zr-V series lightweight refractory multi-principal eutectic alloy according to any one of claims 1 to 3 in the field of aerospace parts.
Citation Information
Patent Citations
Large-size regular billet ingot refractory high-entropy alloy and preparation method thereof
CN110358962A
Refractory high-entropy alloy and forming method thereof
CN111270094A
ZrTi-based eutectic high-entropy alloy and preparation method thereof
CN112267055A
Si-containing eutectic high-entropy alloy and preparation method thereof
CN114657438A
Eutectic high-entropy alloy based on high-activity elements and application of eutectic high-entropy alloy
CN115198160A