3D printing hot work die steel and heat treatment method thereof

By controlling the alloy element content and martensitic transformation temperature in 3D printing hot work die steel, combined with the combination of nickel, cobalt, molybdenum and other elements, the stress and cost problems of traditional materials after printing are solved, and low-cost, strong Carbon-containing 3D printing mold steel with hot workability and high temperature stability expands the application scope of the SLM process.

CN118773522APending Publication Date: 2024-10-15SHANGHAI LAMO TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410766216.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Traditional 3D printing hot work mold materials are prone to residual stress after printing, resulting in size restrictions and high-cost post-processing requirements. Moreover, existing materials are prone to cracking during heat treatment, making it difficult to meet large-scale printing and low-cost requirements.

Method used

3D printing hot work die steel containing carbon elements is used. The alloying element content is controlled within a specific range. The martensitic transformation temperature Ms point is set at 330-280°C. Through the combination of nickel, cobalt, molybdenum, chromium and other elements, the The toughness and high temperature stability of the material avoid the quenching and tempering process, and the strength and hardness are obtained directly through tempering treatment.

Benefits of technology

It has realized low-cost hot-working mold steel that is not easy to crack in large sizes, improved 3D printing performance and high-temperature stability, reduced post-processing costs, and provided a foundation for the application of SLM technology in the mold field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773522A_ABST
    Figure CN118773522A_ABST
Patent Text Reader

Abstract

The invention discloses 3D printing hot work die steel and a heat treatment method thereof. The 3D printing hot work die steel comprises 0.2-0.4 wt% of a carbon element, 2-7 wt% of a chromium element, 1.5-5.0 wt% of a nickel element, 3-7.0 wt% of a cobalt element and the like, and further comprises an iron element. The martensite transformation temperature Ms point is controlled to be 330-280 DEG C while the content of the alloy elements is guaranteed. The 3D printing hot work die steel is heated to 400-650 DEG C after being printed, tempering is carried out for 2-3 times, cooling is carried out after tempering to obtain final strength, hardness and temperature-resistant stability, and finally the carbon-containing 3D printing hot work die steel which supports large-size printing, is high in hot work performance, convenient to heat treatment and low in cost can be obtained. The hot work die steel and the heat treatment method after printing of the hot work die steel belong to the technical field of 3D printing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a 3D printing hot working die steel and a heat treatment method thereof after printing, and specifically to a carbon-containing 3D printing hot working die steel which supports large-size printing, has strong hot working performance, is convenient for heat treatment and is low-cost, and a heat treatment method thereof after printing, and belongs to the field of 3D printing technology. Background Art

[0002] Traditional subtractive processing technology has bottlenecks in manufacturing some complex structural parts (such as conformal water channels inside molds). As a technology that integrates multiple disciplines such as laser processing, material science, and three-dimensional design, 3D printing technology has incomparable advantages in production cycle, design flexibility, and small-batch customization. As a type of 3D printing technology, the selective laser melting (SLM) process has been widely used in the mold industry. Its advantage is that it can build complex conformal water channels inside the mold according to the structural characteristics of the product to improve heat exchange efficiency, thereby improving production efficiency and product quality.

[0003] Existing commercial hot working die materials such as H13 and Dievar have good hot working properties, and their material costs are lower than commonly used 3D printing materials such as 18Ni300. However, due to the rapid cooling and heating process characteristics of SLM technology, traditional die steels with a certain carbon content generally have large residual stresses after printing, which easily lead to stress cracking, thereby limiting the printing size of the workpiece. Commonly used 3D printing materials such as 18Ni300 have much lower tempering and cracking resistance than traditional hot working die steels due to the influence of internal precipitation and matrix alloy elements. In addition, traditional hot working dies need to go through a quenching and tempering process to achieve the best performance of the material, which increases the post-processing cost.

[0004] Therefore, there is an urgent need in the technical field for a hot working die steel material with strong hot working performance, low cost, simple heat treatment, large-size printing and no cracking. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a carbon-containing 3D printing hot working die steel material with low cost, strong hot working performance, convenient heat treatment, and not easy to crack in large size; thereby breaking through the application bottleneck of existing SLM materials in this field.

[0006] In order to solve the above problems, the technical solution adopted by the present invention is: to provide a 3D printing hot working die steel, which includes: 0.2-0.4wt% carbon element, 2-7wt% chromium element, 1.5-5.0wt% nickel element, 3-7.0wt% cobalt element, 0-3.0wt% molybdenum element, 0-1.0wt% vanadium element, 0-1.0wt% silicon element, 0-1.0wt% niobium element, 0-2wt% aluminum element, 0-1.0wt% titanium element, 0-1.0wt% copper element, 0-1.0wt% manganese element, and the remainder of iron element; while ensuring the content of the above alloy elements, the martensitic transformation temperature Ms point is controlled at 330-280°C.

[0007] Preferably, the 3D printing hot working mold material includes: 0.2-0.3wt% carbon element, 3-5wt% chromium element, 4.0-6.0wt% cobalt element, 2.0-3.0wt% nickel element, 2.0-3.0wt% molybdenum element, 0.5-1.0wt% vanadium element, 0.3-1.2wt% silicon element, 0.5-1.0wt% niobium element, 0-1.5wt% aluminum element, 0-0.5wt% titanium element, 0-0.1wt% copper element, 0-0.1wt% manganese element, and the balance of iron element.

[0008] Traditional hot working die steel needs to be quenched and tempered to achieve the required performance. During the heat treatment process, especially during quenching, in order to form martensite inside the workpiece, it is necessary to quickly cool at a high temperature of 20-50°C above the full austenitization degree. However, the internal stress caused by the phase change can easily cause material deformation, increase additional machining costs, and even cause workpiece cracking. The high Ms point of the above materials ensures that the material can be completely transformed into martensite during printing, and there is no need to quench and harden it during post-processing. At the same time, by adding nickel elements to increase the stacking fault energy of the matrix and promote the cross-slip of the material under stress, the toughness of the material can be improved to cope with the stress during printing. In addition, by adding strong carbide precipitation elements to reduce the carbon content in the matrix, the stress of carbon-containing martensite during printing is reduced. The addition of cobalt as a solid solution element is beneficial to improve the strength and toughness of the material at high temperature, and cobalt can hinder the recovery of dislocations in the matrix, further promoting the nucleation of carbides at grain boundaries. Since these special carbides maintain a coherent relationship with the matrix, the toughness of the material will not be impaired by the formation of carbides.

[0009] By regulating the content and size of carbon, molybdenum, chromium, and vanadium carbides, the stability of the material at high temperature after the final heat treatment is guaranteed. The carbon content needs to be controlled between 0.2-0.4wt%. When the carbon content is too low, the elements that fail to form carbides will enter the matrix, which will affect the stability of the material at high temperature. On the contrary, when the carbon content is too high, the carbon in the martensite will cause the internal lattice of the material to be distorted, thereby increasing the stress during printing and affecting the final molding size of the material. The chromium element needs to be controlled at 3-5wt%. In hot working molds, especially in die-casting environments, the oxide film formed by chromium on the surface of the material plays a vital role in the material's oxidation resistance at high temperatures, and the addition of chromium helps to improve the hardenability of steel in the back-end heat treatment. If the chromium content is higher than 5%, it will lead to the formation of M23C7 type carbides with poor high temperature performance, which is not conducive to the high temperature performance of the material. The addition of molybdenum and vanadium can play a role in secondary hardening, and the carbides with strong high temperature stability formed with carbon can nucleate at the grain boundaries, forming a pinning effect, which hinders the recovery of the matrix of the material at high temperatures and improves the material's anti-tempering performance. A small amount of niobium and titanium can refine the austenite grains, avoiding the coarsening and growth of grains during the printing process and subsequent heat treatment. To a certain extent, it also forms fine grain strengthening with the SLM process to further enhance the toughness of the material.

[0010] In order to ensure the stability of the material at high temperatures, the mold cannot be used directly after printing and requires further heat treatment.

[0011] The present invention also provides a heat treatment method for the above-mentioned 3D printing hot working die steel, characterized in that the 3D printing hot working die steel is heated to 400-650°C after printing, tempered 2-3 times, and cooled after tempering to obtain the final strength, hardness and temperature resistance stability.

[0012] The biggest difference between this heat treatment process and traditional heat treatment is that traditional hot working molds need to be quenched to adjust the internal structure of the material after leaving the factory, and then tempered to remove the stress of the material structure phase change. However, the above-mentioned materials do not need to be quenched during heat treatment. During 3D printing, the high Ms point ensures that the structure of the printed matrix is ​​completely martensite. After printing is completed, this material only needs to be tempered to remove stress to obtain reasonable strength, hardness and high temperature stability required for hot working molds.

[0013] Compared with the prior art, the present invention has the following beneficial effects:

[0014] 1. Compared with the current carbon-free SLM mold steel material, the SLM hot working mold steel material obtained by the present invention contains a certain amount of carbon and lower nickel, thereby obtaining better high-temperature stability while ensuring the low cost of the material.

[0015] 2. Compared with the existing traditional mold steel, the present invention achieves better 3D printing performance by regulating the internal structure of the material through innovative component design.

[0016] 3. The low-cost, non-cracking carbon-containing 3D printing stainless steel material obtained by the present invention provides a material basis for the further extensive application of the SLM process in the mold field; the composition and heat treatment method of the carbon-containing hot working die steel developed by the present invention also provide a theoretical basis for the further development of other 3D printing hot working die steel materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a photo of the metallographic structure of Example 1 magnified 100 times;

[0018] Figure 2 This is a photo of the metallographic structure of Example 1 magnified 500 times;

[0019] Figure 3 The tempering hardness of Example 1 at different temperatures;

[0020] Figure 4 This is the tempering hardness curve of Example 1 at 600°C for 100 hours. DETAILED DESCRIPTION

[0021] In order to make the present invention more clearly understood, preferred embodiments are described in detail as follows.

[0022] Example 1

[0023] A 3D printing hot working die steel material, comprising: 0.27wt% carbon, 7wt% chromium, 4.2wt% cobalt, 1.5wt% nickel, 1.5wt% molybdenum, 0.8wt% vanadium, 0.5wt% silicon, 0.05wt% aluminum, 0.05wt% niobium, 0.05wt% manganese, 0.03wt% titanium, 0wt% copper, and the remainder of iron. The composition has Ms=307.0°C and Ac3=879.43°C.

[0024] The heat treatment process after printing is: heating to 650℃ and tempering twice, and air cooling after tempering.

[0025] The hardness after printing is 50HRC, the hardness after heat treatment is 46HRC, the tensile strength is 1650MPa, the yield strength is 1465MPa, and the impact toughness is Akv22.5J.

[0026] The material prepared in this embodiment has the following properties: Figure 1-4 shown.

[0027] Example 2

[0028] A 3D printing hot working die steel material, comprising: 0.33wt% carbon, 5wt% chromium, 4.2wt% cobalt, 1.5wt% nickel, 1.5wt% molybdenum, 1.2wt% vanadium, 0.5wt% silicon, 0.05wt% aluminum, 0.05wt% niobium, 0.05wt% manganese, 0.05wt% copper, 0wt% titanium, and the remainder of iron. The composition has Ms=308.8°C and Ac3=875.19°C.

[0029] The heat treatment process after printing is: heating to 610℃ and tempering twice, and gas cooling after tempering.

[0030] The hardness after printing is 51.5HRC, the hardness after heat treatment is 48.5HRC, the tensile strength is 1774MPa, the yield strength is 1531MPa, and the impact toughness Akv is 17.2J.

[0031] Example 3

[0032] A 3D printing hot working die steel material, comprising: 0.38wt% carbon, 6.4wt% chromium, 7.0wt% cobalt, 2.5wt% nickel, 2.0wt% molybdenum, 1.2wt% vanadium, 0.5wt% silicon, 0.05wt% aluminum, 0.05wt% niobium, 0.05wt% manganese, 0wt% titanium, 0wt% copper, and the remainder of iron. The composition has Ms=282.7°C and Ac3=852°C.

[0033] The heat treatment process after printing is: heating to 610℃ and tempering twice, and oil quenching after tempering.

[0034] The hardness after printing is 52.5HRC, the hardness after heat treatment is 50HRC, the tensile strength is 1861MPa, the yield strength is 1831MPa, and the impact toughness Akv is 15.9J.

Claims

1. A 3D printing hot working die steel, characterized in that: include: Carbon element 0.2-0.4wt%, chromium element 2-7wt%, nickel element 1.5-5.0wt%, cobalt element 3-7.0wt%, molybdenum element 0-3.0wt%, vanadium element 0-1.0wt%, silicon element 0-1.0wt%, niobium element 0-1.0wt%, aluminum element 0-2wt%, titanium element 0-1.0wt%, copper element 0-1.0wt%, manganese element 0-1.0wt%, and the balance iron element; while ensuring the content of the above alloy elements, the martensitic transformation temperature Ms point is controlled at 330-280℃.

2. The 3D printing hot working mold material according to claim 1, characterized in that: include: Carbon element 0.2-0.3wt%, chromium element 3-5wt%, cobalt element 4.0-6.0wt%, nickel element 2.0-3.0wt%, molybdenum element 2.0-3.0wt%, vanadium element 0.5-1.0wt%, silicon element 0.3-1.2wt%, niobium element 0.5-1.0wt%, aluminum element 0-1.5wt%, titanium element 0-0.5wt%, copper element 0-0.1wt%, manganese element 0-0.1wt%, and the balance is iron element.

3. The heat treatment method for 3D printing hot working die steel according to claim 1 or 2, characterized in that: The 3D printing hot working die steel is heated to 400-650°C after printing, tempered 2-3 times, and cooled after tempering to obtain the final strength, hardness and temperature resistance stability.

4. The heat treatment method for 3D printing hot working die steel according to claim 3, characterized in that: The cooling method is air cooling, gas cooling or oil cooling quenching.

Citation Information

Cited By

  • Alloy composition and use thereof

    WO2026149597A1