NiCrAlZr low-expansion metal bonding layer and preparation method thereof

Through the metallurgical combination of the NiCrAlZr low-expansion metal bonding layer and the single crystal high-temperature alloy matrix, the problem of interface instability of the thermal barrier coating at high temperatures is solved, good thermal expansion matching and oxidation corrosion resistance are achieved, and the coating is extended life span.

CN118773553APending Publication Date: 2024-10-15AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410856169.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The thermal expansion coefficient of the existing thermal barrier coating between the ceramic surface layer and the metal matrix is ​​insufficiently matched, resulting in an unstable interface at high temperatures, which limits the long-life development of the thermal barrier coating.

Method used

The NiCrAlZr low-expansion metal bonding layer is deposited by vacuum arc plating. The element composition is 5% Cr, 20%-25% Al, 0.25%-0.5% Zr, and the rest is Ni, combined with single crystal high-temperature alloy The substrate is subjected to mill flow activation, deposition and diffusion treatment to form a metallurgical bond.

Benefits of technology

It achieves good matching with the ceramic surface layer and alloy matrix, improves the resistance to high-temperature oxidation corrosion, slows down the diffusion of elements, enhances the density and strain capacity of the coating, and extends the life of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773553A_ABST
    Figure CN118773553A_ABST
Patent Text Reader

Abstract

The invention discloses a NiCrAlZr low-expansion metal bonding layer and a preparation method thereof, and relates to the technical field of metal bonding layer materials. Metallurgical bonding is formed between the Ni-Cr-Al-Zr alloy and a single-crystal high-temperature alloy matrix, and the Ni-Cr-Al-Zr alloy comprises, by mass, 5% of Cr, 20%-25% of Al, 0.25%-0.5% of Zr and the balance Ni. The metal bonding layer is well bonded with the base body, the thermal expansion coefficient is low under the high-temperature oxidation condition, the matching performance with the alloy base body and the ceramic surface layer is improved, the bonding strength of the thermal barrier coating is improved, and the service life of the thermal barrier coating is prolonged. The anti-oxidation and anti-corrosion requirements of the turbine blade can be met; and the process is simple, industrial production is easy to achieve, and the composite coating is excellent in performance, has application prospects and is suitable for the high-temperature alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal bonding layer materials, and in particular relates to a NiCrAlZr low expansion metal bonding layer and a preparation method thereof. Background Art

[0002] The temperature at the front inlet of the new generation of engines is constantly increasing. Depositing thermal barrier coatings on the surface of blade alloys can increase the operating temperature and high-temperature corrosion resistance of turbine blades. Thermal barrier coating technology is one of the key technologies in the development of advanced aircraft engines. The MCrAlY series of metal bonding layers of thermal barrier coatings are developed from coated anti-oxidation coatings. When used as a single anti-oxidation coating, it has the characteristics of good bonding with the substrate and excellent high-temperature protection performance; when used as a bonding layer, there is insufficient research on the matching of thermal expansion coefficients of alloy / bonding layer / YSZ, the formation law of surface TGO, and the diffusion mechanism of elements, resulting in a decrease in the role of the bonding layer in improving the matching of the ceramic surface layer and the substrate, which fundamentally limits the development of long-life thermal barrier coatings.

[0003] The main difficulty of the low expansion metal bonding layer is that, on the basis of meeting the requirements of high temperature oxidation and thermal corrosion resistance, the thermal expansion coefficient must be well matched with the ceramic surface layer and the metal matrix, and the interface structure must be stable at high temperature. Summary of the invention

[0004] Based on the above background, the purpose of the present invention is to provide a NiCrAlZr coating with a smaller thermal expansion coefficient and good compatibility with a ceramic surface layer and an alloy substrate, and a preparation method thereof.

[0005] In view of this, according to one aspect of an embodiment of the present invention, a NiCrAlZr low expansion metal bonding layer is provided, which forms a metallurgical bond with a single crystal high temperature alloy substrate, wherein the element components are 5% Cr, 20% to 25% Al, 0.25% to 0.5% Zr by mass, and the rest is Ni.

[0006] Optionally, the single crystal high temperature alloy substrate is a DZ125 alloy substrate.

[0007] According to another aspect of an embodiment of the present invention, a method for preparing a NiCrAlZr low expansion metal bonding layer is also provided, and the method for preparing any of the metal bonding layers comprises:

[0008] Step S01: using a NiCrAlZr target material, and installing the target material on a cathode seat of a vacuum arc coating machine;

[0009] Step S02: performing surface activation treatment on the single crystal high temperature alloy substrate;

[0010] Step S03: cleaning and drying the surface of the single crystal high temperature alloy substrate;

[0011] Step S04: depositing a coating on the surface of the single crystal high temperature alloy substrate;

[0012] Step S05: performing diffusion treatment on the deposited coating.

[0013] Optionally, the surface activation treatment method in step S02 is a grinding fluid treatment method.

[0014] Optionally, the grinding fluid treatment method is to use corundum sand with a particle size of 0.154 mm to add it into a liquid sand blowing machine for sand blowing, with a working pressure of 0.2MPa to 0.5MPa and a treatment time of 10min.

[0015] Optionally, step S04 further includes: deposition parameters are arc current I=550A-750A, workpiece bias voltage U=20V-30V, deposition time 100min-150min, vacuum degree 6×10 -3 Pa~7×10 -3 Pa.

[0016] Optionally, step S04 also includes: a preheating step: the vacuum degree reaches 6×10 -3 Pa~7×10 -3 Pa later, bombardment heating, arc current I = 550A ~ 750A, workpiece bias U = 200V ~ 300V, bombardment time is 5min.

[0017] Optionally, step S05 further includes: the vacuum degree of the diffusion process is 1×10 -2 Pa~1×10 -3 Pa, temperature is 850℃-900℃, time is 3h.

[0018] The present invention has the following beneficial effects: (1) The present invention adopts arc ion plating method to prepare NiCrAlZr coating, which has a smaller thermal expansion coefficient, has good compatibility and matching with ceramic surface layer and alloy substrate, and does not cause cracking of coating and interface instability during use; (2) has good resistance to high temperature oxidation corrosion, and improves the resistance to high temperature oxidation corrosion of matrix alloy at high temperature; (3) has good thermal bonding strength with matrix alloy; (4) has low diffusion coefficient, and can slow down the diffusion of elements such as Al and Cr from coating to matrix alloy at high temperature, and can prevent metal elements such as Ti, Mo, W, Ni from alloy substrate to coating. At the same time, since the arc ion plating (ARC) method has the characteristics of moderate deposition rate, good coating density, and metallurgical bonding with substrate, the coating prepared by ARC method has strong compatibility with substrate, good thickness and density, thereby greatly improving the strain capacity of coating. NiCrAlZr coating is prepared by vacuum arc plating technology, and the preparation process is simple, efficient, and low cost, which can meet the demand for long life of protective coating on the outer surface of turbine blades. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is an electron microscope image of a NiCrAlZr low expansion metal bonding layer according to an embodiment of the present invention.

[0020] Figure 2 The figure is a curve diagram showing the variation of thermal expansion coefficient of a NiCrAlZr low expansion metal bonding layer with temperature according to an embodiment of the present invention. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] According to one aspect of an embodiment of the present invention, a NiCrAlZr low expansion metal bonding layer is provided, which forms a metallurgical bond with a single crystal high temperature alloy substrate, wherein the element components are 5% Cr, 20% to 25% Al, 0.25% to 0.5% Zr by mass, and the rest is Ni.

[0023] Furthermore, the single crystal high temperature alloy substrate is a DZ125 alloy substrate.

[0024] According to another aspect of an embodiment of the present invention, a method for preparing a NiCrAlZr low expansion metal bonding layer is provided, wherein the method for preparing any of the metal bonding layers comprises:

[0025] Step S01: using a NiCrAlZr target material, and installing the target material on a cathode seat of a vacuum arc coating machine;

[0026] Step S02: Activate the surface of the single crystal high temperature alloy substrate to enhance the bonding between the bonding layer and the substrate. Further, the surface activation method in step S02 is a grinding flow treatment method.

[0027] Step S03: cleaning and drying the surface of the single crystal high temperature alloy substrate;

[0028] Step S04: depositing a coating on the surface of the single crystal high temperature alloy substrate;

[0029] Step S05: performing diffusion treatment on the deposited coating.

[0030] Furthermore, the grinding fluid treatment method is to use corundum sand with a particle size of 0.154 mm to add it into a liquid sand blowing machine for sand blowing, the working pressure is 0.2MPa~0.5MPa, and the treatment time is 10min.

[0031] Further, step S04 also includes: deposition parameters are arc current I=550A-750A, workpiece bias voltage U=20V-30V, deposition time is 100min-150min, vacuum degree is 6×10 -3 Pa~7×10 -3 Pa.

[0032] Furthermore, step S04 also includes: preheating step: the vacuum degree reaches 6×10 -3 Pa~7×10 -3 After Pa, bombardment heating is performed, the arc current I = 550A ~ 750A, the workpiece bias U = 200V ~ 300V, and the bombardment time is 5min, which is helpful to remove impurities on the substrate surface.

[0033] Furthermore, step S05 also includes: the vacuum degree of the diffusion process is 1×10 -2 Pa~1×10 -3 Pa, temperature is 850-900℃, time is 3h.

[0034] Example

[0035] Prepare the following on multiple 30*10*1.5mm samples: Figure 1 The NiCrAlZr low expansion metal bond layer shown comprises:

[0036] 1. Single crystal high temperature alloy turbine blades are used as the substrate, and the substrate alloy is DZ125 alloy. The NiCrAlZr coating is prepared on the DZ125 alloy using arc ion plating equipment, and the NiCrAlZr target is used to achieve the deposition of the NiCrAlZr coating. Raw materials are selected, and NiCrAlZr targets are used, in which the elements are 5% Cr, 20% to 25% Al, 0.25% to 0.5% Zr by mass, and the rest is Ni. The target is installed on the cathode seat of the vacuum arc coating machine.

[0037] 2. Activate the surface of parts by grinding flow treatment. Add corundum sand with a particle size of 0.154 mm into the liquid sand blasting machine. The working pressure is 0.2MPa~0.5MPa and the treatment time is 10min.

[0038] 3. Clean and dry

[0039] 4. Use a fixture to load the parts into the vacuum chamber of the arc ion plating equipment.

[0040] 5. Install the parts to be coated in the vacuum chamber and evacuate the vacuum to a degree of 6×10 -3 Pa~7×10 - 3 Pa, bombardment heating, arc current I = 550A ~ 750A, workpiece bias U = 200V ~ 300V, bombardment time is 5min, then a layer of NiCrAlZr is deposited on the surface of the part, arc current I = 550A ~ 750A, workpiece bias U = 20V ~ 30V, deposition time is 100min ~ 150min, vacuum degree is 6×10 -3 Pa~7×10 -3 Pa.

[0041] 6. Diffusion treatment of parts with NiCrAlZr coating, diffusion treatment, vacuum degree 10 -2 Pa~10 - 3 Pa, temperature 850-900℃, time 3h.

[0042] from Figure 1 It can be seen that the bonding layer ( Figure 1 The middle layer in the coating has a dense structure and is well bonded to the substrate. After a thermal shock test (5 minutes of heat preservation and 5 minutes of cooling) at 1100 degrees Celsius, the coating has no wrinkling, cracking, peeling, or shedding for more than 4000 times, and is in good condition. Figure 2It can be seen that the expansion coefficient of the NiCrAlZr metal bonding layer of the present invention changes little with temperature. In the temperature range of 50°C to 1150°C, the thermal expansion coefficients of the samples NiAICrZr-1 and NiAICrZr-2 are (12.22 to 16.55) x10 -6 K -1 and (12.35~16.87)x10 -6 K -1 .

[0043] The above is only a specific embodiment of the present invention, and the present invention is described in detail. The unexplained part is a conventional technology. However, the protection scope of the present invention is not limited to this. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. The protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A NiCrAlZr low expansion metal bonding layer, characterized in that: It forms a metallurgical bond with a single crystal high temperature alloy matrix, wherein the element components are 5% Cr, 20%-25% Al, 0.25%-0.5% Zr by mass, and the rest is Ni.

2. The metal bonding layer according to claim 1, characterized in that: The single crystal high temperature alloy substrate is a DZ125 alloy substrate.

3. A method for preparing a NiCrAlZr low expansion metal bonding layer, characterized in that: The method of preparing any one of the metal bonding layers as claimed in claims 1 to 2 comprises: Step S01: using a NiCrAlZr target material, and installing the target material on a cathode seat of a vacuum arc coating machine; Step S02: performing surface activation treatment on the single crystal high temperature alloy substrate; Step S03: cleaning and drying the surface of the single crystal high temperature alloy substrate; Step S04: depositing a coating on the surface of the single crystal high temperature alloy substrate; Step S05: performing diffusion treatment on the deposited coating.

4. The method according to claim 3, characterized in that The surface activation treatment method in step S02 is a grinding fluid treatment method.

5. The method according to claim 4, characterized in that The grinding fluid treatment method is to use corundum sand with a particle size of 0.154 mm to add it into a liquid sand blowing machine for sand blowing. The working pressure is 0.2MPa~0.5MPa and the treatment time is 10min.

6. The method according to claim 3, characterized in that Step S04 also includes: deposition parameters are arc current I=550A-750A, workpiece bias voltage U=20V-30V, deposition time 100min-150min, vacuum degree 6×10 -3 Pa~7×10 -3 Pa.

7. The method according to claim 3, characterized in that Step S04 also includes: Preheating step: vacuum degree reaches 6×10 -3 Pa~7×10 -3 Pa later, bombardment heating, arc current I = 550A ~ 750A, workpiece bias U = 200V ~ 300V, bombardment time is 5min.

8. The method according to claim 3, characterized in that Step S05 also includes: the vacuum degree of the diffusion process is 1×10 -2 Pa~1×10 -3 Pa, temperature is 850℃-900℃, time is 3h.

Citation Information

Patent Citations

  • Gas turbine component with improved thermal barrier coating system

    CN106906471A

  • Thermal barrier coating for single crystal superalloy thermal protection and preparation method thereof

    CN110079770A

  • Aerospace component with protective coating and method of making same

    CN116472363A

  • Thermal barrier coating and preparation method thereof

    CN116479380A

  • Bond coat process for thermal barrier coating

    US20070207339A1