Preparation process of corrosion-resistant lithium magnesium alloy
By forming a uniform phosphate-permanganate conversion film on the surface of magnesium-lithium alloys, the problems of poor corrosion resistance and toxic traditional treatments of magnesium-lithium alloys are solved, and the corrosion resistance of magnesium-lithium alloys is improved.
Patent Information
- Application Number
- CN202410877040.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-15
AI Technical Summary
Magnesium-lithium alloys have poor corrosion resistance, and hexavalent chromium compounds used in traditional chemical conversion treatments are toxic, leading to environmental pollution and limited application.
A conversion solution composed of potassium permanganate and potassium dihydrogen phosphate is used to form a uniform orange film on the surface of the magnesium-lithium alloy. Through grinding, acetone cleaning, alkali cleaning and conversion treatment, a corrosion-resistant phosphate-permanganic acid is formed. Salt conversion coating.
It prolongs the time for corrosion spots to appear on the surface of the magnesium-lithium alloy, improves its corrosion resistance, forms a uniform protective film, and significantly improves the corrosion resistance of the magnesium-lithium alloy.
Smart Images

Figure CN118773594A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alloy surface protection and relates to a preparation process of a corrosion-resistant lithium-magnesium alloy. A uniform orange-yellow film is formed on the surface of the magnesium-lithium alloy to protect the lithium-magnesium alloy and achieve a corrosion-resistant effect. Background Art
[0002] The Mg-Li binary system is a typical eutectic alloy system. According to the relevant phase diagram, when the Li content is between 5-11wt.%, its structure is α and β dual phases, the α solid solution has a hexagonal close-packed structure (hcp), and the β solid solution has a body-centered cubic structure (bcc).
[0003] The corrosion resistance of magnesium-lithium alloy itself is poor. When magnesium-lithium alloy is immersed in liquid ammonia, continuous small bubbles immediately rise on the surface of the sample. This may be due to the corrosion of the substrate by the corrosive medium directly or through the pores of the film layer, resulting in hydrogen evolution caused by the reaction. After immersion for 5 minutes, the surface of the sample is evenly covered with corrosion spots. As the immersion time increases, the area of the corrosion spots gradually expands to the surrounding area. When the immersion reaches 1 hour, compared with the sample before immersion, it can be seen that a large amount of gray-white corrosion products are produced on the surface of the alloy, indicating that the surface of the alloy has been corroded by the corrosive medium. Therefore, for the application of magnesium-lithium alloy, it is necessary to protect its surface to enhance its corrosion resistance.
[0004] Chemical conversion treatment is gaining more and more attention due to its advantages of simple operation, low cost, uniform film formation, etc. Traditional chemical conversion treatment technologies mostly use hexavalent chromium-containing compounds such as chromic anhydride or dichromate as treatment agents to form chromate conversion films on the alloy surface. Although the process is mature and the performance is stable, the hexavalent chromium compounds used in this method are toxic and will cause serious harm to the environment, which greatly limits its application. Therefore, the present invention studies an environmentally friendly chromium-free conversion treatment process. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a preparation process of a corrosion-resistant lithium-magnesium alloy, which protects the lithium-magnesium alloy by forming a uniform orange-yellow film on the surface of the magnesium-lithium alloy, thereby achieving a corrosion-resistant effect.
[0006] The technical solution adopted by the present invention to achieve its purpose is as follows:
[0007] A preparation process of a corrosion-resistant lithium-magnesium alloy comprises the following steps: grinding a magnesium-lithium alloy substrate, cleaning it with acetone, alkali washing it, placing it in a conversion liquid for conversion treatment, and finally air-cooling and drying it to obtain a corrosion-resistant lithium-magnesium alloy, wherein the conversion liquid comprises 40 g / L potassium permanganate and 50 g / L potassium dihydrogen phosphate, the conversion temperature is 55° C., and the conversion time is 20 min.
[0008] Furthermore, the polishing is to polish the surface of the magnesium-lithium alloy substrate using 100-1000# SiC sandpaper.
[0009] Furthermore, the acetone cleaning time is 10 minutes, and the cleaning temperature is room temperature 22-28°C.
[0010] Furthermore, the alkali solution used for alkali washing comprises 37 g / L NaOH, 10 g / L Na3PO4·12H2O, and 17.4 g / L Na2SiO3·9H2O. The alkali washing temperature is 22-28° C., and the alkali washing time is 10 min.
[0011] Furthermore, the chemical composition of the magnesium-lithium alloy matrix is Li 9.5%-10.5%, Zn 2.5%-3.5%, Al 2.5%-3.5% by mass, and the balance is Mg.
[0012] The beneficial effects of the present invention are:
[0013] The present invention forms a uniform orange-yellow film on the surface of the magnesium-lithium alloy to protect the lithium-magnesium alloy and achieve a corrosion-resistant effect. The time for the corrosion point to begin to appear is extended to 330 minutes. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 It is a flow chart of the present invention.
[0015] Figure 2 It is the X-ray diffraction pattern of Mg-10Li-3Al-3Zn alloy.
[0016] Figure 3 This is an optical micrograph of Mg-10Li-3Al-3Zn alloy after being etched with hydrochloric acid alcohol solution for 5-10s.
[0017] Figure 4 This is the macroscopic morphology of Mg-10Li-3Al-3Zn alloy before and after immersion in liquid ammonia solution for 1 hour.
[0018] Figure 5 This is the microscopic morphology of Mg-10Li-3Al-3Zn alloy after being immersed in liquid ammonia solution for 1 hour.
[0019] Figure 6 This is the morphology of Mg-10Li-3Al-3Zn alloy after grinding and alkali washing.
[0020] Figure 7 This is the microscopic morphology of magnesium-lithium alloy after acetone cleaning for 10 minutes.
[0021] Figure 8These are the surface morphologies of Mg-10Li-3Al-3Zn alloy after surface conversion film treatment at different times.
[0022] Fig. 9 These are the macroscopic and microscopic morphologies of the conversion film on the surface of magnesium-lithium alloy.
[0023] Fig.10 It is the electrode potential curve of blank Mg-10Li-3Al-3Zn alloy and converted sample in 3.5% NaCl.
[0024] Fig.11 These are the macroscopic morphologies of the samples treated with permanganate conversion before (a) and after (b) immersion in liquid ammonia.
[0025] Fig.12 This is the microscopic morphology of the sample treated with permanganate conversion after being immersed in liquid ammonia.
[0026] Fig.13 This is a relationship diagram between film forming process and corrosion resistance time. DETAILED DESCRIPTION
[0027] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work should belong to the scope of protection of the present invention. 1. Specific embodiment 1
[0029] Mg-10Li-3Al-3Zn alloy was selected, and the surface of the magnesium-lithium alloy matrix was polished with 1000# SiC sandpaper. After polishing, the microstructure of the alloy matrix was observed. Figure 6 (a), The surface of the magnesium-lithium alloy substrate is covered with many scratches.
[0030] The polished magnesium-lithium alloy substrate was cleaned with acetone at room temperature for 10 min, and then cleaned with running deionized water. After cleaning, the microscopic morphology of the alloy substrate was observed. Figure 7 The surface of the magnesium-lithium alloy substrate is covered with many scratches, which is different from the morphology after polishing. Figure 6 There is no obvious difference compared with (a), indicating that the acetone cleaning process does not cause corrosion of the magnesium-lithium alloy matrix.
[0031] The alloy matrix was placed in an alkali solution for alkali washing. The composition of the alkali solution was 37 g / L NaOH, 10 g / L Na3PO4·12H2O, and 17.4 g / L Na2SiO3·9H2O. The alkali washing temperature was 25°C and the alkali washing time was 10 min. The morphology of the lithium-magnesium alloy after alkali washing can be found in Figure 6(b) As can be seen from the figure, the surface of the sample is still covered with scratches after alkali washing, and there is no obvious difference from the morphology of the sample after sandpaper polishing, indicating that the alkali washing did not cause obvious corrosion to the matrix alloy. The EDX test results show that after the sample was treated with alkali washing, in addition to a large amount of matrix element Mg and a small amount of O, no other elements were detected on the surface. If the alkali washing time is less than 10 minutes, the oil stains on the surface of the sample cannot be completely removed, which will reduce the film quality of the chemical conversion film and fail to achieve a good effect of protecting the matrix; if the alkali washing time is greater than 10 minutes, it will cause corrosion to the matrix itself.
[0032] The alloy matrix is placed in a conversion solution for conversion treatment. The conversion solution includes 40g / L potassium permanganate and 50g / L potassium dihydrogen phosphate. The conversion temperature is 55°C and the conversion time is 20min. Finally, the alloy is air-cooled and dried to obtain a corrosion-resistant lithium-magnesium alloy. After the magnesium-lithium alloy is treated by the above film-forming process, a thin, uniform, orange-yellow chemical conversion film ( Fig. 9 a macro). Fig. 9 b is the microscopic morphology of the corresponding phosphate-permanganate conversion film. It can be seen from the figure that the phosphate-permanganate conversion film is composed of a base film, white granular deposits attached thereto, and irregular microcracks, which are distributed over the entire sample surface.
[0033] The magnesium-lithium alloy used in this embodiment is composed of a magnesium-rich α phase and a lithium-rich β phase, and the potential of the two-phase alloy is related to the thermodynamic equilibrium potential of the different elements that make up the alloy. The standard potential of lithium is -3.045V (NHE), and the standard potential of magnesium is -2.375V (NHE). From the data, it can be seen that the standard potential of lithium is lower than that of magnesium. Therefore, it can be inferred that the potential of the lithium-rich β phase should also be lower than that of the magnesium-rich α phase. As a result, a local battery effect is generated between the α phase and the β phase. When the magnesium-lithium alloy is immersed in the chemical conversion solution, a microcurrent is formed on the surface of the substrate due to the potential difference between the two-phase alloy, which causes the β phase as the anode to begin to dissolve, while the α phase as the cathode undergoes a hydrogen evolution reaction. The released hydrogen causes many microcracks to form on the surface of the substrate during the chemical conversion process, such as Fig. 9 As shown in b. During the test, it was found that a large number of bubbles were indeed generated on the surface of the sample at the beginning of the conversion film treatment. From the EDX spectrum analysis results (Table 1), it can be seen that the element content in different areas of the conversion film is different. There are relatively high contents of O, P, K and Mn in the white sediment, and these elements still have a certain content in the base film. However, the content of Mg is relatively high in the cracks of the conversion film.
[0034] Table 1
[0035] Differentzone Mg,wt.% 0,wt.% P,wt.% Mn,wt.% K,wt.% SpotA 26.36 40.24 16.20 11.13 6.07 SpotB 52.21 24.87 12.14 7.46 3.32 SpotC 74.47 12.45 8.68 2.27 2.13
[0036] 2. The influence of process control on alloy
[0037] The instruments used in the present invention are as follows:
[0038] [1] Metallographic structure observation
[0039] The samples were polished with 100-2000 SiC sandpaper, then polished with polishing agent (magnesium oxide) on a P-1 polishing machine (speed 1350r / min), and finally finely ground on deerskin until there were no scratches on the surface of the sample. The samples were etched with picric acid alcohol solution for 5-10s, and then quickly cleaned with anhydrous ethanol and dried, and finally the metallographic structure was observed with an optical metallographic microscope.
[0040] [2] Scanning electron microscope morphology observation and energy spectrum analysis
[0041] The surface morphology of the samples was analyzed by secondary electron imaging using a Nissan SS-550 scanning electron microscope (SEM), and the cross-sectional morphology of the polished samples was analyzed by backscattered electrons. At the same time, the element distribution on the sample surface was analyzed by an energy dispersive analyzer (EDX).
[0042] [3] X-ray diffraction phase analysis
[0043] The phase composition of the samples was analyzed by X-ray diffractometer (XRD, D / max-RB, Japan). The anode target was CuKa (λ=1.5418A), the tube voltage was 40 kV, and the tube current was 100 mA.
[0044] [4] X-ray photoelectron spectroscopy
[0045] The electron binding energy of the elements of the conversion film was analyzed by MK I X-ray photoelectron spectroscopy (XPS). The anode target was an aluminum target, and the binding energy measured was corrected by standard C (284.60 eV). XPSPEAK4.1 software was used for peak fitting.
[0046] [5] Test method for corrosion resistance of coating
[0047] [5.1] Soak test
[0048] The immersion corrosion test is to completely immerse the sample in the corrosive medium, and record the time difference between the sample immersion time and the first visible corrosion point on the surface as the solution corrosion resistance time of the sample. At the same time, carefully observe the changes in the surface morphology and microstructure of the sample after immersion. The corrosive medium used in this test is 3.5wt.% NaCl aqueous solution, the test temperature is room temperature, and the ratio of the volume of the corrosive medium to the working area of the tested sample is 1cm 2 / 100mL.
[0049] [5.2] Electrochemical test
[0050] The corrosion behavior of the samples was studied using the M352 / M273 electrochemical system from EG&G, USA. A standard three-electrode system was used, with a saturated calomel electrode (SCE) as the reference electrode, graphite as the auxiliary electrode, and the sample to be tested as the working electrode (the non-working area was sealed with paraffin and rosin). The sampling frequency of the test potential-time curve was 5point / s. The scanning range of the test polarization curve was from -0.25V relative to the open circuit potential to a sharp increase in corrosion current, with a scanning rate of 1mV / s. The electrochemical impedance spectroscopy (EIS) was performed on an M273 potentiostat and a 5210 lock-in amplifier, using an M398 AC impedance test system, and the data was fitted using the ZSimpWin fitting software after the test. The scanning frequency range was 100kHz-10mHz, and the amplitude of the disturbance signal was 5mV. There was a delay of about 600s before measuring the polarization curve and EIS.
[0051] 1. Effect of conversion liquid composition on conversion film formation
[0052] The Mg-10Li-3Al-3Zn samples after pre-grinding were used to fully remove the oil stains on the surface with acetone solution and alkaline cleaning solution, and then the samples were immersed in the treatment solutions of different formulations shown in Table 2 to observe the film formation. The film formation, the apparent uniformity of the film, and the time it took for the film-forming samples to begin to corrode significantly after being immersed in a 3.5wt.% NaCl solution were observed, and compared with the conversion solution of the present invention.
[0053] Table 2
[0054]
[0055]
[0056] It can be seen from Table 2 that when the composition of the conversion liquid changes, the film-forming property will be affected. Other conversion liquid components have poor film-forming property, poor corrosion resistance, or even fail to form a film.
[0057] 2. Effect of film forming process on corrosion resistance
[0058] The concentration of KMnO4 in the treatment solution was fixed at 40g / L, and three factors, namely, the concentration of KH2PO4 in the treatment solution, the film-forming temperature and the film-forming time, were selected. Three levels of each factor were selected for orthogonal test, as shown in Table 3. The time it took for the first visible corrosion point to appear on the surface of the film-forming sample after it was immersed in a 3.5wt.% NaCl aqueous solution was used as the evaluation standard for corrosion resistance, and the corresponding test results are shown in Table 4.
[0059] Table 3
[0060]
[0061] Table 4
[0062]
[0063]
[0064] Note: R1, R2 and R3 are the average values of salt water resistance time of the first level, second level and third level of each factor respectively; S represents the range, which is the difference between the maximum and minimum values of the average values R1, R2 and R3 of the corresponding levels of each factor.
[0065] It can be seen directly from Table 4 that the test results of Group 6 are the best, and the time it takes for the conversion film to be immersed in a 3.5wt.% NaCl solution until visible corrosion spots begin to appear is the longest. However, whether this A2B3C1 combination is a suitable combination of the levels of the three factors A, B, and C still requires calculation and analysis of the test results. R1, R2, and R3 in Table 3 are the average values of the salt water resistance time of the first level, the second level, and the third level of each factor, respectively. The range (S) is the difference between the maximum and minimum values of the average values R1, R2, and R3 of the corresponding levels of each factor. Its size reflects the size of the effect of each factor in the test. A large range indicates that this factor has a great impact on the index and is usually an important factor. On the contrary, a small range means a small effect and is an unimportant factor. From the results of the range analysis, we can see that the concentration factor has the greatest impact (the range is 552.37), indicating that the concentration of KH2PO4 in the treatment solution has the most significant effect on the quality of the conversion film. This is because KH2PO4 is not only a reactant, but also plays a role in regulating the total acidity of the treatment solution. Therefore, KH2PO4 plays a vital role in chemical conversion treatment. In comparison, the influence of film-forming temperature (range is 180.67) and film-forming time (range is 128.00) on the quality of the conversion film is far lower than the influence of KH2PO4 concentration on the film quality, and from the range results, we can see that the influence of film-forming temperature is slightly greater than that of film-forming time.
[0066] The relationship between KH2PO4 concentration and corrosion resistance time, the relationship between film forming temperature and corrosion resistance time, and the relationship between film forming time and corrosion resistance time refer to Fig.13 .
[0067] 3. The effect of conversion treatment time on alloy.
[0068] The treatment was carried out with a conversion time of 2 min, 5 min, and 10 min, and compared with the present invention, see Figure 8 .
[0069] When the Mg-10Li-3Al-3Zn alloy was treated in the conversion solution for 2 min ( Figure 8a), there are still scratches on the surface, but compared with the morphology after alkali washing, some microcracks appear in local areas of the sample surface, indicating that a conversion film has begun to form on the substrate surface. At the same time, it can be seen that blocks of different sizes are attached to the surface of the sample. EDX results show that these blocks contain elements in the conversion solution such as P, Mn, and K in addition to the matrix element Mg, indicating that the magnesium-lithium alloy matrix has reacted with the conversion solution at this time, forming these blocks on the surface.
[0070] When the treatment time is 5 min, the sample surface undergoes obvious changes ( Figure 8 b), the scratches become lighter and the surface is almost covered by the film layer. At the same time, the area with microcracks increases significantly, indicating that the film layer has grown rapidly.
[0071] When the treatment time is 10 min, the surface morphology of the sample does not change significantly ( Figure 8 c), which indicates that after a rapid growth period, the conversion film enters a relatively stable formation stage.
[0072] The treatment time of the present invention is 20 minutes, and a uniform phosphate-permanganate conversion film with microcracks is formed on the surface ( Figure 8 d).
[0073] 4. Corrosion resistance of the lithium-magnesium alloy prepared in Example 1 4.1
[0075] Fig.10 Potential-time curves of blank Mg-10Li-3Al-3Zn alloy and the corrosion-resistant lithium-magnesium alloy prepared in Example 1 in 3.5wt.% NaCl. Fig.10 Curve 1 shows that the open circuit potential (OCP) of the blank Mg-10Li-3Al-3Zn alloy slowly increases from -1.64V at the beginning to -1.62V. During the test time, the open circuit potential of the blank magnesium-lithium alloy increases by about 20mV. Compared with the sample treated with the conversion film (whose stable potential is about -1.60V), the open circuit potential at the stable state is relatively low, only -1.62V. This shows that the stability of the blank magnesium-lithium alloy in the 3.5wt.% NaCl solution is not as good as that of the sample after the conversion treatment of the present invention.
[0076] However, the magnesium-lithium alloy samples after transformation showed completely different changes. Fig.10Curve 2 clearly shows that the corrosion process of the sample after conversion treatment can be divided into two stages. In the first stage, an obvious potential jump occurred, and the open circuit potential of the conversion film in 3.5% NaCl solution dropped rapidly from -1.63V at the beginning to the lowest point -1.68V, and then quickly rose to the highest point -1.57V. Due to the inhomogeneity of the composition and structure of the conversion film, a more complex multiphase or multiphase reaction occurred with the solution at the beginning of immersion, which caused the violent fluctuation of the open circuit potential in this stage. In the second stage (II), the fluctuation amplitude of the open circuit potential of the sample with conversion film slowed down significantly, the potential began to slowly decrease, and finally stabilized at about -1.60V. The relatively stable open circuit potential change indicates that some slow and regular reactions occurred between the conversion film and the solution during this immersion stage. In the entire test time range, the open circuit potential of the sample after conversion treatment increased by 30mV. The stable open circuit potential of the conversion film is higher than that of the blank magnesium-lithium alloy, indicating that the stability of the magnesium-lithium alloy after conversion treatment in 3.5wt.% NaCl solution is higher than that of the blank alloy sample, that is, the conversion film of the present invention can improve the corrosion resistance of the magnesium-lithium alloy.
[0077] 4.2 Immersion experiment
[0078] The blank magnesium-lithium alloy and the converted sample were immersed in a liquid ammonia solution at room temperature. The changes on the sample surface were carefully observed, and the time it took for the first visible corrosion point to appear on the sample surface was recorded as the corrosion time of the sample solution. The experiment found that the blank alloy was severely corroded in the NaCl solution, and a large amount of gray-white corrosion products were produced on the sample surface after immersion for 20 hours. The converted samples showed different corrosion processes. After immersion in liquid ammonia solution for 10 hours, local corrosion appeared on the sample surface. As the immersion time increased, the corrosion area on the sample surface gradually expanded, but the trend of the corrosion area expansion was smaller than that of the blank alloy. Compared with the unimmersed samples, the surface of the converted sample was also covered with more obvious corrosion products after immersion for 20 hours ( Fig.11 , a is before immersion, b is after immersion). Fig.12 This is the microscopic morphology of the treated sample after being immersed in liquid ammonia for 20 hours. It can be seen from the figure that the sample after conversion treatment shows a typical pitting morphology.
Claims
1. A process for preparing a corrosion-resistant lithium-magnesium alloy, characterized in that: The magnesium-lithium alloy substrate was polished, cleaned with acetone, and then placed in a conversion solution for conversion treatment after alkali washing. Finally, it was air-cooled and dried to obtain a corrosion-resistant lithium-magnesium alloy. The conversion solution included 40 g / L potassium permanganate and 50 g / L potassium dihydrogen phosphate. The conversion temperature was 55°C and the conversion time was 20 min.
2. The process for preparing a corrosion-resistant lithium-magnesium alloy according to claim 1, characterized in that: The polishing is to use 100-1000# SiC sandpaper to polish the surface of the magnesium-lithium alloy substrate.
3. The process for preparing a corrosion-resistant lithium-magnesium alloy according to claim 1, characterized in that: The acetone cleaning time is 10 minutes, and the cleaning temperature is room temperature 22-28°C.
4. The process for preparing a corrosion-resistant lithium-magnesium alloy according to claim 1, characterized in that: The alkali solution used for alkali washing contains 37 g / L NaOH, 10 g / L Na3PO4·12H2O and 17.4 g / L Na2SiO3·9H2O. The temperature of alkali washing is 22-28°C and the time of alkali washing is 10 min.
5. The process for preparing a corrosion-resistant lithium-magnesium alloy according to claim 1, characterized in that: The chemical composition of the magnesium-lithium alloy matrix is Li 9.5%-10.5%, Zn 2.5%-3.5%, Al 2.5%-3.5% by mass, and the balance is Mg.