A thermal cleaning furnace magnetic steel production line and method for continuously stripping organic coatings

By designing a continuous heat cleaning furnace production line, the organic coating of NdFeB magnetic steel is removed by using a series heating and combustion system, and combined with micro acid, ultrasonic and vacuum treatment, the low coating removal efficiency and degradation of magnetic properties in the prior art are solved. The problem of this achieves efficient and environmentally friendly magnetic steel surface treatment and film thickness consistency.

CN118773620BActive Publication Date: 2024-12-06NANTONG ZHENGHAI MAGNET CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411253298.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-12-06
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

In the process of removing organic coatings on the surface of NdFeB magnets, there are problems such as fast chemical solvent volatility, large safety hazards, low mechanical peeling efficiency, high magnetic attenuation rate and dust influence in the prior art, resulting in low surface treatment efficiency and degradation of magnetic properties. .

Method used

A continuous thermal cleaning furnace production line is designed, including thermal cleaning furnace, microacid cleaning module, ultrasonic cleaning module, blow drying module and vacuum treatment module. The continuous organic coating is achieved through series heating system, combustion system and powder collection system. Remove and achieve an efficient and environmentally friendly production process through control systems and guide rails.

Benefits of technology

The continuous organic coating removal of the magnetic steel surface is achieved, the magnetic attenuation rate is less than 1%, the surface is clean and powder-free, which meets the requirements of recoating, the tooling has good electrical conductivity, high film thickness consistency, and improved production efficiency and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773620B_ABST
    Figure CN118773620B_ABST
Patent Text Reader

Abstract

The present invention discloses a thermal cleaning furnace magnetic steel production line and method for continuously stripping organic coatings, comprising a loading platform and a coating stripping module, a slightly acid cleaning module, an ultrasonic cleaning module, a blow-drying module, a drying module and a control system connected to the loading platform in sequence through a track; the coating stripping module comprises at least one thermal cleaning furnace, the thermal cleaning furnace comprises a first and a second heating system, a combustion system, a powder collection system and an inlet and an outlet, the first and the second heating systems are in series structure and are arranged in the first and the second chambers, and the combustion system is arranged behind the first and the second heating systems; the inlet of the thermal cleaning furnace is connected to the track of the loading platform, and the outlet is connected to the slightly acid cleaning module. After stripping, the surface cleanliness of the tooling / magnetic steel is high, meeting the requirements for continued coating, and having good conductivity. The epoxy layer film thickness range R<0.5mm of the product produced by the same tooling, the long-term process capability of the film thickness CPK>1.33, and the average magnetic flux attenuation rate of the magnetic steel is less than 1%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surface treatment and deplating of NdFeB magnetic steel, and in particular relates to a thermal cleaning furnace magnetic steel production line and a stripping method for continuously stripping organic coatings. Background Art

[0002] NdFeB magnets need to be loaded with different types of tools such as hangers, carriers, hooks, etc. before surface treatment, especially the coating process of organic coatings such as epoxy, electrostatic powder coating, and electrostatic spraying. Absolute electrical contact is required when applying organic coatings. During the coating process, the magnets are usually placed on hangers, carriers, and other tools, and the tools and magnets are coated together. Conventional methods for removing organic coatings are usually chemical solution methods, high-temperature decomposition methods, and mechanical stripping methods.

[0003] Patent EP1319694A1 discloses an agent and method for stripping paint from a metal surface, especially from a metal surface made of non-ferrous metal (such as aluminum or aluminum alloy), wherein the main component of the organic paint stripper involved is an alcohol organic solvent. Since the paint stripper contains an alkoxylated alkyl alcohol as an additional component, a good paint stripping effect is achieved.

[0004] Patent EP0614707A1 uniformly heats the metal wall to at least 200°C and up to 350°C by medium frequency induction heating, and then immediately externally heats the coating in the presence of oxygen to thermally decompose it at a temperature of at least 400°C and up to 550°C, but the metal wall will not exceed 400°C, and then mechanical cleaning of the product cannot be achieved.

[0005] Patent CN105015141A provides a method for mechanical stripping of an organic coating of a composite material, comprising the following steps: placing the composite material coated with the organic coating on the tooling of a plastic spraying machine; adjusting the equipment parameters of the plastic spraying machine, maintaining the nozzle pressure at 20 to 40 psi (0.138-0.276 MPa), and the plastic spraying medium flow at 60 to 75 m / s, and using the plastic spraying machine to spray the composite material with the plastic spraying medium until the organic coating of the composite material is completely removed.

[0006] Patent CN217109592U discloses an environmentally friendly and efficient heat cleaning furnace, which can remove the organic coating on the surface of the workpiece more thoroughly through the coordination of various structures inside, and achieve pollution-free gas emission as much as possible; and can stably achieve the discharge and removal of more workpieces.

[0007] Among the above methods, when the chemical removal method is conventionally used, the organic solvent evaporates quickly and is flammable, which poses a great safety hazard and is not conducive to the health of employees; when using a sandblaster to peel off different types of tooling (such as hangers, carriers, hooks, etc.) to load magnetic steel, different equipment parameters need to be adjusted. At the same time, the use of a single thermal cleaning furnace requires the furnace door to be opened each time, and most of the heat in the furnace is dissipated, resulting in a lower temperature in the furnace when processing the next batch of tooling and / or magnetic steel, and it takes a certain amount of time to raise the temperature in the furnace to the preset temperature again, thereby reducing the working efficiency of the thermal cleaning furnace. At the same time, when the tooling in the thermal cleaning furnace is densely stacked and there is a lot of powder residue in the furnace, it will affect the stripping effect of the coating on the tooling, and it is easy to have incomplete stripping. In addition, after the magnetic steel is baked in a dusty atmosphere, the magnetic attenuation is usually above 5%, which affects the use of the magnetic steel. Summary of the invention

[0008] In order to solve the above problems, the present invention provides a thermal cleaning furnace magnetic steel production line and a stripping method for continuously stripping organic coatings, which can continuously strip the organic coating on the surface of the magnet.

[0009] In order to achieve the above object, the present invention provides the following technical solutions:

[0010] A magnetic steel production line of a thermal cleaning furnace for continuously stripping organic coatings, comprising a loading platform and a coating stripping module, a slightly acid cleaning module, an ultrasonic cleaning module, a blowing module and a drying module connected to the loading platform in sequence through a track, and a control system for controlling the operation of each module; the coating stripping module comprises at least one thermal cleaning furnace, and the thermal cleaning furnace comprises a first heating system, a second heating system, a combustion system, a powder collecting system, and an inlet and an outlet, the first heating system and the second heating system are of a series structure, relatively independently arranged in a first chamber and a second chamber respectively, the combustion system is arranged behind the first and second heating systems, and is used to process the decomposition gases of the first and second heating systems; the powder collecting system is used to collect powders of the first and second heating systems; the inlet of the thermal cleaning furnace is connected to the track of the loading platform, and the outlet is connected to the slightly acid cleaning module.

[0011] In a preferred embodiment of the present invention, the powder collection system includes a powder collection box, an exhaust fan and a powder extraction pipeline; a U-shaped collection pipeline is arranged in the middle position of the thermal cleaning furnace, and the U-shaped opening of the U-shaped collection pipeline is connected to the bottom of the thermal cleaning furnace, so that the powder can be scattered into the U-shaped tube; the fan pipeline of the exhaust fan is connected to the U-shaped collection pipeline and the powder collection box. When the exhaust fan is turned on, the powder in the thermal cleaning furnace is cleaned into the powder collection box through the U-shaped collection pipeline and the fan pipeline.

[0012] Among them, the exhaust fans have different powers. When the amount of powder in the furnace is large, a high-power and high-air volume mode can be used, and when the amount of powder is small, a low-power and low-air volume mode can be used.

[0013] In a preferred embodiment of the present invention, the slightly acid cleaning module includes a cleaning tank and a filtration circulation system; the filtration circulation system is a bag filter, and the filter inlet and outlet are connected to the cleaning tank. The filtration circulation system is used to enhance the contact between the acid solution and the tooling / product, and remove solid impurities in the solution to increase the cleaning effect.

[0014] In a preferred embodiment of the present invention, the cleaning tank is a plastic tank or a stainless steel tank, and the material may be PP, PVC, 304 stainless steel, etc.

[0015] In a preferred embodiment of the present invention, the ultrasonic cleaning module includes an ultrasonic cleaning tank, a filtering circulation system and a vibration system; the vibration system is arranged outside the ultrasonic cleaning tank, and the inlet and outlet of the filtering circulation system are connected to the ultrasonic cleaning tank; the filtering circulation system is configured to enhance the contact between the water washing liquid and the tooling / product, while removing solid impurities in the solution.

[0016] In a preferred embodiment of the present invention, the frequency of the ultrasonic cleaning tank is 20-28KHZ, and the ultrasonic time is 1-5min.

[0017] In a preferred embodiment of the present invention, the cleaning tank is a stainless steel tank, and the material may be 304 or 316 stainless steel.

[0018] In a preferred embodiment of the present invention, the filtration circulation system is a bag filter, and the inlet and outlet of the filter are connected to the ultrasonic cleaning tank.

[0019] In a preferred embodiment of the present invention, the thermal cleaning furnace production line further comprises a vacuum processing module, and the vacuum processing module has at least one vacuum high-temperature single-chamber furnace.

[0020] Since the magnetic steel is damaged when the organic coating is peeled off, the magnetic attenuation usually exceeds 5%. By adding a vacuum treatment module to the magnetic steel, the problem of high magnetic flux attenuation of the product can be solved, thereby improving defective products into qualified products.

[0021] In a preferred embodiment of the present invention, the inlet and outlet of the heat cleaning furnace are gate-type closed structures to ensure that they can be closed in time to reduce the heat dissipation of the heat cleaning furnace;

[0022] In a preferred embodiment of the present invention, the thermal cleaning furnace deplating and stripping production line is a continuous production line, and the coating stripping module, micro-acid cleaning module, ultrasonic cleaning module, blow drying module, drying module and vacuum processing module are all driven by guide rails and hoisting.

[0023] The present invention also provides a method for continuously stripping an organic coating using the thermal cleaning furnace magnetic steel production line, comprising:

[0024] S10, placing the tooling and / or magnetic steel on the loading platform and sending them into the hot cleaning furnace through the hot cleaning furnace guide rail;

[0025] S20, using the first heating system to heat the tooling and / or magnetic steel in the first chamber to volatilize and remove the organic solvent in the organic coating, making the coating brittle; then the tooling and / or magnetic steel are sent to the second chamber through the guide rail, and the tooling and / or magnetic steel are heated by the second heating system to calcine the organic matter in the organic coating of the magnet; after the gas decomposition products of the first and second heating systems enter the combustion system, the temperature in the combustion system is controlled at 800-1000°C, and after high-temperature treatment, they are converted into CO2 and water vapor and discharged through the chimney;

[0026] S30, after the heating is completed, the guide rail automatically transports the loading tooling and / or magnetic steel out, and the tooling and / or magnetic steel use a hoist to sequentially hoist the loading platform into the slightly acid cleaning module, ultrasonic cleaning module, drying module and drying module for cleaning and drying;

[0027] S40, tooling and / or magnetic steel are cut, and the obtained tooling and / or magnetic steel can be coated again.

[0028] In a preferred embodiment of the present invention, the heating temperature in the first chamber is 180° C.-250° C., and the heating time is 20-40 min.

[0029] In a preferred embodiment of the present invention, the heating temperature in the second chamber is 380° C. - 450° C., and the heating time is 150-200 min.

[0030] In a preferred embodiment of the present invention, after the magnetic steel and the tooling are unloaded, the magnetic steel is placed in a vacuum treatment module for vacuum treatment, and the vacuum degree in the furnace is controlled at 10*e -2 ~100Pa; preferably 10*e -2 ~20Pa; the processing temperature is 400-700℃, and the processing time is 200-300min.

[0031] In a preferred embodiment of the present invention, in step S20, the control system always ensures that the decomposition speed and the concentration of gas decomposition products are strictly controlled within a certain range; the control system automatically controls the atmosphere in the furnace so that the oxygen content is not less than 18%, so that the organic matter on the surface of the product to be treated is gradually decomposed into gas. When the oxygen content is lower than 18%, the oxygen content is too low, the combustion is not sufficient, the decomposition effect is affected, and the powder on the tooling and magnetic steel is easy to be peeled off incompletely.

[0032] In a preferred embodiment of the present invention, the drying module comprises a drying air knife, and the air temperature during drying is controlled at 100-150° C., and the drying time is 1-5 minutes.

[0033] In a preferred embodiment of the present invention, the drying module is a drying furnace. During drying, the wind temperature is controlled at 100-150° C. and the drying time is 30-60 minutes.

[0034] In a preferred embodiment of the present invention, the cleaning tank of the slightly acidic cleaning module is filled with a weak acid solution with a pH value of 5-6.5, and the weak acidic cleaning solution is acetic acid or oxalic acid; the cleaning time is 5-20 minutes.

[0035] In a preferred embodiment of the present invention, during ultrasonic cleaning, the frequency of the ultrasonic tank is 20-28 KHZ, and the ultrasonic time is 1-5 min.

[0036] In a preferred embodiment of the present invention, in step S30, after the loading tooling enters the ultrasonic cleaning module, the vibration motor drives the vibration frame and the loading tooling to vibrate, thereby enhancing the contact between the water washing liquid and the tooling / product and enhancing the cleaning ability.

[0037] In a preferred embodiment of the present invention, the amplitude of vibration of the loading tooling is 2-3 mm.

[0038] In a preferred embodiment of the present invention, the loading tooling after ultrasonic cleaning passes through a filtering circulation system to expand the concentration range of the surface material, while removing solid impurities in the solution to enhance the cleaning effect.

[0039] The loading platform and the hot cleaning furnace guide rails in the present invention can be called auxiliary equipment, which can handle multiple toolings at a time.

[0040] Beneficial effects of the present invention:

[0041] 1) The deplating and stripping production line of the present invention can continuously strip the organic coating on the surface of the magnet. After the organic coating is stripped, the surface of the magnetic steel is clean and powder-free and can be used for re-coating. The cleanliness can reach ≤9 for Class B particles and ≤8 for Class C particles.

[0042] 2) After the organic coating is stripped, the average magnetic flux attenuation rate of the magnetic steel is less than 1%. Magnetic attenuation refers to the average magnetic flux attenuation rate of the sintered NdFeB workpiece after vibration stripping, that is, magnetic attenuation = (magnetic flux NOM before stripping) - (magnetic flux NOM after stripping) / (magnetic flux NOM before stripping).

[0043] 3) After the organic coating is stripped, the conductivity of the tooling is good, the resistance between any two points of the tooling is R < 5Ω, and the surface is clean and free of powder, meeting the requirements for continued coating. The thickness range of the epoxy layer produced by the same tooling is R < 0.5μm, the film thickness consistency is good, and the long-term process capability of the film thickness CPK > 1.33.

[0044] 4) The present invention adopts a continuous thermal cleaning furnace deplating stripping method, which is more environmentally friendly. The thermal cleaning furnace is a travel bridge thermal cleaning furnace, which is entered and exited through a gate-type closed door. Except for intermittent operation of loading and unloading, the rest of the production line can be continuously mechanized through the production line to meet the requirements of mass production. The processed tooling can be directly used for re-coating production. The conductivity-related parameters of the coating production process are stable, and the product film thickness consistency is high.

[0045] 5) The organic coating stripping method of the present invention does not use chemical reagents. During the operation, only slight acids are exposed, and no highly toxic chemicals such as organic solvents are exposed. This solves the problem of rapid evaporation of organic solvents during chemical coating removal, which poses a great safety hazard and damages the health of employees, and also solves the problem of low efficiency of continuous mechanical stripping. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 It is a schematic diagram of the overall process of the hot cleaning furnace magnetic steel production line of the present invention;

[0047] Figure 2 It is a structural schematic diagram of the coating stripping module of the present invention;

[0048] Figure 3 It is a structural schematic diagram of the slightly acid cleaning module of the present invention;

[0049] Figure 4 It is a structural schematic diagram of the ultrasonic cleaning module of the present invention. DETAILED DESCRIPTION

[0050] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0051] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0052] Example 1

[0053] 1) Place the electrophoresis tooling and magnet on the loading platform, and coat it with epoxy resin with a coating thickness of 15μm. The specifications of the electrophoresis tooling are 400mm*300mm; the specifications of the magnet are 40mm*30mm*3mm. It is sent into the hot cleaning furnace through the hot cleaning furnace guide rail, first heated to 200℃ in the first chamber by the first heating system, and treated for 30min; then it enters the second chamber of the hot cleaning furnace through the guide rail, and is heated to 390℃ by the second heating system, and treated for 180min to calcine the organic matter in the organic coating of the magnet; after the heating time is reached, the guide rail automatically transports the loading tooling out.

[0054] The control system automatically controls the atmosphere in the furnace so that the oxygen content is not less than 18%, so that the organic matter on the surface of the product to be treated is gradually decomposed into gas. The gas decomposition products of the first heating system and the second heating system enter the combustion system. The temperature of the combustion system is 1000℃. After high-temperature treatment, they are converted into CO2 and water vapor and discharged through the chimney. The workpiece / magnetic steel and powdered inorganic matter that is not affected by temperature remain in the thermal cleaning furnace.

[0055] 2) After heating is completed, use a hoist to lift the electrophoresis tooling and magnetic steel into the slightly acid cleaning module on the loading platform. The cleaning tank is filled with acetic acid, the pH is controlled at 5.5, and the cleaning time is 10 minutes.

[0056] 3) After the powder is cleaned, the electrophoresis tooling and magnetic steel are hoisted into the ultrasonic cleaning module with a hoist. The frequency of the ultrasonic tank is 25KHZ, the ultrasonic time is 3min, and the amplitude of the vibration of the loading tooling is 2mm.

[0057] 4) After ultrasonic cleaning, the electrophoresis tooling and magnetic steel are hoisted into the drying module with the loading platform, the air temperature is controlled at 130℃, and the drying time is 3 minutes.

[0058] 5) After the electrophoresis tooling and magnetic steel are blown dry, the loading platform is hoisted into the drying module, the wind temperature is controlled at 120℃, and the drying time is 40 minutes.

[0059] 6) Place the dried electrophoresis tooling and magnetic steel into a vacuum monomer furnace, control the vacuum degree at 15Pa, the processing temperature at 510℃, and the processing time for 220min.

[0060] The electrophoretic tooling and magnetic steel processed by the continuous thermal cleaning furnace production line for stripping organic coatings can be used directly, the surface of the magnetic steel is clean and powder-free, the Class B particles of the magnetic steel are level 8, and the Class C particles are level 7.

[0061] The treated magnetic steel is hung on the treated tooling for electrophoresis treatment, and the resistance values ​​of any three corners and the center point of the tooling are randomly measured, and the average value is recorded as R. R=1.1Ω.

[0062] The extreme difference of epoxy layer thickness of products using the same hanger is 0.3μm, and the consistency of film thickness is good; 5 pieces of magnetic steel are randomly taken every day to measure the thickness of the electrophoretic layer, and the sampling is carried out for 25 days. The long-term process capability CPK of the film thickness is 1.68.

[0063] Example 2

[0064] 1) Place the powder spraying tooling and magnet on the loading platform. The coating is polyurethane with a coating thickness of 100μm. The specifications of the powder spraying tooling are 800mm*500mm; the specifications of the magnet are 50mm*40mm*3mm. It is sent into the hot cleaning furnace through the hot cleaning furnace guide rail. First, it is treated in the first chamber of the hot cleaning furnace with a temperature of 210℃ for 30min; then it enters the second chamber of the hot cleaning furnace with a temperature of 420℃ through the guide rail for 150min to calcine the organic matter in the organic coating of the magnet; after the heating time is reached, the guide rail automatically transports the loading tooling out.

[0065] The control system automatically controls the atmosphere in the furnace so that the oxygen content is not less than 18%, so that the organic matter on the surface of the product to be treated is gradually decomposed into gas. The gas decomposition products of the first heating system and the second heating system enter the combustion system. The temperature of the combustion system is 900℃. After high-temperature treatment, they are converted into CO2 and water vapor and discharged through the chimney. The workpiece / magnetic steel and powdered inorganic matter that are not affected by temperature remain in the thermal cleaning furnace.

[0066] 2) After heating is completed, the loading platform is hoisted to lift the powder spraying tooling and magnetic steel into the slightly acid cleaning module. The cleaning tank is filled with oxalic acid, the pH is controlled at 5.0, and the cleaning time is 10 minutes.

[0067] 3) After the powder is cleaned, the powder spraying tooling and magnets are hoisted into the ultrasonic cleaning module. The frequency of the ultrasonic tank is 25KHZ, the ultrasonic time is 2.5min, and the amplitude of the vibration of the loading tooling is 3mm.

[0068] 4) After ultrasonic cleaning, the powder spraying tooling and magnetic steel are hoisted into the drying module with a hoist. The wind temperature is controlled at 120℃ and the drying time is 2 minutes.

[0069] 5) After drying, the powder spraying tooling and magnetic steel are used, and the loading platform is hoisted into the drying module. The wind temperature is controlled at 130℃ and the drying time is 45 minutes.

[0070] 6) Place the dried powder spraying tooling and magnetic steel into a vacuum monomer furnace, control the vacuum degree at 15Pa, the processing temperature at 500℃, and the processing time for 280min.

[0071] The powder spraying tooling and magnetic steel processed by the continuous thermal cleaning furnace production line for stripping organic coatings can be used directly, the surface of the magnetic steel is clean and powder-free, the Class B particles of the magnetic steel are Class 9, and the Class C particles are Class 8.

[0072] The treated magnetic steel is hung on the treated tooling for electrostatic powder spraying. The resistance values ​​of any three corners and the center point of the tooling are randomly measured, and the average value is recorded as R. R=2.3Ω, indicating that the conductivity is good, the surface is clean and free of powder, and meets the requirements for continued coating.

[0073] The thickness range of the epoxy layer using the same hanger product is 0.2μm, indicating that the film thickness is uniform and consistent. Five magnetic steels are randomly selected every day to measure the film thickness of the powder spray layer. The sampling lasts for 25 days, and the long-term process capability CPK of the film thickness is 1.73.

[0074] Example 3

[0075] 1) Place the spraying tooling and magnet on the loading platform. The coating is acrylic resin with a coating thickness of 20μm. The specifications of the spraying tooling are 1000mm*1000mm; the specifications of the magnet are 70mm*20mm*3.5mm. It is sent into the hot cleaning furnace through the hot cleaning furnace guide rail, and first treated in the first chamber of the hot cleaning furnace at a temperature of 230℃ for 30min; then it enters the second chamber of the hot cleaning furnace at a temperature of 400℃ through the guide rail and is treated for 180min to calcine the organic matter in the organic coating of the magnet; after the heating time is reached, the guide rail automatically transports the loading tooling out.

[0076] The control system automatically controls the atmosphere in the furnace so that the oxygen content is not less than 18%, so that the organic matter on the surface of the product to be treated is gradually decomposed into gas. The gas decomposition products of the first heating system and the second heating system enter the combustion system. The temperature of the combustion system is 900℃. After high-temperature treatment, they are converted into CO2 and water vapor and discharged through the chimney. The workpiece / magnetic steel and powdered inorganic matter that are not affected by temperature remain in the thermal cleaning furnace.

[0077] 2) After heating is completed, use a hoist to lift the spraying tooling and magnetic steel onto the loading platform into the slightly acid cleaning module. The cleaning tank is filled with acetic acid, the pH is controlled at 6, and the cleaning time is 15 minutes.

[0078] 3) After the powder is cleaned, the spraying tooling and magnets are hoisted into the ultrasonic cleaning module. The frequency of the ultrasonic tank is 28KHZ, the ultrasonic time is 4 minutes, and the amplitude of the vibration of the loading tooling is 2mm.

[0079] 4) After ultrasonic cleaning, the spraying tooling and magnetic steel are hoisted into the drying module with a hoist. The air temperature is controlled at 120°C and the drying time is 4 minutes.

[0080] 5) After the spraying tooling and magnets are dried, the loading platform is hoisted into the drying module, the air temperature is controlled at 150°C, and the drying time is 40 minutes. The dried tooling is removed from the platform and is ready for re-coating.

[0081] 6) Place the dried magnetic steel back into the vacuum monomer furnace, control the vacuum degree at 15Pa, the processing temperature at 520℃, and the processing time for 240min.

[0082] The spraying tooling and magnetic steel processed by the continuous thermal cleaning furnace production line for stripping organic coatings can be used directly, the surface of the magnetic steel is clean and powder-free, the Class B particles of the magnetic steel are level 8, and the Class C particles are level 8.

[0083] The treated magnetic steel is hung on the treated tooling for spraying. The resistance values ​​of any three corners and the center point of the tooling are randomly measured, and the average value is recorded as R. R=3.4Ω, indicating that the conductivity is good, the surface is clean and free of powder, and meets the requirements for continued coating.

[0084] The extreme difference of the spray coating thickness of the products using the same hanger is 0.15μm, and the consistency of the coating thickness is good; 5 pieces of magnetic steel are randomly taken every day to measure the coating thickness of the spray coating, and the sampling is carried out for 25 days. The long-term process capability CPK of the coating thickness is 1.78.

[0085] Comparative Example 1

[0086] The preparation method is the same as that of Example 1, except that:

[0087] In step 1), there is no heating treatment step in the first chamber. The electrophoresis tooling and magnetic steel directly enter the second chamber of the thermal cleaning furnace at a temperature of 420°C through the guide rail, and the treatment time is 210 minutes.

[0088] After treatment, the Class B particles on the surface of the magnetic steel are level 13, and the Class C particles are level 12.

[0089] Hang the treated magnetic steel on the treated tooling for electrophoretic coating, randomly measure the resistance values ​​of any three corners and the center point of the tooling, calculate the average value and record it as R, R=230Ω. This indicates that the conductivity is average, and continue coating after loading the product.

[0090] The film thickness range of products using the same hanger is 1.5μm, and the film thickness consistency is good; 5 pieces of magnetic steel are randomly taken every day to measure the film thickness, and the sampling is carried out for 25 days. The long-term process capability CPK of the film thickness is 0.87.

[0091] Comparative Example 2

[0092] The preparation method is the same as that of Example 2, except that:

[0093] There is no heating treatment step in the second chamber in step 1). The electrophoresis tooling and magnetic steel directly enter the first chamber of the thermal cleaning furnace through the guide rail at a temperature of 230°C, and the treatment time is 210 minutes.

[0094] After processing, there is powder residue on the surface of the magnetic steel.

[0095] The processed magnetic steel is hung on the processed tooling for electrophoretic coating, and the surface of the product is not coated with an electrophoretic layer.

[0096] Comparative Example 3

[0097] The preparation method is the same as that of Example 3, except that step 6 is not included and there is no vacuum treatment step.

[0098] After treatment, the Class B particles on the surface of the magnetic steel are level 9, and the Class C particles are level 8.

[0099] The treated magnetic steel is hung on the treated tooling for electrophoretic coating. The resistance values ​​of any three corners and the center point of the tooling are randomly measured, and the average value is recorded as R, R=1.3Ω.

[0100] The film thickness range of products using the same hanger is 1.2μm, and the film thickness consistency is good; 5 pieces of magnetic steel are randomly taken every day to measure the film thickness, and the sampling is carried out for 25 days. The long-term process capability CPK of the film thickness is 1.71.

[0101] After treatment, the magnetic flux attenuation rate of the magnetic steel is 5.2%.

[0102] Test Case

[0103] Resistance value: Randomly measure the resistance values ​​of any three points on the tooling and the center point, and calculate the average value, which is recorded as R.

[0104] Film thickness CPK: Use the treated hanger and magnetic steel to produce continuous coating, take 5 pieces every day to measure the film thickness, take 25 consecutive days, and take 125 pieces in total. First calculate the average value X of the film thickness of 5 pieces of magnetic steel every day and the standard deviation s of 125 products. The upper specification limit of the product film thickness is USL, and the lower specification limit is LSL.

[0105] CPK= Min[ (USL- X) / 3s, (X- LSL) / 3s]

[0106] Cleanliness test: refer to ISO16232 cleanliness standard, and the product sampling quantity is 30 pieces.

[0107] Magnetic flux attenuation rate: 30 pieces of each of the above samples 1-3 and comparison sample 1 were randomly selected, and magnetic flux tests were performed before and after deplating to compare the changes in magnetic properties of the sintered NdFeB workpieces before and after deplating. MAX, MIN, and NOM respectively represent the maximum, minimum, and average magnetic flux values ​​in each tested sample; the magnetic flux before deplating represents the magnetic flux value of the sintered NdFeB workpiece before the deplating liquid is used to deplating the coating; the magnetic flux after deplating represents the magnetic flux value of the sintered NdFeB workpiece after the coating is deplated through the stripping line.

[0108] Magnetic attenuation refers to the average magnetic flux attenuation rate of the sintered NdFeB workpiece after vibration stripping, that is, magnetic attenuation = ((magnetic flux NOM before stripping) - (magnetic flux NOM after stripping))) / (magnetic flux NOM before stripping).

[0109] The test results of Examples 1-3 and Comparative Examples 1-3 are shown in Table 1 below.

[0110] Table 1

[0111]

[0112] As can be seen from Table 1, the average resistance R in Examples 1-3 is less than 5Ω, indicating good conductivity, clean surface without powder, and meeting the requirements for continued coating. However, R in Comparative Example 1 is 230Ω, with poor conductivity, but coating can continue, and the product film thickness CPK is low, indicating that the hanger state reduces the consistency of the film thickness. In Comparative Example 2, there is residue on the surface, and coating cannot continue, which does not meet the functional requirements.

[0113] The purpose of heating in the first chamber is mainly to volatilize and remove the organic solvent in the organic coating to make the coating brittle; the purpose of heating in the second chamber by using the second heating system is to calcine the organic matter in the organic coating of the magnet.

[0114] In Comparative Example 1, there is no heating step in the first chamber. From the data in Table 1, it can be seen that the average resistance R is relatively high, indicating poor conductivity, residual powder on the surface, the cleanliness level (Type B particles) is 13, and the cleanliness level (Type C particles) is 12, which means the cleanliness is relatively low, and the magnetic steel film thickness CPK after coating is relatively low.

[0115] In Comparative Example 2, there is no step of heating in the first chamber. From the data in Table 1, it can be seen that the surface is in an open circuit state, the organic coating on the surface is not effectively stripped off, and the requirement for continued coating cannot be met.

[0116] In Example 1-3, after the organic coating is stripped, the average magnetic flux attenuation rate of the magnetic steel is less than 1%. In Comparative Example 1-2, the average magnetic flux attenuation rate of the magnetic steel is also less than 1%, but higher than that of Example 1-3.

[0117] In comparative example 3, there is no vacuum treatment step, and the average magnetic flux attenuation rate of the magnetic steel is 5.2%, indicating that this vacuum treatment step can repair the magnetic steel (improve the appearance of defective products to qualified products) and improve the magnetic flux attenuation rate of the product. After treatment, the B-type particles on the surface of the magnetic steel are level 9, and the C-type particles are level 8. Although the surface cleanliness is good, the magnetic flux attenuation rate of the product is poor.

[0118] The tooling and / or magnetic steel after the stripping treatment of the present invention can be reused after simultaneous treatment, or can be reused after separate treatment, without affecting the conductivity of the tooling and the magnetic properties of the magnetic steel. For example, the magnetic steel of Example 1 can be used in combination with the powder spraying tooling of Example 2. In addition, the electrophoresis tooling after stripping of Example 1 is used to directly electrophoretically treat a new product, or the magnetic steel after stripping of Example 2 is used in combination with a new powder spraying tooling, both of which can obtain product performance equivalent to that of a new tooling and a new magnetic steel.

[0119] The above is only a preferred application implementation of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A continuous thermal cleaning furnace magnetic steel production line for stripping organic coatings, characterized in that: It includes a loading platform, a coating stripping module, a slightly acid cleaning module, an ultrasonic cleaning module, a drying module and a drying module which are sequentially connected to the loading platform through a track, and a control system for controlling the operation of each module; The coating stripping module includes at least one thermal cleaning furnace, which includes a first heating system, a second heating system, a combustion system, a powder collection system, an inlet and an outlet. The first heating system and the second heating system are in series and are relatively independently arranged in the first chamber and the second chamber respectively. The combustion system is arranged behind the first and second heating systems to process the decomposition gases of the first and second heating systems; the powder collection system is used to collect powders of the first and second heating systems; the inlet of the thermal cleaning furnace is connected to the track of the loading platform, and the outlet is connected to the slightly acid cleaning module; The heat cleaning furnace magnetic steel production line also includes a vacuum processing module, which has at least one vacuum high-temperature single-chamber furnace.

2. The hot cleaning furnace magnetic steel production line according to claim 1 is characterized in that: The powder collection system comprises a powder collection box, an exhaust fan and a powder extraction pipeline; A U-shaped collecting pipeline is provided at a middle position in the heat cleaning furnace, and a U-shaped opening of the U-shaped collecting pipeline is connected to the bottom of the heat cleaning furnace so that powder is scattered into the U-shaped tube; The fan pipeline of the exhaust fan is connected to the U-shaped collecting pipeline and the powder collecting box. When the exhaust fan is turned on, the powder in the heat cleaning furnace is cleaned into the powder collecting box through the U-shaped collecting pipeline and the fan pipeline.

3. The hot cleaning furnace magnetic steel production line according to claim 1 is characterized in that: The micro-acid cleaning module includes a cleaning tank and a filtering circulation system; the filtering circulation system is a bag filter, and the inlet and outlet of the filter are connected to the cleaning tank; the filtering circulation system is used to enhance the contact between the acid solution and the tooling / product, while removing solid impurities in the solution to increase the cleaning effect.

4. The hot cleaning furnace magnetic steel production line according to claim 1 is characterized in that: The ultrasonic cleaning module comprises an ultrasonic cleaning tank, a filtering circulation system and a vibration system; the vibration system is arranged outside the ultrasonic cleaning tank, and the inlet and outlet of the filtering circulation system are connected to the ultrasonic cleaning tank.

5. The hot cleaning furnace magnetic steel production line according to claim 1, characterized in that: The inlet and outlet of the heat cleaning furnace are gate-type closed structures that can be closed in time to reduce the heat dissipation of the heat cleaning furnace when passing through; the heat cleaning furnace cloth has a multi-stroke transmission chain, which is a multi-stroke bridge-type heat cleaning furnace.

6. A method for stripping an organic coating using a magnetic steel production line for a thermal cleaning furnace for stripping an organic coating continuously according to any one of claims 1 to 5, characterized in that: include: S10, placing the tooling and / or magnetic steel on the loading platform and sending them into the hot cleaning furnace through the hot cleaning furnace guide rail; S20, using a first heating system to heat the tooling and / or magnetic steel in the first chamber to volatilize and remove the organic solvent in the organic coating, making the coating brittle; Then, the tooling and / or magnetic steel are sent into the second chamber through the guide rail, and the tooling and / or magnetic steel are heated by the second heating system to calcine the organic matter in the organic coating of the magnet; after the gas decomposition products of the first and second heating systems enter the combustion system, the temperature in the combustion system is controlled at 800-1000℃, and after high-temperature treatment, they are converted into CO2 and water vapor and discharged through the chimney; S30, after the heating is completed, the guide rail automatically transports the loading tooling and / or magnetic steel out, and the tooling and / or magnetic steel use a hoist to sequentially hoist the loading platform into the slightly acid cleaning module, ultrasonic cleaning module, drying module and drying module for cleaning and drying; S40, cutting the tooling and / or magnetic steel, and the obtained tooling and / or magnetic steel can be coated again; After the magnetic steel and tooling are unloaded, the magnetic steel is placed in a vacuum treatment module for vacuum treatment. The vacuum degree in the furnace is controlled at 10*e -2 ~100Pa; treatment temperature is 400-700℃, treatment time is 200-300min; In step S20, the heating temperature in the first chamber is 180-250° C., and the heating time is 20-40 min; the heating temperature in the second chamber is 380-450° C., and the heating time is 150-200 min.

7. The method according to claim 6, characterized in that The vacuum degree in the furnace is controlled at 10*e -2 ~20Pa.

8. The method according to claim 6, characterized in that In step S20, the control system automatically controls the atmosphere in the furnace so that the oxygen content is not less than 18%, so that the organic matter on the surface of the product to be processed is gradually decomposed into gas.

9. The method according to claim 6, characterized in that The drying module includes a drying air knife, and the air temperature is controlled at 100-150°C during drying, and the drying time is 1-5 minutes; the drying module is a drying furnace, and the air temperature is controlled at 100-150°C during drying, and the drying time is 30-60 minutes; The cleaning tank of the slightly acid cleaning module is filled with a weak acid solution with a pH value of 5-6.5, and the weak acid solution is acetic acid or oxalic acid; the cleaning time is 5-20 minutes.

10. The method according to claim 6, characterized in that In step S30, after the loading tooling enters the ultrasonic cleaning module, the vibration motor drives the vibration frame and the loading tooling to vibrate, thereby enhancing the contact between the water washing liquid and the tooling / product, thereby enhancing the cleaning ability; the loading tooling after ultrasonic cleaning passes through the filtration circulation system to expand the concentration range of the surface material, and at the same time removes the solid impurities in the solution to increase the cleaning effect; the amplitude of the vibration of the loading tooling is 2-3mm.