Method for conditioning and hydrolyzing extruded films
By using co-extrusion technology and perfluorosulfonyl fluoride membrane pretreatment method in PEM electrolytic cells, the problem of high production cost of PEM electrolytic cells is solved, the ionic conductivity of the membrane and the efficiency of the electrolyzer are improved, and economical Efficient membrane pretreatment and electrolyzer performance improvement.
Patent Information
- Application Number
- CN202410397668.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-03
- Filing Date
- 2024-04-03
- Publication Date
- 2024-10-15
AI Technical Summary
The production cost of existing PEM electrolytic cells is high, and traditional planar stacking systems have limitations in improving cost and performance parameters, especially when using corrosion-sensitive electrodes, making it difficult to achieve cost-effective membrane pretreatment.
Tubular cells are fabricated through co-extrusion technology using multi-aqueous electrolyzers and fuel cells, using perfluorosulfonyl fluoride membranes for pretreatment, exchanging fluoride groups through sodium hydroxide, and using triethylsilanol to hydrolyze sulfonyl fluoride groups , improve the ionic conductivity of the membrane, and optimize the reaction parameters through measurement technology to improve the proton diffusion and stability of the membrane.
A method to reduce the production cost of PEM electrolytic cells in the presence of corrosion-sensitive electrodes is realized, which improves the ionic conductivity of the membrane and the efficiency of the electrolyzer, reduces production costs, and at the same time improves the functional performance of the electrolyzer.
Smart Images

Figure CN118773669A_ABST
Abstract
Description
Technical Field
[0001] The disclosed invention generally falls within the field of electrochemical batteries. More specifically, embodiments of the disclosed invention provide a method for conditioning and / or hydrolyzing extruded membranes. Background Art
[0002] Electrochemical cells, which can be planar, tubular, or monolithic in design, are the fundamental building blocks of electrochemical devices. Various designs have several drawbacks; for example, planar solid oxide fuel cells (SOFCs) have long start-up times, and tubular SOFCs have low volumetric power density. Electrochemical fuel cells generate direct current (DC) electricity by converting the chemical bond energy potential of the fuel into electrical energy. Currently, fuel cells are being researched as an alternative to traditional power plants and battery storage systems.
[0003] Electrical energy storage is crucial in the context of energy conversion, as renewable energy laws may jeopardize the technical and economic stability of the power grid due to the increasing production of renewable and inherently unstable energy sources. To absorb and release different types of energy across different timescales, multiple storage technologies must be integrated. Storage solutions must meet the requirements of high energy efficiency, low cost, and resource conservation. In addition to mechanical (compressed air, water column) and thermal storage options, electrochemical devices (batteries, electrolysis / fuel cells) are also an important component of these options.
[0004] Industrial water electrolysis is primarily carried out in two different types of batteries. In alkaline electrolytes, high currents can be generated using relatively inexpensive electrode materials, but this typically occurs at high overvoltages, leading to low energy efficiency and poor energy storage. Low overvoltages are feasible for PEM electrolysis, which is conducted under acidic conditions; however, this relies on the use of valuable metals such as platinum and iridium as catalysts. From an economic and raw material perspective, large-scale use is problematic.
[0005] Alkaline water electrolyzers are becoming more widely used in commercial applications, and proton exchange membrane water electrolyzers (PEMFEs) are gaining more attention due to their low gas cross-linking through the membrane, high conversion efficiency, fewer corrosion problems, and compact design. However, several challenges remain to be addressed. One of these is the high cost of conventional planar electrolyzers, stemming from the high cost of bipolar plates, porous transport layers, platinum group metal (PGM) catalysts, and membranes. A shift from planar to tubular cell geometry could be a strategy to reduce production and assembly costs.
[0006] Anodes and cathodes, two porous electrodes, and a dense solid electrolyte and / or membrane separating the electrodes are commonly used in batteries that constitute solid-state electrochemical devices.
[0007] The electrolysis apparatus described in WO2008 / 048103A1 includes an outer wall container vertically divided into four chambers connected in series, with electrodes placed in the first and last chambers. These chambers are separated from each other by a semi-permeable membrane, which is substantially permeable to cations and preferably substantially impermeable to polyvalent cations. However, gas diffusion is not addressed in WO2008 / 048103A1.
[0008] Document DE102016005144A1 describes a composite, which is a longitudinal device with a tubular cross-section, suitable as a building block of an electrochemical cell, and is formed of structural elements including or included by an inner electrode, which is a porous electrode or a gas diffusion layer, and wherein the structural elements in the contact region between the inner electrode and the included structural elements are shaped to form flow channels, or wherein the structural elements in the contact region between the outer electrode and the included structural elements are shaped to form flow channels. With structural elements having these shapes, the resistance along the composite is significantly reduced, and the voltage drop along the electrochemical cell is mitigated, which is generally detrimental during the use of the electrochemical cell.
[0009] Since hydrogen is used both as an energy carrier and a feedstock in the chemical industry, the combination of water electrolysis for producing hydrogen and oxygen with a fuel cell for repurposing the energy contained in fuel H2 in this invention is particularly economically attractive. Its unique added value stems from its dual functionality.
[0010] In this regard, reducing the production cost of PEM electrolytic cells is a goal pursued by many organizations using various strategies, but it has always been a steady increase in cost and performance parameters through the use of technical parameters available in conventional planar stacking systems. By utilizing a completely novel manufacturing method in the field of electrolysis technology, this invention aims to provide the possibility of an alternative method for membrane pretreatment that can be used in the presence of corrosion-sensitive electrodes (e.g., electrodes coated with catalysts in electrolyzers or fuel cells).
[0011] Therefore, based on the above discussion, there is an urgent need for a technical solution to overcome the aforementioned limitations. This disclosure focuses on a method for conditioning and / or hydrolyzing extruded membranes. Summary of the Invention
[0012] The following is a summary description of exemplary embodiments of the present invention. It is provided as a preamble to help those skilled in the art to more quickly understand the detailed design discussion that follows, and is not intended to limit in any way the scope of the claims appended herein specifically to point out the invention.
[0013] According to exemplary embodiments, this disclosure focuses on a method for separately conditioning pretreatment, such as hydrolysis, of extruded membranes. The extrusion of the membrane gives the electrolytic cell a tubular structure. After the extrusion process, the membrane must be pretreated to ensure its ionic conductivity. The proton conductivity of the membrane is essential for the efficiency of water electrolysis and the function of the electrolyzer.
[0014] According to one aspect of this disclosure, a method for conditioning / pretreatment / hydrolysis extruded membranes is disclosed. The method for pretreating the cation exchange membrane includes converting water into hydrogen using multiple water electrolyzers (WEs) and fuel cells, as well as flow batteries. The method also includes sealing half-cells of tubular cells manufactured via co-extrusion technology to achieve a higher electrode volume / membrane area ratio. The method further includes extruding a perfluorosulfonyl fluoride membrane from perfluorosulfonyl fluoride particles comprising polymers of perfluoropolymer chains substituted with sulfonyl fluoride groups. The method also includes using a pretreatment technique to increase the ionic conductivity of the extruded perfluorosulfonyl fluoride membrane prior to use in the electrolytic cell. The method further includes applying a milder pretreatment technique by activating SF bonds to perform nucleophilic exchange of fluoride groups. The method also includes hydrolyzing the sulfonyl fluoride groups to sulfonic acid using triethylsilanol.
[0015] In one embodiment of the invention, the perfluorosulfonyl fluoride membrane is industrially pretreated and sodium hydroxide is used to exchange the fluoride groups for hydroxyl groups.
[0016] In one embodiment of the invention, when the perfluorosulfonyl fluoride membrane is industrially pretreated, the sodium sulfonate groups are protonated by storing the perfluorosulfonyl fluoride membrane in 1M sulfuric acid.
[0017] In one embodiment of the present invention, the industrially pretreated perfluorosulfonyl fluoride membrane includes multiple parameters, such as, but not limited to, proton diffusion, in-plane conductivity, ion exchange capacity, water absorption rate, etc.
[0018] In one embodiment of the invention, the method includes using measurement techniques to calculate parameters such as water absorption rate, swelling factor, and ion exchange capacity.
[0019] In one embodiment of the present invention, the measurement technique includes Raman spectroscopy, nuclear magnetic resonance (NMR) technique, etc.
[0020] In one embodiment of the invention, the method further includes transferring fluoride ions from a strong covalent bond to a leaving group, which, when a catalyst is used, is achieved by reacting with H+. + and / or R3Si + It is assisted by the interaction of the two.
[0021] In one embodiment of the invention, the catalyst comprises triethylsilane in the presence of 1,8-diazabicyclo(5.4.0)undec-7-ene (DBU).
[0022] In one embodiment of the invention, the reaction is a sulfur(VI)-fluoride exchange (SuFEx), which involves the exchange of fluoride groups to form silanyl esters and release F. - And deprotected esters to obtain sulfonic acid groups.
[0023] In one embodiment of the present invention, the method includes optimizing a plurality of reactants.
[0024] In one embodiment of the invention, the perfluorosulfonyl fluoride membrane is conditioned / treated for a predetermined conditioning time at room temperature with an optimized reactant concentration.
[0025] In one embodiment of the invention, the predetermined conditioning time is increased at 24-hour intervals, and after each interval, the perfluorosulfonic acid (PFSA) membrane is stored in water for 24 hours and then in 1M H2SO4 for another 24 hours.
[0026] According to an embodiment of the present invention, the method includes hydrolyzing a perfluorosulfonyl fluoride membrane with a certain concentration of reactants to adjust the perfluorosulfonyl fluoride membrane.
[0027] In one embodiment of the invention, the method includes hydrolyzing a perfluorosulfonyl fluoride membrane in Et3SiOH and storing it in a 1M H2SO4 solution until the measured conductivity is higher than 90 mS / cm.
[0028] In one embodiment of the invention, the method includes measuring the conductivity of the perfluorosulfonic acid membrane.
[0029] In one embodiment of the present invention, co-extrusion technology includes simple extrusion, multilayer extrusion, fabric extrusion, etc.
[0030] In one embodiment of the invention, the method includes optimizing hydrolysis reaction parameters and evaluating the stability of the half-cell.
[0031] These and other advantages will be apparent from the embodiments described herein in this application.
[0032] The preceding is a simplified summary of the invention to provide an understanding of some embodiments of the invention. This summary is neither a broad nor an exhaustive overview of the invention and its various embodiments. It presents selected concepts of embodiments of the invention in a simplified form as an introduction to the more detailed description that follows. As will be understood, other embodiments of the invention may utilize one or more features set forth above or described in detail below, either alone or in combination. Attached Figure Description
[0033] To more clearly describe the embodiments of this disclosure or the technical solutions in the prior art, the accompanying drawings required for the embodiments or the prior art are briefly described below. Obviously, the drawings in the following description only illustrate some embodiments of this disclosure, and those skilled in the art can derive other implementations from these drawings without creative effort. All embodiments or implementations should fall within the protection scope of this disclosure.
[0034] Figure 1A A perspective view of a tubular water electrolysis cell for generating hydrogen and oxygen according to an embodiment of the present invention is shown.
[0035] Figure 1B Another perspective view of a tubular water electrolysis cell according to an embodiment of the invention disclosed herein is shown;
[0036] Figure 2 A top view showing a SEM image of a porous anodic electrode of a tubular water electrolysis cell for generating hydrogen and oxygen according to an embodiment of the invention disclosed herein;
[0037] Figure 3A A cross-sectional view of a porous anodic electrode of a tubular water electrolysis cell for generating hydrogen and oxygen according to an embodiment of the invention disclosed herein is shown.
[0038] Figures 3B to 3C Images of the membrane before (left) and after (right) Raman measurements according to one or more embodiments of the invention disclosed herein are shown;
[0039] Figure 3D An H-cell (H-cell) for measuring proton diffusion of an extruded membrane according to an embodiment of the invention disclosed herein is shown.
[0040] Figure 4 Perspective views of various components of a PEME water electrolyzer according to embodiments of the invention disclosed herein are shown; and
[0041] Figure 5 A flowchart is shown of a method for conditioning and / or hydrolyzing an extruded membrane according to an embodiment of the invention disclosed herein.
[0042] Electrochemical cell systems and methods for conditioning and / or hydrolyzing extruded membranes are illustrated in the accompanying drawings, in which the same reference numerals denote corresponding parts. It should be noted that the drawings are intended to illustrate exemplary embodiments of the present disclosure. These drawings are not intended to limit the scope of the disclosure. It should also be noted that these drawings are not necessarily drawn to scale. Detailed Implementation
[0043] Those skilled in the art will recognize that variations and modifications can be made to this disclosure other than those specifically described. It should be understood that this disclosure includes all such variations and modifications. This disclosure also includes all such steps, features, compositions, and compounds individually or collectively mentioned or indicated in this specification, as well as any and all combinations of any one or more of these steps or features.
[0044] For convenience, specific terms and embodiments used in this specification are compiled herein before further description of this disclosure. These definitions should be read in accordance with the remainder of this disclosure and as understood by those skilled in the art. The terms used herein have meanings recognized and known to those skilled in the art; however, for convenience and completeness, specific terms and their meanings are listed below.
[0045] The articles “a,” “one,” and “the” are used to refer to one or more (i.e., at least one) articles.
[0046] The terms “comprising” and “including” are used in an inclusive, open-ended sense, meaning that additional elements may be included. It should not be construed as “consisting only of…”. In this specification, unless the context otherwise requires, the word “comprising” and variations such as “including” and “containing” will be understood to imply the inclusion of the stated element or step or group of elements or steps, but do not exclude any other element or step or component or group of steps.
[0047] The term "including" is used to mean "including but not limited to". "Including" and "including but not limited to" are used interchangeably.
[0048] Anodizing is a commonly used method in industry for nanostructuring.
[0049] In this invention, for convenience, SEM and scanning electron microscope can be used interchangeably.
[0050] In this invention, for convenience, PEM and polymer electrolyte membranes can be used interchangeably.
[0051] In this invention, for convenience, inductively coupled plasma atomic emission spectrometry and ICP-OES can be used interchangeably.
[0052] In this invention, for convenience, IEC and ion exchange chromatography can be used interchangeably.
[0053] In this invention, for convenience, polytetrafluoroethylene and PTFE can be used interchangeably.
[0054] In this invention, for convenience, DMF and dimethylformamide can be used interchangeably.
[0055] In this invention, for convenience, the following abbreviations can be used interchangeably:
[0056] XRD for X-ray powder diffraction
[0057] TEM for transmission electron microscopy
[0058] EDX for Energy Dispersive X-ray Analysis
[0059] AFM for atomic force microscopy
[0060] BET for Bruno Emmett Teller
[0061] GC-MS for gas chromatography-mass spectrometry
[0062] ICP-MS for Inductively Coupled Plasma Mass Spectrometry
[0063] AAS for atomic absorption spectroscopy
[0064] TOC (Total Organic Carbon)
[0065] IC for ion chromatography
[0066] ADL for electrocatalytic active materials
[0067] PFSA for perfluorosulfonic acid
[0068] Figure 1A A perspective view of a tubular water electrolysis cell 100 for generating hydrogen and oxygen according to an embodiment of the present invention is shown. The tubular water electrolysis cell 100 includes an external current collector 1, an external electrode 2, an ion exchange membrane 3, an internal electrode 4, an internal current collector 5, etc.
[0069] According to an embodiment of the present invention, the tubular battery 100 may further include an external current collector 1 defining an outer region of the tubular electrochemical battery 100. The external current collector 1 may include an elongated hollow portion for including an external electrode 2 having multiple physical, chemical, and mechanical parameters. Using additive manufacturing 102, the external electrode 2 is molded, such as... Figure 1B shown.
[0070] Additive manufacturing 102 can allow the fabrication of porous metal outer electrodes 2 and inner electrodes 4 with configurable microstructures, macrostructures, and regular constructions, as well as three-dimensional porous structures suitable for desired voltage distributions.
[0071] According to embodiments of the present invention, multiple physical, chemical, and mechanical parameters include high porosity, large active reaction area, water and air permeability for transporting reactants and reaction products, high electrical and thermal conductivity, good corrosion resistance, and sufficient strength and dimensional stability under certain flow pressure.
[0072] Additionally, the external current collector 1 includes an ion exchange membrane 3 for exchanging ions from the external electrode to the internal electrode 4 within an internal region. The ion exchange membrane 3 can be disposed within the inner cavity of the external electrode 2, directly on the internal electrode 4, using various extrusion techniques.
[0073] Now refer to Figure 2 , Figures 3A to 3D Various embodiments of the present invention are described.
[0074] Figure 2 A top view 200 shows a SEM image of a porous anodized electrode of a tubular water electrolysis cell 100 for generating hydrogen and oxygen according to an embodiment of the present invention. In particular, planar high-purity metal samples can be anodized under precise temperature and potential control to form correspondingly virtually flawless cylindrical hole shapes and arrangements. Furthermore, anodizing can be used for the first time for structural titanium workpieces.
[0075] In one or more embodiments of the present invention, the diameter and length of the pores formed on the outer electrode 2 and the inner electrode 4 can be adjusted. Furthermore, using atomic layer deposition (ALD) 104, the inner pore walls of the outer electrode 2 and the inner electrode 4 can be uniformly coated with a thin (20 nm) to ultrathin (2 nm) layer of electrocatalytic active material, as well as... Figure 3A As shown. Atomic layer deposition (ALD) has an extraordinary ability to uniformly cover even deep pores by using oxides, sulfides and / or any other noble metals and electrocatalytically active materials.
[0076] In an exemplary scenario, a tubular geometry is used for PEM fuel cells. Specifically, in tubular cells, only half of the cell is sealed at the end, resulting in a high electrode volume to membrane area ratio. Furthermore, the half-cell can be manufactured in a single step via a co-extrusion process, allowing for continuous industrial cell production and reducing the number of components required for stacking assembly processes.
[0077] According to an embodiment of the present invention, in a co-extrusion process, the perfluorosulfonyl fluoride membrane is extruded from perfluorosulfonyl fluoride particles. Furthermore, the perfluorosulfonyl fluoride membrane undergoes pretreatment before being used as an ion exchange membrane.
[0078] According to one embodiment of the invention, for industrial pretreatment, sodium hydroxide is used to exchange fluoride groups for hydroxyl groups. Subsequently, the sodium sulfonate groups are protonated by storing the membrane in 1M sulfuric acid.
[0079] The following reactions occur:
[0080]
[0081] To fabricate tubular batteries, the membrane is extruded onto a tubular electrode, which is fabricated in the example of TiAIV coated with a catalyst. These materials can corrode during sodium hydroxide pretreatment. A milder pretreatment process may be needed to hydrolyze the stable SF bonds in the membrane to withstand harsh reaction conditions. The stable SF bonds can be activated in the presence of a suitable catalyst, and the fluoride groups can undergo nucleophilic exchange in a reaction known as sulfide (VI)-fluoride exchange (SuFEx). This reaction—click chemistry—has been used in polymer chemistry to build the core backbone of polymers and functionalize monomers as side chains, providing post-polymerization modification of the polymer.
[0082] In the presence of a sufficient catalyst, fluoride ions react with H+. + and / or R3Si + The interaction between the strong covalent bond and the leaving group is transferred.
[0083] Therefore, in this invention, in order to achieve hydrolysis using less corrosive chemicals, triethylsilane is used as a catalyst in the presence of 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU). The reaction is a two-step reaction, wherein the first step is the formation of an intermediate, and the second step is the protonation of this intermediate to obtain the desired sulfonic acid group. The feasibility of hydrolyzing sulfonyl fluoride groups to sulfonic acids using a less aggressive method with triethylsilane is shown in the following reaction:
[0084]
[0085] In particular, the pretreated membrane is characterized by ensuring good proton diffusion, in-plane conductivity, ion exchange capacity, water absorption and stability of the co-extruded half-cell during the pretreatment process.
[0086] According to an embodiment of the invention, a tubular cation exchange membrane is manufactured by extruding VM-Fumasep FFT (FumaTech BWT), a perfluorosulfonyl fluoride / PTFE copolymer granular material with a particle size of 2 mm. To hydrolyze the sulfonyl fluoride groups, N,N-dimethylformamide (DMF ≥ 99.9%, UV / IR grade, Carl Roth GmbH), DBU (> 99%, Sigma Aldrich), triethylsilanol (97%, Thermo Scientific), and sodium hydroxide (10%, Carl Roth GmbH) are used. For protonation, 1M sulfuric acid (diluted from 75% sulfuric acid, pure, Carl Roth GmbH) is used. Alternatively, ultrapure water can be used. Ultra, Elga LabWater).
[0087] In embodiments of the present invention, the hydrolysis of the sulfonyl fluoride group is carried out via the SuFEx reaction (reaction 2). Specifically, the membrane is stored in a solution containing Et3SiOH, DBU, and DMF at 70°C with shaking at 200 rpm for 24 hours. The membrane is then washed with water and stored in water at room temperature for 24 hours. The water is changed at least three times during storage. Additionally, the membrane is protonated in 1M sulfuric acid at room temperature and 60 rpm for 24 hours and stored overnight in 1M sulfuric acid at room temperature. The membrane is then dried at 80°C for 5 hours and weighed to obtain the dry weight. The water absorption rate is calculated using the following equation:
[0088] W uptake (%) = [(W) wet -W dry ) / W dry ]×100, where:
[0089] W wet -Wet mass of the membrane
[0090] W dry - Quality after drying
[0091] In addition, the membrane was stored in 0.5 M NaCl solution at room temperature for 24 hours to allow all protonated sulfonic acid groups to exchange with sodium cations. Then, the membrane was stored in 1 M sulfuric acid for 24 hours, and the final Na+ concentration was measured by inductively coupled plasma optical emission spectrometry (ICP-OES). + Concentration. IEC uses the following equation for calculation:
[0092]
[0093] in,
[0094] [Na] is the sodium concentration in mg / L, measured using ICP-OES.
[0095] V H2SO4 This is the volume of 1M sulfuric acid used in heavy protonation membranes, in liters (L).
[0096] W dry It is the dry mass of the membrane, in grams.
[0097] Mw Na This is the molar mass of sodium, expressed in mg / mmol.
[0098] In embodiments of the present invention, the ion exchange membrane 3 may include a polymer electrolyte membrane (PEM).
[0099] In an embodiment of the invention, the membrane was subjected to Raman spectroscopy after being stored overnight in 1M sulfuric acid at room temperature. Measurements were performed using a sample holder with a water reservoir, thus maintaining membrane hydration. A confocal microscopy Raman spectrometer (Invia Reglex, Renishaw, Kingswood, UK) was used, with a laser beam (He-Ne, 633nm, 0.85mW) focused through a 50x objective lens (DM 2500, Leica, Mannheim, Germany) having a 1mm spot size and a high-resolution diffraction grating density of 1800 grooves mm⁻¹. Individual spectra were acquired by integrating 50 spectra over an integration time of 10 s. To determine thermal degradation of the membrane, images were collected before and after image acquisition, as shown in the image. Figure 3B and Figure 3C shown.
[0100] refer to Figure 3D and Figure 3D Proton diffusion was measured using an H-cell, in which two compartments are separated by a membrane. The membrane was cut, enrolled, and sandwiched between two PTFE gaskets. The usable surface area of the membrane was 0.196 cm². 2 The sealing area is specified by the gasket. One compartment is filled with 0.1M HCl, and the other compartment is filled with 0.5M NaCl. Due to H... + Different concentrations of protons result in diffusion from high-concentration compartments to low-concentration compartments. After increasing the proton concentration in the NaCl compartment, the pH value was measured over 30 minutes, and the proton diffusion of the membrane was calculated using an equation.
[0101] JH d =n B / A·t.
[0102] Among them, J H d It is proton diffusion, with units of μmol / cm. 2 min,
[0103] n B This represents the increase in proton concentration in the NaCl compartment, measured in μmol.
[0104] A is the area of the membrane, in cm². 2 ,as well as
[0105] t is time, measured in seconds (s).
[0106] Before measuring in-plane conductivity, the membrane was protonated overnight in sulfuric acid at room temperature and washed several times with water to remove sulfuric acid residue. A four-electrode MK3 cell (FUMATECH BWT) was used, with the membrane placed on the four platinum electrodes of the probe tip and the probe tip cap placed on the membrane, with the insulating PTFE (Teflon) side of the cap facing the sample. The cap was manually secured using two screws. To prevent membrane dehydration, the cell was immersed in softened water at room temperature. A Gamry potentiostat (Gamry Reference 3000 potentiostat / galvanostat / ZRA) was used at 1000 Hz, open-circuit voltage, and 10 mV amplitude. Proton conductivity was calculated using the equation σ = L / W·T·R, where σ is the in-plane conductivity in S / cm, L is the distance between electrodes in cm, B is the membrane width in cm, D is the membrane thickness in cm, and R is the resistance in Ohms.
[0107] In a preferred embodiment of the invention, stability tests were performed on the co-extruded half-cell using optimized hydrolysis reaction parameters. The reactant concentrations and reaction durations were varied until the optimal proton conductivity was achieved. First, the reactants were optimized, and the concentrations used are listed in Table 1:
[0108] Table 1: Relationship between the concentration of different reactants and different parameters
[0109]
[0110] Using 5 mL of DMF as a solvent, the reaction was carried out at 70 °C and 200 rpm for 24 hours, and the measured conductivity was compared with that of the commercial PFSA planar membrane Fumasep F10100 (FumaTech BWT). The conductivity obtained with the membrane for 1 day was comparable to that of the commercial membrane. Therefore, these reactant concentrations (1 equivalent of membrane, 1 equivalent of Et3SiOH, and 1 equivalent of DBU) were used.
[0111] Table 2 shows the reproducibility of the results. Two extruded membranes were adjusted to optimal reactant concentrations (1 equivalent of membrane, 1 equivalent of Et3SiOH, and 1 equivalent of DBU), and their proton conductivity was measured and compared with that of the sample at day 1. The conductivity of the three membranes hydrolyzed with the same reactant concentrations was also measured. Since the standard deviation is 3%, it can be concluded that the hydrolysis reaction has sufficient reproducibility.
[0112] Table 2: Reproducibility Study of Membrane Pretreatment
[0113] membrane thickness Conductivity name μm mS / cm 1d 50 94 2a 50 96 2b 50 90
[0114] The hydrolysis reaction was carried out by pretreating the membrane with an optimized reactant concentration at room temperature. The settling time was increased in 24-hour intervals. After each interval, the membrane was stored in water for 24 hours, then in 1 M H₂SO₄ for another 24 hours, after which the conductivity was measured, and the membrane was stored in the same solution for another 24 hours. The reaction time was increased until the conductivity > 90 mS / cm. Table 3 shows the reaction time and membrane conductivity, respectively.
[0115] Table 3: Reaction time and membrane conductivity under optimized reaction time parameters
[0116]
[0117] In one embodiment of the invention, the stability test of the co-extruded half-cell includes physicochemical characterization. All membranes are characterized after the hydrolysis reaction to ensure that their physicochemical properties are regulated. The water absorption swelling factor and ion exchange capacity are calculated, and Raman and NMR measurements are performed.
[0118] The ion exchange membrane 3 may include a tubular membrane welded or extruded to the internal electrode 4, as shown in Figure 1 and Figure 4 shown.
[0119] According to embodiments of the present invention, multiple extrusion technologies include simple extrusion, multilayer extrusion, fabric extrusion, etc.
[0120] The internal electrode 4 may include a first end and a second end molded by additive manufacturing 102. In an embodiment of the invention, the internal electrode 4 includes a Ti-Fleece GDE.
[0121] The outer current collector 1 and the inner current collector 5 can further utilize various extrusion technologies to manufacture the tubular water electrolysis battery 100 based on extrusion.
[0122] The external electrode 2 and the internal electrode 4 may include porous external electrode 2 and internal electrode 4, which have an effective active surface area for increasing electrochemical reactions, depending on the open porosity and pore size.
[0123] The outer electrode 2 and the inner electrode 4 may include varying geometric parameters of the holes and coating.
[0124] In one embodiment of the invention, the diameter and length of the holes formed on the outer electrode 2 and the inner electrode 4 can be adjustable. Furthermore, the inner walls of the holes on the outer electrode 2 and the inner electrode 4 can be uniformly coated with a thin (<20 nm) to ultrathin (<2 nm) electrocatalytic active material layer by means of atomic layer deposition (ALD) 104.
[0125] The tubular electrochemical cell 100 also includes an internal current collector 5 embedded in the surrounding wall of the longitudinally extending internal electrode 4. Furthermore, the internal current collector 5 may extend through the first and second ends of the internal current electrode 4.
[0126] Furthermore, as additional components of this battery, the inner current collector 5 and the outer current collector 1 can also be produced by extrusion 106, which could potentially greatly simplify the manufacturing of the tubular water electrolysis battery 100.
[0127] Figure 4 A perspective view of the various components of a PEM water electrolyzer according to an embodiment of the present invention is shown. One half-cell, serving as the flow electrode, is formed by a tubular membrane electrode assembly made of titanium hollow fibers and titanium nonwoven fabric, respectively. The other half-cell is made of graphite felt. Besides a simple arrangement with flow channels, a titanium flow field with multiple initiating spirals can also be used. The two half-cells are separated by a tubular ion exchange membrane.
[0128] Figure 5 A flowchart of method 500 for conditioning and / or hydrolyzing an extruded membrane according to an embodiment of the present invention is shown.
[0129] At point 502, multiple water electrolyzers (WEs) are used to convert water into hydrogen.
[0130] At 504, the half-cell of the tubular battery 100 manufactured by co-extrusion technology is sealed to obtain a higher electrode volume ratio per unit film area.
[0131] At position 506, a perfluorosulfonyl fluoride membrane is extruded from the perfluorosulfonyl fluoride particles. In one embodiment of the invention, the perfluorosulfonyl fluoride membrane is industrially pretreated, and sodium hydroxide is used to exchange the fluoride groups for hydroxyl groups. When the perfluorosulfonyl fluoride membrane is industrially pretreated, the sodium sulfonate groups are protonated with 1M sulfuric acid.
[0132] At point 508, a pretreatment technique is used to increase the ionic conductivity of the extruded perfluorosulfonyl fluoride membrane before using the perfluorosulfonate membrane as a cation exchange membrane.
[0133] At 510, a milder pretreatment technique is applied by activating the SF bond to perform nucleophilic exchange of the fluoride group. According to one embodiment of the invention, the reaction can be a sulfur(VI)-fluoride exchange (SuFEx) involving the exchange of the fluoride group. Alternatively, storage in sulfuric acid can include deprotection of the ester to obtain a sulfonic acid group.
[0134] At position 512, triethylsilyl alcohol is used to hydrolyze the sulfonyl fluoride group into a sulfonic acid group.
[0135] In one embodiment of the present invention, the industrially pretreated perfluorosulfonic acid (PFSA) perfluorosulfonyl fluoride membrane includes multiple parameters, such as, but not limited to, proton diffusion, in-plane conductivity, ion exchange capacity, water absorption rate, etc.
[0136] In one embodiment of the invention, method 500 further includes calculating parameters such as water absorption rate, expansion factor, and ion exchange capacity using measurement techniques. According to embodiments of the invention, the measurement techniques may include Raman spectroscopy, nuclear magnetic resonance (NMR) techniques, etc.
[0137] In one embodiment of the invention, the method further includes the transfer of fluoride ions from a strong covalent bond to a leaving group, which, when a catalyst is used, is achieved through interaction with H+. + and / or R3Si + The interaction between the catalyst and the surrounding environment is aided by the catalyst. In the presence of 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), the catalyst contains triethylsilanol.
[0138] According to one embodiment of the invention, method 500 may include optimizing a plurality of reactants. The perfluorosulfonyl fluoride membrane is conditioned at room temperature with optimized reactant concentrations for a predetermined conditioning time. In embodiments of the invention, the predetermined conditioning time is increased at 24-hour intervals, and after each interval, the pretreated perfluorosulfonyl fluoride membrane is stored in water for 24 hours and then in 1M H₂SO₄ for another 24 hours.
[0139] Although the invention has been described in conjunction with what are now considered to be the most practical and various embodiments, it will be understood that the invention is not limited to the disclosed embodiments, but rather is intended to cover various modifications and equivalent arrangements included within the scope of the appended claims.
[0140] Those skilled in the art will recognize that, based on the examples described in the embodiments disclosed in this specification, the units and algorithm steps can be implemented by electronic hardware, computer software, or a combination thereof.
Claims
1. A method (500) for conditioning and / or hydrolyzing an extruded film, the method comprising: The ion exchange process is carried out in a separate electrochemical cell using a cation exchange membrane; as well as Pretreatment of perfluorosulfonyl fluoride membranes extruded from particles of a polymer comprising perfluorinated polymer chains substituted with sulfonyl fluoride groups; Using a pretreatment technique to increase the ionic conductivity of the extruded perfluorosulfonyl fluoride membrane; applying the pretreatment technique by activating SF bonds to perform nucleophilic exchange of fluoride groups of the extruded membrane in a reaction of hydrolyzing the sulfonyl fluoride groups to sulfonic acid using triethylsilanol; comprising optimizing the concentration of reactants and the duration of said reaction to obtain a polymer comprising perfluorinated polymer chains substituted with sulfonic acid groups; as well as As a cation exchange membrane, a perfluorosulfonic acid membrane comprising said polymer having perfluorinated polymer chains substituted with sulfonic acid groups is used.
2. The method (500) of claim 1, wherein the preprocessing technique further calculates proton diffusion, in-plane conductivity, ion exchange capacity, water absorption, or any combination thereof.
3. The method (500) of claim 2, wherein the method (500) comprises calculating the parameters, such as water absorption, expansion factor and the ion exchange capacity, using measurement techniques.
4. The method (500) of claim 3, wherein the measurement technique comprises Raman spectroscopy, nuclear magnetic resonance (NMR) technique, or any combination thereof.
5. The method (500) of claim 1, wherein the method (500) further comprises: + and / or R3Si + The hydrolysis of fluoride ions is assisted by the interaction of the hydrolysis catalyst.
6. The method (500) of claim 5, wherein the catalyst comprises triethylsilanol in the presence of 1,8 diazabicyclo[5.4.0]undecene-7-ene (DBU).
7. The method (500) of claim 1, wherein the reaction is a sulfur (VI)-fluoride exchange (SuFEx), comprising: The fluoride group is exchanged to form an intermediate, and the intermediate is protonated to obtain the sulfonic acid group.
8. The method (500) of claim 7, wherein the perfluorosulfonyl fluoride membrane is pre-treated at room temperature for a predetermined conditioning time.
9. The method (500) of claim 8, wherein the predetermined pretreatment time is increased in intervals of 24 hours and after each interval, the pretreated perfluorosulfonyl fluoride membrane is stored in water for 24 hours and in 1 M H2SO4 for another 24 hours.
10. The method (500) of claim 1, wherein the method (500) comprises hydrolyzing the perfluorosulfonyl fluoride membrane with a concentration of reactants for pretreating the perfluorosulfonyl fluoride membrane to obtain increased conductivity.
11. The method (500) of claim 1, wherein the method (500) comprises measuring the conductivity of the hydrolyzed perfluorosulfonic acid (PFSA) membrane.
12. The method (500) of claim 1, wherein the method (500) comprises storing the hydrolyzed perfluorosulfonic acid (PFSA) membrane in water and a 1M H2SO4 solution, and measuring the conductivity of the hydrolyzed perfluorosulfonic acid membrane until the conductivity is greater than 90 mS / cm.
13. The method (500) according to claim 1, wherein the co-extrusion technology comprises simple extrusion, multi-layer extrusion, fabric extrusion or any combination thereof.
14. The method (500) of claim 1, wherein the method (500) comprises physicochemically characterizing the hydrolyzed perfluorosulfonic acid (PFSA) membrane by calculating the water absorption expansion factor and ion exchange capacity of the hydrolyzed perfluorosulfonic acid (PFSA) membrane and measuring Raman and NMR of the hydrolyzed perfluorosulfonic acid (PFSA) membrane, thereby performing stability testing on the co-extruded half-cell.