High-speed copper plating solution for solid welding wire and copper plating process of high-speed copper plating solution
By optimizing the copper plating solution formula and electroplating process parameters, the copper plating speed and corrosion resistance of the welding wire are improved, and the problems of slow copper plating speed and insufficient corrosion resistance in the existing technology are solved.
Patent Information
- Application Number
- CN202411036434.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-15
AI Technical Summary
The existing welding wire copper plating technology has a slow copper plating speed, which affects the processing efficiency, and the corrosion resistance of the coating is insufficient.
A high-speed copper plating solution, including specific proportions of water-soluble copper salts, brighteners, levelers, additives, inhibitors, and accelerators, was designed for solid metal plating by optimizing electroplating process parameters such as current density and plating temperature. The welding wire undergoes high-speed replacement copper plating.
Significantly improves the plating rate, tensile strength and corrosion resistance of the welding wire.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper plating solutions, and in particular to a high-speed copper plating solution for solid welding wire and a copper plating process thereof. Background Art
[0002] At present, the processing of welding wire is to use special metal strips with thicker diameters and then make them into thinner welding wires of various specifications through a series of drawing. In order to prevent rust and improve the conductivity of the welding wire, the welding wire needs to be copper-plated.
[0003] For example, Chinese patent CN108165959B proposes a chemical copper plating solution, which includes a water-soluble copper salt, a reducing agent, a complexing agent, a leveling agent, a buffer, a stabilizer, a surfactant, and deionized water; wherein, by weight, the deionized water is 1000 parts, the water-soluble copper salt is 20-35 parts, the reducing agent is 15-32 parts, the complexing agent is 10-20 parts, the leveling agent is 5-15 parts, the buffer is 2-12 parts, the stabilizer is 1-15 parts, and the surfactant is 0.01-0.2 parts; the water-soluble copper salt is selected from one or more of copper sulfate, copper chloride, copper nitrate, and copper methanesulfonate.
[0004] However, in the above patent, the copper plating speed is relatively slow, which affects the processing efficiency of the entire welding wire; and the corrosion resistance of the coating needs to be improved.
[0005] Based on this, the present invention designs a high-speed copper plating solution for solid welding wire and a copper plating process thereof to solve the above problems. Summary of the invention
[0006] In view of the above-mentioned shortcomings of the prior art, the present invention provides a high-speed copper plating solution for solid welding wire and a copper plating process thereof.
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0008] A high-speed copper plating solution for solid welding wire;
[0009] The high-speed copper plating solution includes 32-46 parts of water-soluble copper salt, 5-8 parts of brightener, 20-27 parts of leveler, 4-12 parts of additive, 3-6 parts of inhibitor, 2-5 parts of accelerator, and 900 parts of deionized water;
[0010] The additive is a mixture of 2-thiazoline polydithiopropane sulfonate sodium and N,N-dimethyldithioformamide propane sulfonate sodium;
[0011] The accelerator is selected from one or both of piperazine-1,4-dithiocarboxylic acid potassium salt and 2,3-dimercaptopropanesulfonic acid sodium salt.
[0012] Furthermore, the water-soluble copper salt is composed of a mixture of copper sulfate and copper nitrate; and the molar ratio of the copper sulfate to the copper nitrate is (20-40):(4-8).
[0013] Furthermore, the mass ratio of the 2-thiazoline polydithiopropane sulfonate sodium and the N,N-dimethyldithiocarboxamide propane sulfonate sodium is (2-3): (3-5).
[0014] Furthermore, the leveling agent is selected from one or more of butynediol, hydroxypropyl propargyl ether, and butynediol diethoxy ether.
[0015] Furthermore, the brightener is selected from one or more of 2-mercaptothiazoline, bisbenzenesulfonimide, and sodium polyanisole sulfonate.
[0016] Furthermore, the inhibitor is a mixture of polyethylene glycol and sodium chloride.
[0017] Furthermore, the mass ratio of polyethylene glycol to sodium chloride is (25-32):(16-24).
[0018] A high-speed copper plating process for solid welding wire, wherein the surface of the solid welding wire is roughened and then preheated to 50-65° C., and the high-speed copper plating solution is used to perform high-speed displacement copper plating on the solid welding wire;
[0019] The current density is 13-16A / dm 2 , the electroplating temperature is 68-75℃.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The present invention significantly improves the electroplating rate, tensile strength and corrosion resistance of the welding wire by optimizing various parameters of the electroplating process and optimizing the formula of the copper plating solution. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Embodiment 1
[0024] This embodiment provides a copper plating process for a solid welding wire, comprising the following steps:
[0025] Step 1: preparing a high-speed copper plating solution;
[0026] Weigh the raw material: 46 kg of a mixture of copper sulfate and copper nitrate; the molar ratio of copper sulfate to copper nitrate is 40:8;
[0027] 8kg brightener: 2-mercaptothiazoline, bisbenzenesulfonimide, sodium polyanisole sulfonate;
[0028] 27kg leveling agent: butynediol, hydroxypropyl propargyl ether, butynediol diethoxy ether;
[0029] 12kg additives: sodium 2-thiazoline polydithiopropane sulfonate and sodium N,N-dimethyldithiocarboxamide propane sulfonate in a mass ratio of 3:5;
[0030] 6kg inhibitor: polyethylene glycol and sodium chloride in a mass ratio of 32:24;
[0031] 5kg accelerator: piperazine-1,4-dithiocarboxylate potassium salt;
[0032] 900kg deionized water;
[0033] The solid wire surface was roughened and preheated to 65°C. The high-speed copper plating solution was used at a current density of 16A / dm 2 , high-speed displacement copper plating was performed on solid welding wire at an electroplating temperature of 75°C.
[0034] Embodiment 2
[0035] This embodiment provides a copper plating process for a solid welding wire, comprising the following steps:
[0036] Step 1: preparing a high-speed copper plating solution;
[0037] Weigh the raw materials: 32 kg of a mixture of copper sulfate and copper nitrate; the molar ratio of copper sulfate to copper nitrate is 20:4;
[0038] 5kg brightener: 2-mercaptothiazoline;
[0039] 20kg leveling agent: butynediol diethoxy ether;
[0040] 4kg additives: sodium 2-thiazoline polydithiopropane sulfonate and sodium N,N-dimethyldithiocarboxamide propane sulfonate in a mass ratio of 2:3;
[0041] 3kg inhibitor: polyethylene glycol and sodium chloride in a mass ratio of 25:16;
[0042] 2kg accelerator: 2,3-dimercaptopropanesulfonic acid sodium salt;
[0043] 900kg deionized water;
[0044] The solid wire surface was roughened and preheated to 50°C. The high-speed copper plating solution was used at a current density of 13A / dm 2 , high-speed displacement copper plating was performed on solid welding wire at an electroplating temperature of 68°C.
[0045] Embodiment 3
[0046] This embodiment provides a copper plating process for a solid welding wire, comprising the following steps:
[0047] Step 1: preparing a high-speed copper plating solution;
[0048] Weigh the raw materials: 40 kg of a mixture of copper sulfate and copper nitrate; the molar ratio of copper sulfate to copper nitrate is 25:6;
[0049] 7kg brightener: 2-mercaptothiazoline, bisbenzenesulfonimide;
[0050] 25kg leveling agent: hydroxypropyl propargyl ether, butynediol diethoxy ether;
[0051] 10kg additives: sodium 2-thiazoline polydithiopropane sulfonate and sodium N,N-dimethyldithiocarboxamide propane sulfonate in a mass ratio of 2.5:3.8;
[0052] 5kg inhibitor: polyethylene glycol and sodium chloride in a mass ratio of 30:21;
[0053] 4kg accelerator: piperazine-1,4-dithiocarboxylate potassium salt;
[0054] 900kg deionized water;
[0055] The solid wire surface was roughened and preheated to 61°C. The high-speed copper plating solution was used at a current density of 15A / dm 2 , high-speed displacement copper plating was performed on solid welding wire at an electroplating temperature of 70°C.
[0056] Comparative Example 1
[0057] Different from the third embodiment, no additive is added.
[0058] This embodiment provides a copper plating process for a solid welding wire, comprising the following steps:
[0059] Step 1: preparing a high-speed copper plating solution;
[0060] Weigh the raw materials: 40 kg of a mixture of copper sulfate and copper nitrate; the molar ratio of copper sulfate to copper nitrate is 25:6;
[0061] 7kg brightener: 2-mercaptothiazoline, bisbenzenesulfonimide;
[0062] 25kg leveling agent: hydroxypropyl propargyl ether, butynediol diethoxy ether;
[0063] 5kg inhibitor: polyethylene glycol and sodium chloride in a mass ratio of 30:21;
[0064] 4kg accelerator: piperazine-1,4-dithiocarboxylate potassium salt;
[0065] 900kg deionized water;
[0066] The solid wire surface was roughened and preheated to 61°C. The high-speed copper plating solution was used at a current density of 15A / dm 2 , high-speed displacement copper plating was performed on solid welding wire at an electroplating temperature of 70°C.
[0067] Comparative Example 2
[0068] Different from the third embodiment, no accelerator is added.
[0069] This embodiment provides a copper plating process for a solid welding wire, comprising the following steps:
[0070] Step 1: preparing a high-speed copper plating solution;
[0071] Weigh the raw materials: 40 kg of a mixture of copper sulfate and copper nitrate; the molar ratio of copper sulfate to copper nitrate is 25:6;
[0072] 7kg brightener: 2-mercaptothiazoline, bisbenzenesulfonimide;
[0073] 25kg leveling agent: hydroxypropyl propargyl ether, butynediol diethoxy ether;
[0074] 10kg additives: sodium 2-thiazoline polydithiopropane sulfonate and sodium N,N-dimethyldithiocarboxamide propane sulfonate in a mass ratio of 2.5:3.8;
[0075] 5kg inhibitor: polyethylene glycol and sodium chloride in a mass ratio of 30:21;
[0076] 900kg deionized water;
[0077] The solid wire surface was roughened and preheated to 61°C. The high-speed copper plating solution was used at a current density of 15A / dm 2 , high-speed displacement copper plating was performed on solid welding wire at an electroplating temperature of 70°C.
[0078] Comparative Example 3
[0079] Different from the third embodiment, the electroplating temperature is 60°C.
[0080] This embodiment provides a copper plating process for a solid welding wire, comprising the following steps:
[0081] Step 1: preparing a high-speed copper plating solution;
[0082] Weigh the raw materials: 40 kg of a mixture of copper sulfate and copper nitrate; the molar ratio of copper sulfate to copper nitrate is 25:6;
[0083] 7kg brightener: 2-mercaptothiazoline, bisbenzenesulfonimide;
[0084] 25kg leveling agent: hydroxypropyl propargyl ether, butynediol diethoxy ether;
[0085] 10kg additives: sodium 2-thiazoline polydithiopropane sulfonate and sodium N,N-dimethyldithiocarboxamide propane sulfonate in a mass ratio of 2.5:3.8;
[0086] 5kg inhibitor: polyethylene glycol and sodium chloride in a mass ratio of 30:21;
[0087] 4kg accelerator: piperazine-1,4-dithiocarboxylate potassium salt;
[0088] 900kg deionized water;
[0089] The solid wire surface was roughened and preheated to 61°C. The high-speed copper plating solution was used at a current density of 15A / dm 2 , high-speed displacement copper plating was performed on solid welding wire at an electroplating temperature of 60°C.
[0090] The solid welding wires after high-speed displacement copper plating of Examples 1 to 3 and Comparative Examples 1 to 3 were tested respectively, and the corrosion resistance was tested according to the standard of GB / T 20854-2007, and the tensile strength was tested according to the standard of GB / T 10423-2002;
[0091] The results are as follows:
[0092] project Embodiment 1 Embodiment 2 Embodiment 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Plating rate (μm / min) 8.1 7.9 8.0 7.8 6.6 6.3 Tensile strength(MPa) 502 498 501 480 495 499 Corrosion resistance (%) 0.13 0.12 0.14 0.16 0.13 0.11
[0093] It can be seen from the above table that the present invention significantly improves the electroplating rate, tensile strength and corrosion resistance of the welding wire by optimizing various parameters of the electroplating process and optimizing the formula of the copper plating solution.
[0094] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A high-speed copper plating solution for solid welding wire, characterized in that: The high-speed copper plating solution includes 32-46 parts of water-soluble copper salt, 5-8 parts of brightener, 20-27 parts of leveler, 4-12 parts of additive, 3-6 parts of inhibitor, 2-5 parts of accelerator, and 900 parts of deionized water; The additive is a mixture of 2-thiazoline polydithiopropane sulfonate sodium and N,N-dimethyldithiocarboxamide propane sulfonate sodium; The accelerator is selected from one or both of piperazine-1,4-dithiocarboxylic acid potassium salt and 2,3-dimercaptopropanesulfonic acid sodium salt.
2. The high-speed copper plating solution according to claim 1, characterized in that The water-soluble copper salt is composed of a mixture of copper sulfate and copper nitrate; and the molar ratio of the copper sulfate to the copper nitrate is (20-40): (4-8).
3. The high-speed copper plating solution according to claim 2, characterized in that: The mass ratio of the 2-thiazoline polydithiopropane sulfonate sodium and the N,N-dimethyldithiocarboxamide propane sulfonate sodium is (2-3): (3-5).
4. The high-speed copper plating solution according to claim 3, characterized in that: The leveling agent is selected from one or more of butynediol, hydroxypropyl propargyl ether, butynediol diethoxy ether.
5. The high-speed copper plating solution according to claim 4, characterized in that: The brightener is selected from one or more of 2-mercaptothiazoline, bisbenzenesulfonimide, and sodium polyanisole.
6. The high-speed copper plating solution according to claim 5, characterized in that: The inhibitor is a mixture of polyethylene glycol and sodium chloride.
7. The high-speed copper plating solution according to claim 6, characterized in that: The mass ratio of the polyethylene glycol to sodium chloride is (25-32):(16-24).
8. A high-speed copper plating process for solid welding wire, characterized in that: After roughening the surface of the solid welding wire, preheat it to 50-65° C., and use the high-speed copper plating solution described in any one of claims 1-7 to perform high-speed displacement copper plating on the solid welding wire; The current density is 13-16A / dm 2 , the electroplating temperature is 68-75℃.
Citation Information
Cited By
Preparation process of high-strength gas shielded welding wire and high-strength gas shielded welding wire
CN120023526A
Preparation process of a high-strength gas shielded welding wire and the high-strength gas shielded welding wire
CN120023526B