Laminated substrate

By using a dummy wafer during the growth of gallium nitride layers to control the silicon concentration distribution, the problem of in-plane non-uniformity of silicon concentration in large-diameter multilayer substrates is solved, thereby improving the production efficiency and performance of semiconductor devices.

CN118773732APending Publication Date: 2024-10-15SUMITOMO CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410391010.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-06
Filing Date
2024-04-02
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the prior art, the silicon concentration of gallium nitride layers on large-diameter laminated substrates has an in-plane non-uniformity problem, especially the silicon concentration on the outer periphery is significantly higher than that in the center, which affects the production efficiency and performance of semiconductor devices.

Method used

By epitaxially growing a gallium nitride layer on a substrate and using a dummy wafer during the growth process to reduce silicon incorporation from the substrate edge, the silicon concentration distribution is controlled, ensuring that the silicon concentration at the periphery is higher than that at the center but is controlled within a certain range to avoid excessive non-uniformity.

Benefits of technology

It effectively suppresses in-plane non-uniformity of silicon concentration in gallium nitride layers, improves the production efficiency and performance of semiconductor devices, and reduces the impact on resistance and withstand voltage characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773732A_ABST
    Figure CN118773732A_ABST
Patent Text Reader

Abstract

Provided is a laminated substrate in which in-plane unevenness of Si concentration distribution in a GaN layer is suppressed. This laminated substrate is provided with: a base substrate; and a gallium nitride layer epitaxially grown above the base substrate and comprising gallium nitride containing silicon, the gallium nitride layer having an upper surface having a radius of 50 mm or more, the thickness of the gallium nitride layer being 4 [mu] m or more, and the silicon concentration of the upper surface of the gallium nitride layer having a distribution in which the center silicon concentration at the center of the upper surface is greater than the center silicon concentration at the center of the upper surface. The outer peripheral silicon concentration at a radial position 10 mm from the edge of the upper surface is high, the central silicon concentration is 4 * 1015 cm <-3 > or more and less than 2 * 1016 cm <-3 >, and the outer peripheral silicon mixing concentration, which is the excess amount of the outer peripheral silicon concentration exceeding the central silicon concentration, is 1.2 * 1015 cm <-3 > or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a laminate substrate. Background Art

[0002] A stacked substrate having a gallium nitride (GaN) layer epitaxially grown on various base substrates is used as a material for manufacturing semiconductor devices (for example, see Patent Document 1). In order to improve the production efficiency of semiconductor devices, the stacked substrate is being enlarged. Silicon (Si) is used as an n-type impurity added to the GaN layer.

[0003] As described in detail later, the inventors conducted research on a stacked substrate with a large diameter, a low added Si concentration and a thick GaN layer, and found that in-plane unevenness of the Si concentration distribution in the GaN layer (specifically, unevenness such that the Si concentration becomes higher on the outer peripheral side of the GaN layer) is easily produced.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2018-199601 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] An object of the present invention is to provide a multilayer substrate in which in-plane non-uniformity of Si concentration distribution in a GaN layer is suppressed.

[0009] Solutions for solving problems

[0010] According to one embodiment of the present invention, there is provided a laminated substrate comprising:

[0011] a base substrate; and

[0012] a gallium nitride layer epitaxially grown on the base substrate and composed of gallium nitride containing silicon,

[0013] The gallium nitride layer has an upper surface with a radius of more than 50 mm,

[0014] The thickness of the gallium nitride layer is greater than 4 μm,

[0015] The silicon concentration of the upper surface of the gallium nitride layer has a distribution in which a peripheral silicon concentration at a radial position 10 mm from an edge of the upper surface is high relative to a central silicon concentration at the center of the upper surface.

[0016] The central silicon concentration is 4×10 15 cm -3 More than and less than 2×10 16 cm-3 ,

[0017] The excess of the peripheral silicon concentration over the central silicon concentration, i.e., the peripheral silicon mixed concentration, is 1.2×10 15 cm -3 the following.

[0018] Effects of the Invention

[0019] The present invention provides a multilayer substrate in which in-plane non-uniformity of Si concentration distribution in a GaN layer is suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic cross-sectional view of a laminated substrate according to an exemplary embodiment.

[0021] Figure 2 This is a top view of a GaN layer for explaining a method for measuring the Si concentration in the GaN layer.

[0022] Figure 3 It is a schematic side view showing a GaN layer manufacturing apparatus according to an embodiment.

[0023] Figure 4 This is a graph showing an example of Si concentration distribution on the upper surface of the GaN layer according to the first example of the embodiment.

[0024] Figure 5 is a schematic representation of Figure 4 This is a graph of Si concentration distribution of the same first example.

[0025] Figure 6 This is a graph showing an example of Si concentration distribution on the upper surface of the GaN layer according to the second example of the embodiment.

[0026] Figure 7 is a schematic representation of Figure 6 The graph of Si concentration distribution of the second example is similar.

[0027] Figure 8 It is a schematic side view showing a manufacturing apparatus of a GaN layer of a comparative method.

[0028] Fig. 9 This is a graph showing an example of Si concentration distribution on the upper surface of a GaN layer of a comparative example.

[0029] Fig.10 is a schematic representation of Fig. 9 A graph of Si concentration distribution in a similar manner is shown for comparison.

[0030] Description of Reference Numerals

[0031] 10…base structure, 20…GaN layer, 25…upper surface (of GaN layer), 30…upper layer, 40…wafer, 50…dummy wafer, 60…full wafer, 100…laminated substrate, 200…manufacturing device, 210…susceptor, 211…inner periphery of susceptor, 212…outer periphery of susceptor, 213…upper surface of susceptor edge, 220…raw material gas, 230…Si-containing deposit DETAILED DESCRIPTION

[0032] A laminated substrate 100 according to an embodiment of the present invention will be described. Figure 1 1 is a schematic cross-sectional view illustrating a laminate substrate 100 . The laminate substrate 100 includes at least a base structure 10 and a gallium nitride (GaN) layer 20 formed on the base structure 10 .

[0033] The base structure 10 has at least a base substrate as a crystal substrate for epitaxially growing the GaN layer 20. The base structure 10 may also have a buffer layer between the base substrate and the GaN layer 20 as required. The structure of the buffer layer can be appropriately selected as required.

[0034] As the base substrate, a GaN substrate, a sapphire substrate, a silicon (Si) substrate, a silicon carbide (SiC) substrate, etc. can be appropriately used. For example, when the base substrate is a GaN substrate, the base structure 10 can be a GaN substrate. In addition, for example, when the base substrate is a Si substrate, the base structure 10 can have a Si substrate and an aluminum nitride (AlN) layer provided as a nucleation layer, etc.

[0035] The laminated substrate 100 may include an upper layer 30 formed on the GaN layer 20 as required. The structure of the upper layer 30 may be appropriately selected according to the operation of the semiconductor device to be manufactured using the laminated substrate 100. The upper layer 30 may be, for example, a group III nitride layer epitaxially grown on the GaN layer 20.

[0036] The GaN layer 20 of the embodiment has the following features. The GaN layer 20 has an upper surface 25 with a radius of 50 mm or more (a diameter of 100 mm or more). That is, the laminated substrate 100 has a circular shape with a diameter of 100 mm or more. It should be noted that the laminated substrate 100 may have a positioning plane or a notch as needed.

[0037] GaN layer 20 contains silicon (Si) as an n-type impurity. The Si concentration of upper surface 25 of GaN layer 20 has a distribution in which a peripheral Si concentration C1 at the periphery of upper surface 25 is higher than a central Si concentration C0 at the center of upper surface 25 .

[0038] The center Si concentration C0 is 10 15 cm -3The concentration change of the order of magnitude will have an impact on the low concentration, specifically, 4×10 15 cm -3 More than and less than 2×10 16 cm -3 The Si concentration C0 in the center is less than 1×10 16 cm -3 (i.e. 10 15 cm -3 The effect is more significant in the case of the method with the order of magnitude of . The excess of the peripheral Si concentration C1 over the central Si concentration C0, i.e., the peripheral Si mixed concentration Δ (i.e., C1-C0), is 1.2×10 15 cm -3 That is, the peripheral Si concentration C1 is higher than the central Si concentration C0, but the peripheral Si mixed concentration Δ, which is the difference between the two, is suppressed to 1.2×10 15 cm -3 The thickness of the GaN layer 20 is 4 μm or more. The thickness of the GaN layer 20 is, for example, 40 μm or less.

[0039] The GaN layer 20 is a layer that functions as at least a part of the operating layer in the semiconductor element including the stacked substrate 100. Therefore, the GaN layer 20 preferably has both withstand voltage characteristics and resistance characteristics in a balanced manner. From the viewpoint of improving the withstand voltage, the central Si concentration C0 of the GaN layer 20 is preferably less than 2×10 16 cm -3 In addition, from the viewpoint of increasing the withstand voltage, the thickness of the GaN layer 20 is preferably 4 μm or more. From the viewpoint of reducing the resistance, the central Si concentration C0 of the GaN layer 20 is preferably 4×10 15 cm -3 Furthermore, from the viewpoint of reducing the resistance, the thickness of the GaN layer 20 is preferably 40 μm or less.

[0040] As described later, the peripheral Si mixing concentration Δ is the concentration of Si mixed into the periphery of the GaN layer 20 due to the Si-containing sediment 23. The central Si concentration C0 is substantially equal to the target added concentration as the concentration of Si added intentionally. The peripheral Si mixing concentration Δ is the excess amount of the peripheral Si mixing concentration exceeding the central Si concentration C0 caused by the mixing of Si. The GaN layer 20 of the embodiment has a feature that the peripheral Si mixing concentration Δ is suppressed compared to the comparative method.

[0041] In the following description, the radius of the GaN layer 20 is 50 mm, the thickness of the GaN layer 20 is 4 μm, and the target concentration of Si added in the GaN layer 20 is 9×10 15 cm -3 Such conditions are common in the embodiment and the comparative embodiment.

[0042] A method for measuring the Si concentration in the GaN layer 20 will be described. Figure 2 1 is a plan view of the GaN layer 20 for explaining a method of measuring the Si concentration in the GaN layer 20. An XY orthogonal coordinate system is set on the upper surface 25 of the GaN layer 20, with the center of the upper surface 25 as the origin.

[0043] First, the measurement positions within the surface are described. As measurement points for the Si concentration on the upper surface 25, at least a central measurement point and four peripheral measurement points are set, for a total of five measurement points. The central measurement point is set at the center of the upper surface 25. The four peripheral measurement points are set at radial positions 10 mm from the edge of the upper surface 25 for the positive X direction, the negative X direction, the positive Y direction, and the negative Y direction (i.e., every 90° along the circumferential direction). Here, as a representative position of the periphery when specifying the Si concentration at the periphery of the upper surface 25, a radial position 10 mm from the edge of the upper surface 25 is set.

[0044] The Si concentration at the central measurement point is the central Si concentration C0. The Si concentration obtained by averaging the Si concentration CX+ at the peripheral measurement point in the positive X direction, the Si concentration CX- at the peripheral measurement point in the negative X direction, the Si concentration CY+ at the peripheral measurement point in the positive Y direction, and the Si concentration CY- at the peripheral measurement point in the negative Y direction is the peripheral Si concentration C1. That is, the peripheral Si concentration C1 represents the Si concentration averaged in the peripheral direction. The excess of the peripheral Si concentration C1 over the central Si concentration C0, that is, C1-C0, is the peripheral Si mixing concentration Δ.

[0045] In this example, the radius of the upper surface 25 is 50 mm. Four peripheral measurement points are set at radial positions 40 mm from the center in the positive X direction, the negative X direction, the positive Y direction, and the negative Y direction.

[0046] In addition to the central measurement point and the four peripheral measurement points, an intermediate measurement point can also be set at a radial position between the central measurement point and the peripheral measurement point. In this example, the intermediate measurement point is set at a radial position of 10 mm, 20 mm, and 30 mm from the center for the positive X direction, negative X direction, positive Y direction, and negative Y direction, respectively. Figure 2 In order to facilitate illustration, large black dots are used to represent the central measurement points and the peripheral measurement points, and small black dots are used to represent the intermediate measurement points.

[0047] It should be noted that, in the case where the radius of the upper surface 25 of the GaN layer 20 exceeds 50 mm, the four peripheral measurement points are also set at radial positions 10 mm from the edge of the upper surface 25. In addition, in the case where the radius of the upper surface 25 of the GaN layer 20 exceeds 50 mm, the intermediate measurement points may also be set at radial positions every 10 mm from the center for the positive X direction, the negative X direction, the positive Y direction, and the negative Y direction.

[0048] The Si concentration obtained by averaging the Si concentrations at four measurement points in the positive X direction, the negative X direction, the positive Y direction, and the negative Y direction set at equal radial positions from the center of the upper surface 25, that is, the Si concentration obtained by circumferentially averaging the radial positions is called the average Si concentration. The peripheral Si concentration C1 is the average Si concentration at the periphery.

[0049] As described later, the growth of the GaN layer 20 is carried out in a uniform manner in the circumferential direction. However, in reality, even between the four measurement points set at equal radial positions, there will be deviations in Si concentration. In order to reduce the influence of such deviations, the Si concentration obtained by circumferential averaging, that is, the average Si concentration, is used to evaluate the radial distribution of Si concentration in the GaN layer 20. The concentration of mixed Si is the excess of the average Si concentration at each radial position over the central Si concentration C0.

[0050] Next, the measurement position in the height direction is described. As the Si concentration in the GaN layer 20, the Si concentration of the upper surface 25 is measured by secondary ion mass spectrometry (SIMS). Among them, the "Si concentration of the upper surface 25" is not exactly the Si concentration at the height of the upper surface 25, but as described below, it refers to the Si concentration near the upper surface 25. In the mode where the upper layer 30 is not stacked, the upper surface 25 is the uppermost surface of the stacked substrate 100, and in the mode where the upper layer 30 is stacked, the upper surface 25 is the interface between the upper layer 30 and the GaN layer 20.

[0051] In general, the reliability of SIMS measurement at the surface position is not high. Therefore, it is preferred to perform SIMS measurement at a height slightly from the upper surface 25 to the side of the base structure 10, that is, slightly inside the GaN layer 20. In addition, it is preferred to use a measurement value obtained by averaging a certain degree of height range (depth range, thickness range). Here, for each measurement point in the surface, the value obtained by averaging the SIMS measurement values ​​of the depth range of more than 100nm and less than 200nm from the upper surface 25 is defined as the Si concentration of the upper surface 25. For example, in a method in which the thickness of the GaN layer 20 is 4μm, the average value of the Si concentration based on SIMS measurement in the range of more than 3.8μm and less than 3.9μm from the lower surface of the GaN layer 20 is defined as the Si concentration of the upper surface 25.

[0052] Before further describing the embodiment, a comparative method will be described. Figure 8 1 is a schematic side view of a manufacturing apparatus 200 for manufacturing a GaN layer 20 in a comparative manner. The manufacturing apparatus 200 is a metal organic vapor phase epitaxy (MOVPE) apparatus having a susceptor 210 for mounting a wafer 40. The wafer 40 is an object to be processed (an intermediate of the laminated substrate 100) in the stage of the growth processing of the GaN layer 20 by the manufacturing apparatus 200, and specifically, is the base structure 10 at the start of the growth of the GaN layer 20, and is a laminate of the base structure 10 and the GaN layer 20 after the growth of the GaN layer 20 starts.

[0053] The manufacturing device 200 is a cross-flow MOVPE device that supplies a raw material gas 220 in a direction parallel to the upper surface of the wafer 40. The raw material gas 220 includes a GaN raw material gas for growing GaN constituting the GaN layer 20, and a Si doping raw material gas for supplying Si added to the GaN layer 20. The GaN raw material gas includes a gallium (Ga) raw material gas and a nitrogen (N) raw material gas. As the Ga raw material gas, for example, trimethyl gallium (TMG) gas is used, and as the N raw material gas, for example, ammonia (NH3) gas is used. As the Si doping raw material gas, for example, silane (SiH4) gas is used.

[0054] The growth temperature can be selected in the range of 900°C to 1400°C, for example, and the flow rate ratio of the V group source gas to the III group source gas, i.e., the V / III ratio, can be selected in the range of 10 to 5000, for example. The Si doping source gas is added to the GaN layer 20 at a target concentration of 4×10 15 cm -3 More than and less than 2×10 16 cm -3 A specified value within the range of 9×10 15 cm -3 supplied in the form of .

[0055] The susceptor 210 holds the wafer 40 so as to rotate the wafer 40 about the center of the wafer 40 . By growing the GaN layer 20 while performing such rotation, the growth conditions of the GaN layer 20 are made uniform in the circumferential direction of the wafer 40 .

[0056] The susceptor inner peripheral edge 211 is a position of the edge of the susceptor 210 where the wafer 40 is placed in a plan view. The susceptor edge upper surface 213 is an upper surface of the susceptor 210 between the susceptor inner peripheral edge 211 and the susceptor outer peripheral edge 212 .

[0057] As the GaN layer 20 is grown, the Si-containing deposit 230 is attached to the upper surface 213 of the susceptor edge, so that Si is mixed into the GaN layer 20 from the Si-containing deposit 230. The Si-containing deposit 230 is a defect of GaN and contains Si. It is speculated that the main source of Si contained in the Si-containing deposit 230 may be Ga raw material gas or Si-doped raw material gas (one or both of them), but the details are not clear. In addition, it is unrealistic to prevent the Si-containing deposit 230 from being attached to the upper surface 213 of the susceptor edge. The mixing of Si from the Si-containing deposit 230 into the GaN layer 20 cannot be controlled in the prior art.

[0058] The concentration of Si mixed in from the Si-containing deposit 230 increases as it is closer to the inner peripheral edge 211 of the susceptor, that is, closer to the outer peripheral side of the edge of the wafer 40. The inclusion of Si in the GaN layer 20 due to the Si-containing deposit 230 is referred to as "mixing", which is distinguished from "addition" in which Si is intentionally included in the GaN layer 20 by Si doping the raw material gas.

[0059] Ideally, the concentration of Si contained in the GaN layer 20 is controlled to be the target concentration to be added by the Si doping source gas over the entire region of the upper surface 25. Therefore, as described in the embodiment described later, it is preferable to minimize the amount of Si mixed in from the Si-containing deposit 230.

[0060] The concentration of Si mixed into the GaN layer 20 from the Si-containing deposit 230 is about the same during the growth within the above growth condition range and during the growth within the above target addition concentration range. Specifically, as described later, the concentration of Si mixed into the outer periphery (10 mm radial position from the edge of the wafer 40, 10 mm radial position from the inner peripheral edge 211 of the susceptor in the comparative method) is 1.6×10 15 cm -3 about.

[0061] Fig. 9 1 is a graph showing an example of Si concentration distribution on the upper surface 25 of the GaN layer 20 of the comparative method. The horizontal axis represents the measurement position in the plane in mm units, and the vertical axis represents the measurement position in 10 15 cm -3 The unit represents the Si concentration. The Si concentration of each measurement point in the X direction is represented by a black circle, and the Si concentration of each measurement point in the Y direction is represented by a hollow quadrilateral. The average Si concentration is represented by a cross. This representation method is related to the implementation method. Figure 4 as well as Figure 6 The same is true in the chart of .

[0062] The central Si concentration C0 is 9×10 15 cm -3Furthermore, the Si concentration at about 10 mm from the center is approximately constant. Therefore, it can be said that the mixed Si does not reach the center of the wafer 40.

[0063] At radial positions about 20 mm or more from the center, the excess of the central Si concentration C0, that is, the concentration of mixed Si, becomes significantly higher. In addition, the concentration of mixed Si increases toward the outer peripheral side.

[0064] In the comparison method, the central Si concentration C0 is 9.01×10 15 cm -3 The peripheral Si concentration C1 is 10.65×10 15 cm -3 The peripheral Si mixing concentration Δ is 1.64×10 15 cm -3 .

[0065] Fig.10 is a schematic representation of Fig. 9 A graph of Si concentration distribution in a similar manner is shown for comparison. Fig.10 In FIG. 1 , for easy understanding, the wafer 40 and the susceptor inner peripheral edge 211 are shown together with the Si concentration distribution.

[0066] The addition distribution D0 is a Si concentration distribution that is equal to and constant to the central Si concentration C0 in the entire region within the surface of the wafer 40, and schematically represents the Si concentration distribution caused by Si added by the Si doping raw material gas. The mixing distribution D1 schematically represents the Si concentration distribution caused by Si mixed in by the Si-containing deposit 230. The overall Si concentration distribution is represented as the sum of the addition distribution D0 and the mixing distribution D1.

[0067] Si caused by the Si-containing deposit 230 is mixed into a width of about 40 mm in the radial direction from the edge of the wafer 40. In the case of a large-diameter wafer 40, such as a 50 mm radius, as in this example, Si mixing does not occur at the center. On the other hand, if a method is used in which a wafer with a smaller diameter, such as a 25 mm radius, is used, Si mixing will also occur at the center of the wafer.

[0068] In the case of a small diameter structure where Si is mixed in the center, mixed Si from both sides of the center overlaps in the center, so that the Si concentration caused by the mixed Si also becomes high in the center. As a result, the Si concentration distribution caused by the mixed Si becomes nearly uniform in the plane.

[0069] In contrast, in a large-diameter wafer 40 where Si is not mixed in the center as in this example, the Si concentration distribution caused by the mixed Si becomes a non-uniform distribution with a large difference between the center and the periphery. Thus, in a large-diameter wafer 40, specifically, a wafer with a radius of 50 mm or more, the in-plane non-uniformity of the Si concentration distribution caused by the mixed Si becomes significant.

[0070] Although a method with a radius of 50 mm is illustrated, in a wafer 40 with a radius exceeding 50 mm, the concentration of mixed Si in the periphery (a radial position of 10 mm from the edge of the wafer 40, and a radial position of 10 mm from the inner peripheral edge 211 of the base in the comparison method) is also at the same level as that in the case of a radius of 50 mm.

[0071] In the comparison method, the peripheral Si mixed concentration Δ, which is the Si concentration difference between the center and the periphery, is 1.64×10 15 cm -3 On the other hand, the target Si addition concentration, i.e., the center Si concentration C0, is 10 15 cm -3 Therefore, the influence of the peripheral Si mixed concentration Δ on the Si concentration distribution in the plane becomes significant.

[0072] Thus, when the radius of the upper surface 25 is greater than 50 mm and the central Si concentration C0 is 4×10 15 cm -3 More than and less than 2×10 16 cm -3 (and thus less than 1×10 16 cm -3 ) in the GaN layer 20, the difference in Si concentration between the center and the periphery caused by the Si mixing becomes significant. As described below, in the embodiment, a technology capable of suppressing such in-plane non-uniformity of Si concentration compared with the comparative method, that is, a technology capable of suppressing the peripheral Si mixing concentration Δ compared with the comparative method is proposed.

[0073] It should be noted that, as a general trend, the thicker the GaN layer 20 is, the greater the peripheral Si mixing concentration Δ is. This is because the longer the growth time of the GaN layer 20 is, the more Si-containing deposits 230 adhere to the susceptor edge upper surface 213 will be.

[0074] The comparative method (and the embodiment) exemplifies the peripheral Si mixing concentration Δ of the GaN layer 20 with a thickness of 4 μm. If the thickness of the GaN layer 20 is sufficiently thin, the mixing of Si caused by the Si-containing sediment 230 may not cause the in-plane non-uniformity described above. However, when a GaN layer 20 with a thickness of 4 μm (or more than 4 μm) is grown, the in-plane non-uniformity described above will occur. As described below, in the embodiment, a technology is proposed that can reduce the peripheral Si mixing concentration Δ in the GaN layer 20 with a thickness of 4 μm compared to the comparative method, and further, a technology is proposed that can similarly reduce the peripheral Si mixing concentration Δ even in a GaN layer 20 thicker than 4 μm.

[0075] The implementation method is further described. Figure 3 1 is a schematic side view showing a manufacturing apparatus 200 of the GaN layer 20 according to the embodiment. The manufacturing apparatus 200 according to the embodiment is a lateral flow MOVPE apparatus similar to the comparative embodiment.

[0076] In the embodiment, the GaN layer 20 is grown in a state where a ring-shaped dummy wafer 50 is arranged outside the wafer 40 in a top view. The dummy wafer 50 has a radial width WD and has the same thickness as the wafer 40. As the material of the dummy wafer 50 (dummy base substrate) at the beginning of the growth of the GaN layer 20, a material that becomes a base for epitaxial growth of GaN, such as GaN, and another material such as sapphire is used. After the growth of the GaN layer 20 starts, a structure in which the grown GaN layer is stacked on the dummy base substrate becomes the dummy wafer 50.

[0077] The full wafer 60 is a structure in which the wafer 40 and the dummy wafer 50 are combined. In the embodiment, the processing object of the manufacturing apparatus 200 is the full wafer 60. The edge of the full wafer 60, that is, the outer peripheral edge where the dummy wafer 50 is arranged, is the susceptor inner peripheral edge 211.

[0078] In the embodiment, by arranging the dummy wafer 50 further outside the wafer 40, Si released from the Si-containing deposit 230 is preferentially mixed into the GaN grown on the dummy wafer 50. Si released from the Si-containing deposit 230 and crossing the width WD of the dummy wafer 50 is mixed into the GaN layer 20 of the wafer 40. In this way, by using the dummy wafer 50, Si mixed into the GaN layer 20 from the Si-containing deposit 230 can be reduced compared with the comparative method.

[0079] Next, a first example of the embodiment will be described. In the first example of the embodiment, an example in which the width WD of the dummy wafer 50 is 10 mm is exemplified. The growth conditions of the GaN layer 20 in the first example of the embodiment are the same as those in the above-mentioned comparative example.

[0080] Figure 4 : is a graph showing an example of Si concentration distribution on the upper surface 25 of the GaN layer 20 of the first example of the embodiment. As in the comparative example, in the first example of the embodiment, Si mixing on the outer peripheral side is observed, but it is suppressed compared with the comparative example.

[0081] In the first example of the embodiment, specifically, the central Si concentration C0 is 9.00×10 15 cm -3 The peripheral Si concentration C1 is 10.05×10 15 cm -3 The peripheral Si mixing concentration Δ is 1.05×10 15 cm -3 , compared with the peripheral Si mixing concentration Δ1.64×10 15 cm -3 Compared to being suppressed.

[0082] The peripheral Si contamination concentration is less than Δ1.64×10 15 cm -3 The first concentration reference value is set to 1.2×10 15 cm -3 In the first example of the embodiment, the peripheral Si mixing concentration Δ is suppressed to the first concentration reference value 1.2×10 15 cm -3 the following. Figure 4 (and Fig. 9 ), the first concentration reference value is represented as Δ1.2.

[0083] Figure 5 is a schematic representation of Figure 4 A graph of Si concentration distribution in the first example of the same embodiment. Figure 5 In FIG. 1 , for easy understanding, the wafer 40 , the dummy wafer 50 , and the susceptor inner periphery 211 are shown together with the Si concentration distribution.

[0084] The mixed distribution D1 in the comparative method is shown on the central side of the wafer 40, and the mixed distribution D1 in the first example of the embodiment is shown on the outer peripheral side of the wafer 40. Compared with the comparative method, the dummy wafer 50 has the effect of moving the inner peripheral edge 211 of the susceptor away from the outer side of the wafer 40. Therefore, compared with the comparative method, the mixed distribution D1 can be moved to the outer peripheral side of the wafer 40 according to the width 10 mm of the dummy wafer 50. In this way, in the first example of the embodiment, compared with the comparative method, the mixed Si concentration can be suppressed to a low level on the lower side of the mixed distribution D1.

[0085] Next, a second example of the embodiment is described. In the second example of the embodiment, a mode in which the width WD of the dummy wafer 50 is 20 mm is exemplified. The growth conditions of the GaN layer 20 in the second example of the embodiment are the same as those in the above-mentioned comparative mode (or the first example of the embodiment).

[0086] Figure 6 1 is a graph showing an example of Si concentration distribution on the upper surface 25 of the GaN layer 20 of the second embodiment. As in the comparative method and the first embodiment, in the second embodiment, Si mixing on the peripheral side is also observed, but it is further suppressed compared with the first embodiment.

[0087] In the second example of the embodiment, specifically, the central Si concentration C0 is 8.91×10 15 cm -3 The peripheral Si concentration C1 is 9.44×10 15 cm -3 The peripheral Si mixing concentration Δ is 0.53×10 15 cm -3 , which is different from the peripheral Si mixing concentration Δ1.05×10 15 cm -3 was further suppressed.

[0088] The first concentration reference value is 1.2×10 15 cm -3 The second and third low concentration reference values ​​are set to 0.9×10 15 cm -3 and 0.6×10 15 cm -3 The peripheral Si contamination concentration Δ in the second example of the embodiment is also suppressed to the first concentration reference value of 1.2×10 15 cm -3 The peripheral Si contamination concentration Δ in the second example of the embodiment is preferably suppressed to the second concentration reference value of 0.9×10 15 cm -3 Below, it is more preferably suppressed to the third concentration reference value of 0.6×10 15 cm -3 the following. Figure 6 , the third concentration reference value is represented as Δ0.6.

[0089] Figure 7 is a schematic representation of Figure 6 A graph showing Si concentration distribution in a second example of the same embodiment is shown. Figure 7In FIG. 1 , for easy understanding, the wafer 40 , the dummy wafer 50 , and the susceptor inner periphery 211 are shown together with the Si concentration distribution.

[0090] The mixed distribution D1 in the comparative method is shown on the central side of the wafer 40, and the mixed distribution D1 in the second example of the embodiment is shown on the outer peripheral side of the wafer 40. In the second example of the embodiment, compared with the comparative method, the mixed distribution D1 can be moved to the outer peripheral side of the wafer 40 according to the width 20 mm of the dummy wafer 50. In this way, in the second example of the embodiment, compared with the first example of the embodiment, the mixed Si concentration can be suppressed to a lower level on the lower side of the mixed distribution D1.

[0091] By further increasing the width WD of the dummy wafer 50 as in the second example, the mixing of Si into the outer periphery of the wafer 40 can be further suppressed. However, increasing the width WD of the dummy wafer 50 increases the area of ​​the full wafer 60, that is, the area of ​​the GaN layer to be grown.

[0092] The cross-flow MOVPE device has the following characteristics: the larger the area of ​​the growing GaN layer, the lower the raw material efficiency (the proportion of raw materials that contribute to the growth). In the embodiment, since a thicker GaN layer 20 with a thickness of more than 4 μm is grown, the reduction in raw material efficiency leads to a deterioration in production efficiency and an increase in cost. In addition, the larger the growth area, the more likely it is that the downstream side will be depleted of raw materials.

[0093] Therefore, from the viewpoint of favorably growing the GaN layer 20 in the wafer 40 , the area of ​​the entire wafer 60 , that is, the width WD of the dummy wafer 50 is preferably a smaller value within a range in which the effect of suppressing the incorporation of Si can be appropriately obtained.

[0094] Therefore, the width WD of the dummy wafer 50 is not excessively increased in order to make the peripheral Si mixed concentration Δ zero. Specifically, the fourth concentration reference value is set to 0.3×10 15 cm -3 The width WD of the dummy wafer 50 is limited to the outer periphery, and the Si mixed concentration Δ is the fourth concentration reference value 0.3×10 15 cm -3 The size of the above degree.

[0095] Thus, in the embodiment, the peripheral Si mixed concentration Δ is suppressed by using the dummy wafer 50, but the peripheral Si mixed concentration Δ is not reduced to zero. That is, the characteristic that the peripheral Si concentration C1 is higher than the central Si concentration C0 is retained. Specifically, the peripheral Si mixed concentration Δ is suppressed to the first concentration reference value of 1.2×10 15 cm -3 Below, it is preferably suppressed to the second concentration reference value of 0.9×10 15 cm-3 Below, it is more preferably suppressed to the third concentration reference value of 0.6×10 15 cm -3 Below. The peripheral Si mixed concentration Δ is the fourth concentration reference value 0.3×10 15 cm -3 above.

[0096] It should be noted that when “peripheral Si concentration C1 is higher than central Si concentration C0” is defined, not only the first condition that the peripheral Si concentration C1 is larger than the central Si concentration C0 but also the second condition described below is satisfied.

[0097] The peripheral Si concentration C1 is the average value of the four peripheral measurement points. If only the average value is considered, for example, there is (hypothetically) a deviation such as the Si concentration at three peripheral measurement points is lower than the central Si concentration C0, but the Si concentration at one peripheral measurement point is extremely high, which may include an inappropriate situation in which the average value, that is, the peripheral Si concentration C1 is higher than the central Si concentration C0.

[0098] In the embodiment, as described above, the GaN layer 20 is grown while rotating in a manner that achieves uniformity in the circumferential direction. Therefore, it is preferable to also consider the provision that uniformity is achieved in the circumferential direction. Here, when it is stipulated that "the peripheral Si concentration C1 is higher than the central Si concentration C0", as an additional second condition, it is set to also meet the condition that the Si concentration of at least 3 (preferably 4) of the 4 peripheral measurement points is higher than the central Si concentration C0.

[0099] In the above description, the thickness of the GaN layer 20 is 4 μm. As described above, the longer the growth time of the GaN layer 20 is, that is, the thicker the GaN layer 20 is, the more Si-containing deposits 230 tend to be. Therefore, when the width WD of the dummy wafer 50 is constant, the thicker the GaN layer 20 is, the greater the peripheral Si mixing concentration Δ is.

[0100] Therefore, in the case where the thickness of the GaN layer 20 is thicker than 4 μm, it is preferable to appropriately increase the width WD of the dummy wafer 50 according to the thickness of the GaN layer 20, so as to reduce the peripheral Si mixing concentration Δ to a predetermined value, compared with the case where the thickness of the GaN layer 20 is 4 μm. In this way, by appropriately increasing the width WD of the dummy wafer 50 according to the thickness of the GaN layer 20, the peripheral Si mixing concentration Δ can be reduced to a predetermined value even in the case where the thickness of the GaN layer 20 is thicker than 4 μm.

[0101] The following further describes the features of the GaN layer 20 of the embodiment. As described above, in the embodiment, the peripheral Si mixed concentration Δ is suppressed by using the dummy wafer 50. As a result, the area on the center side of the upper surface 25 of the GaN layer 20 with a low concentration of mixed Si can be expanded to the outer side compared to the comparative method. In other words, the width of the area on the outer side of the upper surface 25 of the GaN layer 20 with a high concentration of mixed Si can be made smaller than that of the comparative method.

[0102] The concentration of Si mixed in is higher than the lower limit of the target added concentration, that is, the lower limit of the central Si concentration C0 by 4×10 15 cm -3 The Si concentration exceeds 10%, which is 0.4×10 15 cm -3 The area is called the Si mixed high concentration area. Figure 4 In the study, the Si concentration (0.4×10 15 cm -3 ) is represented by ΔSi. The high Si concentration region is an annular region on the edge side of the upper surface 25 of the GaN layer 20. The circular region (the entire region) further inside the annular region as the high Si concentration region is an annular region is an Si low concentration region. The width of the annular region from the edge of the upper surface 25 that becomes the Si high concentration region is W1, and the diameter of the circular region that becomes the Si low concentration region is W0.

[0103] The width W1 of the Si high concentration region is Fig. 9 ) is approximately 30 mm. In contrast, in the first example ( Figure 4 ) and the second example ( Figure 6 ) is reduced to about 20 mm. The width W1 in the second example is smaller than the width W1 in the first example. The width W1 of the mixed Si high concentration region in the first and second examples of the embodiment is suppressed to less than 20 mm.

[0104] Thus, the GaN layer 20 of the embodiment has the following characteristics: the concentration of mixed Si (the amount by which the average Si concentration exceeds the central Si concentration C0) is 0.4×10 15 cm -3 the following.

[0105] In the embodiment (and the comparative embodiment), the concentration of mixed Si decreases monotonically from the outer periphery to the center of the GaN layer 20. Therefore, the GaN layer 20 of the embodiment has the following characteristics: the intermediate Si concentration C2 at the radial position between the center and the periphery is higher than the central Si concentration C0 and lower than the peripheral Si concentration C1.

[0106] The intermediate Si concentration C2 is set to be, for example, the average Si concentration at a radial position 30 mm from the center. Figure 4 In the first example of the embodiment shown, the intermediate Si concentration C2 (9.40×10 15 cm -3 ) is higher than the central Si concentration C0 (9.00×10 15 cm -3 ), which is lower than the peripheral Si concentration C1 (10.05×10 15 cm -3 ). In addition, Figure 6 In the second example of the embodiment shown, the intermediate Si concentration C2 (9.25×10 15 cm -3 ) is higher than the central Si concentration C0 (8.91×10 15 cm -3 ), which is lower than the peripheral Si concentration C1 (9.44×10 15 cm -3 ).

[0107] <Preferred Mode of the Invention>

[0108] Preferred embodiments of the present invention are described below.

[0109] (Note 1)

[0110] A laminate substrate, characterized by comprising: a base substrate; and

[0111] a gallium nitride layer epitaxially grown on the base substrate and composed of gallium nitride containing silicon,

[0112] The gallium nitride layer has an upper surface with a radius of more than 50 mm,

[0113] The thickness of the gallium nitride layer is greater than 4 μm,

[0114] The silicon concentration of the upper surface of the gallium nitride layer has a distribution in which a peripheral silicon concentration at a radial position 10 mm from an edge of the upper surface is high relative to a central silicon concentration at the center of the upper surface.

[0115] The central silicon concentration is 4×10 15 cm -3 More than and less than 2×1016 cm -3 ,

[0116] The excess of the peripheral silicon concentration over the central silicon concentration, i.e., the peripheral silicon mixed concentration, is 1.2×10 15 cm -3 Less than (preferably 0.9×10 15 cm -3 Below, more preferably 0.6×10 15 cm -3 the following).

[0117] (Note 2)

[0118] The laminated substrate according to Supplementary Note 1, wherein in a circular region further inside the circular region having a width of 20 mm from the edge of the upper surface, the excess amount of the silicon concentration of the upper surface of the gallium nitride layer over the central silicon concentration is 0.4×10 15 cm -3 the following.

[0119] (Note 3)

[0120] The stacked substrate according to Supplement 1 or 2, wherein the silicon concentration of the upper surface of the gallium nitride layer has the following distribution: the intermediate silicon concentration at a radial position 30 mm from the center of the upper surface is higher than the central silicon concentration and lower than the peripheral silicon concentration.

Claims

1. A laminate substrate, characterized in that: have: a base substrate; and a gallium nitride layer epitaxially grown on the base substrate and composed of gallium nitride containing silicon, The gallium nitride layer has an upper surface with a radius of more than 50 mm, The thickness of the gallium nitride layer is greater than 4 μm. The silicon concentration of the upper surface of the gallium nitride layer has a distribution in which a peripheral silicon concentration at a radial position 10 mm from an edge of the upper surface is high relative to a central silicon concentration at the center of the upper surface. The central silicon concentration is 4×10 15 cm -3 More than and less than 2×10 16 cm -3 , The excess of the peripheral silicon concentration over the central silicon concentration, i.e., the peripheral silicon mixed concentration, is 1.2×10 15 cm -3 the following.

2. The laminate substrate according to claim 1, wherein In a circular region further inside the circular region with a width of 20 mm from the edge of the upper surface, the excess amount of the silicon concentration of the upper surface of the gallium nitride layer over the central silicon concentration is 0.4×10 15 cm -3 the following.

3. The laminated substrate according to claim 1 or 2, wherein: The silicon concentration of the upper surface of the gallium nitride layer has a distribution in which a middle silicon concentration at a radial position 30 mm from the center of the upper surface is higher than the central silicon concentration and lower than the peripheral silicon concentration.