Winding mechanism for preparing polypropylene filament yarn and method for preparing filament yarn by using winding mechanism

By adding liquid crystal polymer during the spinning process and using isothermal annealing technology, the polypropylene crystals of the polypropylene filament are oriented along the fiber axis, which solves the problems of insufficient strength of the polypropylene filament and uneven cooling during the spinning process, and achieves Preparation of polypropylene filament with high strength and high thermal stability.

CN118773756AInactive Publication Date: 2024-10-15扬州市奕轩纤维有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410714745.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing polypropylene filament has insufficient strength, which limits its application in industrial products. In addition, uneven air-cooling in the traditional spinning process leads to shortcomings such as breakage and wool, which affects the tensile orientation and crystallization of the fiber.

Method used

Using a combination of liquid crystal polymer and polypropylene masterbatch, the liquid crystal units are oriented along the fiber axis by heating and melting, using capillary force and traction during the spinning process, and then isothermal annealing is performed during the stretching process to make the polypropylene heavy. Crystallization uses the induction effect of liquid crystal units to orient along the axial direction, thereby improving the strength of the fiber.

Benefits of technology

The preparation of high-strength polypropylene filament is achieved, with a breaking strength of ≥7.0 cN/dtex and an elongation at break of less than 18%. The equipment requirements are simplified and the cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773756A_ABST
    Figure CN118773756A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of polymer fiber preparation, and particularly relates to a winding mechanism for preparing polypropylene filament yarn and a method for preparing filament yarn by using the same. In the spinning process, liquid crystal elements in the liquid crystal polymer are oriented in the axial direction of the fiber under the action of capillary force and traction acting force; then, in the stretching process, polypropylene in the fiber is recrystallized by utilizing an isothermal annealing treatment technology, and the recrystallized polypropylene crystal is oriented in the axial direction under the induction action of a liquid crystal unit, so that the high-thermal-stability and high-strength polypropylene filament yarn is obtained. The preparation of the high-strength polypropylene filament yarn can be directly realized on the existing polypropylene filament yarn spinning equipment, and the equipment requirement is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer fiber preparation, and in particular to a winding mechanism for preparing polypropylene filaments and a method for preparing the filaments using the mechanism. Background Art

[0002] Polypropylene is a synthetic fiber made from propylene, a byproduct of petroleum refining, through polymerization and melt spinning. It is also called polypropylene fiber. The varieties of polypropylene include filaments (including undeformed filaments and expanded deformed filaments), staple fibers, bristle fibers, film-split fibers, hollow fibers, shaped fibers, various composite fibers and non-woven fabrics. In 2021, China's polypropylene production was 428,000 tons, a year-on-year increase of 3.8%. The price of polypropylene yarn is 15,000-20,000 yuan / ton, and the output value exceeds 5 billion yuan. Due to its low price, polypropylene synthetic fiber is currently mainly used in civilian clothing, but with the rapid changes in the chemical fiber market, synthetic fibers are developing towards differentiation and functionalization. However, polypropylene is limited to clothing due to its insufficient strength on the market. Various products that withstand high strength, such as geotextiles, conveyor belts, nets, tarpaulins, etc. made of special materials, now mainly use polyamide products. As raw materials, they have good performance but high cost. Some products also use fine-denier polypropylene filaments, which are plyed to achieve coarse denier to meet the requirements on fineness, but there are two disadvantages: first, the plying of fine-denier filaments requires additional equipment and labor energy consumption, thereby increasing the cost of raw materials; second, although the fineness requirements are met after plying, the product performance is not improved, and the strength and elongation do not meet the requirements, which cannot meet the needs of industrial products. Therefore, it is of great significance to develop high-strength polypropylene yarns.

[0003] At present, the production of polypropylene filaments is all done through one-step spinning. Since the crystallization temperature of polypropylene is between 120 and 130°C, and the crystallinity is proportional to time, the temperature of the filaments ejected from the spinneret is about 200°C in the traditional side-blowing air cooling. After the air-blowing air cooling, the temperature gradually drops to room temperature. When the temperature of the filaments drops to 120-130°C, the filaments will produce partial (or full) crystallization, among which the radial crystallization of the filaments will affect the tensile orientation of the fiber, thereby reducing the tensile orientation degree, and then affecting its crystallization setting, and finally affecting the strength of the finished filaments; in addition, due to uneven air cooling, the production process often has shortcomings such as broken ends and hairy filaments, and the strength is a certain distance away from that of polyester. The strength of the produced polypropylene filaments is generally below 6.5 cN / dtex. Therefore, how to make the polypropylene crystals oriented along the axial direction of the fiber is an important means to improve the strength of polypropylene filaments. Summary of the invention

[0004] In order to solve some problems existing in the above-mentioned prior art, the present invention provides a winding mechanism for preparing polypropylene filaments, including a winding mechanism, the winding mechanism includes a winding unit frame, the winding unit frame is provided with a unit shell, a winding drive motor is arranged on the outside of the unit shell, a fixed winding drum is arranged on one side of the unit shell, an arc-shaped movable slide groove is arranged below the fixed winding drum, the movable slide groove is arranged at two ends of one side of the unit shell, an auxiliary winding drum is arranged outside the movable slide groove, a winding moving part is arranged inside the winding unit frame, a limiting mechanism is arranged on the other side of the unit shell, a limiting plate is arranged below the limiting mechanism, the limiting mechanism includes a fixed block arranged between the winding unit frame and the limiting plate, a support column is arranged between the fixed blocks, a limiting slider is slidably arranged on the support column, the other side of the limiting slider is cooperated with a driving shaft, and the winding moving part includes a rotating shaft connected to the auxiliary winding drum.

[0005] As a further improvement of the present invention, in order to ensure stable linkage between the winding drive motor and internal components, the winding drive motor is cooperated with a plurality of groups of transmission belts, the winding drive motor is connected with a winding auxiliary wheel, each of the winding auxiliary wheels is connected with a fixed winding drum through a transmission belt, the fixed winding drum is connected with a first transmission wheel, and the auxiliary winding drum is connected with a second transmission wheel.

[0006] As a further improvement of the present invention, in order to ensure stable driving of the limiting sliding wheel and the limiting mechanism, the auxiliary winding drum is arranged with a protruding movable slide groove, and a limiting sliding wheel is arranged on the other side of the auxiliary winding drum. The limiting sliding wheel is connected with reinforcing ribs, and the reinforcing ribs of the limiting sliding wheels at both ends are concentrated at one point and connected to the driving shaft.

[0007] To achieve the above object, the present invention also provides a method for preparing polypropylene filaments, and the steps of preparing the polypropylene filaments are as follows: Step 1: Polypropylene masterbatch needs to be pre-treated before use. The polypropylene masterbatch needs to be dried. Drying can remove moisture from the raw materials to avoid bubbles or affect product quality during subsequent processing; Step 2: Add polypropylene masterbatch, 1-5% liquid crystal polymer, and 1-5% cooling masterbatch into a hopper, wherein the liquid crystal polymer is one or more of poly(diphenyl terephthalate), poly(naphthalene terephthalate), poly(hydroquinone terephthalate), and poly(ethylene terephthalate); Step 3: The raw materials in the above step 1 are heated and melted at 250-320°C, and extruded into a spinning box through a twin screw at a temperature of 220-280°C at a pressure of 7.0-10.0MPa; Step 4: Control the temperature of the spinning box to 200-260°C and the pressure to 5.0-10.0MPa, so that the liquid crystal polymer enters the liquid crystal state and the polypropylene is in the molten state; Step 5: The mixture in the spinning box is spun into a tow through a spinneret, and the tow enters a cooling water tank for water cooling. The water temperature is controlled at 10-20°C, and the spinneret is 3-10 cm away from the water surface; Step 6: After being cooled by water, the tow enters a horizontal stretching machine for stretching, wherein the temperature of the hot roller of the stretching machine is controlled at 80-135°C and the stretching speed is 50-200 m / min; Step 7: After the stretching in step 5 is completed, the filament is cooled to room temperature in a cooling room for 5-20 m and wound to obtain a high-strength polypropylene filament.

[0008] A method for preparing polypropylene filaments, wherein the specific steps of winding and forming in step seven are as follows: Step 1: After the tow is cooled by water, it enters the horizontal stretching machine for stretching. After the stretching, it passes through a cooling room for 5-20m to cool down to room temperature; Step 2: The wire bundle will first contact the fixed winding drum on the winding mechanism, the winding drive motor will start, the wire bundle will be wound around the fixed winding drum, the fixed winding drum will rotate, and the winding auxiliary wheel will rotate; Step 3: The fixed winding drum rotates, and the rotating shaft connected to the fixed winding drum rotates synchronously; Step 4: The fixed winding drum is synchronously driven with the first transmission wheel, and the auxiliary winding drum is synchronously driven with the second transmission wheel; Step 5: The first transmission wheel cooperates with the second transmission wheel of the auxiliary winding drum through the transmission belt, and the second transmission wheel drives the auxiliary winding drum to perform auxiliary winding under the action of the first transmission wheel and the transmission belt; Step six: The auxiliary winding drum slides in the movable slide groove through the limiting sliding wheel. The reinforcing ribs of the limiting sliding wheels at both ends are concentrated at one point and are connected to the driving shaft. The driving shaft is connected to the limiting slider. When the limiting slider moves downward, it drives the limiting sliding wheel to extend to both sides and simultaneously drives the auxiliary winding drum to slide to both sides; when the limiting slider moves upward, it drives the limiting sliding wheel to extend inwardly and simultaneously drives the auxiliary winding drum to slide inwardly for auxiliary winding.

[0009] When the present invention is working, the purpose of the present invention is to provide a high-strength polypropylene filament and a preparation method thereof, in view of the defect that the radial crystallization of the filament bundle will affect the tensile orientation of the fiber during the traditional side-blowing air cooling during polypropylene spinning, thereby reducing the tensile orientation degree, further affecting its crystallization setting, and finally affecting the strength of the finished filament. The high-strength polypropylene filament has a breaking strength of ≥7.0 cN / dtex and a breaking elongation of less than ≤18%. The preparation method of the high-strength polypropylene filament is as follows: liquid crystal polymer is added to polypropylene pellets, first heated and melted; during the spinning process, the liquid crystal unit in the liquid crystal polymer is oriented along the fiber axis under the action of capillary force and traction force; then, during the stretching process, the polypropylene in the fiber is recrystallized by using isothermal annealing treatment technology, and under the induction of the liquid crystal unit, the recrystallized polypropylene crystals are oriented along the axial direction, thereby obtaining high-strength polypropylene filament with high thermal stability.

[0010] The beneficial effects of the present invention are as follows: a small amount of liquid crystal polymer is used in the method for preparing high-strength polypropylene filaments of the present invention, and during the spinning process, the liquid crystal unit in the liquid crystal polymer is oriented along the fiber axis under the action of capillary force and traction force; then, during the stretching process, the polypropylene in the fiber is recrystallized by using an isothermal annealing treatment technology, and under the induction of the liquid crystal unit, the recrystallized polypropylene crystals are oriented along the axial direction, thereby obtaining high-strength polypropylene filaments with high thermal stability; the polypropylene crystals of the polypropylene filaments prepared by the method of the present invention are oriented along the fiber axis, the strength is high, the breaking strength is ≥7.0 cN / dtex, and the breaking elongation is less than ≤18%; the method is simple to operate, and can directly realize the preparation of high-strength polypropylene filaments on existing polypropylene filament spinning equipment, and the equipment requirements are low. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] In order to facilitate the understanding of those skilled in the art, the present invention is further described below with reference to the accompanying drawings: Figure 1 It is a front view structural diagram of the present invention.

[0012] Figure 2 It is a side structural diagram of the present invention.

[0013] Figure 3 It is a rear structural diagram of the present invention.

[0014] Figure 4 This is a structural diagram of the present invention without the unit casing.

[0015] Figure 5 It is the internal structure diagram of the present invention.

[0016] Among them, 1 is a winding unit frame, 2 is a unit casing, 3 is a winding drive motor, 4 is a fixed winding drum, 5 is a movable slide, 6 is an auxiliary winding drum, 7 is a winding movable part, 8 is a limiting mechanism, 801 is a fixed block, 802 is a support column, 803 is a limiting slider, 804 is a driving shaft, 9 is a limiting plate, 10 is a transmission belt, 11 is a winding auxiliary wheel, 12 is a first transmission wheel, 13 is a second transmission wheel, 14 is a limiting sliding wheel, and 15 is a reinforcing rib. DETAILED DESCRIPTION

[0017] In order to enable those skilled in the art to better understand the technical solution in this application, Figure 1-5 The present invention is further described. The following examples are only used to more clearly illustrate the technical solution of the present invention, and are not intended to limit the protection scope of the present invention.

[0018] like Figure 1-5 A winding mechanism for preparing polypropylene filaments shown in the figure includes a winding mechanism, the winding mechanism includes a winding unit frame 1, the winding unit frame 1 is provided with a unit housing 2, a winding drive motor 3 is arranged outside the unit housing 2, a fixed winding drum 4 is arranged on one side of the unit housing 2, an arc-shaped moving slide 5 is arranged below the fixed winding drum 4, the moving slide 5 is arranged at both ends of one side of the unit housing 2, an auxiliary winding drum 6 is arranged outside the moving slide 5, and the winding unit frame 1 is arranged inside There is a winding moving part 7, a limiting mechanism 8 is arranged on the other side of the unit casing 2, a limiting plate 9 is arranged below the limiting mechanism 8, the limiting mechanism 8 includes a fixed block 801 arranged between the winding unit frame 1 and the limiting plate 9, a support column 802 is arranged between the fixed block 801, a limiting slider 803 is slidably arranged on the support column 802, and a driving shaft 804 is cooperated with the other side of the limiting slider 803, and the winding moving part 7 includes a rotating shaft 701 arranged to be connected to the auxiliary winding drum 6.

[0019] The winding drive motor 3 is equipped with several groups of transmission belts 10, and the winding drive motor 3 is connected to a winding auxiliary wheel 11. Each of the winding auxiliary wheels 11 is connected to a fixed winding drum 4 through a transmission belt 10. The fixed winding drum 4 is connected to a first transmission wheel 12, and the auxiliary winding drum 6 is connected to a second transmission wheel 13.

[0020] The auxiliary winding drum 6 is arranged to protrude from the movable slide groove 5, and a limiting sliding wheel 14 is arranged on the other side of the auxiliary winding drum 6. The limiting sliding wheel 14 is connected with a reinforcing rib 15. The reinforcing ribs 15 of the limiting sliding wheels 14 at both ends are concentrated at one point and are connected to the driving shaft 804.

[0021] A method for preparing polypropylene filaments, the steps of preparing the polypropylene filaments are as follows: Step 1: Polypropylene masterbatch needs to be pre-treated before use. The polypropylene masterbatch needs to be dried. Drying can remove moisture from the raw materials to avoid bubbles or affect product quality during subsequent processing; Step 2: Add polypropylene masterbatch, 1-5% liquid crystal polymer, and 1-5% cooling masterbatch into a hopper, wherein the liquid crystal polymer is one or more of poly(diphenyl terephthalate), poly(naphthalene terephthalate), poly(hydroquinone terephthalate), and poly(ethylene terephthalate); Step 3: The raw materials in the above step 1 are heated and melted at 250-320°C, and extruded into a spinning box through a twin screw at a temperature of 220-280°C at a pressure of 7.0-10.0MPa; Step 4: Control the temperature of the spinning box to 200-260°C and the pressure to 5.0-10.0MPa, so that the liquid crystal polymer enters the liquid crystal state and the polypropylene is in the molten state; Step 5: The mixture in the spinning box is spun into a tow through a spinneret, and the tow enters a cooling water tank for water cooling. The water temperature is controlled at 10-20°C, and the spinneret is 3-10 cm away from the water surface; Step 6: After being cooled by water, the tow enters a horizontal stretching machine for stretching, wherein the temperature of the hot roller of the stretching machine is controlled at 80-135°C and the stretching speed is 50-200 m / min; Step 7: After the stretching in step 5 is completed, the filament is cooled to room temperature in a cooling room for 5-20 m and wound to obtain a high-strength polypropylene filament.

[0022] The specific steps of winding forming in step seven are as follows: Step 1: After the tow is cooled by water, it enters the horizontal stretching machine for stretching. After the stretching, it passes through a cooling room for 5-20m to cool down to room temperature; Step 2: The wire bundle first contacts the fixed winding drum 4 on the winding mechanism, the winding drive motor runs, the wire bundle is wound onto the fixed winding drum 4, the fixed winding drum 4 rotates, and the winding auxiliary wheel 11 rotates; Step 3: The fixed winding drum 4 rotates, and the rotating shaft 701 connected to the fixed winding drum 4 rotates synchronously; Step 4: The fixed winding drum 4 and the first transmission wheel 12 are driven synchronously, and the auxiliary winding drum 6 and the second transmission wheel 13 are driven synchronously; Step 5: The first transmission wheel 12 cooperates with the second transmission wheel 13 of the auxiliary winding drum 6 through the transmission belt 10. Under the action of the first transmission wheel 12 and the transmission belt 10, the second transmission wheel 13 drives the auxiliary winding drum 6 to perform auxiliary winding; Step six: The auxiliary winding drum 6 slides in the movable slide groove 5 through the limiting sliding wheel 14. The reinforcing ribs 15 of the limiting sliding wheels 14 at both ends are concentrated at one point and are connected to the driving shaft 804. The driving shaft 804 is connected to the limiting slider 803. When the limiting slider 803 moves downward, it drives the limiting sliding wheel 14 to extend to both sides, and simultaneously drives the auxiliary winding drum 6 to slide to both sides; when the limiting slider 803 moves upward, it drives the limiting sliding wheel 14 to extend inwardly, and simultaneously drives the auxiliary winding drum 6 to slide inwardly for auxiliary winding.

[0023] When the present invention is working, in view of the defect that the radial crystallization of the filament bundle will affect the tensile orientation of the fiber during the traditional side-blowing air cooling during polypropylene spinning, thereby reducing the tensile orientation degree, further affecting its crystallization setting, and finally affecting the strength of the finished fiber, a high-strength polypropylene filament and a preparation method thereof are provided, wherein the breaking strength of the high-strength polypropylene filament is ≥7.0 cN / dtex, and the breaking elongation is less than ≤18%. The preparation method of the high-strength polypropylene filament is as follows: liquid crystal polymer is added to polypropylene pellets, and first heated and melted; during the spinning process, the liquid crystal unit in the liquid crystal polymer is oriented along the axial direction of the fiber under the action of capillary force and traction force; then, during the stretching process, the polypropylene in the fiber is recrystallized by using isothermal annealing treatment technology, and under the induction of the liquid crystal unit, the recrystallized polypropylene crystals are oriented along the axial direction, thereby obtaining high-strength polypropylene filament with high thermal stability; the following describes an embodiment of the preparation method of the present invention, but the following embodiment is used to illustrate the present invention and does not constitute any limitation to the claims of the present invention. Example 1

[0024] Step 1: Add polypropylene masterbatch, 2% poly(diphenyl terephthalate), and 2% cooling masterbatch into the hopper; Step 2: The raw materials in the above step 1 are heated and melted at 310°C, and extruded into a spinning box through a twin screw at a pressure of 7.0 MPa, wherein the temperature of zone 1 of the screw extruder is 240-250°C, the temperature of zone 2 is 250-260°C, the temperature of zone 3 is 260-280°C, the temperature of zone 4 is 260-270°C, and the temperature of zone 5 is 250-260°C; Step 3: Control the temperature of the spinning box to 210°C and the pressure to 5.0 MPa, so that the liquid crystal polymer enters the liquid crystal state and the polypropylene is in the molten state; Step 4: The mixture in the spinning box is spun into a tow through a spinneret, and the tow enters a cooling water tank for water cooling. The water temperature is controlled at 20°C, and the spinneret is 8 cm away from the water surface; Step 5: After being cooled by water, the tow enters a horizontal stretching machine for stretching, wherein the temperature of the hot roller of the stretching machine is controlled at 130°C and the stretching speed is 150m / min; Step 6: After the stretching in step 5 is completed, the filament is cooled to room temperature in a cooling room for 10 m and wound to obtain a high-strength polypropylene filament.

[0025] The breaking strength of the high-strength polypropylene filament is 7.4 cN / dtex, and the breaking elongation is 17.2%. Example 2

[0026] Step 1: Add polypropylene masterbatch, 4% poly(diphenyl terephthalate), and 2% cooling masterbatch into the hopper; Step 2: The raw materials in the above step 1 are heated and melted at 310°C, and extruded into a spinning box through a twin screw at a pressure of 7.0 MPa, wherein the temperature of zone 1 of the screw extruder is 240-250°C, the temperature of zone 2 is 250-260°C, the temperature of zone 3 is 260-280°C, the temperature of zone 4 is 260-270°C, and the temperature of zone 5 is 250-260°C; Step 3: Control the temperature of the spinning box to 210°C and the pressure to 5.0 MPa, so that the liquid crystal polymer enters the liquid crystal state and the polypropylene is in the molten state; Step 4: The mixture in the spinning box is spun into a tow through a spinneret, and the tow enters a cooling water tank for water cooling. The water temperature is controlled at 20°C, and the spinneret is 8 cm away from the water surface; Step 5: After being cooled by water, the tow enters a horizontal stretching machine for stretching, wherein the temperature of the hot roller of the stretching machine is controlled at 130°C and the stretching speed is 150m / min; Step 6: After the stretching in step 5 is completed, the filament is cooled to room temperature in a cooling room for 10 m and wound to obtain a high-strength polypropylene filament.

[0027] The breaking strength of the high-strength polypropylene filament is 8.5 cN / dtex, and the breaking elongation is 16.1%. Example 3

[0028] Step 1: Add polypropylene masterbatch, 2% polyhydroquinone terephthalate, and 2% cooling masterbatch into the hopper; Step 2: The raw materials in the above step 1 are heated and melted at 310°C, and extruded into a spinning box through a twin screw at a pressure of 7.0 MPa, wherein the temperature of zone 1 of the screw extruder is 240-250°C, the temperature of zone 2 is 250-260°C, the temperature of zone 3 is 260-280°C, the temperature of zone 4 is 260-270°C, and the temperature of zone 5 is 250-260°C; Step 3: Control the temperature of the spinning box to 210°C and the pressure to 5.0 MPa, so that the liquid crystal polymer enters the liquid crystal state and the polypropylene is in the molten state; Step 4: The mixture in the spinning box is spun into a tow through a spinneret, and the tow enters a cooling water tank for water cooling. The water temperature is controlled at 20°C, and the spinneret is 8 cm away from the water surface; Step 5: After being cooled by water, the tow enters a horizontal stretching machine for stretching, wherein the temperature of the hot roller of the stretching machine is controlled at 130°C and the stretching speed is 150m / min; Step 6: After the stretching in step 5 is completed, the filament is cooled to room temperature in a cooling room for 10 m and wound to obtain a high-strength polypropylene filament.

[0029] The breaking strength of the high-strength polypropylene filament is 7.9 cN / dtex, and the breaking elongation is 16.8%. Example 4

[0030] Step 1: Add polypropylene masterbatch, 1% poly(diphenyl terephthalate), 1% poly(hydroquinone terephthalate), and 2% cooling masterbatch into the hopper; Step 2: The raw materials in the above step 1 are heated and melted at 310°C, and extruded into a spinning box through a twin screw at a pressure of 7.0 MPa, wherein the temperature of zone 1 of the screw extruder is 240-250°C, the temperature of zone 2 is 250-260°C, the temperature of zone 3 is 260-280°C, the temperature of zone 4 is 260-270°C, and the temperature of zone 5 is 250-260°C; Step 3: Control the temperature of the spinning box to 210°C and the pressure to 5.0 MPa, so that the liquid crystal polymer enters the liquid crystal state and the polypropylene is in the molten state; Step 4: The mixture in the spinning box is spun into a tow through a spinneret, and the tow enters a cooling water tank for water cooling. The water temperature is controlled at 20°C, and the spinneret is 8 cm away from the water surface; Step 5: After being cooled by water, the tow enters a horizontal stretching machine for stretching, wherein the temperature of the hot roller of the stretching machine is controlled at 130°C and the stretching speed is 150m / min; Step 6: After the stretching in step 5 is completed, the filament is cooled to room temperature in a cooling room for 10 m and wound to obtain a high-strength polypropylene filament.

[0031] The breaking strength of the high-strength polypropylene filament is 7.7 cN / dtex, and the breaking elongation is 17.0%. Example 5

[0032] Step 1: Add polypropylene masterbatch, 2% poly(diphenyl terephthalate), and 2% cooling masterbatch into the hopper; Step 2: The raw materials in the above step 1 are heated and melted at 310°C, and extruded into a spinning box through a twin screw at a pressure of 7.0 MPa, wherein the temperature of zone 1 of the screw extruder is 240-250°C, the temperature of zone 2 is 250-260°C, the temperature of zone 3 is 260-280°C, the temperature of zone 4 is 260-270°C, and the temperature of zone 5 is 250-260°C; Step 3: Control the temperature of the spinning box to 210°C and the pressure to 7.0 MPa, so that the liquid crystal polymer enters the liquid crystal state and the polypropylene is in the molten state; Step 4: The mixture in the spinning box is spun into a tow through a spinneret, and the tow enters a cooling water tank for water cooling. The water temperature is controlled at 20°C, and the spinneret is 8 cm away from the water surface; Step 5: After being cooled by water, the tow enters a horizontal stretching machine for stretching, wherein the temperature of the hot roller of the stretching machine is controlled at 130°C and the stretching speed is 150m / min; Step 6: After the stretching in step 5 is completed, the filament is cooled to room temperature in a cooling room for 10 m and wound to obtain a high-strength polypropylene filament.

[0033] The breaking strength of the high-strength polypropylene filament is 7.1 cN / dtex, and the breaking elongation is 17.7%. Example 6

[0034] Step 1: Add polypropylene masterbatch, 2% poly(diphenyl terephthalate), and 2% cooling masterbatch into the hopper; Step 1: The raw materials in the above step 1 are heated and melted at 310°C, and extruded into a spinning box through a twin-screw extruder at a pressure of 7.0 MPa, wherein the temperature of zone 1 of the screw extruder is 240-250°C, the temperature of zone 2 is 250-260°C, the temperature of zone 3 is 260-280°C, the temperature of zone 4 is 260-270°C, and the temperature of zone 5 is 250-260°C; Step 3: Control the temperature of the spinning box to 210°C and the pressure to 5.0 MPa, so that the liquid crystal polymer enters the liquid crystal state and the polypropylene is in the molten state; Step 4: The mixture in the spinning box is spun into a tow through a spinneret, and the tow enters a cooling water tank for water cooling. The water temperature is controlled at 20°C, and the spinneret is 8 cm away from the water surface; Step 5: After being cooled by water, the tow enters a horizontal stretching machine for stretching, wherein the temperature of the hot roller of the stretching machine is controlled at 125°C and the stretching speed is 150m / min; Step 6: After the stretching in step 5 is completed, the filament is cooled to room temperature in a cooling room for 10 m and wound to obtain a high-strength polypropylene filament.

[0035] The breaking strength of the high-strength polypropylene filament is 7.6 cN / dtex, and the breaking elongation is 17.0%. Example 7

[0036] Step 1: Add polypropylene masterbatch, 2% poly(diphenyl terephthalate), and 2% cooling masterbatch into the hopper; Step 2: The raw materials in the above step 1 are heated and melted at 310°C, and extruded into a spinning box through a twin screw at a pressure of 7.0 MPa, wherein the temperature of zone 1 of the screw extruder is 240-250°C, the temperature of zone 2 is 250-260°C, the temperature of zone 3 is 260-280°C, the temperature of zone 4 is 260-270°C, and the temperature of zone 5 is 250-260°C; Step 3: Control the temperature of the spinning box to 210°C and the pressure to 5.0 MPa, so that the liquid crystal polymer enters the liquid crystal state and the polypropylene is in the molten state; Step 4: The mixture in the spinning box is spun into a tow through a spinneret, and the tow enters a cooling water tank for water cooling. The water temperature is controlled at 20°C, and the spinneret is 8 cm away from the water surface; Step 5: After being cooled by water, the tow enters a horizontal stretching machine for stretching, wherein the temperature of the hot roller of the stretching machine is controlled at 130°C and the stretching speed is 200m / min; Step 6: After the stretching in step 5 is completed, the filament is cooled to room temperature in a cooling room for 10 m and wound to obtain a high-strength polypropylene filament.

[0037] The breaking strength of the high-strength polypropylene filament is 7.8 cN / dtex, and the breaking elongation is 16.9%. Example 8

[0038] Step 1: Add polypropylene masterbatch, 2% poly(diphenyl terephthalate), and 2% cooling masterbatch into the hopper; Step 2: The raw materials in the above step 1 are heated and melted at 310°C, and extruded into a spinning box through a twin screw at a pressure of 7.0 MPa, wherein the temperature of zone 1 of the screw extruder is 240-250°C, the temperature of zone 2 is 250-260°C, the temperature of zone 3 is 260-280°C, the temperature of zone 4 is 260-270°C, and the temperature of zone 5 is 250-260°C; Step 3: Control the temperature of the spinning box to 210°C and the pressure to 5.0 MPa, so that the liquid crystal polymer enters the liquid crystal state and the polypropylene is in the molten state; Step 4: The mixture in the spinning box is spun into a tow through a spinneret, and the tow enters a cooling water tank for water cooling. The water temperature is controlled at 20°C, and the spinneret is 8 cm away from the water surface; Step 5: After being cooled by water, the tow enters a horizontal stretching machine for stretching, wherein the temperature of the hot roller of the stretching machine is controlled at 130°C and the stretching speed is 150m / min; Step 6: After the stretching in step 5 is completed, the filament is cooled to room temperature in a cooling room for 20 m and wound to obtain a high-strength polypropylene filament.

[0039] The breaking strength of the high-strength polypropylene filament is 7.9 cN / dtex, and the breaking elongation is 16.4%.

[0040] Comparative Example 1 Step 1: Add polypropylene masterbatch and 2% cooling masterbatch into the hopper; Step 2: The raw materials in the above step 1 are heated and melted at 310°C, and extruded into a spinning box through a twin screw at a pressure of 7.0 MPa, wherein the temperature of zone 1 of the screw extruder is 240-250°C, the temperature of zone 2 is 250-260°C, the temperature of zone 3 is 260-280°C, the temperature of zone 4 is 260-270°C, and the temperature of zone 5 is 250-260°C; Step 3: Control the temperature of the spinning box to 210°C and the pressure to 5.0MPa to keep the polypropylene in a molten state; Step 4: The mixture in the spinning box is spun into a tow through a spinneret, and the tow enters a cooling water tank for water cooling. The water temperature is controlled at 20°C, and the spinneret is 8 cm away from the water surface; Step 5: After being cooled by water, the tow enters a horizontal stretching machine for stretching, wherein the temperature of the hot roller of the stretching machine is controlled at 130°C and the stretching speed is 150m / min; Step 6: After the stretching in step 5 is completed, the filament is cooled to room temperature in a cooling room for 10 m and wound to obtain a high-strength polypropylene filament.

[0041] The breaking strength of the high-strength polypropylene filament is 6.2 cN / dtex, and the breaking elongation is 20.2%.

[0042] The present invention is not limited to the above-mentioned embodiments. On the basis of the technical solution disclosed in the present invention, technicians in this field can make some substitutions and deformations to some technical features therein according to the disclosed technical content without creative labor, and these substitutions and deformations are all within the protection scope of the present invention.

Claims

1. A winding mechanism for preparing polypropylene filaments, comprising a winding mechanism, characterized in that: The winding mechanism comprises a winding unit frame (1), the winding unit frame (1) being provided with a unit housing (2), a winding drive motor (3) being provided outside the unit housing (2), a fixed winding drum (4) being provided on one side of the unit housing (2), an arc-shaped movable slide groove (5) being provided below the fixed winding drum (4), the movable slide groove (5) being provided at two ends of one side of the unit housing (2), an auxiliary winding drum (6) being provided outside the movable slide groove (5), a winding movable component (7) being provided inside the winding unit frame (1), and the unit housing (2) being provided with a plurality of winding drive motors (3). A limiting mechanism (8) is arranged on the other side of the shell (2), a limiting plate (9) is arranged below the limiting mechanism (8), the limiting mechanism (8) comprises a fixed block (801) arranged between the winding unit frame (1) and the limiting plate (9), a support column (802) is arranged between the fixed blocks (801), a limiting slider (803) is slidably arranged on the support column (802), a driving shaft (804) is matched with the other side of the limiting slider (803), and the winding moving component (7) comprises a rotating shaft (701) arranged to be connected to the auxiliary winding drum (6).

2. A winding mechanism for preparing polypropylene filaments according to claim 1, characterized in that: The winding drive motor (3) is provided with a plurality of groups of transmission belts (10) in cooperation with the winding drive motor (3), the winding drive motor (3) is connected to a winding auxiliary wheel (11), each of the winding auxiliary wheels (11) is connected to a fixed winding drum (4) via a transmission belt (10), the fixed winding drum (4) is connected to a first transmission wheel (12), and the auxiliary winding drum (6) is connected to a second transmission wheel (13).

3. A winding mechanism for preparing polypropylene filaments according to claim 1, characterized in that: The auxiliary winding drum (6) is arranged to protrude from the movable slide groove (5), and a limited sliding wheel (14) is arranged on the other side of the auxiliary winding drum (6). The limited sliding wheel (14) is connected to a reinforcing rib (15), and the reinforcing ribs (15) of the limited sliding wheels (14) at both ends are concentrated at one point and are connected to the driving shaft (804).

4. The method for preparing polypropylene filament according to claim 1, characterized in that: The preparation method of the polypropylene filament comprises the following steps: Step 1: Polypropylene masterbatch needs to be pre-treated before use. The polypropylene masterbatch needs to be dried. Drying can remove moisture from the raw materials to avoid bubbles or affect product quality during subsequent processing; Step 2: Add polypropylene masterbatch, 1-5% liquid crystal polymer, and 1-5% cooling masterbatch into a hopper, wherein the liquid crystal polymer is one or more of poly(diphenyl terephthalate), poly(naphthalene terephthalate), poly(hydroquinone terephthalate), and poly(ethylene terephthalate); Step 3: The raw materials in the above step 1 are heated and melted at 250-320°C, and extruded into a spinning box through a twin screw at a temperature of 220-280°C at a pressure of 7.0-10.0MPa; Step 4: Control the temperature of the spinning box to 200-260°C and the pressure to 5.0-10.0MPa, so that the liquid crystal polymer enters the liquid crystal state and the polypropylene is in the molten state; Step 5: The mixture in the spinning box is spun into a tow through a spinneret, and the tow enters a cooling water tank for water cooling. The water temperature is controlled at 10-20°C, and the spinneret is 3-10 cm away from the water surface; Step 6: After being cooled by water, the tow enters a horizontal stretching machine for stretching, wherein the temperature of the hot roller of the stretching machine is controlled at 80-135°C and the stretching speed is 50-200 m / min; Step 7: After the stretching in step 5 is completed, the filament is cooled to room temperature in a cooling room for 5-20 m and wound to obtain a high-strength polypropylene filament.

5. The method for preparing polypropylene filament according to claim 4, characterized in that: The specific steps of winding forming in step seven are as follows: Step 1: After the tow is cooled by water, it enters the horizontal stretching machine for stretching. After the stretching, it passes through a cooling room for 5-20m to cool down to room temperature; Step 2: The wire bundle first contacts the fixed winding drum (4) on the winding mechanism, the winding drive motor runs, the wire bundle is wound onto the fixed winding drum (4), the fixed winding drum (4) rotates, and the winding auxiliary wheel (11) rotates; Step 3: The fixed winding drum (4) rotates, and the rotating shaft (701) connected to the fixed winding drum (4) rotates synchronously; Step 4: The fixed winding drum (4) and the first transmission wheel (12) are driven synchronously, and the auxiliary winding drum (6) and the second transmission wheel (13) are driven synchronously; Step 5: The first transmission wheel (12) cooperates with the second transmission wheel (13) of the auxiliary winding drum (6) through the transmission belt (10), and the second transmission wheel (13) drives the auxiliary winding drum (6) to perform auxiliary winding under the action of the first transmission wheel (12) and the transmission belt (10); Step 6: The auxiliary winding drum (6) slides in the movable slide groove (5) through the limit sliding wheel (14), and the reinforcing ribs (15) of the limit sliding wheels (14) at both ends are concentrated at one point and connected to the drive shaft (804). The drive shaft (804) is connected to the limit sliding block (803). When the limit sliding block (803) moves downward, it drives the limit sliding wheel (14) to extend to both sides and simultaneously drives the auxiliary winding drum (6) to slide to both sides; when the limit sliding block (803) moves upward, it drives the limit sliding wheel (14) to extend inwardly and simultaneously drives the auxiliary winding drum (6) to slide inwardly to perform auxiliary winding.