Method for preparing SiC fiber by in-situ regulation and control of fiber surface carbon
By controlling the pyrolytic carbon deposition by adjusting the pressure in the high-temperature furnace, the thickness of the carbon-rich layer on the surface of the SiC fiber is controlled in situ, which solves the problems of high SiC fiber preparation cost and limited resistivity adjustment range in the existing technology, and achieves high mechanical properties. and SiC fibers of various resistivities.
Patent Information
- Application Number
- CN202411029405.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-15
AI Technical Summary
Existing SiC fiber preparation methods have problems such as high preparation cost, limited resistivity adjustment range, and damaged mechanical properties. It is difficult to take into account the mechanical properties and electrical properties of the fiber, and cannot meet the requirements of the fiber as a load-bearing phase and a functional phase.
Polycarbosilane is melt-spun and oxidatively cross-linked to obtain infusible fibers, which are fired in a high-temperature furnace. The pressure in the furnace is adjusted to control the deposition of pyrolytic carbon on the fiber surface to achieve the thickness of the carbon-rich layer on the surface of the SiC fiber. Through in-situ control, SiC fibers with different resistivities were prepared.
The preparation of SiC fibers with different resistivities has been achieved, and the fibers have excellent mechanical properties and low cost, simplifying the synthesis process and avoiding complicated unmelting or firing processes.
Smart Images

Figure CN118773776A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing SiC fiber, and in particular to a method for preparing SiC fiber by in-situ regulating carbon on the fiber surface, and belongs to the technical field of silicon carbide fiber. Background Art
[0002] The high-speed development of weapons and equipment is an important trend in future development. The high-speed flight of aircraft in the atmosphere will cause the surface temperature of the aircraft to rise. At the same time, the high-temperature components in the engine will also strongly scatter radar waves, becoming the main source of radar scattering in the rear of the aircraft. In short, the radar exposure symptoms of high-temperature parts on high-speed aircraft are more significant, which greatly limits its penetration capability and combat power improvement. Due to the constraints of power, aerodynamics and other conditions, there are fewer stealth technologies available, and high-temperature absorbing materials have become an important way to solve the problem of stealth of high-temperature components of aircraft.
[0003] Continuous fiber reinforced ceramic matrix composites (CMC) have the characteristics of high temperature resistance, low density and excellent mechanical properties. At the same time, by adjusting its composition structure, it can achieve the function of wave absorption. Therefore, it is widely studied as a high-temperature structural functional integrated material with both load-bearing and wave absorption. SiC fiber has the advantages of high temperature resistance, oxidation resistance, high specific strength and specific modulus, and has become an important reinforcing fiber variety in CMC. In addition to the above characteristics, SiC fiber also has a wide range of electrical performance regulation. Japan's UBE company reported semiconductor-grade SiC fiber, and its different grades of products correspond to 10 -1 ~10 6 The resistivity is in the Ωcm range. Japan Carbon Corporation also reported a 10 3 ~10 4 Ωcm NL200, 10 6 ~10 7 Ωcm NL400, 10 -1 ~10 0 Ωcm of NL500, and 10 -1 There are different brands of products such as NL607 with Ωcm. However, none of the above products report the methods of achieving different resistivities.
[0004] Polycarbosilane (PCS) fibers are transformed into SiC fibers after air infusibility treatment and sintering. SiC fibers can be considered to be composed of SiC phase, free carbon phase and Si-OC amorphous phase. The three phases have obvious resistivity differences. The resistivity of SiC fibers can be controlled by adjusting the composition ratio of the three phases. Chollon sintered the electron beam irradiated polycarbosilane infusible fibers at different temperatures to obtain SiC fibers with an oxygen content of less than 1%. The resistivity of the obtained SiC fibers is related to the sintering temperature. In addition, Chollon also studied the effect of the sintering atmosphere on the resistivity. When the infusible fibers were sintered in a hydrogen-containing atmosphere, the carbon content in the obtained SiC fibers decreased as the hydrogen content increased, and the resistivity increased accordingly (Journal of the European Ceramic Society, 1998, 18: 125-133). Gou et al. (Journal of the European Ceramic Society, 2017, 37: 517-522) conducted a similar study. When the firing atmosphere contains hydrogen or ammonia, the resistivity increases due to the reduction of free carbon in the obtained SiC fiber or the formation of silicon nitride phase, but at the same time the fiber strength decreases significantly from 2.9 GPa to 1.6 GPa. Some researchers have used electron beam irradiation or chemical vapor crosslinking instead of air oxidation crosslinking to treat polycarbosilane infusibility, reduce the oxygen content in the obtained SiC fiber, increase the carbon content, and reduce the resistivity of the fiber (Journal of Inorganic Materials, 2012, 27: 162-168). Wang Juan et al. prepared polycarbosilane with a high carbon content by co-cracking polydimethylsilane and polyvinyl chloride, which made the carbon content in the final SiC fiber higher and prepared low resistivity SiC fiber, but the tensile strength of the obtained fiber was low (<1.8) and decreased with the decrease of resistivity (Journal of the Chinese Society of Nonferrous Metals, 2001, 11: 377-381). Wang Yifei et al. introduced titanium into polycarbosilane to obtain SiC fiber containing titanium. The fiber resistivity increased from 10 to 10 with the increase of Ti content. 6 Ωcm can be reduced to 10 3 Ωcm, and the strength is less than 2.0GPa.
[0005] At the same time, the surface microstructure of SiC fibers, especially the thickness of the carbon-rich layer on the fiber surface, has a significant effect on the fiber resistivity. Hu Tianjiao et al. continuously and rapidly passed the infusible fibers through a high-temperature furnace, and the pyrolytic carbon produced by the pyrolysis of polycarbosilane was deposited on the fiber surface, thereby obtaining a resistivity of 10 0 -10 1 Ωcm SiC fiber. If there is no pyrolytic carbon deposition, the resistivity of the obtained SiC fiber is 10 5Ωcm. However, due to the continuous and rapid passage of the fiber through the high-temperature furnace, the obtained SiC fiber was not completely sintered, and the strength was less than 1.8GPa, which was seriously low (Materials Science and Engineering B, 2011, 176: 706-710). OKAMURA et al. oxidized titanium-containing SiC fiber to obtain an oxide layer on the fiber surface, thereby increasing the resistance of the fiber, but the strength was damaged. Tan et al. also conducted similar work and obtained a fiber with improved resistivity (Journal of Material Science, 2009, 44: 1172-1179).
[0006] The above publicly reported methods for changing the resistivity of SiC fibers have the problems of increasing the synthesis process, using complex infusibility or sintering processes, high preparation costs, limited resistivity adjustment range, and impaired mechanical properties. It is difficult to take into account both the mechanical and electrical properties of the fibers, and it is impossible to meet the requirements of the fibers being both load-bearing and functional phases. Therefore, it is urgent to develop a simple and efficient method for preparing silicon carbide fibers. Summary of the invention
[0007] In view of the shortcomings of the prior art, the present invention aims to provide a method for preparing SiC fibers by in-situ regulating the carbon on the fiber surface. The method is simple, low-cost, and can obtain SiC fibers with different resistivities and excellent mechanical properties.
[0008] In order to achieve the above technical objectives, the present invention provides a method for preparing SiC fibers by in-situ regulating the carbon on the fiber surface, the method comprising melt-spinning polycarbosilane to obtain precursor fibers, then heating the precursor fibers for oxidative cross-linking to obtain infusible fibers, and then placing the infusible fibers in a high-temperature furnace for firing; wherein, during the firing process, the pressure in the high-temperature furnace is adjusted to 100Pa to 130kPa.
[0009] Since the polycarbosilane infusible fiber is converted into SiC fiber through high-temperature sintering, carbon source substances such as alkanes and olefins are released during the sintering process, and the carbon source substances are converted into pyrolytic carbon at high temperature. Whether these pyrolytic carbons are deposited on the surface of the obtained SiC fiber and the deposition thickness directly affect the resistivity of the obtained fiber. The present invention utilizes the adjustment of the furnace pressure during the sintering process to control the deposition process of pyrolytic carbon on the fiber surface, thereby achieving in-situ regulation of the thickness of the carbon-rich layer on the surface of the SiC fiber, and preparing SiC fibers with different resistivities. At the same time, the fiber of the present invention is not damaged during the preparation process, so that the prepared SiC fiber has higher mechanical properties.
[0010] As a preferred solution, the carbon-rich layer on the surface of the SiC fiber has a thickness of 0 to 100 nm and a resistivity of 1 to 9×10 -2 ~1~9×106 Ωcm.
[0011] As a preferred solution, when the pressure in the high-temperature furnace is 100Pa to 9kPa, the SiC fiber surface obtained has no carbon-rich layer and the resistivity is 1 to 9×10 5 ~1~9×10 6 Ωcm, more preferably 8×10 5 ~5×10 6 Ωcm.
[0012] As a preferred solution, when the pressure in the high-temperature furnace is 10 kPa to 90 kPa, the carbon-rich layer on the surface of the SiC fiber obtained has a thickness of 1 to 5 nm and a resistivity of 1 to 9×10 3 ~1~9×10 4 Ωcm, more preferably 2×10 3 ~9×10 3 Ωcm.
[0013] As a preferred solution, when the pressure in the high-temperature furnace is 100 kPa to 104 kPa, the carbon-rich layer on the surface of the SiC fiber obtained has a thickness of 6 to 15 nm and a resistivity of 1 to 9×10 1 ~1~9×10 2 Ωcm, more preferably 1×10 2 ~7×10 2 Ωcm.
[0014] As a preferred solution, when the pressure in the high-temperature furnace is 105 kPa to 115 kPa, the carbon-rich layer on the surface of the SiC fiber has a thickness of 16 to 30 nm and a resistivity of 1 to 9 × 10 -1 ~1~9×10 0 Ωcm, more preferably 3×10 -1 ~9×10 -1 Ωcm.
[0015] As a preferred solution, when the pressure in the high-temperature furnace is 116 kPa to 130 kPa, the carbon-rich layer on the surface of the SiC fiber is 31 to 100 nm thick and has a resistivity of 1 to 9×10 -2 Ωcm, more preferably 1×10 -2 ~7×10 -2 Ωcm.
[0016] As a preferred solution, the diameter of the raw silk is 10-16 um.
[0017] As a preferred solution, the temperature of the oxidative cross-linking is 180-210°C.
[0018] As a preferred solution, the oxygen content in the infusible fiber is 5-16 wt %.
[0019] As a preferred solution, the sintering process is: heating to 1000-1400° C. under a protective atmosphere and then maintaining the temperature for 0.5-2 hours.
[0020] As a preferred solution, the protective atmosphere includes nitrogen and / or an inert gas.
[0021] As a preferred solution, the heating rate is 1-10°C / min.
[0022] As a preferred solution, the average single-filament tensile strength of the SiC fiber is not less than 2.5 GPa.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) By adopting the in-situ adjustment method of the present invention, the thickness of the carbon-rich layer on the surface of the obtained SiC fiber can be regulated by adjusting the pressure in the furnace during the sintering process, thereby preparing SiC fibers with different resistivities, without adding a complicated synthesis process, or using a special infusibility method, and a special sintering gas, which is simple, easy and low-cost;
[0025] (2) The mechanical properties of the SiC fiber produced are excellent. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0027] Figure 1 This is the surface Auger electron spectrum of the SiC fiber obtained in Example 1.
[0028] Figure 2 This is the surface Auger electron spectrum of the SiC fiber obtained in Example 3.
[0029] Figure 3 This is the surface Auger electron spectrum of the SiC fiber obtained in Example 4.
[0030] Figure 4 This is the surface Auger electron spectrum of the SiC fiber obtained in Example 5. DETAILED DESCRIPTION
[0031] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1
[0033] A method for preparing SiC fiber by in-situ regulating the carbon on the fiber surface, the specific steps are as follows:
[0034] S1: 2kg of PCS was melt-spun to produce 0.5k (500 strands / bundle) of continuous fibrils with a diameter ranging from 14um to 16um.
[0035] S2: The raw fibers were placed in a forced air oven for oxidation treatment at 200°C to obtain infusible fibers with an oxygen content of 11 wt%.
[0036] S3: Put the infusible fiber into a high-temperature furnace, replace the air in the furnace with high-purity nitrogen repeatedly for 3 times, turn on the vacuum pump, control the pressure in the furnace at 120Pa through the pressure sensor in the furnace and the solenoid valve on the gas line, and the heating rate is 8℃ / min. The furnace temperature is raised from room temperature to 1200℃ and kept warm for 0.5h to complete the sintering.
[0037] S4: When the high temperature furnace starts to cool down, turn off the vacuum pump and fill the furnace with nitrogen to normal pressure. Keep the nitrogen flowing in the high temperature furnace during the cooling process.
[0038] S5: The furnace temperature drops below 100°C, the furnace door is opened, and the SiC fiber is taken out.
[0039] S6: According to GB / T 34520.6-2017 "Continuous Silicon Carbide Fiber Test Method Part 6: Resistivity", the resistivity of the obtained SiC fiber was tested, and the resistivity was 1.5×10 6 Ωcm, and the fiber strength is 2.6GPa.
[0040] The Auger electron spectrum of the SiC fiber obtained in this example is as follows Figure 1 As shown, there is no oxygen-rich layer on the fiber surface.
[0041] Example 2
[0042] S1: 2kg of PCS was melt-spun to produce 0.5k (500 strands / bundle) of continuous fibrils with a diameter in the range of 12um-14um.
[0043] S2: The raw fibers were placed in a forced air oven for oxidation treatment at 195° C. to obtain infusible fibers with an oxygen content of 10 wt %.
[0044] S3: Put the infusible fiber into a high-temperature furnace, replace the air in the furnace with high-purity nitrogen repeatedly for 3 times, turn on the vacuum pump, control the pressure in the furnace at 70 kPa through the pressure sensor in the furnace and the solenoid valve on the gas line, and the heating rate is 5 ° C / min. The furnace temperature is raised from room temperature to 1300 ° C and kept warm for 1 hour to complete the sintering.
[0045] S4: When the high temperature furnace starts to cool down, turn off the vacuum pump and fill the furnace with nitrogen to normal pressure. Keep the nitrogen flowing in the high temperature furnace during the cooling process.
[0046] S5: The furnace temperature drops below 100°C, the furnace door is opened, and the SiC fiber is taken out.
[0047] S6: According to GB / T 34520.6-2017 "Continuous Silicon Carbide Fiber Test Method Part 6: Resistivity", the resistivity of the obtained SiC fiber was tested and the resistivity was 5.2×10 3 Ωcm, the fiber strength is 2.8GPa, and there is a carbon-rich layer about 3nm thick on the fiber surface.
[0048] Example 3
[0049] S1: 2kg of PCS was melt-spun to produce 0.5k (500 strands / bundle) of continuous fibrils with a diameter in the range of 13um-15um.
[0050] S2: The raw fibers were placed in a forced air oven for oxidation treatment at 190° C. to obtain infusible fibers with an oxygen content of 9 wt %.
[0051] S3: Put the infusible fiber into a high-temperature furnace, replace the air in the furnace with high-purity nitrogen repeatedly for 3 times, then turn off the vacuum pump and keep nitrogen flowing into the furnace. The pressure in the furnace is controlled at 100 kPa through the pressure sensor in the furnace and the solenoid valve on the gas line. The heating rate is 5 °C / min, and the furnace temperature is raised from room temperature to 1200 °C and kept warm for 1.5 hours to complete the sintering.
[0052] S4: Keep nitrogen flowing in the high-temperature furnace during the cooling process.
[0053] S5: The furnace temperature drops below 100°C, the furnace door is opened, and the SiC fiber is taken out.
[0054] S6: According to GB / T 34520.6-2017 "Continuous Silicon Carbide Fiber Test Method Part 6: Resistivity", the resistivity of the obtained SiC fiber was tested, and the resistivity was 4×10 2 Ωcm, and the fiber strength is 3.2GPa.
[0055] The Auger electron spectrum of the SiC fiber obtained in this example is as follows Figure 2As shown, there is a carbon-rich layer about 7 nm thick on the fiber surface.
[0056] Example 4
[0057] S1: 2kg of PCS was melt-spun to produce 0.5k (500 strands / bundle) of continuous fibrils with a diameter ranging from 11um to 13um.
[0058] S2: The raw fibers were placed in a forced air oven for oxidation treatment at 205°C to obtain infusible fibers with an oxygen content of 14 wt%.
[0059] S3: Put the infusible fiber into a high-temperature furnace, replace the air in the furnace with high-purity nitrogen repeatedly for 3 times, then turn off the vacuum pump and keep nitrogen flowing into the furnace. The pressure in the furnace is controlled at 112 kPa through the pressure sensor in the furnace and the solenoid valve on the gas line. The heating rate is 5 °C / min, and the furnace temperature is raised from room temperature to 1300 °C and kept for 2 hours to complete the sintering.
[0060] S4: Keep nitrogen flowing in the high-temperature furnace during the cooling process.
[0061] S5: The furnace temperature drops below 100°C, the furnace door is opened, and the SiC fiber is taken out.
[0062] S6: According to GB / T 34520.6-2017 "Continuous Silicon Carbide Fiber Test Method Part 6: Resistivity", the resistivity of the obtained SiC fiber was tested, and the resistivity was 6×10 -1 Ωcm, and the fiber strength is 3.5GPa.
[0063] The Auger electron spectrum of the SiC fiber obtained in this example is as follows Figure 3 As shown, there is a carbon-rich layer about 20 nm thick on the fiber surface.
[0064] Example 5
[0065] S1: 2kg of PCS was melt-spun to produce 0.5k (500 strands / bundle) of continuous fibrils with a diameter in the range of 12um-14um.
[0066] S2: The raw fibers were placed in a forced air oven for oxidation treatment at 180° C. to obtain infusible fibers with an oxygen content of 7 wt %.
[0067] S3: Put the infusible fiber into a high-temperature furnace, replace the air in the furnace with high-purity nitrogen repeatedly for 3 times, then turn off the vacuum pump and keep nitrogen flowing into the furnace. The pressure in the furnace is controlled at 122 kPa through the pressure sensor in the furnace and the solenoid valve on the gas line. The heating rate is 6 °C / min, and the furnace temperature is raised from room temperature to 1350 °C and kept for 2 hours to complete the sintering.
[0068] S4: Keep nitrogen flowing in the high-temperature furnace during the cooling process.
[0069] S5: The furnace temperature drops below 100°C, the furnace door is opened, and the SiC fiber is taken out.
[0070] S6: According to GB / T 34520.6-2017 "Continuous Silicon Carbide Fiber Test Method Part 6: Resistivity", the resistivity of the obtained SiC fiber was tested, and the resistivity was 4×10 -2 Ωcm, and the fiber strength is 2.8GPa.
[0071] The Auger electron spectrum of the SiC fiber obtained in this example is as follows Figure 4 As shown, there is a carbon-rich layer about 65 nm thick on the fiber surface.
[0072] Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing SiC fiber by in-situ regulating the carbon on the fiber surface, characterized in that: The polycarbosilane is melt-spun to obtain a raw fiber, and then the raw fiber is heated to perform oxidative cross-linking to obtain an infusible fiber, and then the infusible fiber is placed in a high-temperature furnace for firing; wherein, during the firing process, the pressure in the high-temperature furnace is adjusted to 100Pa to 130kPa.
2. The method for preparing SiC fiber by in-situ regulating carbon on the fiber surface according to claim 1, characterized in that: The carbon-rich layer on the surface of the SiC fiber has a thickness of 0 to 100 nm and a resistivity of 1 to 9×10 -2 ~1~9×10 6 Ωcm.
3. The method for preparing SiC fiber by in-situ regulating carbon on the fiber surface according to claim 1 or 2, characterized in that: When the pressure in the high-temperature furnace is 100Pa~9kPa, the SiC fiber surface has no carbon-rich layer and the resistivity is 1~9×10 5 ~1~9×10 6 Ωcm; When the pressure in the high-temperature furnace is 10 kPa to 90 kPa, the carbon-rich layer on the surface of the SiC fiber has a thickness of 1 to 5 nm and a resistivity of 1 to 9 × 10 3 ~1~9×10 4 Ωcm; When the pressure in the high-temperature furnace is 100 kPa to 104 kPa, the carbon-rich layer on the surface of the SiC fiber is 6 to 15 nm thick and has a resistivity of 1 to 9×10 1 ~1~9×10 2 Ωcm; When the pressure in the high-temperature furnace is 105 kPa to 115 kPa, the carbon-rich layer on the surface of the SiC fiber has a thickness of 16 to 30 nm and a resistivity of 1 to 9 × 10 -1 ~1~9×10 0 Ωcm; When the pressure in the high-temperature furnace is 116 kPa to 130 kPa, the carbon-rich layer on the surface of the SiC fiber has a thickness of 31 to 100 nm and a resistivity of 1 to 9 × 10 -2 Ωcm.
4. The method for preparing SiC fiber by in-situ regulating carbon on the fiber surface according to claim 1, characterized in that: The diameter of the raw silk is 10-16 um.
5. The method for preparing SiC fiber by in-situ regulating carbon on the fiber surface according to claim 1, characterized in that: The temperature of the oxidative crosslinking is 180-210°C.
6. The method for preparing SiC fiber by in-situ regulating carbon on the fiber surface according to claim 1 or 5, characterized in that: The oxygen content in the infusible fiber is 5-16 wt %.
7. A method for preparing SiC fiber by in-situ regulating carbon on the fiber surface according to claim 1, characterized in that: The sintering process is: heating to 1000-1400° C. under a protective atmosphere and then maintaining the temperature for 0.5-2 hours.
8. The method for preparing SiC fiber by in-situ regulating carbon on the fiber surface according to claim 7, characterized in that: The protective atmosphere includes nitrogen and / or an inert gas.
9. The method for preparing SiC fiber by in-situ regulating carbon on the fiber surface according to claim 7 or 8, characterized in that: The heating rate is 1-10°C / min.
10. The method for preparing SiC fiber by in-situ regulating carbon on the fiber surface according to claim 1, characterized in that: The average single-filament tensile strength of the SiC fiber is not less than 2.5 GPa.
Citation Information
Patent Citations
Preparation method of continuous SiC fiber having surface carbon-rich structure
CN103160955A
Preparation method of continuous silicon carbide ceramic fiber thermistor
CN106810262A
Preparation method for in-situ growth of carbon coating on surface of silicon carbide fiber
CN118390294A
Product Of Lenticular Transferring Printed Matter Heat-Adhered By Hot-Melt Resin
KR1020210029935A
Cited By
Preparation method of silicon carbide fiber with adjustable resistivity
CN121161456A