Semiconductor structure and forming method thereof
By using an anti-thermal diffusion medium with a thermal conductivity lower than that of the substrate in the semiconductor structure, heat diffusion is suppressed, the heating efficiency of the heating device of the thermo-optical modulator is improved, the problem of low heating efficiency in the existing technology is solved, and the semiconductor structure is reduced of power consumption.
Patent Information
- Application Number
- CN202310354874.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-15
AI Technical Summary
The heating device of the existing thermo-optical modulator has low heating efficiency, resulting in poor performance.
The thermal diffusion prevention medium is introduced into the semiconductor structure, and its thermal conductivity is lower than that of the substrate, which inhibits heat diffusion and improves the heating efficiency of the heating device.
By reducing the substrate dissipation probability of heat, the heating efficiency of the heating device is improved and the power consumption of the semiconductor structure is reduced.
Smart Images

Figure CN118778291A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the field of semiconductor manufacturing, and in particular to a semiconductor structure and a method for forming the same. Background Art
[0002] Optical modulators are important devices in optical devices. Optical modulators based on optical waveguide structures have attracted extensive attention due to their compact structure, easy device integration and large-scale production. Among them, thermo-optical modulators have the advantages of simple production, low cost and easy integration.
[0003] The principle of thermo-optic modulator is thermo-optic effect, which is to change the molecular arrangement of crystal by heating or cooling it, thereby changing the optical properties of crystal, and then changing the refractive index of waveguide, so as to control the phase of light wave. Among them, the heating efficiency of the heating device is the key performance indicator of thermo-optic modulator.
[0004] However, the heating efficiency of current heating devices still needs to be improved, resulting in poor performance of thermo-optical modulators. Summary of the invention
[0005] The problem solved by the embodiments of the present invention is to provide a semiconductor structure and a method for forming the same, so as to improve the heating efficiency of a heating device, thereby ensuring the performance of the semiconductor structure.
[0006] To solve the above problems, an embodiment of the present invention provides a semiconductor structure, comprising: a substrate; a waveguide layer located on the substrate; a dielectric layer located on the substrate and covering the waveguide layer; a heating device buried in the dielectric layer and located above the top of the waveguide layer; and an anti-heat diffusion medium located in the substrate at the bottom of the waveguide layer, wherein the thermal conductivity of the anti-heat diffusion medium is lower than the thermal conductivity of the substrate.
[0007] Correspondingly, an embodiment of the present invention also provides a method for forming a semiconductor structure, comprising: providing a substrate, on which a waveguide layer is formed; forming a dielectric layer covering the waveguide layer and a heating device buried in the dielectric layer on the substrate, wherein the heating device is located above the top of the waveguide layer; and forming an anti-heat diffusion medium located at the bottom of the waveguide layer in the substrate, wherein the thermal conductivity of the anti-heat diffusion medium is lower than the thermal conductivity of the substrate.
[0008] Compared with the prior art, the technical solution of the embodiment of the present invention has the following advantages:
[0009] The semiconductor structure provided by the embodiment of the present invention has an anti-heat diffusion medium located in the substrate at the bottom of the waveguide layer. Since the thermal conductivity of the anti-heat diffusion medium is lower than the thermal conductivity of the substrate, the anti-heat diffusion medium is beneficial to suppressing the diffusion of heat generated by the heater, and correspondingly helps to reduce the probability of the heat generated by the heater being dissipated through the substrate, thereby improving the heating efficiency of the heater, enabling the heater to better heat the waveguide layer, thereby reducing the power consumption of the semiconductor structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 It is a schematic diagram of a semiconductor structure;
[0011] Figure 2 A schematic diagram showing an embodiment of a semiconductor structure of the present invention is shown;
[0012] Figures 3 to 5 It is a schematic structural diagram corresponding to each step in an embodiment of a method for forming a semiconductor structure of the present invention. DETAILED DESCRIPTION
[0013] As can be seen from the background, the heating efficiency of the heating device is a key performance indicator of the thermo-optical modulator, but the heating efficiency of the heating device needs to be improved.
[0014] Now, combined with a semiconductor structure, we analyze the reasons why the heating efficiency of the heating device needs to be improved. Figure 1 , Figure 1 It is a schematic diagram of a semiconductor structure.
[0015] The semiconductor structure includes: a substrate 50 ; a waveguide layer 30 located on the substrate 50 ; a dielectric layer 20 located on the substrate 50 and covering the waveguide layer 30 ; and a heating device 10 located on the dielectric layer 20 above the top of the waveguide layer 30 .
[0016] The heating device 10 is realized by the upper metal resistor, such as Figure 1 As shown, after the heating device 10 is powered on for heating, the heat generated by the heating device 10 will be dissipated to the surroundings, thereby heating the surrounding waveguide layer 30. However, since the thermal conductivity of the substrate 50 is generally relatively high (currently, the material of the substrate 50 is generally silicon, and the thermal conductivity of silicon material is relatively high), the heat is easily dissipated to the surroundings, resulting in a large power consumption of the heating device 10, and thus a decrease in the heating efficiency of the heating device.
[0017] In order to solve the technical problem, an embodiment of the present invention provides a semiconductor structure, comprising: a substrate; a waveguide layer located on the substrate; a dielectric layer located on the substrate and covering the waveguide layer; a heating device buried in the dielectric layer and located above the top of the waveguide layer; and an anti-heat diffusion medium located in the substrate at the bottom of the waveguide layer, wherein the thermal conductivity of the anti-heat diffusion medium is lower than the thermal conductivity of the substrate.
[0018] The semiconductor structure provided by the embodiment of the present invention has an anti-heat diffusion medium located in the substrate at the bottom of the waveguide layer. Since the thermal conductivity of the anti-heat diffusion medium is lower than the thermal conductivity of the substrate, the anti-heat diffusion medium is beneficial to suppressing the diffusion of heat generated by the heater, and correspondingly helps to reduce the probability of the heat generated by the heater being dissipated through the substrate, thereby improving the heating efficiency of the heater, enabling the heater to better heat the waveguide layer, thereby reducing the power consumption of the semiconductor structure.
[0019] In order to make the above-mentioned purposes, features and advantages of the embodiments of the present invention more obvious and understandable, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0020] Figure 2 It is a schematic structural diagram of an embodiment of a semiconductor structure of the present invention.
[0021] refer to Figure 2 In this embodiment, the semiconductor structure includes: a substrate 500; a waveguide layer 400, located on the substrate 500; a dielectric layer 200, located on the substrate 500 and covering the waveguide layer 400; a heating device 300, buried in the dielectric layer 200 and located above the top of the waveguide layer 400; and an anti-heat diffusion medium 900, located in the substrate 500 at the bottom of the waveguide layer 400, wherein the thermal conductivity of the anti-heat diffusion medium 900 is lower than that of the substrate 500.
[0022] The substrate 500 is used to provide a process platform for forming the semiconductor structure.
[0023] In this embodiment, the material of the substrate 500 is silicon. In other embodiments, the material of the substrate may also be other materials such as germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium, and the substrate may also be other types of substrates such as silicon on insulator substrates or germanium on insulator substrates.
[0024] The waveguide layer 400 is used to control the phase of the light wave.
[0025] In this embodiment, the waveguide layer 400 is a thermo-optic modulator. The working principle of the thermo-optic modulator is the thermo-optic effect, which is to change the molecular arrangement of the waveguide layer 400 by heating or cooling the waveguide layer 400, thereby changing the optical properties of the waveguide layer 400, and then changing the refractive index of the waveguide (the refractive index becomes smaller after heating), thereby achieving control of the phase of the light wave.
[0026] In this embodiment, the material of the waveguide layer 400 is silicon. By selecting the waveguide layer 400, it is convenient to dope it according to the requirements.
[0027] The dielectric layer 200 is located on the substrate 500 and covers the waveguide layer 400 .
[0028] The dielectric layer 200 is used to achieve electrical isolation between various devices or conductive components, and is also used to protect various components located therein.
[0029] As an example, the material of the dielectric layer 200 is a dielectric material, such as silicon oxide, silicon nitride, or silicon oxynitride. In other embodiments, the material of the dielectric layer may also be a resin material.
[0030] The heating device 300 is used to heat the waveguide layer 400, thereby achieving control over the phase of the light wave. The heating efficiency of the heating device 300 is a key performance indicator of the semiconductor structure.
[0031] In this embodiment, the material of the heating device 300 is one or more of metal and metal nitride, so as to achieve heating through metal resistance. Specifically, the material of the heating device 300 includes one or more of titanium nitride, titanium, tantalum nitride, tantalum, copper and aluminum.
[0032] It should be noted that the size of the heating device 300 is adjusted accordingly according to the size of the waveguide layer 400 .
[0033] In this embodiment, the heating device 300 and the waveguide layer 400 are spaced apart in the longitudinal direction, so as to ensure that the heating device 300 can work independently and avoid adverse effects caused by direct contact.
[0034] The anti-heat diffusion medium 900 is used to limit the heat dissipation to improve the efficiency of the heating device 300 .
[0035] Since the thermal conductivity of the anti-heat diffusion medium 900 is lower than that of the substrate 500, the anti-heat diffusion medium 900 is conducive to suppressing the diffusion of heat generated by the heater 300, and correspondingly helps to reduce the probability of the heat generated by the heater 300 being dissipated through the substrate 500, thereby improving the heating efficiency of the heater 300, so that the heater 300 can better heat the waveguide layer 400, thereby reducing the power consumption of the semiconductor structure.
[0036] In this embodiment, the heat diffusion prevention medium 900 includes a cavity. In other words, the heat diffusion prevention medium 900 is an air medium.
[0037] The thermal conductivity of air is much lower than that of semiconductor materials (eg, silicon) or dielectric materials (eg, silicon oxide). By using the air cavity, the anti-heat diffusion medium 900 can better limit the heat dissipation.
[0038] In this embodiment, along the normal direction of the surface of the substrate 500, the height H of the anti-heat diffusion medium 900 at the bottom of the waveguide layer 400 should not be too small or too large. If the height H of the anti-heat diffusion medium 900 at the bottom of the waveguide layer 400 is too small, it is easy to cause the anti-heat diffusion medium 900 to have a poor effect of limiting heat dissipation; if the height H of the anti-heat diffusion medium 900 at the bottom of the waveguide layer 400 is too large, it is easy to have an adverse effect on the mechanical strength of the remaining substrate 500, thereby having an adverse effect on the yield of the semiconductor structure. For this reason, in this embodiment, along the normal direction of the surface of the substrate 500, the height H of the anti-heat diffusion medium 900 at the bottom of the waveguide layer 400 is 3 microns to 10 microns.
[0039] Specifically in this embodiment, the height H of the anti-heat diffusion medium 900 at the bottom of the waveguide layer 400 is the height of the cavity at the bottom of the waveguide layer 400 .
[0040] In this embodiment, the semiconductor structure further includes an opening 600 located at a side of the waveguide layer 400 and penetrating the dielectric layer 200 .
[0041] The opening 600 is also an air medium. Therefore, the opening 600 is helpful to further suppress the diffusion of the heat generated by the heater 300, thereby further improving the heating efficiency of the heating device 300.
[0042] In this embodiment, the anti-heat diffusion medium 900 is a cavity, and the cavity is connected to the opening 600 .
[0043] Accordingly, when forming the cavity, the cavity can be formed via the opening 600 , that is, the opening 600 provides a process basis for forming the cavity.
[0044] By forming the cavity through the opening 600, the influence of the cavity on the existing process can be reduced, or the influence of the existing process on the cavity can be reduced, thereby improving process reliability. For example, by first forming the opening 600 and then forming the cavity, the flatness of each film layer when forming various components on the substrate 500 can be improved, or the dielectric layer 200 can be prevented from being filled into the cavity again.
[0045] In this embodiment, the projection shape of the opening 600 on the substrate 500 includes a square. The square opening 600 has a larger volume, so it is beneficial to further improve the effect of the opening 600 for suppressing heat diffusion. In addition, the larger volume of the square opening 600 also reduces the process difficulty of forming the cavity, for example, it is convenient for etching gas to enter.
[0046] In other implementations, the projection shape of the opening on the substrate may also be other shapes, such as a circle.
[0047] Specifically, there are a plurality of openings 600 , and the plurality of openings 600 are distributed around the waveguide layer 400 .
[0048] There are multiple openings 600, and the multiple openings 600 are respectively and separately arranged in the dielectric layer 200, which is beneficial to increase the number of the openings 600 and improve the effect of the openings 600 in suppressing heat diffusion. Moreover, this is beneficial to ensure that the dielectric layer 200 above the waveguide layer 400 has sufficient mechanical strength and reduce the probability of collapse of the waveguide layer 400 and the dielectric layer 200 above it. In addition, when a cavity is formed through the openings 600, it is beneficial to improve the efficiency of forming the cavity.
[0049] The plurality of openings 600 are distributed around the waveguide layer 400, which is beneficial to improving the uniformity of the effect of suppressing heat diffusion. In addition, when a cavity is formed through the openings 600, it is beneficial to improve the etching uniformity when forming the cavity, which is not only beneficial to improving the formation quality of the cavity, but also beneficial to reducing the impact on the surrounding area.
[0050] The size of the opening 600 should not be too small or too large. If the size of the opening 600 is too small, it is easy to cause the opening 600 to have a poor effect in limiting the heat dissipation, or when a cavity is formed through the opening 600, it is easy to cause the etching gas to be unable to enter, thereby having an adverse effect on the formation of the cavity; if the size of the opening 600 is too large, it is easy to have an adverse effect on the mechanical strength of the remaining dielectric layer 200. For this reason, in this embodiment, the size of the opening 600 is 4 microns to 20 microns.
[0051] In this embodiment, the thickness W of the dielectric layer 200 between the side wall of the opening 600 and the side wall of the heating device 300 is 5 micrometers to 30 micrometers along the direction perpendicular to the side wall of the opening 600. If the thickness W of the dielectric layer 200 between the side wall of the opening 600 and the side wall of the heating device 300 is too large, it is easy to cause heat to diffuse through the dielectric layer 200 above the waveguide layer 400, thereby affecting the heating efficiency of the heating device 300; if the thickness W of the dielectric layer 200 between the side wall of the opening 600 and the side wall of the heating device 300 is too small, it is easy to cause the mechanical strength of the dielectric layer 200 above the waveguide layer 400 to be poor, thereby reducing the probability of collapse of the waveguide layer 400 and the dielectric layer 200 above it.
[0052] It should be noted that, in the present embodiment, in a direction parallel to the surface of the substrate 500, the anti-heat diffusion medium 900 also extends to the bottom of the dielectric layer 200 on the side of the opening 600 away from the waveguide layer 400, which is conducive to increasing the volume of the anti-heat diffusion medium 900, thereby further enhancing the effect of the anti-heat diffusion medium 900 for suppressing heat diffusion, so as to further improve the heating efficiency of the heating device 300.
[0053] Moreover, in one embodiment, the cavity is formed by an isotropic etching process, and therefore, affected by the characteristics of the isotropic etching process, the dielectric layer 200 on the side of the opening 600 away from the waveguide layer 400 is also laterally etched, so the cavity also extends to the bottom of the dielectric layer 200 on the side of the opening 600 away from the waveguide layer 400.
[0054] In this embodiment, the semiconductor structure further includes: an isolation layer 700 located between the substrate 500 and the waveguide layer 400 .
[0055] The isolation layer 700 is used to prevent light from diffusing during propagation.
[0056] Correspondingly, the cavity is surrounded by the isolation layer 700 and the substrate 500 .
[0057] In one embodiment, the substrate 500, the isolation layer 700 and the waveguide layer 400 are prepared by a SOI (Silicon-On-Insulator) substrate. In other words, the substrate 500 is the bottom semiconductor layer in the SOI substrate, the isolation layer 700 is the insulating layer in the SOI substrate, and the waveguide layer 400 is obtained by patterning the top semiconductor layer in the SOI substrate.
[0058] In this embodiment, the isolation layer 700 between the substrate 500 and the waveguide layer 400 is retained.
[0059] Among them, since the materials of the isolation layer 700 and the dielectric layer 200 are the same or similar, retaining the isolation layer 700 at the bottom of the dielectric layer 200 is beneficial to reducing process risks. For example, if the isolation layer 700 at the bottom of the dielectric layer 200 is removed, part of the dielectric layer 200 may also be removed.
[0060] In this embodiment, the isolation layer 700 is made of an insulating material, and the insulating material includes silicon oxide.
[0061] In this embodiment, the semiconductor structure further includes: an interconnection structure 100 buried in the dielectric layer 200 and located on the top of the heating device 300 , and the interconnection structure 100 is electrically connected to the heating device 300 .
[0062] The interconnection structure 100 is an interconnection structure 100 formed by a back-end process. The interconnection structure 100 is used for electrical connection of specific devices, so as to lead out the electrical properties of each device or realize electrical connection between devices.
[0063] In this embodiment, the heating device 300 is electrically connected to the interconnection structure 100 located thereon, so that the heating device 300 is powered by the interconnection structure 100 .
[0064] As an example, the material of the interconnection structure 100 is copper. In other embodiments, the material of the interconnection layer may also be other conductive materials, such as aluminum.
[0065] In this embodiment, the opening 600 is located at the side of the waveguide layer 400 and penetrates the dielectric layer 200, and the interconnection structure 100 is buried in the dielectric layer 200. In other words, the opening 600 is formed after the interconnection structure 100 in the back-end process is formed. On the one hand, this reduces the impact of the opening 600 on the existing process, and on the other hand, it also increases the depth of the opening 600, thereby further improving the effect of the opening 600 for suppressing heat diffusion.
[0066] Specifically, an external interface exposing the top of the interconnect structure 100 is formed in the dielectric layer 200 , and the interconnect structure 100 with the external interface exposed is used to achieve electrical connection with an external circuit, for example, the interconnect structure 100 with the external interface exposed is used as a pad.
[0067] Accordingly, the opening 600 penetrates the entire dielectric layer 200 where the interconnect structure 100 is located until the substrate 500 is exposed. That is, the opening 600 is formed after the entire back-end process is completed, thereby minimizing the impact of the opening 600 on the existing process and maximizing the depth of the opening 600.
[0068] Accordingly, the present invention also provides a method for forming a semiconductor structure. Figures 3 to 5 It is a schematic structural diagram corresponding to each step in an embodiment of a method for forming a semiconductor structure of the present invention.
[0069] refer to Figure 3 , providing a substrate 500 on which a waveguide layer 400 is formed.
[0070] The substrate 500 is used to provide a process platform for subsequent processes.
[0071] In this embodiment, the material of the substrate 500 is silicon. In other embodiments, the material of the substrate may also be other materials such as germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium, and the substrate may also be other types of substrates such as silicon on insulator substrates or germanium on insulator substrates.
[0072] The waveguide layer 400 is used to control the phase of the light wave.
[0073] In this embodiment, the waveguide layer 400 is a thermo-optic modulator. The working principle of the thermo-optic modulator is the thermo-optic effect, which is to change the molecular arrangement of the waveguide layer 400 by heating or cooling the waveguide layer 400, thereby changing the optical properties of the waveguide layer 400, and then changing the refractive index of the waveguide (the refractive index becomes smaller after heating), thereby achieving control of the phase of the light wave.
[0074] In this embodiment, the material of the waveguide layer 400 is silicon.
[0075] It should be noted that the waveguide layer 400 is formed by patterning a material corresponding to the waveguide layer 400 .
[0076] In this embodiment, in the step of providing the substrate 500 , an isolation layer 700 is further formed between the substrate 500 and the waveguide layer 400 .
[0077] The isolation layer 700 is used to prevent light from diffusing during propagation.
[0078] In this embodiment, the material of the isolation layer 700 is an insulating material, and the insulating material includes silicon oxide. In one embodiment, the substrate 500, the isolation layer 700 and the waveguide layer 400 are made of a SOI (Silicon-On-Insulator) substrate.
[0079] Specifically, the step of providing a substrate 500, an isolation layer 700 and a waveguide layer 400 includes: providing an SOI substrate, including an optical modulation device region (not shown) for forming the waveguide layer 400, and the SOI substrate includes a bottom semiconductor layer, an insulating layer located on the bottom semiconductor layer, and a top semiconductor layer located on the insulating layer; patterning the top semiconductor layer in the optical modulation device region to form the waveguide layer 400 located in the optical modulation device region, the insulating layer is used as the isolation layer 700, and the bottom semiconductor layer serves as the substrate 500.
[0080] Continue to refer Figure 3 A dielectric layer 200 covering the waveguide layer 400 and a heating device 300 buried in the dielectric layer 200 are formed on the substrate 500 , and the heating device 300 is located above the top of the waveguide layer 400 .
[0081] The dielectric layer 200 is used to achieve electrical isolation between various devices or conductive components, and is also used to protect various components located therein.
[0082] As an example, the material of the dielectric layer 200 is a dielectric material, such as silicon oxide, silicon nitride, or silicon oxynitride. In other embodiments, the material of the dielectric layer may also be a resin material.
[0083] The heating device 300 is used to heat the waveguide layer 400, thereby achieving control over the phase of the light wave. The heating efficiency of the heating device 300 is a key performance indicator of the semiconductor structure.
[0084] In this embodiment, the material of the heating device 300 is one or more of metal and metal nitride, so as to achieve heating through metal resistance. Specifically, the material of the heating device 300 includes one or more of titanium nitride, titanium, tantalum nitride, tantalum, copper and aluminum.
[0085] It should be noted that the size of the heating device 300 is adjusted accordingly according to the size of the waveguide layer 400 .
[0086] In this embodiment, the heating device 300 and the waveguide layer 400 are spaced apart in the longitudinal direction, so as to ensure that the heating device 300 can work independently and avoid adverse effects caused by direct contact.
[0087] It should be noted that, in the step of forming the dielectric layer 200 covering the waveguide layer 400 and the heating device 300 buried in the dielectric layer 200 on the substrate 500, an interconnection structure 100 buried in the dielectric layer 200 and located on the top of the heating device 300 is also formed, and the interconnection structure 100 is electrically connected to the heating device 300.
[0088] The interconnection structure 100 is an interconnection structure 100 formed by a back-end process. The interconnection structure 100 is used for electrical connection of specific devices, so as to lead out the electrical properties of each device or realize electrical connection between devices.
[0089] In this embodiment, the heating device 300 is electrically connected to the interconnection structure 100 located thereon, so that the heating device 300 is powered by the interconnection structure 100 .
[0090] As an example, the material of the interconnection structure 100 is copper. In other embodiments, the material of the interconnection layer may also be other conductive materials, such as aluminum.
[0091] Specifically, an external interface exposing the top of the interconnect structure 100 is formed in the dielectric layer 200 , and the interconnect structure 100 with the external interface exposed is used to achieve electrical connection with an external circuit, for example, the interconnect structure 100 with the external interface exposed is used as a pad.
[0092] refer to Figure 4The method for forming the semiconductor structure further includes: forming an opening 600 on a side of the waveguide layer 400 that penetrates the dielectric layer 200 and exposes the substrate 500 .
[0093] The opening 600 is also an air medium, so the opening 600 is helpful to further suppress the diffusion of the heat generated by the heater 300, thereby improving the heating efficiency of the heating device 300.
[0094] It should be noted that, in one embodiment, a cavity is subsequently formed in the substrate 500, and therefore, the opening 600 is formed to provide a process basis for the subsequent formation of the cavity, that is, the cavity can be formed through the opening 600. Among them, by forming the cavity through the opening 600, the influence of the cavity on the existing process can be reduced, or the influence of the existing process on the cavity can be reduced, thereby improving process reliability. For example, forming the opening 600 first and then forming the cavity can improve the flatness of each film layer when forming various components above the substrate 500, or avoid the dielectric layer 200 from being filled into the cavity again.
[0095] In this embodiment, the projection shape of the opening 600 on the substrate 500 includes a square. The volume of the square opening 600 is larger, so it is beneficial to further enhance the effect of the opening 600 for suppressing heat diffusion. In addition, the volume of the square opening 600 is larger, which also reduces the difficulty of forming the cavity, for example, it is convenient for etching gas to enter. In other implementations, the projection shape of the opening on the substrate can also be other shapes, such as a circle.
[0096] Specifically, in the step of forming an opening 600 penetrating the dielectric layer 200 and exposing the substrate 500 on the side of the waveguide layer 400 , there are multiple openings 600 , and the multiple openings 600 are distributed around the waveguide layer 400 .
[0097] There are multiple openings 600, and the multiple openings 600 are respectively and separately arranged in the dielectric layer 200, which is conducive to increasing the number of the openings 600, and improving the effect of the openings 600 in suppressing heat diffusion. Moreover, this is conducive to making the dielectric layer 200 above the waveguide layer 400 have sufficient mechanical strength, reducing the probability of collapse of the waveguide layer 400 and the dielectric layer 200 above it. In addition, when a cavity is formed through the openings 600, it is conducive to improving the efficiency of forming the cavity.
[0098] The plurality of openings 600 are distributed around the waveguide layer 400, which is beneficial to improving the uniformity of the effect of suppressing heat diffusion. In addition, when a cavity is formed through the openings 600, it is beneficial to improve the etching uniformity when forming the cavity, which is not only beneficial to improving the formation quality of the cavity, but also beneficial to reducing the impact on the surrounding area.
[0099] The size of the opening 600 should not be too small or too large. If the size of the opening 600 is too small, it is easy to cause the opening 600 to have a poor effect in limiting the heat dissipation, or when a cavity is formed through the opening 600, it is easy to cause the etching gas to be unable to enter, thereby having an adverse effect on the formation of the cavity; if the size of the opening 600 is too large, it is easy to have an adverse effect on the mechanical strength of the remaining substrate 500. For this reason, in the step of forming the opening 600 in this embodiment, the size of the opening 600 is 4 microns to 20 microns.
[0100] In this embodiment, in the step of forming the opening 600, the thickness W of the dielectric layer 200 between the side wall of the opening 600 and the side wall of the heating device 300 is 5 micrometers to 30 micrometers along the direction perpendicular to the side wall of the opening 600. If the thickness W of the dielectric layer 200 between the side wall of the opening 600 and the side wall of the heating device 300 is too large, it is easy to cause heat to diffuse through the dielectric layer 200 above the waveguide layer 400, thereby affecting the heating efficiency of the heating device 300; if the thickness W of the dielectric layer 200 between the side wall of the opening 600 and the side wall of the heating device 300 is too small, it is easy to cause the mechanical strength of the dielectric layer 200 above the waveguide layer 400 to be poor, thereby reducing the probability of collapse of the waveguide layer 400 and the dielectric layer 200 above it.
[0101] In this embodiment, the interconnection structure 100 is also buried in the dielectric layer 200. In other words, the opening 600 is formed after the interconnection structure 100 in the back-end process is formed. On the one hand, this reduces the impact of the opening 600 on the existing process. On the other hand, it also increases the depth of the opening 600, thereby further enhancing the effect of the opening 600 for suppressing heat diffusion.
[0102] In this embodiment, an external interface exposing the top of the interconnect structure 100 is also formed in the dielectric layer 200. Accordingly, the opening 600 penetrates the entire dielectric layer 200 where the interconnect structure 100 is located until the substrate 500 is exposed. That is to say, the opening 600 is formed after the entire back-end process is completed, thereby minimizing the impact of the opening 600 on the existing process and maximizing the depth of the opening 600.
[0103] In this embodiment, the step of forming the opening 600 includes: etching the dielectric layer 200 on the side of the waveguide layer 400 using an anisotropic etching process to form the opening 600 penetrating the dielectric layer 200 and exposing the substrate 500 .
[0104] The anisotropic etching process has the characteristic of anisotropic etching, which is beneficial to improving the quality of the etching profile, thereby improving the morphology quality and dimensional accuracy of the opening 600 .
[0105] In one embodiment, the anisotropic etching process includes a deep silicon etching process. Since the interconnection structure 100 is also buried in the dielectric layer 200, the depth of the opening 600 is relatively large, and the deep silicon etching technology can perform a relatively deep etching of the semiconductor structure, so the deep silicon etching process is used to improve the reliability of the etching process.
[0106] It should be noted that the etching time of the anisotropic etching process should not be too long or too short. If the etching time of the anisotropic etching process is too short, it is easy to cause the depth of the opening 600 to be too small, resulting in poor effect of the opening 600 in suppressing heat diffusion, or it is easy to cause the opening 600 to fail to expose the substrate 500, thereby causing adverse effects on the step of forming a cavity through the opening 600. For this reason, in this embodiment, the etching time of the anisotropic etching process ranges from 40 seconds to 80 seconds.
[0107] It should also be noted that an isolation layer 700 is formed between the substrate 500 and the waveguide layer 400 . Therefore, in the process of forming the opening 600 , the isolation layer 700 exposed by the dielectric layer 200 is further etched. Therefore, the opening 600 penetrates the isolation layer 700 .
[0108] Specifically, a mask layer (not shown) is formed to cover the dielectric layer 200 and the interconnect structure 100, and a mask opening (not shown) is formed in the mask layer and is located at a side of the waveguide layer 400; the mask layer is used as a mask to etch the dielectric layer 200 along the mask opening to form an opening 600 exposing the substrate 500.
[0109] As an example, the material of the mask layer is photoresist. In other embodiments, the mask layer may also be made of other suitable materials.
[0110] In this embodiment, after forming the opening 600, the mask layer is retained, so that the mask layer is used to continue to protect the dielectric layer 200 and the interconnect structure 100 during the subsequent cavity formation process. In other embodiments, the mask layer may also be removed after forming the opening to reduce the difficulty of the etching gas entering the opening and contacting the substrate 500 when etching the substrate 500 later.
[0111] refer to Figure 5 , a heat diffusion prevention medium 900 is formed in the substrate 500 and is located at the bottom of the waveguide layer 400 , and the thermal conductivity of the heat diffusion prevention medium 900 is lower than the thermal conductivity of the substrate 500 .
[0112] The anti-heat diffusion medium 900 is used to limit the heat dissipation to improve the efficiency of the heating device 300 .
[0113] Since the thermal conductivity of the anti-heat diffusion medium 900 is lower than that of the substrate 500, the anti-heat diffusion medium 900 is conducive to suppressing the diffusion of heat generated by the heater, and correspondingly helps to reduce the probability of the heat generated by the heater being dissipated through the substrate 500, thereby improving the heating efficiency of the heating device 300, so that the heating device 300 can better heat the waveguide layer 400, thereby reducing the power consumption of the semiconductor structure.
[0114] In this embodiment, the step of forming the heat diffusion prevention medium 900 at the bottom of the waveguide layer 400 in the substrate 500 includes: forming a cavity at the bottom of the waveguide layer 400 in the substrate 500. In other words, the heat diffusion prevention medium 900 is an air medium.
[0115] The thermal conductivity of air is much lower than that of semiconductor materials (eg, silicon) or dielectric materials (eg, silicon oxide). By using the air cavity, the anti-heat diffusion medium 900 can better limit the heat dissipation.
[0116] In this embodiment, in the step of forming the heat diffusion prevention medium 900, the height H of the heat diffusion prevention medium 900 at the bottom of the waveguide layer 400 along the normal direction of the surface of the substrate 500 should not be too small or too large. If the height H of the heat diffusion prevention medium 900 at the bottom of the waveguide layer 400 is too small, it is easy to cause the heat diffusion prevention medium 900 to have a poor effect of limiting the heat dissipation; if the height H of the heat diffusion prevention medium 900 at the bottom of the waveguide layer 400 is too large, it is easy to have an adverse effect on the mechanical strength of the remaining substrate 500, thereby having an adverse effect on the yield of the semiconductor structure. For this reason, in this embodiment, along the normal direction of the surface of the substrate 500, the height H of the heat diffusion prevention medium 900 at the bottom of the waveguide layer 400 is 3 microns to 10 microns.
[0117] Specifically in this embodiment, the height H of the anti-heat diffusion medium 900 at the bottom of the waveguide layer 400 is the height of the cavity at the bottom of the waveguide layer 400 .
[0118] In this embodiment, before the heat diffusion prevention medium 900 located at the bottom of the waveguide layer 400 is formed in the substrate 500, an opening penetrating the dielectric layer 200 and exposing the substrate 500 is formed on the side of the waveguide layer 400. Therefore, the step of forming the heat diffusion prevention medium 900 located at the bottom of the waveguide layer 400 in the substrate 500 includes: forming a cavity located at the bottom of the waveguide layer 400 in the substrate 500 via the opening 600, and correspondingly, the cavity is connected to the opening 600.
[0119] In this embodiment, the step of forming a cavity at the bottom of the waveguide layer 400 in the substrate 500 includes: etching the substrate 500 at the side of the waveguide layer 400 using an isotropic etching process until a portion of the thickness of the substrate 500 at the bottom of the waveguide layer 400 is removed to form a cavity at the bottom of the waveguide layer 400.
[0120] Since the isotropic etching process has the characteristic of isotropic etching, lateral etching is achieved, thereby being able to remove a portion of the thickness of the substrate 500 at the bottom of the waveguide layer 400. In addition, directly using the isotropic etching process for etching is conducive to increasing the remaining thickness of the substrate 500 at the bottom of the cavity while forming the cavity, thereby improving the heating efficiency of the heating device 300 while ensuring that the remaining substrate 500 has a higher mechanical strength.
[0121] In other embodiments, the cavity may also be formed by two-step etching. Specifically, the step of forming the cavity at the bottom of the waveguide layer in the substrate includes: performing a first etching on the substrate at the side of the waveguide layer using an anisotropic etching process to form a groove in the substrate; and performing a second etching on the substrate exposed by the groove using an isotropic etching process until a portion of the thickness of the substrate at the bottom of the waveguide layer is removed to form a cavity at the bottom of the waveguide layer.
[0122] In this embodiment, the isotropic etching process includes a deep silicon etching process, and the anisotropic etching process includes a deep silicon etching process.
[0123] Since the deep silicon etching technology can perform relatively deep etching on the semiconductor structure, the substrate 500 of the bottom portion of the waveguide layer 400 can be removed through the opening 600, thereby improving the formation quality of the cavity.
[0124] In other embodiments, the isotropic etching process may also be a wet etching process.
[0125] It should be noted that, in the step of using an isotropic etching process to etch the substrate 500 on the side of the waveguide layer 400 until a portion of the thickness of the substrate 500 at the bottom of the waveguide layer 400 is removed to form a cavity at the bottom of the waveguide layer 400, the time of the isotropic etching process should not be too short or too long. If the time of the isotropic etching process is too long, the mechanical strength of the semiconductor structure will deteriorate; if the time of the isotropic etching process is too short, the etching will be incomplete. Therefore, in this embodiment, the time range of the isotropic etching process is 150 seconds to 250 seconds.
[0126] In this embodiment, in a direction parallel to the surface of the substrate 500, the anti-heat diffusion medium 900 also extends to the bottom of the dielectric layer 200 on the side of the opening 600 away from the waveguide layer 400, which is conducive to increasing the volume of the anti-heat diffusion medium 900, thereby further enhancing the effect of the anti-heat diffusion medium 900 for suppressing heat diffusion, so as to further improve the heating efficiency of the heating device 300.
[0127] Moreover, specifically in this embodiment, since an isotropic etching process is adopted to etch away a portion of the thickness of the substrate 500 at the side of the waveguide layer 400, based on the characteristics of isotropic etching, the etching process etches the substrate 500 in all directions. Accordingly, after the cavity is formed, in a direction parallel to the surface of the substrate 500, the cavity also extends to the bottom of the dielectric layer 200 on the side of the opening 600 away from the waveguide layer 400.
[0128] In this embodiment, since an isolation layer 700 is also formed between the substrate 500 and the waveguide layer 400, in the step of forming the heat diffusion prevention medium 900 located at the bottom of the waveguide layer 400 in the substrate 500, the isolation layer 700 between the substrate 500 and the waveguide layer 400 is retained.
[0129] Among them, since the materials of the isolation layer 700 and the dielectric layer 200 are the same or similar, retaining the isolation layer 700 at the bottom of the dielectric layer 200 is beneficial to reducing process risks. For example, if the isolation layer 700 at the bottom of the dielectric layer 200 is removed, part of the dielectric layer 200 may also be removed.
[0130] In this embodiment, the anti-heat diffusion medium 900 is a cavity. Accordingly, in the step of forming a cavity at the bottom of the waveguide layer 400 in the substrate 500 , the cavity is surrounded by the isolation layer 700 and the substrate 500 .
[0131] It should be noted that the semiconductor structure described in the above embodiments can be obtained by using the formation method described in this embodiment, and can also be obtained by using other formation methods.
[0132] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A semiconductor structure, characterized in that: include: substrate; a waveguide layer, located on the substrate; a dielectric layer, located on the substrate and covering the waveguide layer; a heating device buried in the dielectric layer and located above the top of the waveguide layer; The anti-heat diffusion medium is located in the substrate at the bottom of the waveguide layer, and the thermal conductivity of the anti-heat diffusion medium is lower than the thermal conductivity of the substrate.
2. The semiconductor structure according to claim 1, wherein: The anti-thermal diffusion medium includes a cavity.
3. The semiconductor structure according to claim 1 or 2, characterized in that: Along the normal direction of the substrate surface, the height of the heat diffusion prevention medium at the bottom of the waveguide layer is 3 microns to 10 microns.
4. The semiconductor structure according to claim 1 or 2, characterized in that: The semiconductor structure further includes an opening located at a side of the waveguide layer and penetrating the dielectric layer.
5. The semiconductor structure according to claim 4, characterized in that There are multiple openings, and the multiple openings are distributed around the waveguide layer.
6. The semiconductor structure according to claim 4, wherein: The opening has an opening size of 4 micrometers to 20 micrometers.
7. The semiconductor structure according to claim 4, wherein: Along a direction perpendicular to the sidewall of the opening, a thickness of the dielectric layer between the sidewall of the opening and the sidewall of the heater is 5 micrometers to 30 micrometers.
8. The semiconductor structure according to claim 4, wherein: A projected shape of the opening on the substrate includes a square.
9. The semiconductor structure according to claim 4, characterized in that The semiconductor structure further includes an interconnection structure buried in the dielectric layer and located on the top of the heating device, wherein the interconnection structure is electrically connected to the heating device.
10. The semiconductor structure according to claim 2, wherein: The semiconductor structure further includes an opening located at a side of the waveguide layer and penetrating the dielectric layer, and the cavity is connected to the opening.
11. The semiconductor structure according to claim 2, wherein: The semiconductor structure further includes: an isolation layer located between the substrate and the waveguide layer; The cavity is surrounded by the isolation layer and the substrate.
12. A method for forming a semiconductor structure, characterized in that: include: providing a substrate, on which a waveguide layer is formed; forming a dielectric layer covering the waveguide layer and a heating device buried in the dielectric layer on the substrate, wherein the heating device is located above the top of the waveguide layer; An anti-heat diffusion medium is formed in the substrate and located at the bottom of the waveguide layer, wherein the thermal conductivity of the anti-heat diffusion medium is lower than the thermal conductivity of the substrate.
13. The method for forming a semiconductor structure according to claim 12, wherein: The step of forming a heat diffusion prevention medium in the substrate at the bottom of the waveguide layer includes forming a cavity in the substrate at the bottom of the waveguide layer.
14. The method for forming a semiconductor structure according to claim 12 or 13, characterized in that: The method for forming a semiconductor structure further includes: forming an opening on a side of the waveguide layer that penetrates the dielectric layer and exposes the substrate.
15. The method for forming a semiconductor structure according to claim 14, wherein: The step of forming the anti-heat diffusion medium at the bottom of the waveguide layer in the substrate includes: forming a cavity at the bottom of the waveguide layer in the substrate through the opening.
16. The method for forming a semiconductor structure according to claim 14, wherein: The step of forming the opening includes: etching the dielectric layer at the side of the waveguide layer using an anisotropic etching process to form an opening penetrating the dielectric layer and exposing the substrate.
17. The method for forming a semiconductor structure according to claim 16, wherein: The anisotropic etching process includes a deep silicon etching process.
18. The method for forming a semiconductor structure according to claim 13, wherein: The step of forming a cavity at the bottom of the waveguide layer in the substrate comprises: etching the substrate at the side of the waveguide layer by an isotropic etching process until a portion of the thickness of the substrate at the bottom of the waveguide layer is removed to form a cavity at the bottom of the waveguide layer; or, An anisotropic etching process is used to perform a first etching on the substrate at the side of the waveguide layer to form a groove in the substrate; an isotropic etching process is used to perform a second etching on the substrate exposed by the groove until a portion of the thickness of the substrate at the bottom of the waveguide layer is removed to form a cavity at the bottom of the waveguide layer.
19. The method for forming a semiconductor structure according to claim 18, wherein: The isotropic etching process includes a deep silicon etching process, and the anisotropic etching process includes a deep silicon etching process.
20. The method for forming a semiconductor structure according to claim 13, wherein: In the step of providing a substrate, an isolation layer is further formed between the substrate and the waveguide layer; In the step of forming a cavity in the substrate at the bottom of the waveguide layer, the cavity is surrounded by the isolation layer and the substrate.