Coating and baking method of thick-layer photoresist
By dynamically dispensing glue on a rotating glass substrate and using a stepped temperature baking method, the problem of uniformity and photosensitivity of thick-layer photoresist coating is solved, and a thick-layer photoresist with uniform thickness and good photosensitivity is achieved, which reduces the cost Reduce production costs and improve efficiency.
Patent Information
- Application Number
- CN202410949284.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-10-20
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-15
AI Technical Summary
The coating uniformity of thick-layer photoresist in the prior art is poor, and the photosensitive properties of the upper and lower layers are uneven, resulting in missing or deformed microstructures. Simultaneous X-ray exposure costs are high and production efficiency is low.
A rotating glass substrate is used for dynamic dispensing, and photoresist layers with different dilution ratios are coated multiple times, and a step-heating baking method is used to form a thick layer of photoresist with uniform thickness and good photosensitivity.
A thick layer of photoresist with large thickness, uniform glue surface and good photosensitivity is achieved, which avoids the reduction of the photoresist sensitivity of the underlying photoresist due to multiple baking, and improves production efficiency and cost-effectiveness.
Smart Images

Figure CN118778364A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semiconductor integrated circuit manufacturing photolithography process, in particular to a coating and baking method for thick-layer photoresist. Background Art
[0002] In the global semiconductor industry, with the rapid rise of the Internet of Things, such as smart driving, smart logistics, and smart homes, the consumer demand for sensors is increasing day by day. MEMS sensors refer to micro sensor devices manufactured on silicon wafers using semiconductor technology. MEMS is the abbreviation of Micro-Electro Mechanical System, which is an independent intelligent system.
[0003] MEMS processing technology is a process for making microstructures on various substrates (such as silicon substrates, glass substrates, quartz substrates, sapphire substrates, etc.) according to product requirements. Microstructures are mainly used as various sensors and actuators, and are made into different movable structures (such as gears, cantilever beams, cavities, bridge structures, etc.) and various functional materials according to different sensor types. Since the mechanical structure inside the MEMS sensor is at the micron level or even the nanometer level, the traditional mechanical processing method is obviously unable to meet the production needs of MEMS.
[0004] The MEMS micromachining technologies currently used in industry include: bulk silicon micromachining, surface micromachining and LIGA process (combination of photolithography, electroforming and injection molding). The LIGA process can produce microstructures with high aspect ratio, high precision and complex structure. In order to obtain microstructures with complete structure and large size, the thickness of thick layer photoresist used for MEMS generally reaches tens or even hundreds of microns. The coated photoresist needs to be baked to remove the solvent in the photoresist layer to improve the adhesion and photosensitivity of the film. Therefore, the photosensitivity, thickness uniformity and adhesion between the photoresist layer and the substrate will directly affect the integrity of the microstructure.
[0005] The thickness of a single coating of the commonly used coating method can only reach about 20um at most. Generally, the same type and viscosity of photoresist are used for multiple coatings to obtain a thicker photoresist layer. The photoresist coated by this conventional method has poor uniformity of the coating surface. Since the second layer of photoresist is coated, the substrate is all photoresist layer, the fluidity between photoresists deteriorates, the dripping track is obvious, and the coating surface is not smooth. Poor uniformity of the photoresist layer thickness will lead to missing or even deformation of the microstructure size.
[0006] Moreover, the thickness of the photoresist layer makes it more difficult to photosensitize the bottom layer of photoresist, and synchronized X-ray exposure with strong penetrating power is required. Otherwise, the lower layer of photoresist is not fully exposed and the microstructure cannot be developed. However, the synchrotron radiation source is expensive, the production efficiency of X-ray exposure is low, the mask life is short, and the production cost is high. The UV-LIGA technology, which is formed by combining ultraviolet thick resist lithography technology with LIGA technology, can avoid the problem of X-ray exposure. However, the energy of ultraviolet light is much lower than that of X-rays, and higher requirements are placed on the photosensitivity and uniformity of thick layers of photoresist, which increases the technical difficulty of thick resist coating and baking.
[0007] The prior art invention patent CN201510415328.4 controls the thickness of the photoresist film by controlling the evaporation rate of the photoresist through airflow, and strengthens the evaporation mechanism during the coating process. Although this coating method can obtain a uniform film, it is only suitable for thin layers of photoresist with a thickness of 0.2um-1.2um, and cannot coat high-viscosity and high-thickness photoresists. Summary of the invention
[0008] In view of the existing problems of poor uniformity in coating thick-layer photoresist and uneven photosensitivity of upper and lower layers, the present invention provides a coating and baking method for thick-layer photoresist, which can obtain thick-layer photoresist with large thickness, uniform surface and good photosensitivity.
[0009] To achieve the above object, the embodiments of the present invention adopt the following technical solutions:
[0010] A coating and baking method for thick-layer photoresist includes a glass substrate, a surface of the glass substrate is coated with an oxide film, and the coating and baking method includes:
[0011] Rotate the glass substrate to dynamically drip the photoresist from the edge of the glass substrate toward the center;
[0012] A first photoresist is applied to form a first photoresist layer, wherein the volume ratio of the photoresist stock solution of the first photoresist to the diluent is a first dilution ratio R 1 ;
[0013] Baking the first photoresist layer, baking the first photoresist layer in a step-by-step temperature increase manner to form a film of the first photoresist layer;
[0014] A second photoresist is coated on the surface of the first photoresist layer to form a second photoresist layer, wherein the volume ratio of the photoresist stock solution of the second photoresist to the diluent is a second dilution ratio R 2 ;
[0015] Baking the second photoresist layer, baking the second photoresist layer in a step-by-step temperature increase manner to form a film of the second photoresist layer;
[0016] placing the baked glass substrate in a clean environment to cool the photoresist and the glass substrate to room temperature;
[0017] The first dilution ratio R 1 Greater than the second dilution ratio R 2 .
[0018] In some embodiments, the step-by-step heating method is at least a three-stage step-by-step heating method, and baking the first photoresist layer specifically includes: in the first stage, heating the first photoresist layer from room temperature to a first temperature t 1 , keep warm for 10 to 20 minutes; in the second stage, the first photoresist layer is heated from the first temperature t 1 Heating to the second temperature t 2 , keep warm for 10 to 20 minutes; in the third stage, the first photoresist layer is heated from the second temperature t 2 Heating to the third temperature t 3 , keep warm for 10 to 50 minutes; the first temperature t 1 <Second temperature t 2 <Third temperature t 3 .
[0019] In some embodiments, baking the second photoresist layer specifically includes: in the first stage, heating the second photoresist layer from room temperature to a fourth temperature t 4 , keep warm for 10 to 20 minutes; in the second stage, the second photoresist layer is heated from the fourth temperature t 4 Heating to the fifth temperature t 5 , keep warm for 10 to 20 minutes; in the third stage, the second photoresist layer is heated from the fifth temperature t 5 Heating to the sixth temperature t 6 , keep warm for 10 to 50 minutes; the fourth temperature t 4 <Fifth temperature t 5 <Sixth temperature t 6 , the third temperature t 3 <Sixth temperature t 6 .
[0020] In some embodiments, after the second photoresist layer is baked, a third photoresist is coated and baked on the surface of the second photoresist layer, and then an Nth photoresist is coated and baked to form an Nth photoresist layer. The volume ratio of the photoresist stock solution of the Nth photoresist to the diluent is the Nth dilution ratio Rn, and the Nth dilution ratio Rn is the minimum dilution ratio.
[0021] In some embodiments, baking the Nth photoresist layer, using a step-by-step temperature increase method to bake the Nth photoresist layer, includes: in a first stage, heating the Nth photoresist layer from room temperature to a seventh temperature t 3(N-1)+1 , keep warm for 10 to 20 minutes; in the second stage, the Nth photoresist layer is heated from the seventh temperature t3(N-1)+1 Heating to the eighth temperature t 3(N-1)+2 , keep warm for 10 to 20 minutes; in the third stage, the Nth photoresist layer is heated from the eighth temperature t 3(N-1)+2 Heating to the ninth temperature t 3(N-1)+3 , keep warm for 10 to 50 minutes; the seventh temperature t 3(N-1)+1 <Second temperature t 3(N-1)+2 <Third temperature t 3(N-1)+3 .
[0022] In some embodiments, rotating the glass substrate specifically includes: uniformly accelerating the glass substrate to a rotation speed of 150-400 rpm, and dynamically dripping the photoresist from the edge of the glass substrate toward the center through a hose.
[0023] In some embodiments, coating the first photoresist specifically includes: accelerating the glass substrate to a rotation speed of 500 to 3000 rpm for spin coating, the spin coating time is 5 to 30 seconds, forming a first photoresist layer, the thickness of the first photoresist layer is a first thickness T 1 .
[0024] In some embodiments, coating the second photoresist on the surface of the first photoresist layer specifically includes: accelerating the glass substrate to a uniform speed of 1000-3000 rpm for spin coating, the spin coating time is 5-30s, forming a second photoresist layer, the thickness of the second photoresist layer is a second thickness T 2 , the first thickness T 1 >Second thickness T 2 .
[0025] In some embodiments, the diluent is propylene glycol methyl ether acetate.
[0026] In some embodiments, the coating and baking method further includes: cleaning the surface of the glass substrate by a DIP cleaning device;
[0027] A layer of chromium oxide or chromium oxynitride is coated on the surface of the glass substrate by a coating machine.
[0028] In a second aspect, the present invention provides a photomask, which includes a glass substrate and a photoresist layer disposed on the surface of the glass substrate. The photoresist layer is formed on the surface of the glass substrate by the above-mentioned coating and baking method.
[0029] Advantages of the implementation of the present invention: The technical solution provides a method for coating and baking a thick layer of photoresist, and its process flow includes coating a first photoresist layer, baking the first photoresist layer by step-by-step temperature increase, coating a second photoresist layer again, baking the second photoresist layer by step-by-step temperature increase, until coating the Nth photoresist layer, and baking the Nth photoresist layer by step-by-step temperature increase, so as to complete the coating of the thick layer of photoresist. Different layers of photoresist use different dilution ratios. Since the upper layer of photoresist has low viscosity and good leveling properties, it can fill the surface undulations of the lower layer of high viscosity photoresist, so that the final film surface has no undulations and good thickness uniformity. Different layers of photoresist are all subjected to step-by-step temperature increase, and the temperature nodes of each layer of photoresist are set differently. The lower layer of photoresist coated first has a lower baking temperature and a shorter baking time, so as to protect the photosensitivity of the bottom layer of photoresist from loss after multiple baking to the maximum extent. This technical solution can improve the fluidity of the upper photoresist coating and avoid reducing the photosensitivity of the bottom photoresist due to multiple baking. By coating photoresists of different viscosities multiple times, a thick layer of photoresist with large thickness, uniform surface and good photosensitivity can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0031] Figure 1 The present invention is a process flow chart of a method for coating and baking a thick layer of photoresist. DETAILED DESCRIPTION
[0032] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0033] In addition, the terms "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, a feature defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "plurality" means two or more.
[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] like Figure 1 As shown, a coating and baking method of a thick layer of photoresist includes a glass substrate, which is subjected to chemical mechanical polishing by a single-sided polishing device, and rough polishing and fine polishing are respectively performed to remove impurities, flaws and other defects on the surface of the glass substrate. Then, the surface of the glass substrate is cleaned by a DIP cleaning device to remove foreign matter such as particles, polishing powder, and oil stains on the surface of the glass substrate. The initial cleaning of the glass substrate is completed.
[0036] A layer of chromium oxide or chromium oxynitride is coated on the surface of the glass substrate by magnetron sputtering through a coating machine to increase the adhesion between the photoresist and the substrate. The coated glass substrate is DIP cleaned again to remove particulate impurities on the surface of the glass substrate.
[0037] Then, photoresist is coated on a clean glass substrate with a chrome layer.
[0038] The coating and baking method of the thick layer photoresist of this embodiment comprises the following steps:
[0039] (1) Applying the first photoresist layer
[0040] Propylene glycol methyl ether acetate is used as a diluent to dilute the high viscosity photoresist stock solution to form a first photoresist. In this step, the volume ratio of the photoresist stock solution to the diluent is a first dilution ratio R 1 , according to the first dilution ratio R 1 After the first photoresist with the proper proportion is evenly mixed, the glass substrate is uniformly accelerated to a rotation speed of 150-400 rpm for rotation, and the photoresist is dynamically dripped from the edge of the glass substrate toward the center through a hose.
[0041] Apply the first photoresist, accelerate the glass substrate to a speed of 500-3000 rpm for spin coating, and the spin coating time is 5-30 seconds to form a first photoresist layer, the thickness of the first photoresist layer is a first thickness T 1 .
[0042] (2) Baking the first photoresist layer
[0043] The first photoresist layer is baked by a step-by-step heating method to form a film of the first photoresist layer; the step-by-step heating method is at least a three-stage step-by-step heating method, and the three-stage step-by-step heating method is adopted in this embodiment. Specifically, the first stage includes: heating the first photoresist layer from room temperature to a first temperature t 1 , keep warm for 10 to 20 minutes; in the second stage, the first photoresist layer is heated from the first temperature t 1 Heating to the second temperature t 2 , keep warm for 10 to 20 minutes; in the third stage, the first photoresist layer is heated from the second temperature t 2 Heating to the third temperature t 3 , keep warm for 10 to 50 minutes; the first temperature t 1 <Second temperature t 2 <Third temperature t 3 .
[0044] (3) Applying the second photoresist layer
[0045] Propylene glycol methyl ether acetate is used as a diluent to dilute the high viscosity photoresist stock solution to form a second photoresist. In this step, the volume ratio of the photoresist stock solution to the diluent is a second dilution ratio R 2 , according to the second dilution ratio R 2 After the proportioned second photoresist is evenly mixed, the rotation speed of the glass substrate is adjusted to 150-400 rpm and the photoresist is dynamically dripped from the edge of the first photoresist layer toward the center through a hose.
[0046] The first dilution ratio R 1 Greater than the second dilution ratio R 2 .
[0047] A second photoresist is coated on the surface of the first photoresist layer, and the glass substrate is uniformly accelerated to a rotation speed of 500 rpm to 3000 rpm for spin coating. The spin coating time is 5 to 30 seconds to form a second photoresist layer. The thickness of the second photoresist layer is a second thickness T 2 The first thickness T 1 >Second thickness T 2 .
[0048] (4) Baking the second photoresist layer
[0049] The second photoresist layer is baked by a step-by-step heating method to form a film of the second photoresist layer; the step-by-step heating method is at least a three-stage step-by-step heating method, and the three-stage step-by-step heating method is adopted in this embodiment. Specifically, the first stage is to heat the second photoresist layer from room temperature to a fourth temperature t 4 , keep warm for 10 to 20 minutes; in the second stage, the second photoresist layer is heated from the fourth temperature t 4 Heating to the fifth temperature t5 , keep warm for 10 to 20 minutes; in the third stage, the second photoresist layer is heated from the fifth temperature t 5 Heating to the sixth temperature t 6 , keep warm for 10 to 50 minutes; the fourth temperature t 4 <Fifth temperature t 5 <Sixth temperature t 6 , the third temperature t 3 <Sixth temperature t 6 .
[0050] (5) Applying the Nth photoresist layer
[0051] After the second photoresist layer is baked, the third photoresist can be coated and baked on the surface of the second photoresist layer, and then the Nth photoresist can be coated and baked to form the Nth photoresist layer, that is, the Nth photoresist layer is coated on the glass substrate that has been coated with the N-1th photoresist layer.
[0052] Propylene glycol methyl ether acetate is used as a diluent to dilute the high viscosity photoresist stock solution to form an Nth photoresist. In this step, the volume ratio of the photoresist stock solution to the diluent is the Nth dilution ratio R n , according to the Nth dilution ratio R n After the Nth photoresist with the same proportion is evenly mixed, the rotation speed of the glass substrate is adjusted to 150-400 rpm and the photoresist is dynamically dripped from the edge of the N-1th photoresist layer toward the center through a hose.
[0053] Among them, the dilution ratio of the high viscosity photoresist needs to meet the first dilution ratio R 1 >Second dilution ratio R 2 >…>Nth dilution ratio R n .
[0054] (6) Baking the Nth photoresist layer
[0055] The Nth photoresist layer is baked by a step-by-step heating method, and the step-by-step heating method is at least a three-stage step-by-step heating method. In this embodiment, a three-stage step-by-step heating method is adopted. Specifically, the first stage is to heat the Nth photoresist layer from room temperature to a seventh temperature t 3(N-1)+1 , keep warm for 10 to 20 minutes; in the second stage, the Nth photoresist layer is heated from the seventh temperature t 3(N-1)+1 Heating to the eighth temperature t 3(N-1)+2 , keep warm for 10 to 20 minutes; in the third stage, the Nth photoresist layer is heated from the eighth temperature t 3(N-1)+2 Heating to the ninth temperature t 3(N-1)+3 , keep warm for 10 to 50 minutes; the seventh temperature t 3(N-1)+1 <Second temperature t 3(N-1)+2 <Third temperature t 3(N-1)+3.
[0056] Finally, the baked glass substrate is placed in a clean environment to cool the photoresist and the glass substrate to room temperature, completing the coating of the thick layer of photoresist.
[0057] In this embodiment, the maximum thickness of a single coating of photoresist is 25 μm, and multiple coatings can be performed according to actual needs, and the number of N layers of the Nth photoresist layer can be set according to actual needs. Among them, the dilution ratio of the high-viscosity photoresist satisfies the dilution ratio R 1 >R 2 >…>R n , the thickness of the photoresist layer satisfies the thickness T 1 >T 2 >…>T n Through multiple coatings, the total thickness of the film can reach T 总 =T 1 +T 2 +…+T n The total thickness can reach tens of microns or even hundreds of microns.
[0058] During the step-by-step heating process of baking, the baking temperature t 1 <t 2 <t 3 , t 4 <t 5 <t 6 , t 3 <t 6 By analogy, the nth photoresist layer, t 3(n-1)+1 <t 3(n-1)+2 <t 3(n-1)+3 .
[0059] In some embodiments, the coating and baking method of the thick layer photoresist comprises:
[0060] (1) Applying the first photoresist layer
[0061] ①The volume ratio of AZ4562 photoresist stock solution and diluent is the first dilution ratio of 6:1.
[0062] ②Accelerate from rest to 100rpm at an acceleration of 100rpm / s. The photoresist is dynamically dripped from the edge to the center of the glass substrate, and the moving speed of the dripping arm is 6mm / s. When the dripping arm reaches the center of the substrate, the dripping stops.
[0063] ③ Accelerate from 100 rpm to 350 rpm at an acceleration of 200 rpm / s, continue for 3 seconds, then decelerate to a standstill at an acceleration of 100 rpm / s.
[0064] ④ Accelerate from rest to 610 rpm at an acceleration of 800 rpm / s for 6 seconds.
[0065] ⑤Decelerate to a standstill at an acceleration of 800rpm / s.
[0066] (2) Baking the first photoresist layer
[0067] ① Raise the temperature of the first photoresist layer from room temperature 25°C to a first temperature of 40°C and keep it warm for 10 minutes.
[0068] ② Raise the temperature of the first photoresist layer from a first temperature of 40°C to a second temperature of 60°C and keep it warm for 10 minutes.
[0069] ③ The first photoresist layer is heated from the second temperature of 60° C. to the third temperature of 80° C. and kept at this temperature for 20 minutes. The thickness of the obtained first photoresist layer is 23.6 um.
[0070] (3) Applying the second photoresist layer
[0071] ①The volume ratio of AZ4562 photoresist stock solution and diluent is the second dilution ratio of 5:1.
[0072] ②Accelerate from rest to 100rpm at an acceleration of 100rpm / s. The photoresist is dynamically dripped from the edge to the center of the glass substrate, and the moving speed of the dripping arm is 6mm / s. When the dripping arm reaches the center of the substrate, the dripping stops.
[0073] ③ Accelerate from 100 rpm to 350 rpm at an acceleration of 200 rpm / s, continue for 3 seconds, then decelerate to a standstill at an acceleration of 100 rpm / s.
[0074] ④ Accelerate from rest to 675 rpm at an acceleration of 800 rpm / s for 9 seconds.
[0075] ⑤Decelerate to a standstill at an acceleration of 800rpm / s.
[0076] (4) Baking the second photoresist layer
[0077] ① Raise the temperature of the second photoresist layer from room temperature 25°C to a fourth temperature of 50°C and keep it warm for 10 minutes.
[0078] ② Raise the temperature of the second photoresist layer from the fourth temperature of 50°C to the fifth temperature of 70°C and keep it warm for 10 minutes.
[0079] ③ The second photoresist layer was heated from the fifth temperature of 70° C. to the sixth temperature of 90° C. and kept at this temperature for 30 minutes. The thickness of the obtained second photoresist layer was 16.2 um.
[0080] (5) Applying the third photoresist layer
[0081] ①The volume ratio of AZ4562 photoresist stock solution and diluent is the third dilution ratio of 4:1.
[0082] ②Accelerate from rest to 100rpm at an acceleration of 100rpm / s. The photoresist is dynamically dripped from the edge to the center of the glass substrate, and the moving speed of the dripping arm is 6mm / s. When the dripping arm reaches the center of the substrate, the dripping stops.
[0083] ③ Accelerate from 100 rpm to 350 rpm at an acceleration of 200 rpm / s, continue for 3 seconds, then decelerate to a standstill at an acceleration of 100 rpm / s.
[0084] ④ Accelerate from rest to 1100 rpm at an acceleration of 1000 rpm / s for 6 seconds.
[0085] ⑤Decelerate to a standstill at an acceleration of 1000rpm / s.
[0086] (6) Baking the third photoresist layer
[0087] ① Raise the temperature of the third photoresist layer from room temperature 25°C to the seventh temperature 60°C and keep it warm for 10 minutes.
[0088] ② Raise the temperature of the third photoresist layer from the seventh temperature of 60°C to the eighth temperature of 75°C and keep it warm for 10 minutes.
[0089] ③ The third photoresist layer was heated from the eighth temperature of 75° C. to the ninth temperature of 95° C. and kept warm for 40 minutes. The thickness of the obtained third photoresist layer was 10.5 um.
[0090] The total thickness of the three-layer photoresist film is 23.6um+16.2um+10.5um=50.3um. The film is uniform, without obvious glue dripping tracks left by conventional double-layer glue coating. The product is used by the client, the photolithography is normal, the photoresist microstructure is complete after development, and there is no photoresist residue at the bottom of the microstructure, indicating that the photosensitivity of the bottom layer of photoresist is normal.
[0091] In some embodiments, the coating and baking method of the thick layer photoresist comprises:
[0092] (1) Applying the first photoresist layer
[0093] ①The volume ratio of AZ4562 photoresist stock solution and diluent is the first dilution ratio of 6:1.
[0094] ②Accelerate from rest to 100rpm at an acceleration of 100rpm / s. The photoresist is dynamically dripped from the edge to the center of the glass substrate, and the moving speed of the dripping arm is 6mm / s. When the dripping arm reaches the center of the substrate, the dripping stops.
[0095] ③ Accelerate from 100 rpm to 350 rpm at an acceleration of 200 rpm / s, continue for 3 seconds, then decelerate to a standstill at an acceleration of 100 rpm / s.
[0096] ④ Accelerate from rest to 600 rpm at an acceleration of 800 rpm / s for 5 seconds.
[0097] ⑤Decelerate to a standstill at an acceleration of 800rpm / s.
[0098] (2) Baking the first photoresist layer
[0099] ① Raise the temperature of the first photoresist layer from room temperature 25°C to a first temperature of 40°C and keep it warm for 10 minutes.
[0100] ② Raise the temperature of the first photoresist layer from a first temperature of 40°C to a second temperature of 60°C and keep it warm for 10 minutes.
[0101] ③ The first photoresist layer is heated from the second temperature of 60° C. to the third temperature of 80° C. and kept at this temperature for 20 minutes. The thickness of the obtained first photoresist layer is 20.2 um.
[0102] (3) Applying the second photoresist layer
[0103] ①The volume ratio of AZ4562 photoresist stock solution and diluent is the second dilution ratio of 5:1.
[0104] ②Accelerate from rest to 100rpm at an acceleration of 100rpm / s. The photoresist is dynamically dripped from the edge to the center of the glass substrate, and the moving speed of the dripping arm is 6mm / s. When the dripping arm reaches the center of the substrate, the dripping stops.
[0105] ③ Accelerate from 100 rpm to 350 rpm at an acceleration of 200 rpm / s, continue for 3 seconds, then decelerate to a standstill at an acceleration of 100 rpm / s.
[0106] ④ Accelerate from rest to 920 rpm at an acceleration of 800 rpm / s for 5 seconds.
[0107] ⑤Decelerate to a standstill at an acceleration of 800rpm / s.
[0108] (4) Baking the second photoresist layer
[0109] ① Raise the temperature of the second photoresist layer from room temperature 25°C to a fourth temperature of 60°C and keep it warm for 10 minutes.
[0110] ② Raise the temperature of the second photoresist layer from the fourth temperature of 60°C to the fifth temperature of 75°C and keep it warm for 10 minutes.
[0111] ③ The second photoresist layer was heated from the fifth temperature of 75° C. to the sixth temperature of 95° C. and kept at this temperature for 40 minutes. The thickness of the obtained second photoresist layer was 15.4 μm.
[0112] The total thickness of the two-layer photoresist film is 20.2um+15.4um=35.6um. The film is uniform, and there is no obvious glue dripping track left by conventional double-layer glue coating. The product is used by the client, the photolithography is normal, the photoresist microstructure is complete after development, and there is no photoresist residue at the bottom of the microstructure, indicating that the photosensitivity of the bottom layer of photoresist is normal.
[0113] In this embodiment, different layers of photoresist are diluted using different dilution ratios, and the dilution ratio of the bottom layer of photoresist is the largest, and the thickness is the largest. Since the upper layer of photoresist has low viscosity and good leveling properties, it can fill the surface undulations of the lower layer of high viscosity photoresist, so that the final film surface has no undulations and good thickness uniformity. By applying photoresists of different viscosities multiple times, a thick layer of photoresist with large thickness, uniform surface, and good photosensitivity can be obtained.
[0114] After each layer of photoresist is coated, the photoresist layer is baked in a three-stage step-by-step heating method. If the previous layer of photoresist is not baked before the next layer of photoresist is coated, the fluidity of the next layer of photoresist coating will deteriorate due to the wet film of photoresist on the substrate, and the adhesive surface will be uneven after coating, affecting the uniformity of adhesive thickness. In this embodiment, the photoresists of different layers are all heated in steps, and the temperature nodes of each layer of photoresist are set differently. The lower layer of photoresist coated first has a lower baking temperature and a shorter baking time, so as to protect the photosensitivity of the bottom layer of photoresist from loss after multiple baking to the maximum extent.
[0115] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the art within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.
Claims
1. A method for coating and baking a thick layer of photoresist, comprising a glass substrate, wherein a layer of oxide film is coated on the surface of the glass substrate, characterized in that: The coating and baking method comprises: Rotate the glass substrate to dynamically drip the photoresist from the edge of the glass substrate toward the center; Applying a first photoresist to form a first photoresist layer, wherein the volume ratio of the photoresist stock solution of the first photoresist to the diluent is a first dilution ratio R1; Baking the first photoresist layer, baking the first photoresist layer in a step-by-step temperature increase manner to form a film of the first photoresist layer; Coating a second photoresist on the surface of the first photoresist layer to form a second photoresist layer, wherein the volume ratio of the photoresist stock solution of the second photoresist to the diluent is a second dilution ratio R2; Baking the second photoresist layer, baking the second photoresist layer in a step-by-step temperature increase manner to form a film of the second photoresist layer; placing the baked glass substrate in a clean environment to cool the photoresist and the glass substrate to room temperature; The first dilution ratio R1 is greater than the second dilution ratio R2.
2. The coating and baking method according to claim 1, characterized in that: The step-by-step heating method is at least a three-stage step-by-step heating method, and baking the first photoresist layer specifically includes: In the first stage, the temperature of the first photoresist layer is increased from room temperature to the first temperature t1, and kept warm for 10-20 minutes; in the second stage, the temperature of the first photoresist layer is increased from the first temperature t1 to the second temperature t2, and kept warm for 10-20 minutes; in the third stage, the temperature of the first photoresist layer is increased from the second temperature t2 to the third temperature t3, and kept warm for 10-50 minutes; wherein the first temperature t1<second temperature t2<third temperature t3.
3. The coating and baking method according to claim 2, characterized in that: Baking the second photoresist layer specifically includes: In the first stage, the temperature of the second photoresist layer is increased from room temperature to a fourth temperature t4, and kept warm for 10 to 20 minutes; in the second stage, the temperature of the second photoresist layer is increased from the fourth temperature t4 to a fifth temperature t5, and kept warm for 10 to 20 minutes; in the third stage, the temperature of the second photoresist layer is increased from the fifth temperature t5 to a sixth temperature t6, and kept warm for 10 to 50 minutes; wherein the fourth temperature t4 is less than the fifth temperature t5 and is less than the sixth temperature t6, and the third temperature t3 is less than the sixth temperature t6.
4. The coating and baking method according to any one of claims 1 to 3, characterized in that: After the second photoresist layer is baked, the third photoresist is coated and baked on the surface of the second photoresist layer, and then the Nth photoresist is coated and baked to form an Nth photoresist layer. The volume ratio of the photoresist stock solution of the Nth photoresist to the diluent is the Nth dilution ratio Rn, and the Nth dilution ratio Rn is the minimum dilution ratio.
5. The coating and baking method according to claim 4, characterized in that: The Nth photoresist layer is baked by step-by-step heating, including: in the first stage, the Nth photoresist layer is heated from room temperature to a seventh temperature t 3(N-1)+1 , keep warm for 10 to 20 minutes; in the second stage, the Nth photoresist layer is heated from the seventh temperature t 3(N-1)+1 Heating to the eighth temperature t 3(N-1)+2 , keep warm for 10 to 20 minutes; in the third stage, the Nth photoresist layer is heated from the eighth temperature t 3(N-1)+2 Heating to the ninth temperature t 3(N-1)+3 , keep warm for 10 to 50 minutes; the seventh temperature t 3(N-1)+1 <Second temperature t 3(N-1)+2 <Third temperature t 3(N-1)+3 .
6. The coating and baking method according to any one of claims 1 to 3, characterized in that: The rotating glass substrate specifically includes: uniformly accelerating the glass substrate to a rotation speed of 150-400 rpm, and dynamically dripping the photoresist from the edge of the glass substrate toward the center through a hose.
7. The coating and baking method according to any one of claims 1 to 3, characterized in that: The coating of the first photoresist specifically includes: uniformly accelerating the glass substrate to a rotation speed of 500-3000 rpm for spin coating, the spin coating time is 5-30 seconds, and a first photoresist layer is formed, wherein the thickness of the first photoresist layer is a first thickness T1.
8. The coating and baking method according to any one of claims 1 to 3, characterized in that: The coating of the second photoresist on the surface of the first photoresist layer specifically includes: uniformly accelerating the glass substrate to a rotation speed of 1000-3000 rpm for spin coating, the spin coating time is 5-30s, to form a second photoresist layer, the thickness of the second photoresist layer is a second thickness T2, and the first thickness T1>the second thickness T2.
9. The coating and baking method according to any one of claims 1 to 3, characterized in that: The diluent is propylene glycol methyl ether acetate.
10. The coating and baking method according to any one of claims 1 to 3, characterized in that: The coating and baking method further comprises: cleaning the surface of the glass substrate by a DIP cleaning device; A layer of chromium oxide or chromium oxynitride is coated on the surface of the glass substrate by a coating machine.
11. A photomask, characterized in that: The photomask comprises a glass substrate and a photoresist layer disposed on a surface of the glass substrate. The photoresist layer is formed on the surface of the glass substrate by using the coating and baking method according to any one of claims 1 to 10.
Citation Information
Patent Citations
Spin coating device and method utilizing airflow for controlling thickness of photoresist film
CN105057163A