Water-based copper composite conductive paste and preparation method thereof
By using water-based copper composite conductive slurry, utilizing components such as potassium-based montmorillonite and carboxymethylcellulose, combined with silicide and conductive enhancement phase, the impact of organic carriers on performance and environment is solved, and low-temperature curing and high-temperature curing are achieved. The stability and good electrical conductivity solve the problems of environmental pollution and high energy consumption in the existing technology.
Patent Information
- Application Number
- CN202410913899.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-09
AI Technical Summary
The organic carriers used in the preparation process of existing conductive slurries have adverse effects on performance, leading to environmental pollution and health hazards. At the same time, the curing temperature is high and energy consumption is large, which limits its application scope.
Using water-based copper composite conductive slurry, potassium-based montmorillonite, carboxymethyl cellulose and other additives are used as water-based carriers, combined with siliconizing agent and conductive reinforcing phase, to prepare a product with low-temperature curing, high-temperature stability and good conductive properties. of slurry.
A green, environmentally friendly, low-cost conductive slurry is achieved, which avoids the pollution problem of organic carriers, reduces the curing temperature, improves the conductive performance and stability, and is suitable for high-temperature use.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electronic pastes, and in particular to a water-based copper composite conductive paste and a preparation method thereof. Background Art
[0002] Conductive paste (electronic paste) is a new type of electronic material with the characteristics of high efficiency, environmental protection, energy saving and low cost. It has been widely used in technical fields such as solar cells, aerospace, sensitive components, resistor networks, displays, and electrode materials for lithium-ion batteries.
[0003] At present, the most studied conductive pastes include gold (Au) paste, silver (Ag) paste, copper (Cu) paste, etc. Among them, Au has better stability, but its price is expensive, so it is not conducive to industrial production; Ag has better conductivity and its price is slightly lower than Au, but it is still expensive. At the same time, Ag+ migration will occur during the use of Ag, resulting in the degradation of product performance and limiting its scope of use; Cu is a base metal with a wide source, and its conductivity is only slightly lower than Ag, while its price is only about 1% of Ag. It has been widely favored by people in recent years.
[0004] Conductive paste generally consists of three parts: conductive phase, adhesive phase and organic carrier. Organic carrier usually consists of organic solvent, thickener and additive, etc. Its function is to mix and disperse metal powder, adhesive and other solid powder into paste slurry, control the rheology, viscosity and printability of electronic paste, and have an important influence on the conductivity, surface morphology and adhesion of the film after the paste is cured.
[0005] Organic solvents are selected as the main solvents for organic carriers. The content of organic solvents generally accounts for 70%-95% of the total mass of organic carriers, which can dissolve thickeners and some other auxiliary solvents and have low volatility at room temperature. Commonly used organic solvents include diethylene glycol ether acetate, tributyl phthalate, tributyl citrate, olate, pinene alcohol, etc. Commonly used thickeners are ethyl cellulose, which is a thermoplastic polymer that is soluble in a variety of organic solvents. It is a white powder at room temperature and has a wide range of solubility and viscosity characteristics. Other additives include silane coupling agents, surfactants, etc.
[0006] The main disadvantages of organic carriers are high prices. Organic carriers volatilize into the environment, causing environmental pollution and harming the health of workers. At the same time, the selection and content ratio of organic carriers are also direct factors affecting the performance of electronic paste products. When conductive pastes use organic carriers, some defects in the process of use limit the application range of conductive pastes.
[0007] At the same time, the curing temperature of the existing conductive paste is high, and the general curing and sintering temperature is around 600-800°C, which has high energy consumption and is easy to cause deformation of the conductive film substrate and silicon wafer, which is not conducive to improving the life of the conductive film. Summary of the invention
[0008] The purpose of the present invention is to overcome the problem that the organic carrier has an adverse effect on the performance of the electronic paste and pollutes the environment during the preparation of the electronic paste in the prior art, and to provide a water-based copper composite conductive paste and a preparation method thereof. The conductive paste is green and environmentally friendly, low in cost, has good anti-oxidation properties, and can be cured at low temperature and used at high temperature.
[0009] In order to achieve the above object, the present invention provides a water-based copper composite conductive paste on one hand, wherein the water-based copper composite conductive paste comprises the following components by mass fraction: 55% to 70% of a composite conductive phase, 1% to 10% of a bonding phase, 1% to 10% of potassium-based montmorillonite, 0.2% to 2.5% of carboxymethyl cellulose, 0.5% to 6% of a silicifying agent, 0.1% to 1% of a mineralizer, 0.5% to 6% of polydimethylsiloxane, 0.3% to 3% of a surfactant, and 15% to 30% of water;
[0010] Wherein, the siliconizing agent is an organosilicon monomer and / or an organosilicon compound;
[0011] The mineralizer is selected from ZnO, CaO, MgO and Fe 2 O 3 At least one of;
[0012] The composite conductive phase contains copper powder and a conductive reinforcement phase, and the mass ratio of the conductive reinforcement phase to the copper powder is 0.5 to 5:100.
[0013] Preferably, the silicifying agent is selected from at least one of trimethylchlorosilane, hexamethyldisilazane, tert-butyldimethylchlorosilane, triisopropylsilane, dimethyldiacetoxysilane, di-tert-butyldichlorosilane, trimethylhydroxyethylsilane and methyldiphenylhydroxyethylsilane.
[0014] Preferably, the bonding phase is B503 ceramic resin and / or B9102 silicon-zirconium composite inorganic resin.
[0015] Preferably, the surfactant is Tween-80.
[0016] Preferably, the particle size D of the copper powder is 50 1~10μm;
[0017] Preferably, the copper powder is composed of copper powder a, copper powder b and copper powder c, wherein the particle size D of the copper powder a is 50 is 0.5 to 2 μm, and the particle size D of the copper powder b is50 The particle size D of the copper powder c is 4 to 6 μm. 50 9~10μm;
[0018] Preferably, the mass ratio of the copper powder a, copper powder b and copper powder c is 1:0.8-1.2:0.8-1.2.
[0019] Preferably, the conductive enhancement phase is nanoscale graphene sheets and / or carbon nanotubes.
[0020] A second aspect of the present invention provides a method for preparing the water-based copper composite conductive paste as described above, the method comprising the following steps:
[0021] (1) mixing part of water with potassium-montmorillonite to obtain potassium-montmorillonite gel, and then sealing and aging;
[0022] (2) The matured potassium-montmorillonite gel is mixed with polydimethylsiloxane, carboxymethyl cellulose, a binder phase, a silicifying agent, a mineralizer, a surfactant, remaining water and a copper composite conductive phase to obtain a mixed solution, and the obtained mixed solution is kneaded and rubber-milled.
[0023] Preferably, in step (1), the aging time is 20 to 30 hours.
[0024] Preferably, in step (2), the process of kneading and grinding the mixed solution comprises: placing the mixed solution into a high-speed double planetary continuous kneader for 1 to 5 times of uniform kneading, and then placing the mixed solution into a colloid mill for 1 to 5 times of grinding.
[0025] The technical solution provided by the present invention is a technical route different from that of an organic carrier. In the present invention, water is used as a solvent, potassium montmorillonite is used as a suspending agent, carboxymethyl cellulose is used as a water-based thickener, and auxiliary agents (siliconizer, mineralizer and polydimethylsiloxane, etc.) are added to prepare a water-based carrier, and a composite conductive phase and a bonding phase are added to obtain a water-based copper composite conductive slurry.
[0026] Compared with the prior art, the water-based copper composite conductive paste of the present invention has the following beneficial effects:
[0027] (1) The water-based copper composite conductive slurry of the present invention uses water as a solvent, is green, environmentally friendly and low in cost, and only produces water vapor after curing and sintering and is discharged into the air through pipelines, without producing other toxic and harmful gases, thus not causing harm to the environment or negatively affecting human health;
[0028] (2) In the present invention, potassium montmorillonite, water, carboxymethyl cellulose and other additives are mixed as a water-based carrier to replace the commonly used organic carrier, thereby avoiding the adverse effects of the use of organic carriers on the performance of electronic pastes. At the same time, through the joint action of various raw material components, the obtained water-based copper composite conductive paste has good oxidation resistance, suspension stability, rheology and high temperature stability;
[0029] (3) In the present invention, potassium montmorillonite, carboxymethyl cellulose, other additives and water are mixed as a water-based carrier. The selected raw materials are widely available, energy-saving and environmentally friendly, and low in cost. The preparation process is relatively simple and easy to promote;
[0030] (4) The water-based copper composite conductive paste of the present invention has excellent conductive properties through the combined action of various raw material components;
[0031] (5) The water-based copper composite conductive paste of the present invention has a low curing temperature. It can be cured to form a conductive film layer by keeping the temperature at 150-350°C for 15-100 minutes. During the curing process, a protective film is formed by the reaction of the silicide, thereby preventing the copper conductive film from being oxidized during use. The water-based copper composite conductive paste can be used at a temperature in the range of 500-900°C or below, and has high stability. Therefore, the water-based copper composite conductive paste can be cured at low temperature and used at high temperature. DETAILED DESCRIPTION
[0032] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0033] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0034] The present invention provides a water-based copper composite conductive slurry, which comprises the following components in mass fraction: 55% to 70% of a composite conductive phase, 1% to 10% of a bonding phase, 1% to 10% of potassium-based montmorillonite, 0.2% to 2.5% of carboxymethyl cellulose, 0.5% to 6% of a silicifying agent, 0.1% to 1% of a mineralizer, 0.5% to 6% of polydimethylsiloxane, 0.3% to 3% of a surfactant, and 15% to 30% of water;
[0035] Wherein, the siliconizing agent is an organosilicon monomer and / or an organosilicon compound;
[0036] The mineralizer is selected from ZnO, CaO, MgO and Fe 2 O 3 At least one of;
[0037] The composite conductive phase contains copper powder and a conductive reinforcement phase, and the mass ratio of the conductive reinforcement phase to the copper powder is 0.5 to 5:100.
[0038] In the present invention, polydimethylsiloxane is used as an antioxidant; at the same time, the reaction product of the silicifying agent can form a dense silicified film (also called glass film) on the surface of the conductive film layer of the slurry, thereby protecting the conductive film and preventing oxidation. Therefore, in the present invention, the antioxidant polydimethylsiloxane and the silicifying agent can be used together to improve the antioxidant property of the conductive film.
[0039] In a preferred embodiment, the silicifying agent is selected from at least one of trimethylchlorosilane, hexamethyldisilazane, tert-butyldimethylchlorosilane, triisopropylsilane, dimethyldiacetoxysilane, di-tert-butyldichlorosilane, trimethylhydroxyethylsilane and methyldiphenylhydroxyethylsilane.
[0040] In the present invention, potassium-montmorillonite is used as a suspending agent to evenly suspend the conductive components in deionized water to improve the printing performance of the conductive paste, and the thickener carboxymethyl cellulose assists the suspending agent to improve the printing performance of the paste. The present invention does not impose any particular restrictions on the specific source of potassium-montmorillonite, which can be prepared by itself or directly used as a commercial product.
[0041] In the present invention, by adding a small amount of mineralizer, sintering can be promoted and certain properties of the product can be improved, the sintering temperature can be reduced, and at the same time, a certain reduction effect can be achieved, and copper oxide produced by the occasional oxidation of a small amount of copper powder can be reduced to copper powder.
[0042] In a preferred embodiment, the water-based copper composite conductive slurry comprises the following components by mass fraction: 57% to 65% composite conductive phase, 4% to 8% bonding phase, 3% to 7% potassium-based montmorillonite, 1% to 2.5% carboxymethyl cellulose, 2% to 5% silicifying agent, 0.1 to 1% mineralizer, 1% to 4% polydimethylsiloxane, 0.5 to 2% surfactant, and 15% to 30% water.
[0043] In the present invention, the bonding phase bonds the composite conductive phase and other components to the substrate, improving the room temperature and high temperature bonding properties of the conductive film. In a preferred embodiment, the bonding phase is B503 ceramic resin and / or B9102 silicon-zirconium composite inorganic resin. By selecting the above resins as the bonding phase, the curing temperature of the prepared slurry is lower and can be used at a higher temperature. Among them, B503 ceramic resin is a single-component ceramic resin that can be stored for a long time without losing gloss, has super high temperature resistance, and has good film-forming properties. The curing process is 180-280°C / 30min; B9102 silicon-zirconium composite inorganic resin is a silicon-zirconium composite inorganic resin that can be used alone or mixed with silicone resins, etc. It has the characteristics of good temperature resistance, good compatibility, good ultra-high temperature resistance, good film-forming properties, etc. Its curing process is 200-280°C / 30min.
[0044] In the present invention, the rheological properties of the slurry can be improved by adding a surfactant. In a preferred embodiment, the surfactant is Tween-80.
[0045] In the present invention, the particle size D of the copper powder is 50 1~10μm.
[0046] In a preferred embodiment, the copper powder is composed of copper powder a, copper powder b and copper powder c, wherein the particle size D of the copper powder a is 50 is 0.5 to 2 μm, and the particle size D of the copper powder b is 50 The particle size D of the copper powder c is 4 to 6 μm. 50 The particle size of the conductive film is 9 to 10 μm. By selecting copper powders with different particle sizes for mixing, the density of the conductive film layer formed by the slurry can be improved.
[0047] Further preferably, the mass ratio of the copper powder a, copper powder b and copper powder c is 1:0.8-1.2:0.8-1.2.
[0048] In the most preferred embodiment, the copper powder is composed of copper powder a, copper powder b and copper powder c, wherein the particle size D of the copper powder a is 50 is 1 μm, and the particle size D of the copper powder b is 50 is 5 μm, and the particle size D of the copper powder c is 50 is 10 μm, and their mass ratio is 1:1:1.
[0049] In a preferred embodiment, the conductive enhancement phase is nano-graphene sheets and / or carbon nanotubes. Nano-graphene sheets or carbon nanotubes have extremely high conductivity, and by selecting them as conductive enhancement phases and adding them to copper powder, the conductivity of the conductive film can be improved.
[0050] The present invention does not limit the specific preparation steps of the composite conductive phase, as long as the copper powder and the conductive reinforcement phase can be mixed as uniformly as possible. In a preferred embodiment, the composite conductive phase is prepared according to the following process: copper powder and the conductive reinforcement phase are mixed, and then ball milled, and the copper powder and the conductive reinforcement phase are mixed uniformly by ball milling.
[0051] Further preferably, the composite conductive phase is prepared according to the following process:
[0052] The copper powder is pickled, washed with water, and then dried to obtain treated copper powder;
[0053] The conductive enhancement phase is mixed with anhydrous ethanol, then ultrasonically vibrated, and then dried to obtain a treated conductive enhancement phase;
[0054] The treated copper powder and the conductive enhancement phase are mixed and then ball milled to obtain a composite conductive phase.
[0055] The present invention also provides a method for preparing the water-based copper composite conductive paste as described above, the method comprising the following steps:
[0056] (1) mixing part of water with potassium-montmorillonite to obtain potassium-montmorillonite gel, and then sealing and aging;
[0057] (2) The matured potassium-montmorillonite gel is mixed with polydimethylsiloxane, carboxymethyl cellulose, a binder phase, a silicifying agent, a mineralizer, a surfactant, remaining water and a copper composite conductive phase, and the obtained mixed solution is kneaded and rubber-milled.
[0058] In step (1) of the present invention, the relationship between the amount of water, water and potassium-montmorillonite is not particularly limited in the present invention and can be designed according to actual conditions. In a specific embodiment, the mass ratio of water to potassium-montmorillonite is 0.8 to 2:1.
[0059] In a preferred embodiment, in step (1), the aging time is 20 to 30 hours.
[0060] In specific implementation, step (2) includes: mixing the remaining water and the potassium-montmorillonite gel obtained in step (1) evenly; then adding a binder phase, carboxymethyl cellulose, polydimethylsiloxane, a siliconizing agent, a mineralizer, a surfactant, and a composite conductive phase, and mixing them evenly.
[0061] In a preferred embodiment, in step (2), the process of kneading and grinding the obtained mixed solution comprises: putting the mixed solution into a high-speed double planetary continuous kneader for 1 to 5 times of uniform kneading, and then putting it into a colloid mill for 1 to 5 times of grinding.
[0062] The present invention will be described in detail below by way of examples, but the protection scope of the present invention is not limited thereto. The experimental methods in the following examples, unless otherwise specified, are conventional methods in the art. The experimental materials used in the following examples, unless otherwise specified, are commercially available products.
[0063] Example 1
[0064] The following raw material components were weighed according to mass percentage: composite conductive phase 60%, B503 ceramic resin 5%, potassium montmorillonite 5%, carboxymethyl cellulose 1.8%, silicifying agent (trimethylchlorosilane) 3%, polydimethylsiloxane 3%, mineralizer (ZnO) 0.2%, surfactant (Tween-80) 1%, deionized water 21%;
[0065] Wherein, the composite conductive phase is prepared according to the following process:
[0066] Copper powder particle size D 50 Copper powder a of 1 μm, particle size D 50 Copper powder b with a particle size of 5 μm and particle size D 50 The copper powder c with a diameter of 10 μm is mixed in a mass ratio of 1:1:1, the copper powder is pickled with dilute sulfuric acid with a mass fraction of 5% to remove the oxide film on the surface, and the pickled copper powder is repeatedly washed with distilled water until the distilled water used to wash the copper powder does not produce a white precipitate when barium chloride is detected; the powder after pickling and water washing is placed in a vacuum drying oven, kept warm at 80°C for 3 hours, and dried to obtain a copper powder with a clean surface.
[0067] An appropriate amount of anhydrous ethanol was added to the conductive reinforcing phase (nanographene sheets) accounting for 1% of the copper powder, and then ultrasonically oscillated at room temperature for 50 minutes. The obtained dispersion was placed in a vacuum drying oven and kept warm at 55°C for 3 hours. After drying, a conductive reinforcing phase with high dispersibility was obtained.
[0068] The treated copper powder is mixed with the conductive reinforcing phase and then put into a planetary ball mill for 20 minutes to make the main conductive phase and the conductive reinforcing phase evenly mixed to obtain a composite conductive phase.
[0069] The preparation method of the water-based copper composite conductive slurry comprises the following steps:
[0070] (1) Preparation of potassium montmorillonite gel
[0071] Deionized water of the same mass as potassium-montmorillonite is added to the potassium-montmorillonite, mixed evenly, and stirred in a high-speed stirrer for 9 minutes to prepare potassium-montmorillonite gel, which is then sealed and aged for 25 hours for use.
[0072] (2) Preparation of water-based copper composite conductive slurry
[0073] The remaining deionized water is mixed evenly with the potassium-based montmorillonite gel prepared in step (1); ceramic resin, polydimethylsiloxane, silicifying agent, mineralizer, carboxymethyl cellulose, surfactant and composite conductive phase are then added and mixed evenly to obtain a mixed solution; the entire mixed solution is then put into a high-speed double planetary continuous kneading machine for mixing three times; the mixed solution is then put into a colloid mill for colloid grinding three times to continuously produce electronic slurry, and finally a water-based copper composite conductive slurry is efficiently obtained.
[0074] Example 2
[0075] The following raw material components were weighed according to mass percentage: composite conductive phase 62%, B503 ceramic resin 5%, potassium montmorillonite 5%, carboxymethyl cellulose 1.7%, silicifying agent (trimethylchlorosilane) 3%, polydimethylsiloxane 3%, mineralizer (CaO) 0.3%, surfactant (Tween-80) 1%, deionized water 19%;
[0076] Wherein, the composite conductive phase is prepared according to the following process:
[0077] Copper powder particle size D 50 Copper powder a of 1 μm, particle size D 50 Copper powder b with a particle size of 5 μm and particle size D 50 The copper powder c with a diameter of 10 μm is mixed in a mass ratio of 1:1:1, the metal copper powder is pickled with dilute sulfuric acid with a mass fraction of 6% to remove the oxide film on the surface, and the metal copper powder after pickling is repeatedly washed with distilled water until the distilled water used to wash the copper powder does not produce a white precipitate when detected by barium chloride; the copper powder after pickling and water washing is placed in a vacuum drying oven, kept warm at 80°C for 3 hours, and dried to obtain copper powder with a clean surface.
[0078] An appropriate amount of anhydrous ethanol was added to the conductive reinforcement phase (nanographene sheets) accounting for 1% of the copper powder, and then ultrasonically oscillated at room temperature for 50 minutes, and then the dispersion was placed in a vacuum drying oven and kept at 60°C for 3 hours. After drying, a highly dispersed nanocarbon conductive reinforcement phase was obtained.
[0079] The treated copper powder is mixed with the conductive reinforcing phase and then put into a planetary ball mill for 20 minutes to make the main conductive phase and the conductive reinforcing phase evenly mixed to obtain a composite conductive phase.
[0080] The preparation method of the water-based copper composite conductive slurry comprises the following steps:
[0081] (1) Preparation of potassium montmorillonite gel
[0082] Deionized water of the same mass as potassium-montmorillonite is added to the potassium-montmorillonite, and the mixture is evenly mixed and stirred in a high-speed mixer for 10 minutes to prepare potassium-montmorillonite gel, which is then sealed and aged for 24 hours for use.
[0083] (2) Preparation of water-based copper composite conductive slurry
[0084] The remaining deionized water is mixed evenly with the nano potassium-based montmorillonite gel prepared in step (1); ceramic resin, polydimethylsiloxane, silicifying agent, mineralizer, carboxymethyl cellulose, surfactant and composite conductive phase are added and mixed evenly; then the whole mixed solution is put into a high-speed double planetary continuous kneading machine for mixing three times; then the whole mixed solution is put into a colloid mill for colloid grinding four times to continuously produce electronic slurry, and finally a water-based copper composite conductive slurry is efficiently prepared.
[0085] Example 3
[0086] The following raw material components were weighed according to mass percentage: composite conductive phase 60%, B503 ceramic resin 7%, potassium montmorillonite 6%, polydimethylsiloxane 2%, carboxymethyl cellulose 1.6%, silicifying agent (triisopropylsilane) 3.5%, mineralizer (MgO) 0.4%, surfactant (Tween-80) 1.5%, deionized water 18%;
[0087] Wherein, the composite conductive phase is prepared according to the following process:
[0088] Copper powder particle size D 50 Copper powder a of 1 μm, particle size D 50 Copper powder b with a particle size of 5 μm and particle size D 50 The copper powder c with a diameter of 10 μm is mixed in a mass ratio of 1:1:1, the copper powder is pickled with dilute sulfuric acid with a mass fraction of 6% to remove the oxide film on the surface, and the metal copper powder after pickling is repeatedly washed with distilled water until the distilled water used for washing the copper powder is not detected by barium chloride to obtain a white precipitate; the copper powder after pickling and water washing is placed in a vacuum drying oven, kept warm at 80°C for 3 hours, and dried to obtain copper powder with a clean surface.
[0089] An appropriate amount of anhydrous ethanol was added to the conductive reinforcing phase carbon nanotubes accounting for 1% of the copper powder, and then ultrasonically oscillated at room temperature for 50 minutes, and then the dispersion was placed in a vacuum drying oven and kept at 60°C for 3 hours. After drying, a highly dispersed nano-carbon conductive reinforcing phase was obtained.
[0090] The treated copper powder is mixed with the conductive reinforcing phase and then put into a planetary ball mill for 20 minutes to make the main conductive phase and the conductive reinforcing phase evenly mixed to obtain a composite conductive phase.
[0091] The preparation method of the water-based copper composite conductive slurry comprises the following steps:
[0092] (1) Preparation of potassium montmorillonite gel
[0093] Deionized water of the same mass as potassium-montmorillonite is added to the potassium-montmorillonite, and the mixture is evenly mixed and stirred in a high-speed mixer for 20 minutes to prepare potassium-montmorillonite gel, which is then sealed and aged for 24 hours for use.
[0094] (2) Preparation of water-based copper composite conductive slurry
[0095] The remaining deionized water is mixed evenly with the potassium-based montmorillonite gel prepared in step (1); ceramic resin, polydimethylsiloxane, carboxymethyl cellulose, silicifying agent, mineralizer, surfactant Tween-80 and composite conductive phase are then added and mixed evenly; the entire mixed solution is then put into a high-speed double planetary continuous kneading machine for mixing three times; the mixture is then put into a colloid mill for 5 times of colloid grinding to continuously produce electronic slurry, and finally a water-based copper composite conductive slurry is efficiently prepared.
[0096] Example 4
[0097] The following raw material components were weighed according to mass percentage: composite conductive phase 60%, potassium montmorillonite 4%, B9102 silicon-zirconium composite inorganic resin 6%, polydimethylsiloxane 2.5%, carboxymethyl cellulose 2%, silicifying agent (triisopropylsilane) 4%, mineralizer (ZnO) 0.5%, surfactant (Tween-80) 1%, and deionized water 20%;
[0098] Wherein, the composite conductive phase is prepared according to the following process:
[0099] Copper powder particle size D 50 Copper powder a of 1 μm, particle size D 50 Copper powder b with a particle size of 5 μm and particle size D 50 The copper powder c with a diameter of 10 μm is mixed in a mass ratio of 1:1:1, the metal copper powder is pickled with dilute sulfuric acid with a mass fraction of 6% to remove the oxide film on the surface, and the metal copper powder after pickling is repeatedly washed with distilled water until the distilled water used for washing the copper powder is not detected by barium chloride to obtain a white precipitate; the copper powder after pickling and water washing is placed in a vacuum drying oven, kept at 80°C for 3 hours, and dried to obtain a copper powder with a clean surface.
[0100] An appropriate amount of anhydrous ethanol was added to the conductive reinforcing phase carbon nanotubes accounting for 1% of the copper powder, and then ultrasonically oscillated at room temperature for 50 minutes, and then the dispersion was placed in a vacuum drying oven and kept at 60°C for 3 hours. After drying, a highly dispersed nano-carbon conductive reinforcing phase was obtained.
[0101] The treated copper powder is mixed with the conductive reinforcing phase and then put into a planetary ball mill for 20 minutes to make the main conductive phase and the conductive reinforcing phase evenly mixed to obtain a composite conductive phase.
[0102] The preparation method of the water-based copper composite conductive slurry comprises the following steps:
[0103] (1) Preparation of potassium montmorillonite gel
[0104] Deionized water of the same mass as potassium-montmorillonite is added to the potassium-montmorillonite, and the mixture is evenly mixed and stirred in a high-speed stirrer for 30 minutes to prepare potassium-montmorillonite gel, which is then sealed and aged for 24 hours for use.
[0105] (2) Preparation of water-based copper composite conductive slurry
[0106] The remaining deionized water is mixed evenly with the potassium-based montmorillonite gel prepared in step (1); then B9102 silicon-zirconium composite inorganic resin, polydimethylsiloxane, carboxymethyl cellulose, silicifying agent, mineralizer, surfactant Tween-80 and composite conductive phase are added and mixed evenly; then the entire mixed solution is put into a high-speed double planetary continuous kneading machine for 4 times of mixing; then put into a colloid mill for 3 times of colloid grinding, and the electronic slurry is continuously produced, and finally a water-based copper composite conductive slurry is efficiently prepared.
[0107] Example 5
[0108] The following raw material components were weighed according to mass percentage: potassium-montmorillonite 5%, composite conductive phase 60%, B9102 silicon-zirconium composite inorganic resin 6%, silicifying agent (trimethylchlorosilane) 4%, polydimethylsiloxane 2%, carboxymethyl cellulose 2.4%, mineralizer (ZnO) 0.6%, surfactant (Tween-80) 1%, and deionized water 19%;
[0109] Wherein, the composite conductive phase is prepared according to the following process:
[0110] The copper powder is made of particle size D 50 Copper powder a of 1 μm, particle size D 50 Copper powder b with a particle size of 5 μm and particle size D 50 The copper powder c with a diameter of 10 μm is mixed in a mass ratio of 1:1:1, the metal copper powder is pickled with dilute sulfuric acid with a mass fraction of 6% to remove the oxide film on the surface, and the metal copper powder after pickling is repeatedly washed with distilled water until the distilled water used for washing the copper powder is not detected by barium chloride to obtain a white precipitate; the copper powder after pickling and water washing is placed in a vacuum drying oven, kept at 80°C for 3 hours, and dried to obtain a copper powder with a clean surface.
[0111] An appropriate amount of anhydrous ethanol was added to the conductive reinforcing phase carbon nanotubes accounting for 1% of the copper powder, and then ultrasonically oscillated at room temperature for 50 minutes, and then the dispersion was placed in a vacuum drying oven and kept at 60°C for 3 hours. After drying, a highly dispersed nano-carbon conductive reinforcing phase was obtained.
[0112] The treated copper powder is mixed with the conductive reinforcing phase and then put into a planetary ball mill for 20 minutes to make the main conductive phase and the conductive reinforcing phase evenly mixed to obtain a composite conductive phase.
[0113] The preparation method of the water-based copper composite conductive slurry comprises the following steps:
[0114] (1) Preparation of potassium montmorillonite gel
[0115] Deionized water of the same mass as potassium-montmorillonite is added to the potassium-montmorillonite, and the mixture is evenly mixed and stirred in a high-speed stirrer for 30 minutes to prepare potassium-montmorillonite gel, which is then sealed and aged for 24 hours for use.
[0116] (2) Preparation of water-based copper composite conductive slurry
[0117] The remaining deionized water is mixed evenly with the potassium-based montmorillonite gel prepared in step (1); then B9102 silicon-zirconium composite inorganic resin, polydimethylsiloxane, silicifying agent, mineralizer, carboxymethyl cellulose, surfactant Tween-80 and composite conductive phase are added and mixed evenly; then the entire mixed solution is put into a high-speed double planetary continuous kneading machine for 5 times of mixing; then put into a colloid mill for 3 times of gel grinding, and the electronic slurry is continuously produced, and finally a water-based copper composite conductive slurry is efficiently prepared.
[0118] Example 6
[0119] The following raw material components were weighed according to mass percentage: potassium-montmorillonite 4%, composite conductive phase 60%, B9102 silicon-zirconium composite inorganic resin 6%, silicifying agent (hexamethyldisilazane) 4%, polydimethylsiloxane 1.5%, carboxymethyl cellulose 1.8%, mineralizer (CaO) 0.7%, surfactant (Tween-80) 1%, and deionized water 21%;
[0120] Wherein, the composite conductive phase is prepared according to the following process:
[0121] Copper powder particle size D 50 Copper powder a of 1 μm, particle size D 50 Copper powder b with a particle size of 5 μm and particle size D 50 The copper powder c with a diameter of 10 μm is mixed in a mass ratio of 1:1:1, the metal copper powder is pickled with dilute sulfuric acid with a mass fraction of 6% to remove the oxide film on the surface, and the metal copper powder after pickling is repeatedly washed with distilled water until the distilled water used for washing the copper powder is not detected by barium chloride to obtain a white precipitate; the powder after pickling and water washing is placed in a vacuum drying oven, kept at 80°C for 3 hours, and dried to obtain a copper powder with a clean surface.
[0122] An appropriate amount of anhydrous ethanol is added to the conductive reinforcing phase nanographene sheets accounting for 1% of the copper powder, and then ultrasonically oscillated at room temperature for 50 minutes, and then the dispersion is placed in a vacuum drying oven and kept at 60°C for 3 hours. After drying, a highly dispersed nanocarbon conductive reinforcing phase is obtained.
[0123] The treated copper powder is mixed with the conductive reinforcing phase and then put into a planetary ball mill for 20 minutes to make the main conductive phase and the conductive reinforcing phase evenly mixed to obtain a composite conductive phase.
[0124] The preparation method of the water-based copper composite conductive slurry comprises the following steps:
[0125] (1) Preparation of potassium montmorillonite gel
[0126] Deionized water of the same mass as potassium-montmorillonite is added to the potassium-montmorillonite, and the mixture is evenly mixed and stirred in a high-speed stirrer for 30 minutes to prepare potassium-montmorillonite gel, which is then sealed and aged for 24 hours for use.
[0127] (2) Preparation of water-based copper composite conductive slurry
[0128] The remaining deionized water is mixed evenly with the potassium-based montmorillonite gel prepared in step (1); then B9102 silicon-zirconium composite inorganic resin, polydimethylsiloxane, silicifying agent, mineralizer, carboxymethyl cellulose, surfactant and composite conductive phase are added and mixed evenly; then the entire mixed solution is put into a high-speed double planetary continuous kneading machine for mixing twice; then the mixture is put into a colloid mill for 4 times of colloid grinding to continuously produce electronic slurry, and finally a water-based copper composite conductive slurry is efficiently prepared.
[0129] Example 7
[0130] The method described in Example 1 was used for implementation, except that the particle size D of the copper powder was 50 is 5 μm (i.e., copper powder a and c are replaced by an equal amount of copper powder b).
[0131] Comparative Example 1
[0132] The method described in Example 1 was followed, except that the conductive enhancement phase was replaced with an equal amount of copper powder.
[0133] Comparative Example 2
[0134] The method described in Example 1 was followed, except that the silanizing agent was replaced with an equal amount of polydimethylsiloxane.
[0135] Comparative Example 3
[0136] The method described in Example 1 was followed, except that polydimethylsiloxane was replaced with an equal amount of a siliconizing agent.
[0137] Test Example 1
[0138] The water-based copper composite conductive pastes prepared in Examples 1-7 and Comparative Example 1 were subjected to conductivity tests. The conductivity of the conductive film formed by curing the water-based copper composite conductive paste was measured using a standard four-probe method; the resistivity of the conductive film was tested using a FT-340 digital four-probe resistivity tester produced by Ningbo Ruike Instruments. The square resistance range of the instrument is 1×10 -5 ~2×10 6 Ω / ρ, resistivity range is 1×10 -6 ~2×10 6 Ω·cm. The test results are shown in Table 1 below.
[0139] Table 1
[0140] Test samples Resistivity (mΩ·cm) Curing temperature(℃) Example 1 6.75 200 Example 2 7.86 200 Example 3 7.94 200 Example 4 7.55 200 Example 5 6.72 200 Example 6 7.53 200 Example 7 8.35 200 Comparative Example 1 8.98 200
[0141] It can be seen from the experimental results in Table 1 that the water-based copper composite conductive paste provided by the present invention has excellent conductive properties and a low curing temperature.
[0142] Test Example 2
[0143] After the water-based copper composite conductive pastes prepared in Example 1 and Comparative Examples 2-3 were cured at 200° C., an oxidation resistance test was performed under conditions of 60% humidity and 20° C. The test results are shown in Table 2 below.
[0144] Table 2
[0145] serial number Antioxidant Example 1 No significant change in 500 days Comparative Example 2 No significant change in 400 days Comparative Example 3 No significant change for 419 days
[0146] It can be seen from Table 2 that the water-based copper composite conductive paste provided by the present invention has excellent antioxidant properties. At the same time, by comparing Example 1 with Comparative Examples 2-3, it can be seen that the combined use of polydimethylsiloxane and the silanizing agent also plays an important role in improving the antioxidant properties, and even the lack of one of them will lead to a significant weakening of the antioxidant properties, indicating that polydimethylsiloxane and the silanizing agent play a synergistic role in improving the antioxidant properties of the water-based copper composite conductive paste.
[0147] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A water-based copper composite conductive slurry, characterized in that: The water-based copper composite conductive paste comprises the following components by mass fraction: 55% to 70% composite conductive phase, 1% to 10% bonding phase, 1% to 10% potassium-based montmorillonite, 0.2% to 2.5% carboxymethyl cellulose, 0.5% to 6% silicifying agent, 0.1% to 1% mineralizer, 0.5% to 6% polydimethylsiloxane, 0.3% to 3% surfactant, and 15% to 30% water; Wherein, the siliconizing agent is an organosilicon monomer and / or an organosilicon compound; The mineralizer is selected from at least one of ZnO, CaO, MgO and Fe2O3; The composite conductive phase contains copper powder and a conductive reinforcement phase, and the mass ratio of the conductive reinforcement phase to the copper powder is 0.5 to 5:
100.
2. The water-based copper composite conductive paste according to claim 1, characterized in that: The silicifying agent is selected from at least one of trimethylchlorosilane, hexamethyldisilazane, tert-butyldimethylchlorosilane, triisopropylsilane, dimethyldiacetoxysilane, di-tert-butyldichlorosilane, trimethylhydroxyethylsilane and methyldiphenylhydroxyethylsilane.
3. The water-based copper composite conductive paste according to claim 1, characterized in that: The bonding phase is B503 ceramic resin and / or B9102 silicon-zirconium composite inorganic resin.
4. The water-based copper composite conductive paste according to claim 1, characterized in that: The surfactant is Tween-80.
5. The water-based copper composite conductive paste according to claim 1, characterized in that: The particle size D of the copper powder 50 1~10μm.
6. The water-based copper composite conductive paste according to claim 1 or 5, characterized in that: The copper powder is composed of copper powder a, copper powder b and copper powder c, wherein the particle size D of the copper powder a is 50 is 0.5 to 2 μm, and the particle size D of the copper powder b is 50 The particle size D of the copper powder c is 4 to 6 μm. 50 9~10μm; Preferably, the mass ratio of the copper powder a, copper powder b and copper powder c is 1:0.8-1.2:0.8-1.
2.
7. The water-based copper composite conductive paste according to claim 1, characterized in that: The conductive enhancement phase is nano-scale graphene sheets and / or carbon nanotubes.
8. A method for preparing the water-based copper composite conductive paste according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: (1) mixing part of water with potassium-montmorillonite to obtain potassium-montmorillonite gel, and then sealing and aging; (2) Mixing the matured potassium montmorillonite gel with polydimethylsiloxane, carboxymethyl cellulose, a binder phase, a silicifying agent, a mineralizer, a surfactant, remaining water and a composite conductive phase, and kneading and grinding the obtained mixed solution.
9. The method according to claim 8, characterized in that In step (1), the aging time is 20 to 30 hours.
10. The method according to claim 8, characterized in that In step (2), the process of kneading and grinding the mixed solution comprises: putting the mixed solution into a high-speed double planetary continuous kneader for 1 to 5 times of uniform kneading, and then putting the mixed solution into a colloid mill for 1 to 5 times of grinding.
Citation Information
Patent Citations
Water-based electronic slurry and preparation method thereof
CN109698040A
Conductive copper paste and using method thereof
CN111540503A
Low-temperature curing type three-proofing conductive nickel paste as well as preparation method and application thereof
CN114334220A
Conductive film, connection structure, and method for producing same
CN118922923A
Conductive paste
JP2014011006A