Transparent conductive film
By using a krypton-containing light-transmitting conductive layer and conductive oxide in a transparent conductive film, combined with sputtering and crystallization processes, the problems of high resistance and warpage of the transparent conductive film are solved, and low resistance and Stable transparent electrode performance.
Patent Information
- Application Number
- CN202411017966.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-02
- Filing Date
- 2021-03-18
- Publication Date
- 2024-10-15
AI Technical Summary
Existing transparent conductive films have problems such as high resistance and easy warping in applications. Especially in transparent electrode applications, it is difficult to meet low resistance and stability requirements.
A translucent conductive layer containing krypton is used to form a conductive oxide on the transparent substrate through sputtering. The compressive residual stress of the conductive layer is controlled to be less than 490MPa, and the amorphous conductive layer is crystallized through heating to optimize the conductive layer. structure and thickness for low resistance and resistance to warping.
It achieves low resistance and suppresses warpage of transparent conductive films, and is suitable for transparent electrodes in devices such as liquid crystal displays and touch panels, improving the performance and stability of the devices.
Smart Images

Figure CN118782297A_ABST
Abstract
Description
[0001] This application is a divisional application of an application with a filing date of March 18, 2021, an application number of 202180022465.5, and an invention name of transparent conductive film. Technical Field
[0002] The present invention relates to a transparent conductive film. Background Art
[0003] In the past, a transparent conductive film having a transparent substrate film and a transparent conductive layer (translucent conductive layer) in sequence along the thickness direction is known. The translucent conductive layer is used as a conductor film for patterning transparent electrodes in various devices such as liquid crystal displays, touch panels and optical sensors. In addition, the translucent conductive layer is sometimes also used as an antistatic layer possessed by the device. The translucent conductive layer is formed by forming a film of a conductive oxide on a substrate film, for example, by sputtering. In the sputtering method, inert gases such as argon gas are used as sputtering gases for impacting a target (film forming material supply material) to eject atoms on the target surface. Related technologies regarding this transparent conductive film are described in, for example, the following patent document 1.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 5-334924 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] The light-transmitting conductive layer of a transparent conductive film is required to have low resistance. This requirement is particularly high for a transparent conductive film used as a transparent electrode. In addition, the transparent conductive film is also required to be less prone to warping.
[0009] The present invention provides a transparent conductive film suitable for achieving low resistance of a light-transmitting conductive layer and suppressing warping of the film.
[0010] Solutions for solving problems
[0011] The present invention [1] includes a transparent conductive film, which comprises a transparent substrate and a light-transmitting conductive layer in this order along the thickness direction, wherein the light-transmitting conductive layer contains krypton, and the light-transmitting conductive layer has a compressive residual stress of less than 490 MPa in an in-plane direction perpendicular to the thickness direction.
[0012] The present invention [2] includes the transparent conductive film described in [1] above, wherein the average number of grain boundaries in the in-plane direction of the light-transmitting conductive layer is less than 12 / μm.
[0013] The present invention [3] includes the transparent conductive film described in [1] or [2] above, wherein the light-transmitting conductive layer contains a conductive oxide containing indium.
[0014] The present invention [4] includes the transparent conductive film according to any one of the above [1] to [3], wherein the light-transmitting conductive layer does not contain xenon.
[0015] The present invention [5] comprises the transparent conductive film described in any one of [1] to [4] above, wherein the light-transmitting conductive layer has a thickness of 2.2×10 -4 Resistivity below Ω·cm.
[0016] The present invention [6] includes the transparent conductive film according to any one of [1] to [5] above, wherein the light-transmitting conductive layer has a thickness of 30 nm or more.
[0017] Effects of the Invention
[0018] The transparent conductive film of the present invention is suitable for achieving low resistance of the transparent conductive layer and suppressing warping of the film because the transparent conductive layer on the transparent substrate contains krypton and the transparent conductive layer has a compressive residual stress of less than 490 MPa in its in-plane direction. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic cross-sectional view of one embodiment of the transparent conductive film of the present invention.
[0020] Figure 2 It is a schematic cross-sectional view of a modified example of the transparent conductive film of the present invention. Figure 2 A in FIG. 1 represents a case where the light-transmitting conductive layer includes a first region and a second region in this order from the transparent substrate side. Figure 2 B represents the case where the light-transmitting conductive layer includes the second region and the first region in this order from the transparent substrate side.
[0021] Figure 3 express Figure 1 A method for producing a transparent conductive film is shown in . Figure 3 A represents the process of preparing a transparent resin film, Figure 3 B represents a process of forming a functional layer on a transparent resin film, Figure 3 C represents a step of forming a light-transmitting conductive layer on the functional layer, Figure 3 D represents the crystallization step of the light-transmitting conductive layer.
[0022] Figure 4 express Figure 1 2 shows a case where the light-transmitting conductive layer in the transparent conductive film is patterned.
[0023] Figure 5 This is a graph showing the relationship between the amount of oxygen introduced when a light-transmitting conductive layer is formed by a sputtering method and the resistivity of the formed light-transmitting conductive layer.
[0024] Description of Reference Numerals
[0025] XTransparent Conductive Film
[0026] DThickness direction
[0027] 10 Transparent substrate
[0028] 11. Transparent resin film
[0029] 12 Functional Layer
[0030] 20 Translucent conductive layer
[0031] 21. Area 1
[0032] 22 Second Area DETAILED DESCRIPTION
[0033] Figure 1 : is a schematic cross-sectional view of a transparent conductive film X as an embodiment of the transparent conductive film of the present invention. The transparent conductive film X includes a transparent substrate 10 and a translucent conductive layer 20 in order on one side facing the thickness direction D. The transparent conductive film X, the transparent substrate 10, and the translucent conductive layer 20 each have a shape extending in a direction (surface direction) orthogonal to the thickness direction D. The transparent conductive film X is an element included in a touch sensor device, a dimming element, a photoelectric conversion element, a heat line control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, an image display device, and the like.
[0034] In the present embodiment, the transparent substrate 10 includes a transparent resin film 11 and a functional layer 12 in this order on one side facing the thickness direction D.
[0035] The transparent resin film 11 is a transparent resin film with flexibility. As the material of the transparent resin film 11, for example, polyester resin, polyolefin resin, acrylic resin, polycarbonate resin, polyethersulfone resin, polyarylate resin, melamine resin, polyamide resin, polyimide resin, cellulose resin and polystyrene resin can be listed. As polyester resin, for example, polyethylene terephthalate (PET), polybutylene terephthalate and polyethylene naphthalate can be listed. As polyolefin resin, for example, polyethylene, polypropylene and cycloolefin polymer can be listed. As acrylic resin, for example, polymethacrylate can be listed. As the material of the transparent resin film 11, from the aspect of easily obtaining a transparent resin film 11 with high surface smoothness, it is preferably selected from the group consisting of polyolefin resin, acrylic resin, polycarbonate resin, melamine resin and polyester resin, and PET is more preferably selected. The high surface smoothness of the transparent resin film 11 contributes to the low resistance of the light-transmitting conductive layer 20, and also contributes to obtaining a transparent conductive film X with suppressed warping.
[0036] The surface of the functional layer 12 side of the transparent resin film 11 may be subjected to a surface modification treatment. Examples of the surface modification treatment include corona treatment, plasma treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment.
[0037] The thickness of the transparent resin film 11 is preferably 1 μm or more, more preferably 10 μm or more, and further preferably 30 μm or more. The thickness of the transparent resin film 11 is preferably 300 μm or less, more preferably 200 μm or less, further preferably 100 μm or less, and particularly preferably 75 μm or less. These configurations related to the thickness of the transparent resin film 11 are suitable for ensuring the handling properties of the transparent conductive film X.
[0038] The total light transmittance (JIS K 7375-2008) of the transparent resin film 11 is preferably 60% or more, more preferably 80% or more, and further preferably 85% or more. This configuration is suitable for ensuring the transparency required for the transparent conductive film X when the transparent conductive film X is provided in a touch sensor device, a dimming element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, an image display device, etc. The total light transmittance of the transparent resin film 11 is, for example, 100% or less.
[0039] In this embodiment, the functional layer 12 is located on one surface of the transparent resin film 11 in the thickness direction D. In addition, in this embodiment, the functional layer 12 is used to prevent the exposed surface (in the middle of the transparent conductive layer 20) from being exposed. Figure 1 The upper surface in the middle forms a hard coating with scratches.
[0040] The hard coat layer is a cured product of a curable resin composition. As the resin contained in the curable resin composition, for example, polyester resins, acrylic resins, urethane resins, amide resins, silicone resins, epoxy resins and melamine resins can be listed. In addition, as the curable resin composition, for example, ultraviolet curable resin compositions and thermosetting resin compositions can be listed. Since curing can occur without high temperature heating, from the viewpoint of contributing to improving the manufacturing efficiency of the transparent conductive film X, as the curable resin composition, an ultraviolet curable resin composition is preferably used. As an ultraviolet curable resin composition, specifically, a hard coat forming composition described in Japanese Patent Publication No. 2016-179686 can be listed.
[0041] The surface of the functional layer 12 on the side of the light-transmitting conductive layer 20 may be subjected to a surface modification treatment. Examples of the surface modification treatment include corona treatment, plasma treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment.
[0042] The thickness of the functional layer 12 as a hard coat layer is preferably 0.1 μm or more, more preferably 0.5 μm or more, and further preferably 1 μm or more. This configuration is suitable for allowing the light-transmitting conductive layer 20 to exhibit sufficient scratch resistance. From the viewpoint of ensuring the transparency of the functional layer 12, the thickness of the functional layer 12 as a hard coat layer is preferably 10 μm or less, more preferably 5 μm or less, and further preferably 3 μm or less.
[0043] The thickness of the transparent substrate 10 is preferably 1 μm or more, more preferably 10 μm or more, further preferably 15 μm or more, and particularly preferably 30 μm or more. The thickness of the transparent substrate 10 is preferably 310 μm or less, more preferably 210 μm or less, further preferably 110 μm or less, and particularly preferably 80 μm or less. These configurations related to the thickness of the transparent substrate 10 are suitable for ensuring the handling properties of the transparent conductive film X.
[0044] The total light transmittance (JIS K 7375-2008) of the transparent substrate 10 is preferably 60% or more, more preferably 80% or more, and further preferably 85% or more. This configuration is suitable for ensuring the transparency required for the transparent conductive film X when the transparent conductive film X is provided in a touch sensor device, a dimming element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, an image display device, etc. The total light transmittance of the transparent substrate 10 is, for example, 100% or less.
[0045] In the present embodiment, the light-transmitting conductive layer 20 is located on one surface of the transparent substrate 10 in the thickness direction D. The light-transmitting conductive layer 20 is a crystalline film having both light transmittance and conductivity.
[0046] The light-transmitting conductive layer 20 is a layer formed of a light-transmitting conductive material. The light-transmitting conductive material contains, for example, a conductive oxide as a main component.
[0047] As the conductive oxide, for example, a metal oxide containing at least one metal or semimetal selected from the group consisting of In, Sn, Zn, Ga, Sb, Ti, Si, Zr, Mg, Al, Au, Ag, Cu, Pd, and W can be cited. Specifically, as the conductive oxide, a conductive oxide containing indium and a conductive oxide containing antimony can be cited. As the conductive oxide containing indium, for example, indium tin composite oxide (ITO), indium zinc composite oxide (IZO), indium gallium composite oxide (IGO), and indium gallium zinc composite oxide (IGZO) can be cited. As the conductive oxide containing antimony, for example, antimony tin composite oxide (ATO) can be cited. From the viewpoint of achieving high transparency and good conductivity, as the conductive oxide, a conductive oxide containing indium is preferably used, and ITO is more preferably used. The ITO contains a metal or semimetal other than In and Sn in an amount less than the content of each of In and Sn.
[0048] When ITO is used as a conductive oxide, the ratio of the content of tin oxide in the ITO to the total content of indium oxide (In2O3) and tin oxide (SnO2) is preferably 0.1% by mass or more, more preferably 3% by mass or more, further preferably 5% by mass or more, and particularly preferably 7% by mass or more. The ratio of the number of tin atoms in the ITO used to the number of indium atoms (tin atoms / indium atoms) is preferably 0.001 or more, more preferably 0.03 or more, further preferably 0.05 or more, and particularly preferably 0.07 or more. These structures are suitable for ensuring the durability of the light-transmitting conductive layer 20. In addition, the ratio of the content of tin oxide in the ITO used to the total content of indium oxide (In2O3) and tin oxide (SnO2) is preferably 15% by mass or less, more preferably 13% by mass or less, and further preferably 12% by mass or less. The ratio of the number of tin atoms in the ITO used to the number of indium atoms (tin atoms / indium atoms) is preferably 0.16 or less, more preferably 0.14 or less, and further preferably 0.13 or less. These structures are suitable for obtaining a translucent conductive layer 20 that is easily crystallized by heating. The ratio of the number of tin atoms in ITO to the number of indium atoms is obtained by, for example, determining the existence ratio of indium atoms and tin atoms in the measured object using X-ray photoelectron spectroscopy. The above-mentioned content ratio of tin oxide in ITO is obtained based on the existence ratio of indium atoms and tin atoms determined by, for example, such an operation. The above-mentioned content ratio of tin oxide in ITO can be determined based on the content ratio of tin oxide (SnO2) of the ITO target used in sputtering film formation.
[0049] The light-transmitting conductive layer 20 contains krypton (Kr) as a rare gas atom. In the present embodiment, the rare gas atom in the light-transmitting conductive layer 20 originates from a rare gas atom used as a sputtering gas in the sputtering method described later for forming the light-transmitting conductive layer 20. In the present embodiment, the light-transmitting conductive layer 20 is a film (sputtered film) formed by the sputtering method.
[0050] The light-transmitting conductive layer 20 preferably contains a region in which the content of Kr in a portion of the thickness direction D is preferably 1.0 atomic % or less, more preferably 0.7 atomic % or less, further preferably 0.5 atomic % or less, further preferably 0.3 atomic % or less, particularly preferably 0.2 atomic % or less, and particularly preferably less than 0.1 atomic %. The content of Kr in this region is, for example, 0.0001 atomic % or more. The light-transmitting conductive layer 20 preferably satisfies this Kr content in the entire region in the thickness direction D. Specifically, the content of Kr in the light-transmitting conductive layer 20 in the entire region in the thickness direction D is preferably 1.0 atomic % or less, more preferably 0.7 atomic % or less, further preferably 0.5 atomic % or less, further preferably 0.3 atomic % or less, particularly preferably 0.2 atomic % or less, and particularly preferably less than 0.1 atomic %. These structures are suitable for achieving good crystal growth and forming large grains when the amorphous translucent conductive layer (translucent conductive layer 20' described later) is crystallized by heating to form the translucent conductive layer 20 during the manufacturing process of the transparent conductive film X. Therefore, they are suitable for obtaining a translucent conductive layer 20 with low resistance (the larger the grains in the translucent conductive layer 20, the lower the resistance of the translucent conductive layer 20).
[0051] Whether there are rare gas atoms such as Kr in the light-transmitting conductive layer 20 and their content, for example, the embodiment is identified by using Rutherford Backscattering Spectrometry described later. Whether there are rare gas atoms such as Kr in the light-transmitting conductive layer 20, for example, the embodiment is identified by using fluorescent X-ray analysis described later. For the light-transmitting conductive layer as the analysis object, since the content of rare gas atoms is not above the detection limit (lower limit), it cannot be quantified by Rutherford backscattering analysis, and when the presence of rare gas atoms is identified by fluorescent X-ray analysis, it is judged that the light-transmitting conductive layer contains a region in which the content ratio of rare gas atoms such as Kr is greater than 0.0001 atomic %.
[0052] The content ratio of Kr in the light-transmitting conductive layer 20 may be different in the thickness direction D. For example, the content ratio of Kr may increase or decrease as it moves away from the transparent substrate 10 in the thickness direction D. Alternatively, the partial region where the content ratio of Kr increases as it moves away from the transparent substrate 10 in the thickness direction D may be located on the transparent substrate 10 side, and the partial region where the content ratio of Kr decreases as it moves away from the transparent substrate 10 may be located on the side opposite to the transparent substrate 10. Alternatively, the partial region where the content ratio of Kr decreases as it moves away from the transparent substrate 10 in the thickness direction D may be located on the transparent substrate 10 side, and the partial region where the content ratio of Kr increases as it moves away from the transparent substrate 10 may be located on the side opposite to the transparent substrate 10.
[0053] From the viewpoint of reducing the compressive residual stress of the light-transmitting conductive layer 20 , the light-transmitting conductive layer 20 preferably contains only Kr as the rare gas atom.
[0054] When the light-transmitting conductive layer 20 contains a rare gas atom other than Kr, examples of the rare gas atom other than Kr include argon (Ar) and xenon (Xe). From the viewpoint of reducing the manufacturing cost of the transparent conductive film X, the light-transmitting conductive layer 20 preferably does not contain Xe.
[0055] The content ratio of the rare gas atoms (including Kr) in the light-transmitting conductive layer 20 is preferably 1.2 atomic % or less, more preferably 1.1 atomic % or less, further preferably 1.0 atomic % or less, further preferably 0.8 atomic % or less, further preferably 0.5 atomic % or less, further preferably 0.4 atomic % or less, particularly preferably 0.3 atomic % or less, and particularly preferably 0.2 atomic % or less. This structure is suitable for achieving good crystal growth and forming large grains when the amorphous light-transmitting conductive layer is crystallized by heating to form the light-transmitting conductive layer 20 in the manufacturing process of the transparent conductive film X, and therefore, it is suitable for obtaining a light-transmitting conductive layer 20 with low resistance. In addition, the light-transmitting conductive layer 20 includes a region in which the content ratio of the rare gas atoms is, for example, 0.0001 atomic % or more in at least a portion of the thickness direction D. The content ratio of the rare gas atoms in the light-transmitting conductive layer 20 is, for example, preferably 0.0001 atomic % or more in the entire region of the thickness direction D.
[0056] like Figure 2 As exemplified in FIG. 8 , the light-transmitting conductive layer 20 may contain Kr in a partial region in the thickness direction D. As exemplified in FIG. Figure 2 A in FIG. 2 represents a case where the light-transmitting conductive layer 20 includes the first region 21 and the second region 22 in this order from the transparent substrate 10 side. The first region 21 contains Kr. The second region 22 does not contain Kr, but contains, for example, a rare gas atom other than Kr. Figure 2 B represents the case where the light-transmitting conductive layer 20 includes the second region 22 and the first region 21 in this order from the transparent substrate 10 side. Figure 2 Although the boundary between the first region 21 and the second region 22 is drawn with an imaginary line, the boundary between the first region 21 and the second region 22 is sometimes impossible to clearly distinguish when there is no significant difference in composition between the first region 21 and the second region 22 other than the content of trace amounts of rare gas atoms.
[0057] When the light-transmitting conductive layer 20 includes a first region 21 and a second region 22, from the viewpoint of reducing the compressive residual stress of the light-transmitting conductive layer 20, the light-transmitting conductive layer 20 preferably includes a first region 21 (a region containing Kr) and a second region 22 (a region not containing Kr) in sequence from the transparent substrate 10 side.
[0058] When the light-transmitting conductive layer 20 includes the first region 21 and the second region 22, the ratio of the thickness of the first region 21 to the total thickness of the first region 21 and the second region 22 is preferably 1% or more, more preferably 20% or more, further preferably 30% or more, further preferably 40% or more, and particularly preferably 50% or more. This ratio is less than 100%. In addition, the ratio of the thickness of the second region 22 to the total thickness of the first region 21 and the second region 22 is preferably 99% or less, more preferably 80% or less, further preferably 70% or less, further preferably 60% or less, and particularly preferably 50% or less. In the case where the light-transmitting conductive layer 20 includes the first region 21 and the second region 22, this configuration related to the ratio of the thickness of each of the first region 21 and the second region 22 is preferred from the viewpoint of reducing the compressive residual stress of the light-transmitting conductive layer 20.
[0059] The content ratio of Kr in the first region 21 is preferably 1.0 atomic % or less, more preferably 0.7 atomic % or less, further preferably 0.5 atomic % or less, further preferably 0.3 atomic % or less, further preferably 0.2 atomic % and particularly preferably less than 0.1 atomic % in the entire region of the first region 21 in the thickness direction D. This configuration is suitable for achieving good crystal growth and forming large grains when the amorphous light-transmitting conductive layer is crystallized by heating to form the light-transmitting conductive layer 20 in the manufacturing process of the transparent conductive film X, and therefore is suitable for obtaining a light-transmitting conductive layer 20 with low resistance. In addition, the content ratio of Kr in the first region 21 is, for example, 0.0001 atomic % or more in the entire region of the thickness direction D of the first region 21.
[0060] In addition, the content ratio of Kr in the first region 21 may be different in the thickness direction D of the first region 21. For example, the content ratio of Kr may increase or decrease as it moves away from the transparent substrate 10 in the thickness direction D of the first region 21. Alternatively, the partial region where the content ratio of Kr increases as it moves away from the transparent substrate 10 in the thickness direction D of the first region 21 may be located on the transparent substrate 10 side, and the partial region where the content ratio of Kr decreases as it moves away from the transparent substrate 10 may be located on the side opposite to the transparent substrate 10. Alternatively, the partial region where the content ratio of Kr decreases as it moves away from the transparent substrate 10 in the thickness direction D of the first region 21 may be located on the transparent substrate 10 side, and the partial region where the content ratio of Kr increases as it moves away from the transparent substrate 10 may be located on the side opposite to the transparent substrate 10.
[0061] The thickness of the light-transmitting conductive layer 20 is, for example, greater than 10 nm. The thickness of the light-transmitting conductive layer 20 is preferably greater than 30 nm, more preferably greater than 50 nm, further preferably greater than 80 nm, and particularly preferably greater than 100 nm. This configuration is suitable for achieving low resistance of the light-transmitting conductive layer 20. In addition, the thickness of the light-transmitting conductive layer 20 is, for example, less than 1000 nm, preferably less than 300 nm, more preferably less than 250 nm, further preferably less than 200 nm, further preferably less than 160 nm, particularly preferably less than 150 nm, and most preferably less than 148 nm. This configuration is suitable for reducing the compressive residual stress of the light-transmitting conductive layer 20 and suppressing the warping of the transparent conductive film X.
[0062] The surface resistance of the light-transmitting conductive layer 20 is, for example, 200Ω / □ or less, preferably 100Ω / □ or less, more preferably 50Ω / □ or less, further preferably 20Ω / □ or less, further preferably 15Ω / □ or less, and particularly preferably 13Ω / □ or less. The surface resistance of the light-transmitting conductive layer 20 is, for example, 1Ω / □ or more. These structures related to the surface resistance are suitable for ensuring the low resistance required for the light-transmitting conductive layer 20 when a transparent conductive film X is provided in a touch sensor device, a dimming element, a photoelectric conversion element, a hot wire control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, an image display device, etc. The surface resistance can be measured by a four-terminal method based on JIS K7194.
[0063] The resistivity of the light-transmitting conductive layer 20 is preferably 2.2×10 -4 Ω·cm or less, more preferably 2×10 -4 Ω·cm or less, more preferably 1.9×10 -4 Ω·cm or less, particularly preferably 1.8×10 -4The resistivity of the light-transmitting conductive layer 20 is preferably 0.1×10 -4 Ω·cm or more, more preferably 0.5×10 -4 Ω·cm or more, more preferably 1.0×10 -4 Ω·cm or more, more preferably 1.01×10 -4 Ω·cm or more. These structures related to resistivity are suitable for ensuring the low resistivity required for the translucent conductive layer 20 when a transparent conductive film X is provided in a contact sensor device, a dimming element, a photoelectric conversion element, a hot wire control component, an antenna component, a heater component, an electromagnetic wave shielding component, a lighting device, and an image display device. The resistivity is calculated by multiplying the surface resistance by the thickness. The resistivity can be controlled by, for example, adjusting the content ratio of Kr in the translucent conductive layer 20 and adjusting various conditions when sputtering the translucent conductive layer 20. As such conditions, for example, the temperature of the substrate (the transparent substrate 10 in this embodiment) on which the translucent conductive layer 20 is formed, the amount of oxygen introduced into the film forming chamber, the air pressure in the film forming chamber, and the horizontal magnetic field strength on the target can be listed.
[0064] The total light transmittance (JIS K 7375-2008) of the light-transmitting conductive layer 20 is preferably 60% or more, more preferably 80% or more, and further preferably 85% or more. This configuration is suitable for ensuring the transparency of the light-transmitting conductive layer 20. In addition, the total light transmittance of the light-transmitting conductive layer 20 is, for example, 100% or less.
[0065] The light-transmitting conductive layer 20 has a compressive residual stress of less than 490 MPa in its in-plane direction (orthogonal to the thickness direction D). That is, the compressive residual stress in at least one direction in the plane of the light-transmitting conductive layer 20 is less than 490 MPa. The compressive residual stress is preferably less than 480 MPa, more preferably less than 450 MPa, further preferably less than 400 MPa, and further preferably less than 300 MPa. The compressive residual stress is, for example, more than 1 MPa. The above-mentioned one direction in which the compressive residual stress in the plane of the light-transmitting conductive layer 20 is less than 490 MPa refers to, for example, the TD direction (orthogonal to the MD direction) of the transparent substrate 10 and / or the transparent resin film 11. The compressive residual stress of the light-transmitting conductive layer 20 can be obtained by the method described later for the embodiments.
[0066] The grain diameter of the light-transmitting conductive layer 20 is preferably 40 nm or more, more preferably 50 nm or more, further preferably 90 nm or more, further preferably 120 nm or more, and particularly preferably 150 nm or more. This structure is suitable for reducing the compressive residual stress in the light-transmitting conductive layer 20, and therefore, is suitable for suppressing the warping of the transparent conductive film X. The grain diameter of the light-transmitting conductive layer 20 is preferably 1000 nm or less, more preferably 500 nm or less, further preferably 300 nm or less, further preferably 250 nm or less, and particularly preferably 200 nm or less. This structure is suitable for suppressing the generation of cracks in the light-transmitting conductive layer 20 due to the bending (bending, warping) of the transparent conductive film X. The grain diameter of the light-transmitting conductive layer 20 refers to: the average value of the equivalent circle diameter obtained by the method described later for the examples.
[0067] The average number of grain boundaries in the in-plane direction of the light-transmitting conductive layer 20 is preferably less than 12 / μm, more preferably less than 11 / μm, further preferably less than 10 / μm, and particularly preferably less than 9 / μm. This structure is suitable for reducing the compressive residual stress in the light-transmitting conductive layer 20, and therefore, is suitable for suppressing the warping of the transparent conductive film X. The average number of grain boundaries in the in-plane direction of the light-transmitting conductive layer 20 is preferably more than 2 / μm, more preferably more than 3 / μm, further preferably more than 4 / μm, and particularly preferably more than 5 / μm. This structure is suitable for suppressing the generation of cracks in the light-transmitting conductive layer 20 due to the bending (bending, warping) of the transparent conductive film X. The average number of grain boundaries in the light-transmitting conductive layer 20 refers to: the average number of grain boundaries obtained by the method described later for the examples.
[0068] For example, the following operation can be performed to determine whether the light-transmitting conductive layer is crystalline. First, the light-transmitting conductive layer (the light-transmitting conductive layer 20 on the transparent substrate 10 in the transparent conductive film X) is immersed in hydrochloric acid with a concentration of 5% by mass at 20°C for 15 minutes. Then, the light-transmitting conductive layer is washed with water and then dried. Next, in the exposed plane of the light-transmitting conductive layer (the surface of the light-transmitting conductive layer 20 on the opposite side of the transparent substrate 10 in the transparent conductive film X), the resistance between a pair of terminals with a spacing of 15 mm (terminal resistance) is measured. In this measurement, when the terminal resistance is less than 10 kΩ, the light-transmitting conductive layer is crystalline. In addition, by using a transmission electron microscope to observe the presence of grains in the light-transmitting conductive layer from above, it is also possible to determine that the light-transmitting conductive layer is crystalline. The preparation method and specific observation method of the observation sample for this purpose are the same as the preparation method and specific observation method of the observation sample described below for the method of deriving the grain diameter of the light-transmitting conductive layer in the embodiments described later.
[0069] The transparent conductive film X is produced, for example, as follows.
[0070] First, if Figure 3 As shown in A in FIG. 1 , a transparent resin film 11 is prepared.
[0071] Then, if Figure 3 As shown in FIG. 1B , the functional layer 12 is formed on one surface of the transparent resin film 11 in the thickness direction D. By forming the functional layer 12 on the transparent resin film 11 , the transparent substrate 10 is manufactured.
[0072] The functional layer 12 as a hard coat layer can be formed by applying a curable resin composition on the transparent resin film 11 to form a coating film, and then curing the coating film. When the curable resin composition contains an ultraviolet curable resin, the coating film is cured by ultraviolet irradiation. When the curable resin composition contains a thermosetting resin, the coating film is cured by heating.
[0073] The exposed surface of the functional layer 12 formed on the transparent resin film 11 is subjected to surface modification treatment as needed. When plasma treatment is performed as the surface modification treatment, argon gas, for example, is used as an inert gas. In addition, the discharge power in the plasma treatment is, for example, 10 W or more, and, for example, 5000 W or less.
[0074] Then, if Figure 3 As shown in FIG. 3C , an amorphous light-transmitting conductive layer 20′ is formed on the transparent substrate 10 (film forming step). Specifically, a material is formed on the functional layer 12 in the transparent substrate 10 by sputtering to form an amorphous light-transmitting conductive layer 20′. The light-transmitting conductive layer 20′ is an amorphous film having both light transmittance and conductivity (the light-transmitting conductive layer 20′ is converted into a crystalline light-transmitting conductive layer 20 by heating in a crystallization step described later).
[0075] In the sputtering method, it is preferred to use a sputtering film forming device that can implement a film forming process using a roll-to-roll method. In the manufacture of the transparent conductive film X, when a roll-to-roll method sputtering film forming device is used, a strip-shaped transparent substrate 10 is moved from a take-out roller provided in the device to a take-up roller, and a material is formed on the transparent substrate 10 to form a translucent conductive layer 20'. In addition, in the sputtering method, a sputtering film forming device having one film forming chamber can be used, or a sputtering film forming device having a plurality of film forming chambers sequentially arranged along the travel path of the transparent substrate 10 can be used (in the case of forming the translucent conductive layer 20' including the first region 21 and the second region 22, a sputtering film forming device having a plurality of film forming chambers of two or more is used).
[0076] In the sputtering method, specifically, a sputtering gas (inert gas) is introduced into a film forming chamber of a sputtering film forming device under vacuum conditions, and a negative voltage is applied to a target disposed on a cathode in the film forming chamber. This generates a glow discharge to ionize gas atoms, and the gas ions collide with the target surface at high speed, ejecting target materials from the target surface, and depositing the ejected target materials on the functional layer 12 in the transparent substrate 10.
[0077] As the material of the target disposed on the cathode in the film forming chamber, the conductive oxide described above for the light-transmitting conductive layer 20 is used, preferably a conductive oxide containing indium is used, and ITO is more preferably used. When ITO is used, the ratio of the content of tin oxide in the ITO to the total content of tin oxide and indium oxide is preferably 0.1% by mass or more, more preferably 1% by mass or more, further preferably 3% by mass or more, further preferably 5% by mass or more, particularly preferably 7% by mass or more, and preferably 15% by mass or less, more preferably 13% by mass or less, and further preferably 12% by mass or less.
[0078] The sputtering method is preferably a reactive sputtering method. In the reactive sputtering method, a reactive gas is introduced into the film forming chamber in addition to the sputtering gas.
[0079] In the case where a light-transmitting conductive layer 20' containing Kr is formed in the entire area in the thickness direction D (the first case), the gas introduced into one or more film forming chambers of the sputtering film forming apparatus contains Kr as a sputtering gas and oxygen as a reactive gas. The sputtering gas may contain an inert gas other than Kr. As the inert gas other than Kr, for example, rare gas atoms other than Kr can be listed. As the rare gas atoms, for example, Ar and Xe can be listed. When the sputtering gas contains an inert gas other than Kr, the content ratio thereof is preferably less than 80% by volume, and more preferably less than 50% by volume.
[0080] In the case of forming the light-transmitting conductive layer 20' including the first region 21 and the second region 22 (the second case), the gas introduced into the film forming chamber for forming the first region 21 contains Kr as a sputtering gas and oxygen as a reactive gas. The sputtering gas may contain an inert gas other than Kr. The type and content ratio of the inert gas other than Kr are the same as those described above for the inert gas other than Kr in the first case.
[0081] In the second case, the gas introduced into the film forming chamber for forming the second region 22 contains an inert gas other than Kr as a sputtering gas and oxygen as a reactive gas. As the inert gas other than Kr, the inert gas described above as the inert gas other than Kr in the first case can be cited, and Ar is preferably used.
[0082] In the reactive sputtering method, the ratio of the amount of oxygen introduced into the film forming chamber to the total amount of the sputtering gas and oxygen introduced is, for example, 0.01 flow % or more and, for example, 15 flow % or less.
[0083] The gas pressure in the film forming chamber in film forming by sputtering (sputtering film forming) is, for example, 0.02 Pa or more, and, for example, 1 Pa or less.
[0084] The temperature of the transparent substrate 10 during sputtering is, for example, 100° C. or less. In order to suppress the thermal expansion of the transparent substrate 10 during sputtering, the transparent substrate 10 is preferably cooled. Suppressing the thermal expansion of the transparent substrate 10 during sputtering helps to obtain a translucent conductive layer 20 (crystalline translucent conductive layer) in which the compressive residual stress is suppressed. From this viewpoint, the temperature of the transparent substrate 10 during sputtering is preferably 20° C. or less, more preferably 10° C. or less, further preferably 5° C. or less, particularly preferably 0° C. or less, and, for example, is -50° C. or more, preferably -20° C. or more, more preferably -10° C. or more, further preferably -7° C. or more.
[0085] As a power source for applying a voltage to the target, for example, a DC power source, an AC power source, an MF power source, and an RF power source can be listed. As a power source, a DC power source and an RF power source can also be used in combination. The absolute value of the discharge voltage in the sputtering film formation is, for example, 50V or more, and, for example, 500V or less. The horizontal magnetic field intensity on the target surface is, for example, 10mT or more, preferably 60mT or more, and, for example, 300mT or less. This structure is preferred for suppressing the krypton atoms in the translucent conductive layer 20 from becoming excessive, and therefore, it is preferred for suppressing the warping of the formed translucent conductive layer 20 and the transparent conductive film X.
[0086] In the present manufacturing method, Figure 3As shown in D, the translucent conductive layer 20 is converted from amorphous to crystalline (crystallized) by heating (crystallization process). As heating means, for example, infrared heaters and ovens (heat medium heating ovens, hot air heating ovens) can be listed. The environment during heating can be any of a vacuum environment and an atmospheric environment. Heating is preferably carried out in the presence of oxygen. From the viewpoint of ensuring a high crystallization rate, the heating temperature is, for example, above 100°C, preferably above 120°C. From the viewpoint of suppressing the influence of heating on the transparent substrate 10, the heating temperature is, for example, below 200°C, preferably below 180°C, more preferably below 170°C, and further preferably below 165°C. The heating time is, for example, less than 10 hours, preferably less than 200 minutes, more preferably less than 90 minutes, and further preferably less than 60 minutes, and, for example, more than 1 minute, preferably more than 5 minutes.
[0087] After returning to room temperature after heating in this process, the transparent substrate 10 shrinks. The structure in which the light-transmitting conductive layer 20 contains Kr is suitable for appropriately shrinking the light-transmitting conductive layer 20 on the shrunk transparent substrate 10 in this state after returning to room temperature (the preferred content ratio of Kr in the light-transmitting conductive layer 20 is as described above). The shrinkage of the light-transmitting conductive layer 20 after returning to room temperature helps to reduce the compressive residual stress of the light-transmitting conductive layer 20.
[0088] As described above, a transparent conductive film X is manufactured.
[0089] like Figure 4 As schematically shown in FIG. 1 , the light-transmitting conductive layer 20 in the transparent conductive film X can be patterned. The light-transmitting conductive layer 20 can be patterned by etching the light-transmitting conductive layer 20 through a predetermined etching mask. The patterning of the light-transmitting conductive layer 20 can be performed before or after the above-mentioned crystallization step. The patterned light-transmitting conductive layer 20 functions as, for example, a wiring pattern.
[0090] The light-transmitting conductive layer 20 on the transparent substrate 10 in the transparent conductive film X contains krypton and has a compressive residual stress of less than 490 MPa in the in-plane direction, and the compressive residual stress is preferably 480 MPa or less, more preferably 450 MPa or less, further preferably less than 400 MPa, and further preferably 300 MPa or less. This configuration is suitable for achieving low resistance of the light-transmitting conductive layer 20 and suppressing warping of the transparent conductive film X. Specifically, as shown in the examples and comparative examples described below.
[0091] In the transparent conductive film X, the functional layer 12 may be an adhesion improving layer for achieving high adhesion of the light-transmitting conductive layer 20 to the transparent substrate 10. The configuration in which the functional layer 12 is an adhesion improving layer is suitable for ensuring adhesion between the transparent substrate 10 and the light-transmitting conductive layer 20.
[0092] The functional layer 12 may be an index-matching layer for adjusting the reflectivity of the surface (one surface in the thickness direction D) of the transparent substrate 10. The configuration of the functional layer 12 as the index-matching layer is suitable for making it difficult to observe the pattern shape of the light-transmitting conductive layer 20 when the light-transmitting conductive layer 20 on the transparent substrate 10 is patterned.
[0093] The functional layer 12 may be a peeling functional layer for practically peeling the light-transmitting conductive layer 20 from the transparent substrate 10. The configuration in which the functional layer 12 is a peeling functional layer is suitable for peeling the light-transmitting conductive layer 20 from the transparent substrate 10 and transferring the light-transmitting conductive layer 20 to another member.
[0094] The functional layer 12 can be a composite layer in which multiple layers are arranged in the thickness direction D. The composite layer preferably includes two or more layers selected from the group consisting of a hard coating layer, a adhesion improving layer, a refractive index adjusting layer and a peeling functional layer. This structure is suitable for making the functional layer 12 compositely express the above-mentioned functions of each selected layer. In a preferred embodiment, the functional layer 12 has a adhesion improving layer, a hard coating layer and a refractive index adjusting layer in sequence on one side of the transparent resin film 11 facing the thickness direction D. In other preferred embodiments, the functional layer 12 has a peeling functional layer, a hard coating layer and a refractive index adjusting layer in sequence on one side of the transparent resin film 11 facing the thickness direction D.
[0095] The transparent conductive film X is bonded to an article and is used in a state where the light-transmitting conductive layer 20 is patterned as necessary. The transparent conductive film X is bonded to an article via, for example, an anchoring functional layer.
[0096] Examples of the article include elements, components and devices. Specifically, examples of the article with a transparent conductive film include elements with a transparent conductive film, components with a transparent conductive film and devices with a transparent conductive film.
[0097] As the element, for example, a dimming element and a photoelectric conversion element can be listed. As the dimming element, for example, a current-driven dimming element and an electric field-driven dimming element can be listed. As the current-driven dimming element, for example, an electrochromic (EC) dimming element can be listed. As the electric field-driven dimming element, for example, a PDLC (polymer dispersed liquid crystal) dimming element, a PNLC (polymer network liquid crystal) dimming element and an SPD (suspended particle device) dimming element can be listed. As the photoelectric conversion element, for example, a solar cell can be listed. As the solar cell, for example, an organic thin-film solar cell and a dye-sensitized solar cell can be listed. As the component, for example, an electromagnetic wave shielding component, a hot wire control component, a heater component and an antenna component can be listed. As the device, for example, a contact sensor device, a lighting device and an image display device can be listed.
[0098] As the above-mentioned fixing function layer, for example, an adhesive layer and a bonding layer can be listed. As the material of the fixing function layer, as long as it is a material with transparency and exerting the fixing function, it can be used without particular limitation. The fixing function layer is preferably formed by a resin. As the resin, for example, acrylic resins, silicone resins, polyester resins, polyurethane resins, polyamide resins, polyvinyl ether resins, vinyl acetate / vinyl chloride copolymers, modified polyolefin resins, epoxy resins, fluororesins, natural rubber and synthetic rubber can be listed. From the aspects of showing cohesion, adhesion, appropriate wettability and other adhesive properties, excellent transparency, and excellent weather resistance and heat resistance, as the above-mentioned resin, an acrylic resin is preferably used.
[0099] In order to suppress the corrosion of the translucent conductive layer 20, an antiseptic may be mixed into the fixing functional layer (the resin forming the fixing functional layer). In order to suppress the migration of the translucent conductive layer 20, an anti-migration agent (such as the material disclosed in Japanese Patent Laid-Open No. 2015-022397) may be mixed into the fixing functional layer (the resin forming the fixing functional layer). In addition, in order to suppress the degradation of the article when it is used outdoors, an ultraviolet absorber may be mixed into the fixing functional layer (the resin forming the fixing functional layer). Examples of ultraviolet absorbers include benzophenone compounds, benzotriazole compounds, salicylic acid compounds, oxalic acid anilide compounds, cyanoacrylate compounds, and triazine compounds.
[0100] In addition, when the transparent substrate 10 of the transparent conductive film X is fixed to the article by means of the fixing functional layer, the translucent conductive layer 20 (including the patterned translucent conductive layer 20) is exposed in the transparent conductive film X. In this case, a covering layer can be configured on the exposed surface of the translucent conductive layer 20. The covering layer is a layer covering the translucent conductive layer 20, which can improve the reliability of the translucent conductive layer 20 and inhibit the functional degradation caused by damage to the translucent conductive layer 20. Such a covering layer is preferably formed of a dielectric material, and more preferably formed of a composite material of a resin and an inorganic material. As a resin, for example, the resin described above for the fixing functional layer can be listed. As an inorganic material, for example, inorganic oxides and fluorides can be listed. As an inorganic oxide, for example, silicon oxide, titanium oxide, niobium oxide, aluminum oxide, zirconium dioxide and calcium oxide can be listed. As a fluoride, for example, magnesium fluoride can be listed. In addition, the above-mentioned preservative, anti-migration agent and ultraviolet absorber can be mixed into the covering layer (a mixture of resin and inorganic material).
[0101] The article with a transparent conductive film has a transparent conductive film X that is suitable for reducing the resistance of the light-transmitting conductive layer 20, and is therefore suitable for achieving high performance of a function that is dependent on the light transmittance and conductivity of the light-transmitting conductive layer 20. In addition, the article with a transparent conductive film has a transparent conductive film X that is suitable for suppressing warping, and is therefore suitable for appropriately mounting the transparent conductive film X with good positional accuracy during the manufacturing process, for example.
[0102] Example
[0103] The present invention is specifically described below with reference to the following embodiments. The present invention is not limited to the embodiments. In addition, the specific numerical values of the compounding amount (content), physical property values, parameters, etc. described below can be replaced with the upper limit (numerical value defined in the form of "below" or "less than") or lower limit (numerical value defined in the form of "above" or "exceeding") of the compounding amount (content), physical property values, parameters, etc. corresponding to them described in the above-mentioned "Specific Implementation Methods".
[0104] [Example 1]
[0105] As a transparent substrate, a long strip of PET film with a hard coating on both sides (product name "KB film CANIA", thickness 54 μm, manufactured by KIMOTO Corporation) was prepared (for this transparent substrate, the thermal shrinkage rate of the transparent substrate in the direction of maximum shrinkage after heating at 165°C for 1 hour (maximum thermal shrinkage rate, recorded as thermal shrinkage rate in MD direction in this embodiment) was 0.65%).
[0106] Next, a 130 nm thick amorphous light-transmitting conductive layer was formed on the hard coating layer in the transparent substrate by reactive sputtering (film forming process). In the reactive sputtering, a sputtering film forming device (DC magnetron sputtering device) capable of implementing the film forming process by a roll-to-roll method was used. The conditions for the sputtering film forming in this embodiment are as follows.
[0107] As a target, a sintered body of indium oxide and tin oxide (tin oxide concentration of 10 mass%) was used. As a power source for applying voltage to the target, a DC power source was used. The horizontal magnetic field intensity on the target was set to 90 mT. The film forming temperature (the temperature of the transparent substrate to be laminated with the translucent conductive layer) was set to -5°C. In addition, the film forming chamber was evacuated until the vacuum degree in the film forming chamber of the device reached 0.8×10 -4 After 0.5 Pa, Kr as a sputtering gas and oxygen as a reactive gas were introduced into the film forming chamber, and the gas pressure in the film forming chamber was set to 0.2 Pa. The ratio of the amount of oxygen introduced into the film forming chamber to the total amount of Kr and oxygen introduced was about 2.5% by flow rate. Figure 5 As shown in FIG. 1 , the oxygen introduction amount is within the region R of the resistivity-oxygen introduction amount curve and the resistivity value of the formed film is 6.5×10 -4 The value can be adjusted in Ω·cm manner. Figure 5 The resistivity-oxygen introduction amount curve shown in can be prepared by previously investigating the oxygen introduction amount dependency of the resistivity of the light-transmitting conductive layer when the light-transmitting conductive layer is formed by reactive sputtering under the same conditions as above except for the oxygen introduction amount.
[0108] Next, the light-transmitting conductive layer on the transparent substrate was crystallized by heating in a hot air oven (crystallization step). In this step, the heating temperature was 165° C. and the heating time was 1 hour.
[0109] As described above, a transparent conductive film of Example 1 was prepared. The light-transmitting conductive layer (thickness 130 nm, crystalline) of the transparent conductive film of Example 1 was formed of a single ITO layer containing Kr.
[0110] [Example 2]
[0111] The transparent conductive film of Example 2 was produced in the same manner as the transparent conductive film of Example 1 except that some film forming conditions in the film forming process were changed and the heating conditions in the crystallization process were changed. In the film forming process of this example, the pressure in the film forming chamber was set to 0.6 Pa, the thickness of the formed light-transmitting conductive layer was set to 34 nm, and the resistivity of the light-transmitting conductive layer was set to 5.7×10 -4 In the crystallization step of this example, the heating temperature was set to 140° C. and the heating time was set to 5 hours.
[0112] The light-transmitting conductive layer (34 nm thick, crystalline) of the transparent conductive film of Example 2 was formed of a single ITO layer containing Kr.
[0113] [Example 3]
[0114] In the film forming process, a first sputtering film forming a first area (thickness 50nm) of the translucent conductive layer is formed on the transparent substrate, and a second sputtering film forming a second area (thickness 80nm) of the translucent conductive layer is formed on the first area is performed in sequence. Except for this, the transparent conductive film of Example 3 is prepared in the same manner as the transparent conductive film of Example 1.
[0115] The conditions for the first sputtering film formation in this embodiment are as follows. As a target, a sintered body of indium oxide and tin oxide (tin oxide concentration is 10 mass%) is used. As a power source for applying voltage to the target, a DC power source is used. The horizontal magnetic field intensity on the target is set to 90 mT. The film forming temperature is set to -5°C. In addition, the first film forming chamber is evacuated until the vacuum degree in the first film forming chamber of the device reaches 0.8×10 -4 After the first film forming chamber was heated to 1.5 0.5 Pa, Kr as a sputtering gas and oxygen as a reactive gas were introduced into the first film forming chamber, and the pressure in the film forming chamber was set to 0.2 Pa. The amount of oxygen introduced into the film forming chamber was such that the resistivity of the formed film became 6.5×10 -4 The value can be adjusted in Ω·cm manner.
[0116] The conditions for the second sputtering film formation in this embodiment are as follows. The second film forming chamber is evacuated until the ultimate vacuum degree in the second film forming chamber of the apparatus reaches 0.8×10 -4 After 0.4 Pa, Ar as a sputtering gas and oxygen as a reactive gas were introduced into the second film forming chamber to set the pressure in the film forming chamber to 0.4 Pa. In this embodiment, the other conditions of the second sputtering film forming were the same as those of the first sputtering film forming.
[0117] As described above, a transparent conductive film of Example 3 was prepared. The light-transmitting conductive layer (thickness 130 nm, crystalline) of the transparent conductive film of Example 3 had, in order from the transparent substrate side, a first region (thickness 50 nm) formed by an ITO layer containing Kr and a second region (thickness 80 nm) formed by an ITO layer containing Ar.
[0118] [Examples 4 and 5]
[0119] For the light-transmitting conductive layer formed in the film-forming process, the thickness of the first region is set from 50nm to 66nm (Example 4) or 85nm (Example 5), and the thickness of the second region is set from 80nm to 64nm (Example 4) or 45nm (Example 5). Apart from this, the same operation as the transparent conductive film of Example 3 is performed to produce the transparent conductive films of Examples 4 and 5.
[0120] The light-transmitting conductive layer (thickness 130 nm, crystalline) of the transparent conductive film of Example 4 has, in order from the transparent substrate side, a first region (thickness 66 nm) formed of an ITO layer containing Kr and a second region (thickness 64 nm) formed of an ITO layer containing Ar. The light-transmitting conductive layer (thickness 130 nm) of the transparent conductive film of Example 5 has, in order from the transparent substrate side, a first region (thickness 85 nm) formed of an ITO layer containing Kr and a second region (thickness 45 nm) formed of an ITO layer containing Ar.
[0121] [Example 6]
[0122] The transparent conductive film of Example 6 was produced in the same manner as the transparent conductive film of Example 1 except for the following matters in the sputtering film formation. A mixed gas of krypton and argon (Kr is 90 volume % and Ar is 10 volume %) was used as the sputtering gas. The ratio of the amount of oxygen introduced into the film forming chamber to the total amount of the mixed gas and oxygen introduced was set to about 2.7% by flow rate. The oxygen introduction amount was set so that the resistivity of the formed film would be 5.7×10 -4 The thickness of the formed light-transmitting conductive layer was set to 140 nm.
[0123] The light-transmitting conductive layer (thickness: 140 nm, crystalline) of the transparent conductive film of Example 6 is formed of a single ITO layer containing Kr and Ar.
[0124] [Comparative Example 1]
[0125] In the film forming step, the transparent conductive film of Comparative Example 1 was produced in the same manner as the transparent conductive film of Example 1, except that Ar was used as the sputtering gas instead of Kr and the film forming pressure was set to 0.4 Pa instead of 0.2 Pa. The light-transmitting conductive layer (thickness 130 nm, crystalline) of the transparent conductive film of Comparative Example 1 was formed of a single ITO layer containing Ar.
[0126] [Comparative Example 2]
[0127] In the film forming step, Ar was used instead of Kr as the sputtering gas, and the film forming pressure was set to 0.4 Pa instead of 0.2 Pa, and in the crystallization step, the heating temperature was set to 155° C. instead of 165° C., and the transparent conductive film of Comparative Example 2 was produced in the same manner as in Example 1. The light-transmitting conductive layer (thickness 130 nm, crystalline) of the transparent conductive film of Comparative Example 2 was formed of a single ITO layer containing Ar.
[0128] [Comparative Example 3]
[0129] In the film forming step, the transparent conductive film of Comparative Example 3 was produced in the same manner as the transparent conductive film of Example 3, except that the first sputtering film forming was performed in sequence to form the second region (thickness 75 nm) of the light-transmitting conductive layer on the transparent substrate and the second sputtering film forming was performed to form the first region (thickness 45 nm) of the light-transmitting conductive layer on the second region. The conditions for the first sputtering film forming in this comparative example were the same as the conditions for the second sputtering film forming in Example 3. The conditions for the second sputtering film forming in this comparative example were the same as the conditions for the first sputtering film forming in Example 3.
[0130] The light-transmitting conductive layer (thickness 120 nm, crystalline) of the transparent conductive film of Comparative Example 3 has, in order from the transparent substrate side, a second region (thickness 75 nm) formed by an ITO layer containing Ar and a first region (thickness 45 nm) formed by an ITO layer containing Kr.
[0131] <Thickness of light-transmitting conductive layer>
[0132] The thickness of the light-transmitting conductive layer of each transparent conductive film in Examples 1 to 6 and Comparative Examples 1 to 3 was measured by FE-TEM observation. Specifically, first, the FIB microsampling method was used to prepare samples for cross-sectional observation of each light-transmitting conductive layer in Examples 1 to 6 and Comparative Examples 1 to 3. In the FIB microsampling method, a FIB device (trade name "FB2200", manufactured by Hitachi) was used, and the acceleration voltage was set to 10 kV. Next, the thickness of the light-transmitting conductive layer in the sample for cross-sectional observation was measured by FE-TEM observation. In the FE-TEM observation, a FE-TEM device (trade name "JEM-2800", manufactured by JEOL) was used, and the acceleration voltage was set to 200 kV.
[0133] The thickness of the first region of each translucent conductive layer in Examples 3 to 5 was measured by preparing a cross-sectional observation sample from an intermediate product before forming the second region on the first region and performing FE-TEM observation of the sample. The thickness of the second region of each translucent conductive layer in Examples 3 to 5 was obtained by subtracting the thickness of the first region from the total thickness of each translucent conductive layer in Examples 3 to 5. The ratio of the first region in the thickness direction of the translucent conductive layer was 38.5% in Example 3, 50.8% in Example 4, and 65.4% in Example 5.
[0134] The thickness of the second region of the light-transmitting conductive layer in Comparative Example 3 was measured by preparing a cross-sectional observation sample from an intermediate product before forming the first region on the second region and performing FE-TEM observation of the sample. The thickness of the first region of the light-transmitting conductive layer in Comparative Example 3 was obtained by subtracting the thickness of the second region from the total thickness of the light-transmitting conductive layer in Comparative Example 3. The ratio of the first region in the thickness direction of the light-transmitting conductive layer in Comparative Example 3 was 37.5%.
[0135] 〈Resistivity〉
[0136] The resistivity of the light-transmitting conductive layer was studied for each transparent conductive film of Examples 1 to 6 and Comparative Examples 1 to 3. Specifically, the surface resistance of the light-transmitting conductive layer of the transparent conductive film was measured using a four-terminal method based on JIS K 7194 (1994), and the resistivity (Ω·cm) was calculated by multiplying the surface resistance value by the thickness of the light-transmitting conductive layer. The results are shown in Table 1.
[0137] 〈Warp Amount of Transparent Conductive Film〉
[0138] For each transparent conductive film of Examples 1 to 6 and Comparative Examples 1 to 3, the degree of warping was studied as follows. First, three rectangular samples (10 cm × 10 cm) were cut out from each transparent conductive film. Next, each sample was placed on the loading surface (approximately horizontal surface) of the loading table, and then the distance between each vertex located at the four corners of the sample and the loading surface was measured. Specifically, when the sample is placed on the loading surface in such a way that the transparent substrate side of the sample contacts the loading surface, the distance (mm) in the vertical direction between the vertex deviating from the loading surface and the loading surface is measured as a positive value. In addition, when the sample is placed on the loading surface in such a way that the translucent conductive layer side of the sample contacts the loading surface, the distance (mm) in the vertical direction between the vertex deviating from the loading surface and the loading surface is measured as a negative value. The distance between the vertex that does not deviate from the loading surface and the loading surface is 0 mm. Next, the absolute value of the average value of the measured distances measured for a total of 12 vertices of each transparent conductive film is calculated as the average warping amount (mm). The value is shown in Table 1. In each of the transparent conductive films of Comparative Examples 1 and 2, the measurement samples were bent into a cylindrical shape (a shape in which the light-transmitting conductive layer was located outside and the transparent substrate was located inside), and the amount of warping could not be measured.
[0139] 〈Quantitative Analysis of Rare Gas Atoms in Translucent Conductive Layer〉
[0140] The content of Kr and Ar atoms contained in the translucent conductive layer of each transparent conductive film of Examples 1 to 6 and Comparative Examples 1 to 3 was analyzed by Rutherford backscattering spectroscopy (RBS). The element ratios of the five elements In+Sn (in Rutherford backscattering spectroscopy, it is difficult to measure In and Sn separately, so the evaluation is performed as the sum of the two elements), O, Ar, and Kr as detection elements were calculated, and the content (atomic %) of Kr atoms and Ar atoms in the translucent conductive layer was calculated. The apparatus used and the measurement conditions are as follows. As analysis results, the Kr content (atomic %), the Ar content (atomic %), and the rare gas atom content (atomic %) are shown in Table 1. Regarding the analysis of the Kr content, in Examples 1 to 6 and Comparative Example 3, no exact measurement value above the detection limit (lower limit) could be obtained (the detection limit may vary depending on the thickness of the translucent conductive layer provided for measurement). Therefore, in Table 1, the Kr content of the translucent conductive layer is shown as being less than the detection limit under the thickness of the layer, and is therefore expressed as "< the specific detection limit under the thickness of the translucent conductive layer to be measured" (the same applies to the expression method of the rare gas atom content).
[0141] <Device used>
[0142] Pelletron 3SDH (manufactured by National Electrostatics Corporation)
[0143] <Measurement Conditions>
[0144] Incident ions: 4 He ++
[0145] Incident energy: 2300keV
[0146] Angle of incidence: 0deg
[0147] Scattering angle: 160deg
[0148] Sample current: 6nA
[0149] Beam diameter: 2mmφ
[0150] In-plane rotation: No
[0151] Irradiation: 75μC
[0152] <Confirmation of Kr atoms in the light-transmitting conductive layer>
[0153] The following operation was used to confirm that each of the light-transmitting conductive layers in Examples 1 to 6 and Comparative Example 3 contained Kr atoms. First, a scanning fluorescent X-ray analyzer (trade name "ZSX Primus IV", manufactured by Rigaku Corporation) was used to repeatedly perform fluorescent X-ray analysis measurements 5 times using the following measurement conditions, and the average value of each scanning angle was calculated to prepare an X-ray spectrum. In addition, in the prepared X-ray spectrum, a peak was confirmed to appear near a scanning angle of 28.2°, thereby confirming that the light-transmitting conductive layer contained Kr atoms.
[0154] <Measurement Conditions>
[0155] Spectrum: Kr-KA
[0156] Measuring diameter: 30mm
[0157] Atmosphere: Vacuum
[0158] Target: Rh
[0159] Tube voltage: 50kV
[0160] Tube current: 60mA
[0161] Primary filter: Ni40
[0162] Scanning angle (deg): 27.0~29.5
[0163] Step (deg): 0.020
[0164] Speed (deg / min): 0.75
[0165] Attenuator: 1 / 1
[0166] Slit: S2
[0167] Spectroscopic crystal: LiF(200)
[0168] Detector: SC
[0169] PHA: 100-300
[0170] <Average crystal grain diameter of light-transmitting conductive layer>
[0171] For each transparent conductive film of Examples 1 to 6 and Comparative Examples 1 to 3, the average grain diameter of the light-transmitting conductive layer (crystalline ITO film) when viewed from above was studied. Specifically, a film sheet cut from a transparent conductive film is first fixed to the sample holder of a slicer. Next, after the tip of the slicer is brought into contact with the film surface of the light-transmitting conductive layer in the film sheet at an extremely acute angle, the light-transmitting conductive layer is cut using the slicer to generate a cutting surface that is roughly parallel to the film surface, thereby obtaining an observation sample. Next, the observation sample is observed using a transmission electron microscope, and the observation sample is photographed from above at a magnification that allows the grains to be clearly identified (a direct magnification of 100,000 times or 200,000 times). Next, arbitrarily select grains within the range of 110 to 250 from the plurality of grains in the captured image. Next, through image analysis processing of the captured images, for each region demarcated by a grain boundary (region within the grain boundary), the area of the region is calculated based on the number of pixels present in the region, the diameter of a circle having the same area as the area is calculated as the grain diameter (equivalent circle diameter), and the average value of the equivalent circle diameters of the selected plurality of grains is calculated. The values are shown in Table 1.
[0172] <Average number of grain boundaries in light-transmitting conductive layer>
[0173] For each transparent conductive film of Examples 1 to 6 and Comparative Examples 1 to 3, the average number of grain boundaries in the translucent conductive layer (crystalline ITO film) was studied. Specifically, the above-mentioned image obtained for each transparent conductive film was first printed on paper in order to study the grain diameter. Then, on the printed image, 5 line segments with an actual size equivalent to 1.0 μm were drawn at any position. Then, the grain boundaries existing in each line segment were counted, and the average value of the number of grain boundaries in the 5 line segments was calculated as the average number of grain boundaries (pieces / μm). The values are shown in Table 1.
[0174] 〈Compressive residual stress of light-transmitting conductive layer〉
[0175] The compressive residual stress of the light-transmitting conductive layer (crystalline ITO film) of each transparent conductive thin film of Examples 1 to 6 and Comparative Examples 1 to 3 was indirectly determined based on the lattice strain of the light-transmitting conductive layer.
[0176] First, a rectangular measurement sample (50 mm × 50 mm) is cut out from a transparent conductive film. Next, a powder X-ray diffraction apparatus (trade name "SmartLab", manufactured by Rigaku Corporation) is used to measure the diffraction intensity of the measurement sample every 0.02° in the range of the measurement scattering angle 2θ = 60 to 61.6° (0.15° / minute). Next, based on the peak angle 2θ of the obtained diffraction image (the peak of the (622) surface of ITO) and the wavelength λ of the X-ray source, the lattice spacing d of the translucent conductive layer in the measurement sample is calculated, and the lattice strain ε is calculated based on d. The following formula (1) is used in the calculation of d, and the following formula (2) is used in the calculation of ε.
[0177] 2d sinθ=λ …(1)
[0178] ε=(d-d0) / d0 …(2)
[0179] In equations (1) and (2), λ is the wavelength of the X-ray source (Cu Kα ray) (= 0.15418 nm), and d0 is the lattice plane spacing of ITO in a stress-free state (= 0.1518967 nm). The above-mentioned X-ray diffraction measurement is carried out for the cases where the angle Ψ formed by the normal line of the film surface and the normal line of the ITO crystal surface is 65°, 70°, 75° and 85°, and the lattice strain ε at each Ψ is calculated. The angle Ψ formed by the normal line of the film surface and the normal line of the ITO crystal surface is adjusted by rotating the sample with the MD direction (direction orthogonal to the TD direction) of the transparent substrate in the measurement sample (part of the transparent conductive film) as the center of the rotation axis. The residual stress σ in the in-plane direction of the ITO film is adjusted according to the Sin 2 The slope of the straight line obtained by plotting the relationship between Ψ and lattice distortion ε was determined by the following formula (3). The residual stress σ in the TD direction determined in this way was given as compressive residual stress (MPa) and is shown in Table 1.
[0180]
[0181] In the formula (3), E is the Young's modulus of ITO (=115 GPa), and ν is the Poisson's ratio of ITO (=0.35).
[0182] [Table 1]
[0183]
[0184] Industrial Applicability
[0185] The transparent conductive film of the present invention can be used as a supply material for a conductor film for patterning a transparent electrode in various devices such as a liquid crystal display, a touch panel, and a photosensor.
Claims
1. A transparent conductive film comprising a transparent substrate and a light-transmitting conductive layer in this order along a thickness direction, The transparent substrate comprises a flexible transparent resin film. The light-transmitting conductive layer includes a region containing 0.0001 atomic % or more and less than 0.1 atomic % of krypton in the thickness direction. The light-transmitting conductive layer has a compressive residual stress of less than 490 MPa in an in-plane direction perpendicular to the thickness direction.
2. The transparent conductive film according to claim 1, wherein The average number of grain boundaries in the in-plane direction of the light-transmitting conductive layer is less than 12 / μm.
3. The transparent conductive film according to claim 1 or 2, wherein: The light-transmitting conductive layer contains a conductive oxide containing indium.
4. The transparent conductive film according to any one of claims 1 to 3, wherein The light-transmitting conductive layer does not contain xenon.
5. The transparent conductive film according to any one of claims 1 to 4, wherein The light-transmitting conductive layer has a 2.2×10 -4 Resistivity below Ω·cm.
6. The transparent conductive film according to any one of claims 1 to 5, wherein The light-transmitting conductive layer has a thickness of 30 nm or more.