A silicon-based semiconductor field effect transistor with ultra-low contact resistance and a method for preparing the same

Through the combination of pulsed laser melting and flash annealing, the problem of high contact resistance in traditional silicon-based CMOS technology is solved, and the performance and stability of semiconductor devices are significantly improved, and the ultra-low contact resistance of silicon-based semiconductor field effect transistors is realized. preparation.

CN118782466BInactive Publication Date: 2024-11-15SICHUAN NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411252038.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional silicon-based CMOS technology has weak performance improvement due to high contact resistance in integrated circuits, especially after the device size is reduced, the contact resistance of the source and drain electrodes has an increasing impact on the total resistance, affecting device performance.

Method used

The combination of pulsed laser melting and flash annealing is used to repair the lattice damage caused by ion implantation through pulsed laser melting, form a super-doped silicon layer, and ohmic contact is formed at the metal-semiconductor interface through flash annealing to reduce the contact resistance.

Benefits of technology

It significantly reduces the contact resistance of semiconductor devices, improves the electrical performance and stability of the device, and ensures the success rate and quality of ohmic contacts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782466B_ABST
    Figure CN118782466B_ABST
Patent Text Reader

Abstract

The present invention discloses a silicon-based semiconductor field effect transistor with ultra-low contact resistance and a preparation method thereof, the preparation method comprising: completing ion implantation of a substrate by injecting chalcogen ions; completing patterning of a sample by photolithography technology, preparing a contact pattern on a substrate by photolithography equipment, and performing metal deposition to form a metal layer covering the substrate; depositing metal by electron beam evaporation and forming an electrode; and completing annealing of the electrode by flash lamp annealing to form an ohmic contact. The present invention can form an alloy at the gold-semiconductor interface, realize secondary regulation of the Schottky barrier, and realize monitoring of the contact resistance by a detection step, thereby ensuring that the ohmic contact can be smoothly realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor devices, and in particular to a silicon-based semiconductor field effect transistor with ultra-low contact resistance and a preparation method thereof. Background Art

[0002] In the development history of the semiconductor industry, the integrated circuit industry has developed rapidly following the prediction of "Moore's Law". Due to the advantages of fast response speed, mature industry and low cost, silicon-based complementary metal oxide semiconductor (CMOS) technology is the mainstream technology of integrated circuit technology. However, with the development of science and technology, the requirements for the integration of semiconductor devices are getting higher and higher, and the size of semiconductor devices is getting smaller and smaller. The processing of traditional silicon-based CMOS faces challenges in technology and physical limits. It is difficult to improve the integration of traditional integrated circuits and the performance of semiconductor devices simply by shortening the channel length of MOSFET. In addition, the influence of various short channel effects such as drain-induced barrier lowering effect and punch-through effect on device performance is becoming more and more serious.

[0003] And with the widespread use of semiconductor devices, people have also put forward higher requirements for device performance. There are many factors that affect the performance of semiconductor devices, among which resistance is a very important factor. The total resistance of semiconductor devices is composed of two parts: the bulk resistance of semiconductor materials and the contact resistance of the source and drain electrodes of semiconductor devices. As the size of devices continues to shrink, the proportion of the contact resistance on the source and drain electrodes of semiconductor devices in the total resistance of the entire device is increasing, and the impact on the performance of semiconductor devices is also increasing. It is generally believed that the potential barrier generated at the interface between the metal electrode and the semiconductor material, namely the Schottky barrier, is the main reason for the high contact resistance and low current transmission capacity of the device. There are two main reasons for the formation of Schottky barriers at the metal-semiconductor interface. One is the mismatch between the metal work function and the semiconductor electron affinity, and the other is the Fermi level pinning effect caused by the metal-induced gap state. Therefore, improving the quality of the ohmic contact between the metal and the semiconductor is the key to reducing the contact resistance on the source and drain electrodes of semiconductor devices and improving the performance of semiconductor devices. Summary of the invention

[0004] One of the purposes of the present invention is to provide a method for preparing a silicon-based semiconductor field effect transistor with ultra-low contact resistance, so as to solve the problem in the prior art that the performance of semiconductor devices is poorly improved due to low carrier density and high contact resistivity.

[0005] The present invention is achieved through the following technical scheme, a method for preparing a silicon-based semiconductor field effect transistor with ultra-low contact resistance, comprising the following steps: S100, completing ion implantation of a substrate by injecting chalcogen ions; S200, completing patterning of a sample by photolithography technology; wherein, a contact pattern is prepared on a substrate by using photolithography equipment, and metal deposition is performed to form a metal layer covering the substrate; S300, metal deposition is performed by electron beam evaporation to form an electrode; S400, annealing of the electrode is completed by flash lamp annealing to form an ohmic contact, and the flash lamp annealing time is 1.3~20ms.

[0006] Furthermore, the preparation method also includes a pulse laser melting step, in which a pulse laser is used to melt the substrate after the ion implantation of the substrate is completed. This step can repair the damage to the semiconductor lattice caused by the ion implantation process, and the integrity of the lattice can be restored by melting the substrate with a pulse laser, thereby improving the crystal quality of the material.

[0007] Furthermore, the pulse laser melting step includes using a pulse laser to melt the substrate after ion implantation in ambient air.

[0008] It should be noted that pulsed laser melting can repair lattice damage caused by ion implantation and optimize metal-semiconductor interface contact, thereby significantly reducing contact resistance and improving the electrical performance and stability of the device. At the same time, pulsed laser melting can provide an efficient and controllable process, which plays an important role in improving the overall performance of semiconductor devices.

[0009] Furthermore, the ion implantation in S100 may adopt a chalcogen element super-doping method to prepare a super-doped silicon layer with an electron density of 10^21cm^-3.

[0010] Furthermore, the order of metal deposition in S200 is to deposit an adhesion layer on the substrate by sputtering deposition, and then deposit a conductive anti-corrosion layer on the adhesion layer by electron beam evaporation.

[0011] Furthermore, an adhesion layer is deposited on the substrate, and the adhesion layer is used to regulate the Schottky barrier and block the diffusion of impurity elements into the semiconductor material; the conductive anti-corrosion layer is deposited on the adhesion layer, and the conductive anti-corrosion layer is used to provide conductivity and protect the adhesion layer from oxidation or corrosion.

[0012] Furthermore, the material of the adhesion layer is titanium metal, with a thickness of 4-9 nm; the material of the conductive anti-corrosion layer is gold or silver, with a thickness of 40-90 nm.

[0013] Furthermore, the preparation method may also include a measurement step, connecting a current source at both ends of the semiconductor and passing a constant current between the electrodes; connecting a voltmeter at both ends of the semiconductor and measuring the voltage drop through a probe; and solving the total resistance Rt at both ends of the probe through the measured current and voltage.

[0014] Furthermore, the total resistance R t The calculation method is formula (1), (1), (2), (3); where R sh is the sheet resistance of the material, L T is the equivalent transmission length, ρ c is the contact resistivity, R c is the contact resistance; r is the radius of the probe, d is the distance between the probes, and a linear fit is made to the data points using d as the horizontal axis. The contact resistivity ρ of the sample is calculated by the slope and intercept of the fitting curve. c and contact resistance R c .

[0015] On the other hand, the present invention provides a silicon-based semiconductor field effect transistor with ultra-low contact resistance. The field effect transistor is prepared according to the method for preparing a silicon-based semiconductor field effect transistor with ultra-low contact resistance as described above, and includes a source region, a drain region, a substrate, an oxide, a gate, and a source and a drain with ultra-low contact resistance.

[0016] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0017] 1. The present invention combines pulsed laser melting and flash lamp annealing to form two annealing processes. The first annealing is achieved by pulsed laser melting to repair the lattice damage caused by ion implantation, ensure that the properties of the super-doped silicon layer are not changed, and ensure the success rate and quality of subsequent ohmic contacts.

[0018] 2. The present invention improves metal deposition to form two electroplating layers, in which titanium metal is used as an adhesion layer to prevent other impurity elements from diffusing into the semiconductor material, ensuring that the ultra-doped silicon layer with a high electron density is not affected. At the same time, the height of the Schottky barrier is regulated, and a conductive anti-corrosion layer is deposited on the adhesion layer to further improve the electrical performance of the entire system, creating good structural conditions for the subsequent formation of ultra-low contact resistance.

[0019] 3. The present invention performs secondary annealing treatment on the electrode through millisecond-level flash lamp annealing, which can form an alloy at the gold-semiconductor interface, realize secondary regulation of the Schottky barrier, and monitor the contact resistance through a detection step to ensure that ohmic contact can be successfully achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The drawings described herein are used to provide a further understanding of the embodiments of the present invention, constitute a part of this application, and do not constitute a limitation of the embodiments of the present invention. In the drawings:

[0021] Figure 1 This is a flowchart provided for Example 1 of the present invention.

[0022] Figure 2 This is a flowchart provided for Example 2 of the present invention.

[0023] Figure 3 This is a schematic diagram of measuring the contact resistance of Example 5 of the present invention.

[0024] Figure 4 This is a scanning electron microscope morphology image of the ohmic contact for measuring the contact resistance of Example 5 of the present invention.

[0025] Figure 5 This is a graph showing the IV characteristics of the metal semiconductor junction of Example 5 of the present invention that has not been annealed.

[0026] Figure 6 This is a graph showing the IV characteristics of the metal semiconductor junction of Example 5 of the present invention without pulsed laser melting treatment.

[0027] Figure 7 This is a graph showing the IV characteristics of the metal semiconductor junction after two-step annealing according to Example 5 of the present invention.

[0028] Figure 8 The p is extracted from the ohmic contact formed by the metal semiconductor junction only subjected to flash lamp electrode annealing in Example 5 of the present invention. c and R c Schematic diagram.

[0029] Fig. 9 The ρ extracted from the ohmic contact formed by the metal semiconductor junction after the two-step annealing treatment of pulse laser melting treatment and flash lamp annealing treatment in Example 5 of the present invention c and R c Schematic diagram. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0031] Embodiment 1:

[0032] Figure 1 The flowchart of this embodiment is shown. This embodiment provides a method for preparing a silicon-based semiconductor field effect transistor with ultra-low contact resistance, which specifically includes the following steps:

[0033] Step 1: Complete the ion implantation of the substrate by implanting chalcogen ions.

[0034] Specifically, ion implantation can use chalcogenide super-doping technology to prepare a super-doped silicon layer with an electron density of 10^21 cm^-3. The super-doped silicon layer prepared by super-doping with chalcogenide elements has ultra-high carrier density and thermal stability. Combined with the subsequent flash annealing process, the Schottky barrier at the metal-semiconductor interface can be adjusted, so that the contact electrode can achieve ultra-low contact resistivity.

[0035] Step 2: Use photolithography technology to complete the patterning of the sample, use photolithography equipment to prepare a contact pattern on the substrate, and perform metal deposition to form a metal layer covering the substrate.

[0036] Specifically, the order of metal deposition is to deposit an adhesion layer on the substrate by sputtering, and then deposit a conductive anti-corrosion layer on the adhesion layer by electron beam evaporation. The adhesion layer is deposited on the substrate, and its material is titanium metal with a deposition thickness of 4~9nm, which is used to regulate the Schottky barrier and block the diffusion of impurity elements into the semiconductor material; the material of the electrical anti-corrosion layer is gold or silver, and the deposition thickness is 40~90nm.

[0037] It should be noted that in this embodiment, the Ti layer (titanium layer) is covered on the silicon-based substrate as an adhesion layer. Its purpose is to serve as a diffusion barrier layer to prevent other impurity elements from diffusing into the semiconductor material and affecting the performance of the device. It can also be used to adjust the Schottky barrier height and affect the contact characteristics between the metal and the semiconductor. The purpose of the Au layer (gold layer) or the Ag layer (silver layer) is to serve as a conductive anti-corrosion layer on the Ti layer (titanium layer). Its purpose is to provide excellent conductive properties. Gold and silver, as a precious metal, have good conductivity and chemical stability, are not easy to oxidize, and can effectively reduce resistance. At the same time, since gold and silver are not easy to react with oxygen and other elements in the air, they can also protect the underlying titanium layer and prevent the titanium layer from being oxidized or corroded. Metal contact with low resistance and high stability is achieved by depositing metals of different properties in sequence. Among them, the titanium layer is used to ensure good adhesion and prevent diffusion, and to adjust the Schottky barrier height; while the gold layer or the silver layer provides excellent conductivity and chemical stability.

[0038] Step 3: Deposit metal by electron beam evaporation and form electrodes.

[0039] Step 4: Use flash lamp annealing to complete the annealing treatment of the electrode and form an ohmic contact. The flash lamp annealing time is 1.3 ms.

[0040] Step 5, measurement step, connect current sources at both ends of the semiconductor respectively, and pass a constant current between the electrodes; connect voltmeters at both ends of the semiconductor respectively, and measure the voltage drop through the probe; solve the total resistance Rt at both ends of the probe through the measured current and voltage.

[0041] Specifically, the total resistance R t The calculation method of can be,

[0042] (1);

[0043] (2);

[0044] (3);

[0045] Among them, R sh is the sheet resistance of the material, L T is the equivalent transmission length, ρ c is the contact resistivity, R c is the contact resistance.

[0046] r is the radius of the probe, d is the distance between the probes, and a linear fit is made to the data points using d as the horizontal axis. The contact resistivity ρ of the sample is calculated by the slope and intercept of the fitting curve. cand contact resistance R c .

[0047] In this embodiment, only flash lamp annealing is used to complete the annealing process of the electrode.

[0048] Embodiment 2:

[0049] Figure 2 The flow chart of this embodiment is shown, from which it can be seen that the main steps of this embodiment are exactly the same as those in exemplary embodiment 1, the difference being that after the ion implantation of the substrate is completed in step 1, a pulsed laser melting step is inserted.

[0050] That is, after the ion implantation of the substrate is completed, the substrate is melted in the ambient air using a pulsed laser. This step can repair the damage to the semiconductor lattice caused by the ion implantation process. Melting the substrate with a pulsed laser can restore the integrity of the lattice, thereby improving the crystal quality of the material. This step can be regarded as an annealing treatment for the substrate, the purpose of which is to increase the amount of ion doping.

[0051] Pulsed laser melting can repair the lattice damage caused by ion implantation and optimize the metal-semiconductor interface contact, thereby significantly reducing the contact resistance and improving the electrical performance and stability of the device. At the same time, pulsed laser melting can provide an efficient and controllable process, which plays an important role in improving the overall performance of semiconductor devices.

[0052] In summary, two annealing processes are used in this embodiment. After the substrate is ion-implanted, the entire substrate is treated by pulsed laser melting, which is the first annealing process, and its purpose is to repair the damage caused by ion implantation to the semiconductor lattice and ensure the super-doping concentration of the silicon layer. The second annealing process is to complete the annealing of the electrode by flash lamp annealing, and its purpose is to perform secondary regulation of the Schottky barrier and ensure the formation of ohmic contact.

[0053] Embodiment 3:

[0054] The main steps of this embodiment are exactly the same as those in exemplary embodiment 1, except that step 4 uses flash lamp annealing to complete annealing of the electrode and form an ohmic contact, and the flash lamp annealing time is 11 ms.

[0055] Embodiment 4:

[0056] The main steps of this embodiment are exactly the same as those in exemplary embodiment 2, except that flash lamp annealing is used to complete the annealing of the electrode, and in the step of forming an ohmic contact, the flash lamp annealing time is 5 ms.

[0057] In order to better understand the present invention, the present invention is further explained below in conjunction with the embodiments, but the present invention is not limited to the following embodiments.

[0058] Embodiment 5:

[0059] This embodiment provides a method for preparing a silicon-based semiconductor field effect transistor with ultra-low contact resistance, and its actual application steps include the following steps:

[0060] Step 1: Using interface control technology, chalcogenide elements are used to prepare a super-doped silicon layer with an electron density of 10^21 cm^-3. The prepared super-doped silicon layer has an ultra-high carrier density that can make the Schottky barrier width thin enough to ensure that electrons can directly tunnel through the barrier.

[0061] Step 2: After the ion implantation of the substrate is completed, the substrate is melted in ambient air using a pulsed laser. This step can repair the damage to the semiconductor lattice caused by the ion implantation process. Melting the substrate with a pulsed laser can restore the integrity of the lattice, thereby improving the crystal quality of the material. This step can be regarded as an annealing treatment for the substrate, the purpose of which is to increase the ion doping amount.

[0062] Pulsed laser melting can repair the lattice damage caused by ion implantation and optimize the metal-semiconductor interface contact, thereby significantly reducing the contact resistance and improving the electrical performance and stability of the device. At the same time, pulsed laser melting can provide an efficient and controllable process, which plays an important role in improving the overall performance of semiconductor devices.

[0063] Step 3: Use photolithography technology to complete the patterning of the sample, use photolithography equipment to prepare a contact pattern on the substrate, and perform metal deposition to form a metal layer covering the substrate.

[0064] Specifically, it includes first depositing a Ti layer (titanium layer) on the substrate by sputtering as an adhesion layer covering the silicon-based substrate. The deposition thickness of the Ti layer (titanium layer) is 4~9nm, and its purpose is to be used for regulating the Schottky barrier and blocking the diffusion of impurity elements into the semiconductor material.

[0065] Then, an Au layer (gold layer) with a thickness of 40 to 90 nm is deposited on the Ti layer (titanium layer) by electron beam evaporation, or an Ag layer (silver layer) with a thickness of 40 to 90 nm is deposited by electron beam evaporation as a conductive anti-corrosion layer.

[0066] It should be noted that the purpose of depositing titanium metal by sputtering is to ensure that the titanium metal and the substrate can be closely adhered, thereby providing the possibility of adjusting the Schottky barrier height of the titanium layer. Depositing gold or silver by electron beam evaporation can ensure the thickness and uniformity of the deposition, thereby providing better electrical connection performance.

[0067] Step 4: Metal deposition and electrode formation by electron beam evaporation.

[0068] Step 5: Use flash lamp annealing to complete the annealing treatment of the electrode and form an ohmic contact. The flash lamp annealing time is 20ms.

[0069] Step 6: Connect a current source to both ends of the semiconductor and pass a constant current between the electrodes; connect a voltmeter to both ends of the semiconductor and measure the voltage drop through the probe; use the measured current and voltage to solve the total resistance Rt across the probe.

[0070] Specifically, the total resistance R t The calculation method of can be,

[0071] (1);

[0072] (2);

[0073] (3);

[0074] Among them, R sh is the sheet resistance of the material, L T is the equivalent transmission length, ρ c is the contact resistivity, R c is the contact resistance. d Usually refers to the spacing between probes. In resistance measurements, d As the distance from the center of the probe to the center of another probe, this parameter is an important factor in calculating resistance because it affects the current distribution and the calculation of contact resistance. r Usually represents the radius of the probe or. In the calculation of resistance and current distribution, r Refers to the effective radius of the probe, which affects the distribution of the electric field and the calculation of contact resistance.

[0075] Use d as the horizontal axis to make a linear fit for the data points, and calculate the contact resistivity ρ of the sample through the slope and intercept of the fitting curve. c and contact resistance R c .

[0076] Figure 3 shows a schematic diagram of contact resistance measurement, Figure 4Scanning electron microscope topography of an ohmic contact showing the contact resistance measurements.

[0077] As can be seen from the above figure, the metal-semiconductor contact principle of ohmic contact with ultra-low contact resistance, there are two types of contacts between metal and semiconductor:

[0078] One type conducts electricity unidirectionally between metals and semiconductors, which is called a Schottky contact or a rectifying contact. The other type of contact still exhibits low resistance characteristics after applying positive and reverse bias voltages, and no rectification occurs, which is an ordinary ohmic contact.

[0079] Work function is an important factor affecting contact characteristics. Assuming that the metal and semiconductor are in close contact without an interface layer, when the metal contacts the n-type semiconductor, the ideal post-contact barrier height is given by the following relationship:

[0080] (4);

[0081] Where W M is the work function of metals and semiconductors; χ is the electron affinity of semiconductor materials, which is defined as the potential difference between the bottom of the semiconductor conduction band and the vacuum level.

[0082] By selecting appropriate alloy conditions, its electrical properties can be greatly improved, which also helps to improve the ohmic contact performance and improve the reliability of the device.

[0083] In this embodiment, the millisecond flash lamp annealing is used to anneal the electrode, which can form an alloy at the gold semiconductor interface, thereby achieving the regulation of the Schottky barrier, thereby achieving an ohmic contact with ultra-low contact resistance.

[0084] And according to the metal-semiconductor contact theory, the transport mode of electrons across the metal-semiconductor junction is related to the doping concentration of the semiconductor. The mechanism of field emission to form ohmic contact is the most common choice in today's semiconductor device technology. In order to form ohmic contact, most compound semiconductors at this stage are prepared by heavily doping layers on the surface, so that the energy band bending at the metal-semiconductor contact is very large, and the contact surface semiconductor becomes a degenerate semiconductor, making the barrier layer very thin, so that electrons can easily pass through the barrier region to form a tunneling current.

[0085] Therefore, the super-doped silicon layer prepared by super-doping with chalcogen elements in this embodiment has a 21 cm -3The ultra-high carrier density makes the Schottky barrier width thin enough to ensure that electrons can directly tunnel through the barrier. However, the common chalcogenide element super-doping preparation easily causes the crystal quality of the material to change. Therefore, in order to ensure the crystal quality of the super-doped silicon layer, this embodiment uses pulsed laser melting treatment of the entire substrate after the ion implantation is completed. Repairing the damage to the semiconductor lattice caused by the ion implantation process ensures the integrity of the lattice, improves the quality of the product, and ensures that a stable ohmic contact can be formed in the subsequent process.

[0086] Figure 5 The IV characteristic curve of the metal semiconductor junction without annealing treatment is shown. Figure 6 The IV characteristic curve of the metal semiconductor junction without pulsed laser melting is shown. Figure 7 The IV characteristic curve of the metal semiconductor junction through the two-step annealing in this embodiment is shown.

[0087] It should be noted that Figure 5 The remaining steps are the same as those of the present embodiment, the only difference being that the pulsed laser melting treatment and flash lamp annealing treatment in step 2 and step 5 of the present embodiment are not performed. Figure 6 The remaining steps are the same as those in the present embodiment, with the only difference being that the pulsed laser melting treatment in step 2 of the present embodiment is not performed. Figure 7 The IV characteristic curve of the metal semiconductor junction after pulse laser melting and flash lamp annealing. Comparing the three figures, we can see that Figure 5 The IV curve of the metal-semiconductor junction without annealing treatment shows nonlinear characteristics, which is a typical Schottky contact. Figure 6 After millisecond flash lamp electrode annealing alloying treatment, the IV characteristics of the metal semiconductor junction change linearly, which means that an ohmic contact is formed at the junction interface. Figure 7 The ohmic contact formed after two annealing treatments has a wider range and has better performance than the metal semiconductor junction that has only been annealed by the flash lamp electrode.

[0088] At the same time, in order to further illustrate the ohmic contact with ultra-low contact resistance described in this embodiment, the total resistance of the test electrode ring is calculated by using the slope of the IV curve; by plotting the total resistance as a function of the metal electrode spacing, the ohmic contact ρ is calculated using formulas (1) to (3). c and R c .

[0089] Figure 8 The ρ extracted from the ohmic contact formed by the metal semiconductor junction subjected to flash lamp electrode annealing alone is shown. c and R c ; Fig. 9 The ρ extracted from the ohmic contact formed by the metal semiconductor junction after the two-step annealing treatment of pulsed laser melting and flash lamp annealing is shown. c and R c .

[0090] from Figure 8 It can be seen that the ρ extracted from the metal semiconductor junction only after flash lamp electrode annealing c =(8.3± 2.6) × 10 -9 Ω∙cm 2 This is because the ultra-doped Si layer prepared by ultra-doping with chalcogen elements has a near 10 21 cm -3 The ultra-high carrier density makes the Schottky barrier thin enough to ensure that electrons can directly tunnel through the barrier; and the millisecond flash lamp annealing is used to anneal the electrode to form an alloy at the gold semiconductor interface to achieve the regulation of the Schottky barrier. Fig. 9 It can be seen that the ρ obtained in the metal semiconductor junction after the two-step annealing treatment of pulsed laser melting and flash lamp annealing is c =(2.9 ± 0.6) × 10 -9 Ω∙cm 2 This is because the lattice damage caused by ion implantation is repaired by pulsed laser melting and the metal-semiconductor interface contact is optimized, thereby ensuring that the properties of the super-doped silicon layer are not changed. At the same time, the activation of impurities and the regrowth of the epitaxial layer can be completed, which has a good effect on improving the success rate of ohmic contact in the flash lamp electrode annealing process.

[0091] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a silicon-based semiconductor field effect transistor with ultra-low contact resistance, characterized in that: The preparation method comprises: S100, completing ion implantation of the substrate by implanting chalcogen ions, and after completing the ion implantation of the substrate, performing a melting process on the substrate using a pulsed laser, The ion implantation adopts the chalcogen element super doping method to prepare a 10 21 cm -3 electron-dense super-doped silicon layer; S200, using photolithography technology to complete the patterning of the sample; wherein, using photolithography equipment to prepare a contact pattern on a substrate, and performing metal deposition to form a metal layer covering the substrate, The order of metal deposition is to deposit an adhesion layer on the substrate by sputtering, and then deposit a conductive anti-corrosion layer on the adhesion layer by electron beam evaporation. The adhesion layer is deposited on the substrate, and is used to regulate the Schottky barrier and block the diffusion of impurity elements into the semiconductor material; the conductive anti-corrosion layer is deposited on the adhesion layer, and is used to provide conductivity and protect the adhesion layer from oxidation or corrosion, and the material of the adhesion layer is titanium metal, and the thickness is 4-9nm; the material of the conductive anti-corrosion layer is gold or silver, and the thickness is 40-90nm; S300, depositing metal and forming electrodes by electron beam evaporation; S400, completing annealing of the electrode by flash lamp annealing to form an ohmic contact, wherein the flash lamp annealing time is 1.3-20 ms.

2. The method for preparing a silicon-based semiconductor field effect transistor with ultra-low contact resistance according to claim 1, characterized in that: The preparation method also includes a measurement step, wherein a current source is connected to both ends of the semiconductor and a constant current is passed between the electrodes; a voltmeter is connected to both ends of the semiconductor and a voltage drop is measured through a probe; and a total resistance Rt at both ends of the probe is solved through the measured current and voltage.

3. The method for preparing a silicon-based semiconductor field effect transistor with ultra-low contact resistance according to claim 2, characterized in that: The total resistance R across the probe t The calculation method is, ; ; ; Among them, R sh is the sheet resistance of the material, L T is the equivalent transmission length, ρ c is the contact resistivity, R c is the contact resistance; Use d as the horizontal axis to make a linear fit for the data points, and calculate the contact resistivity ρ of the sample through the slope and intercept of the fitting curve. c and contact resistance R c ; The first group of ρ c and R c Finally, on this basis, the same contact structure of the sample is selected to complete more than 2 repeated tests and fitting calculations.

4. A silicon-based semiconductor field effect transistor with ultra-low contact resistance, characterized in that: The silicon-based semiconductor field effect transistor with ultra-low contact resistance is prepared according to the method for preparing a silicon-based semiconductor field effect transistor with ultra-low contact resistance according to any one of claims 1 to 3, and includes a source region, a drain region, a substrate, an oxide, a gate, and a source and a drain with ultra-low contact resistance.