Hard carbon negative electrode material for sodium ion battery and preparation method of hard carbon negative electrode material
By using precursor carbon sheets and grid carbon sheets combined with cobalt materials in the hard carbon negative electrode material of sodium ion batteries, the uniform distribution of cobalt elements is achieved, which solves the problem of unstable cycle performance caused by the aggregation of cobalt materials and improves the electrochemistry of the battery. performance.
Patent Information
- Application Number
- CN202410915250.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-15
AI Technical Summary
In existing hard carbon anode materials doped with metal elements for sodium-ion batteries, cobalt materials tend to aggregate, resulting in unstable cycle performance and poor energy storage effects.
The precursor carbon sheet and the covered grid carbon sheet are combined with cobalt material and connected through covalent bonds. The hydrothermal reaction and sintering process are used to evenly distribute the cobalt element to form a hard carbon negative electrode material for sodium ion batteries.
It effectively solves the problem of cobalt element aggregation, improves the cycle performance and energy storage effect of the battery, and enhances the stability of the electrochemical performance.
Smart Images

Figure CN118782801A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery electrode materials, and in particular to a hard carbon negative electrode material for a sodium ion battery and a preparation method thereof. Background Art
[0002] Sodium-ion battery is a rechargeable battery that mainly relies on the movement of sodium ions between the positive and negative electrodes to work. Compared with traditional lithium-ion batteries, it has lower costs and wider resource availability. Hard carbon is an important component of the negative electrode material of sodium-ion batteries. Currently, graphite is mostly used as a sodium-ion hard carbon material. However, the limited resources of graphite and the environmental impact caused by mining have greatly affected the use and development of negative electrode materials for sodium-ion batteries.
[0003] Straw is the waste left after the harvest of crops. It is usually used as fuel, feed or waste disposal, which has a large processing burden and fails to achieve the best use of it. Therefore, with the increasing awareness of environmental protection and the development and utilization of renewable resources in recent years, how to make greater use of straw resources has become a hot research issue.
[0004] Based on the above situation, the technical inspiration of using corn stalks for negative electrode materials of sodium ion batteries has been proposed, which has attracted much attention in the field of batteries. For example, the patent with publication number CN107337205A provides a method for converting waste corn stalks into electrode materials of sodium ion batteries. The waste corn stalks are cleaned, dried, carbonized and calcined to prepare a carbon material with a porous structure for producing negative electrode materials of sodium ion batteries. The sodium ion battery assembled with the material as the negative electrode can show good cycle stability, rate performance and high sodium storage capacity.
[0005] Furthermore, structural modification of battery electrode materials is one of the effective means to improve the cycle performance of electrode materials. Electronic structure modification such as element doping can improve electronic conductivity and provide more energy storage active sites for sodium ions. However, in the existing sodium ion battery negative electrode materials doped with metal elements such as cobalt, the doped metal oxide nanoparticles are prone to aggregation, resulting in unstable cycle performance and poor energy storage effect. Summary of the invention
[0006] The technical problems to be solved by the present invention are:
[0007] In the hard carbon negative electrode materials of sodium ion batteries, the performance of electrode materials can usually be improved by modifying the electronic structure such as element doping, such as improving electronic conductivity and providing more energy storage active sites for sodium ions. However, in the existing metal element doped hard carbon negative electrode materials for sodium ion batteries, the doped cobalt materials and other metal oxides are prone to aggregation and poor distribution uniformity, resulting in unstable cycle performance of the negative electrode sheet in button batteries and poor energy storage effect.
[0008] The technical solution adopted by the present invention is:
[0009] The present invention provides a hard carbon negative electrode material for a sodium ion battery, comprising a precursor carbon sheet and a grid carbon sheet covered on the surface of the precursor carbon sheet, wherein the grid carbon sheet is penetrated by a plurality of grids; the grids are doped with cobalt material, and the cobalt material is bonded to the precursor carbon sheet or the grid carbon sheet through a covalent bond.
[0010] Preferably, the aperture of the grid is 15-50 μm, and the distance between two adjacent grids is 5-20 μm.
[0011] Preferably, the grid carbon sheet is prepared by machining nano-carbon material, and the machining methods include but are not limited to weaving, winding, pressing or cutting.
[0012] The method for preparing the hard carbon negative electrode material for sodium ion battery comprises the following steps:
[0013] S1 pretreatment: pre-treating the biomass carbon material by heating and carbonizing it to obtain a precursor carbon material;
[0014] S2: Slicing the precursor carbon material to make precursor carbon sheets;
[0015] S3 structural treatment: a grid carbon sheet is coated on the surface of the precursor carbon sheet, and hot pressed to obtain a composite carbon sheet;
[0016] S4 cobalt doping: placing the composite carbon sheet in a cobalt-doped mixed solution, heating, performing a hydrothermal reaction, and drying to obtain a doped carbon sheet;
[0017] S5 forming process: sintering the doped carbon sheet to obtain the hard carbon negative electrode material for the sodium ion battery.
[0018] Preferably, in step S1, the pretreatment temperature is 590-620°C, and the pretreatment time is 3-10 hours; the carbonization temperature is 1600-1650°C, and the carbonization time is 5-15 hours.
[0019] Preferably, in step S4, the cobalt-doped mixed solution comprises cobalt salt, urea and water, and the cobalt salt comprises one or more of cobalt chloride, cobalt nitrate, cobalt sulfate or cobalt acetate.
[0020] Preferably, the temperature of the hydrothermal reaction is 200-220° C., and the hydrothermal reaction time is 3-10 h.
[0021] Preferably, in step S5, the sintering temperature is 440-480° C., and the sintering time is 2-5 hours.
[0022] The sodium ion battery prepared by using the hard carbon negative electrode material for sodium ion battery or the hard carbon negative electrode material for sodium ion battery prepared by the above-mentioned preparation method comprises a positive electrode shell stacked layer by layer, the hard carbon negative electrode material for sodium ion battery, a diaphragm, a metallic sodium sheet, a gasket, a spring sheet and a negative electrode shell.
[0023] The beneficial effects of the present invention are as follows:
[0024] The hard carbon negative electrode material for sodium ion battery of the present invention uses biomass materials such as straw as hard carbon material substrate, and introduces covalently linked cobalt elements by hydrothermal reaction, and in the doping process, the grid template carbon sheet is used to make the doping elements evenly distributed on the surface of the hard carbon substrate, which can solve the problem that the existing metal dopants are prone to aggregation, thereby affecting the battery's cycle and energy storage performance. The method has a convenient processing process, is suitable for doping treatment of various elements, and can effectively improve the electrochemical performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a schematic structural diagram of the main body of the sodium ion button battery in Example 1;
[0026] Figure 2 This is a SEM image of the hard carbon negative electrode sheet in Example 1 magnified 200 times;
[0027] Figure 3 This is a SEM image of the hard carbon negative electrode sheet in Example 1 magnified 500 times;
[0028] Figure 4 This is a SEM image of the hard carbon negative electrode sheet in Comparative Example 1 magnified 200 times;
[0029] Figure 5 This is a SEM image of the hard carbon negative electrode sheet in Comparative Example 1 magnified 500 times;
[0030] Figure 6 is the XRD spectrum of the hard carbon negative electrode sheet in Example 1;
[0031] Figure 7 This is the TEM image of the hard carbon negative electrode sheet in Example 1. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0033] The present invention provides a hard carbon negative electrode sheet for a sodium ion battery, comprising a precursor carbon sheet and a grid carbon sheet covered on the surface of the precursor carbon sheet, wherein the grid carbon sheet is provided with a plurality of through holes; and the through holes are doped with cobalt material, and the cobalt material is bonded to the precursor carbon sheet or the grid carbon sheet through a covalent bond.
[0034] The aperture of the grid is 15-50 μm, and the distance between two adjacent grids is 5-20 μm; the grid carbon sheet is a sheet-like carbon material with uniformly distributed grids made by weaving, winding, pressing or cutting nano-carbon materials.
[0035] In the present invention, the method for preparing the hard carbon negative electrode sheet for sodium ion battery comprises the following steps:
[0036] (1) Pretreatment
[0037] The straw is repeatedly rinsed until clean, and then dried and crushed to obtain biomass carbon material; the biomass carbon material is placed at a temperature of 590-620°C for 3-10 hours for pretreatment, and then transferred to a vacuum furnace, heated to 1600-1650°C for 5-15 hours for vacuum carbonization to obtain a precursor carbon material.
[0038] (2) Cobalt-doped materials
[0039] The precursor carbon material is processed by grinding, slicing, etc. to prepare a precursor carbon sheet, and then a grid carbon sheet is coated on both surfaces of the precursor carbon sheet, and hot-pressed to obtain a composite carbon sheet;
[0040] The composite carbon sheet is placed in a mixture of cobalt salt, urea and deionized water, heated to 200-220°C for 3-10h of hydrothermal reaction, and dried at 80-100°C after the reaction to obtain a doped carbon sheet.
[0041] The cobalt tetroxide is compounded with the carbon material obtained by carbonizing straw. The straw carbon material serves as a buffer matrix, which can improve the volume change of the metal oxide anode. It can not only significantly improve the conductivity of the metal oxide electrode, but also effectively prevent the aggregation of metal oxide nanoparticles and improve the stability of battery performance.
[0042] (3) Sintering
[0043] The doped carbon sheet is transferred into a muffle furnace, heated to 440-480° C. and sintered for 2-5 hours to obtain a hard carbon negative electrode sheet for a sodium ion battery.
[0044] In the present invention, the straw is one or more of the common corn, cotton, wheat, rice and other straws; the grid carbon sheet is a sheet-like carbon material with a uniformly distributed grid made by weaving, winding or pressing nano-carbon materials; the cobalt salt can be one or more of the cobalt salts such as cobalt chloride, cobalt sulfate, cobalt nitrate or cobalt acetate.
[0045] In the present invention, the hard carbon negative electrode sheet can be used for sodium ion button cells, and the sodium ion button cells are assembled in the following hierarchical order: positive electrode shell, hard carbon negative electrode sheet, diaphragm, metal sodium sheet, gasket, spring sheet, negative electrode shell.
[0046] Example 1
[0047] Step 1: Take corn stalks and cotton stalks of equal mass, rinse them repeatedly with clean water three times, crush them after drying, and mix them evenly; then place them in a carbonization furnace at 600°C for pretreatment for 6.5 hours, and then transfer them to a vacuum furnace, heat to 1600°C and carbonize them for 10 hours to obtain a precursor carbon material.
[0048] Step 2: Press and grind the precursor carbon material and cut it into 5mm×5mm square precursor carbon sheets with a thickness of about 1.0mm; take another carbon sheet woven and wound by carbon nanotubes, and cut out a number of 20μm×20μm perforations according to a matrix distribution, with a spacing of about 10μm between adjacent perforations to form a grid carbon sheet; cover the upper and lower surfaces of the precursor carbon sheet with a layer of grid carbon sheet, and hot press at 80°C to obtain a composite carbon sheet.
[0049] Step 3: Take 1.5g of cobalt chloride hexahydrate and 1.5g of cobalt sulfate heptahydrate, mix them, add 1.2g of urea and 420mL of deionized water, stir and dissolve to obtain a mixed solution; place the composite carbon sheet in the mixed solution, heat to 200°C for hydrothermal reaction for 5h, take out the carbon sheet after the reaction is completed, and place it in a forced air drying oven at 80°C for drying to obtain a doped carbon sheet.
[0050] Step 4: Place the doped carbon sheet in a muffle furnace, heat to 450°C, sinter for 3 hours, and cool to obtain a hard carbon negative electrode sheet.
[0051] Step 5: Take the above hard carbon negative electrode sheet and press Figure 1 The structure shown, namely positive electrode shell-hard carbon negative electrode plate-diaphragm (glass fiber)-metal sodium plate-gasket-spring plate-negative electrode shell, is assembled into a sodium ion button battery.
[0052] Example 2
[0053] Step 1: Take corn stalks and cotton stalks of equal mass, rinse them repeatedly with clean water three times, crush them after drying, and mix them evenly; then place them in a carbonization furnace at 600°C for pretreatment for 6.5 hours, and then transfer them to a vacuum furnace, heat to 1600°C and carbonize them for 10 hours to obtain a precursor carbon material.
[0054] Step 2: Press and grind the precursor carbon material and cut it into 5mm×5mm square precursor carbon sheets with a thickness of about 1.2mm; take another carbon sheet woven and wound by carbon nanotubes, and cut out a number of 20μm×40μm perforations according to a matrix distribution, with a spacing of about 15μm between adjacent perforations to form a grid carbon sheet; cover the upper and lower surfaces of the precursor carbon sheet with a layer of grid carbon sheet, and hot press at 80°C to obtain a composite carbon sheet.
[0055] Step 3: Take 1.5g of cobalt chloride hexahydrate and 1.5g of cobalt sulfate heptahydrate, mix them, add 1.2g of urea and 420mL of deionized water, stir and dissolve to obtain a mixed solution; place the composite carbon sheet in the mixed solution, heat to 200°C for hydrothermal reaction for 5h, take out the carbon sheet after the reaction is completed, and place it in a forced air drying oven at 80°C for drying to obtain a doped carbon sheet.
[0056] Step 4: Place the doped carbon sheet in a muffle furnace, heat to 450°C, sinter for 3 hours, and cool to obtain a hard carbon negative electrode sheet.
[0057] Step 5: Take the above-mentioned hard carbon negative electrode sheet and assemble it into a sodium ion button battery according to the positive electrode shell-hard carbon negative electrode sheet-diaphragm (glass fiber)-metal sodium sheet-gasket-spring sheet-negative electrode shell.
[0058] Example 3
[0059] Step 1: Take corn stalks and cotton stalks of equal mass, rinse them repeatedly with clean water three times, crush them after drying, and mix them evenly; then place them in a carbonization furnace at 600°C for pretreatment for 6.5 hours, and then transfer them to a vacuum furnace, heat to 1600°C and carbonize them for 10 hours to obtain a precursor carbon material.
[0060] Step 2: Press and grind the precursor carbon material and cut it into 5mm×5mm square precursor carbon sheets with a thickness of about 0.8mm; take another carbon sheet woven and wound by carbon nanotubes, and cut out a number of 15μm×15μm perforations according to a matrix distribution, with a spacing of about 5μm between adjacent perforations to form a grid carbon sheet; cover the upper and lower surfaces of the precursor carbon sheet with a layer of grid carbon sheet, and hot press at 80°C to obtain a composite carbon sheet.
[0061] Step 3: Take 1.5g of cobalt chloride hexahydrate and 1.5g of cobalt sulfate heptahydrate, mix them, add 1.2g of urea and 420mL of deionized water, stir and dissolve to obtain a mixed solution; place the composite carbon sheet in the mixed solution, heat to 200°C for hydrothermal reaction for 5h, take out the carbon sheet after the reaction is completed, and place it in a forced air drying oven at 80°C for drying to obtain a doped carbon sheet.
[0062] Step 4: Place the doped carbon sheet in a muffle furnace, heat to 450°C, sinter for 3 hours, and cool to obtain a hard carbon negative electrode sheet.
[0063] Step 5: Take the above-mentioned hard carbon negative electrode sheet and assemble it into a sodium ion button battery according to the positive electrode shell-hard carbon negative electrode sheet-diaphragm (glass fiber)-metal sodium sheet-gasket-spring sheet-negative electrode shell.
[0064] Example 4
[0065] Step 1: Take corn stalks and cotton stalks of equal mass, rinse them repeatedly with clean water three times, crush them after drying, and mix them evenly; then place them in a carbonization furnace at 600°C for pretreatment for 6.5 hours, and then transfer them to a vacuum furnace, heat to 1600°C and carbonize them for 10 hours to obtain a precursor carbon material.
[0066] Step 2: Press and grind the precursor carbon material and cut it into 5mm×5mm square precursor carbon sheets with a thickness of about 1.5mm; take another carbon sheet woven and wound by carbon nanotubes, and cut out a number of 45μm×45μm perforations according to a matrix distribution, with a spacing of about 18μm between adjacent perforations to form a grid carbon sheet; cover the upper and lower surfaces of the precursor carbon sheet with a layer of grid carbon sheet, and hot press at 80°C to obtain a composite carbon sheet.
[0067] Step 3: Take 1.5g of cobalt chloride hexahydrate and 1.5g of cobalt sulfate heptahydrate, mix them, add 1.2g of urea and 420mL of deionized water, stir and dissolve to obtain a mixed solution; place the composite carbon sheet in the mixed solution, heat to 200°C for hydrothermal reaction for 5h, take out the carbon sheet after the reaction is completed, and place it in a forced air drying oven at 80°C for drying to obtain a doped carbon sheet.
[0068] Step 4: Place the doped carbon sheet in a muffle furnace, heat to 450°C, sinter for 3 hours, and cool to obtain a hard carbon negative electrode sheet.
[0069] Step 5: Take the above-mentioned hard carbon negative electrode sheet and assemble it into a sodium ion button battery according to the positive electrode shell-hard carbon negative electrode sheet-diaphragm (glass fiber)-metal sodium sheet-gasket-spring sheet-negative electrode shell.
[0070] Example 5
[0071] Step 1: Take corn stalks and cotton stalks of equal mass, rinse them repeatedly with clean water three times, crush them after drying, and mix them evenly; then place them in a carbonization furnace at 600°C for pretreatment for 6.5 hours, and then transfer them to a vacuum furnace, heat to 1600°C and carbonize them for 10 hours to obtain a precursor carbon material.
[0072] Step 2: Press and grind the precursor carbon material and cut it into 5mm×5mm square precursor carbon sheets with a thickness of about 1.0mm; take another carbon sheet woven and wound by carbon nanotubes, and cut out a number of 20μm×20μm perforations according to a matrix distribution, with a spacing of about 10μm between adjacent perforations to form a grid carbon sheet; only a layer of grid carbon sheet is covered on the upper surface of the precursor carbon sheet, and hot pressed at 80°C to obtain a composite carbon sheet.
[0073] Step 3: Take 1.5g of cobalt chloride hexahydrate and 1.5g of cobalt sulfate heptahydrate, mix them, add 1.2g of urea and 420mL of deionized water, stir and dissolve to obtain a mixed solution; place the composite carbon sheet in the mixed solution, heat to 200°C for hydrothermal reaction for 5h, take out the carbon sheet after the reaction is completed, and place it in a forced air drying oven at 80°C for drying to obtain a doped carbon sheet.
[0074] Step 4: Place the doped carbon sheet in a muffle furnace, heat to 450°C, sinter for 3 hours, and cool to obtain a hard carbon negative electrode sheet.
[0075] Step 5: Take the above-mentioned hard carbon negative electrode sheet and assemble it into a sodium ion button battery according to the positive electrode shell-hard carbon negative electrode sheet-diaphragm (glass fiber)-metal sodium sheet-gasket-spring sheet-negative electrode shell.
[0076] Example 6
[0077] Step 1: Take corn stalks and cotton stalks of equal mass, rinse them repeatedly with clean water three times, crush them after drying, and mix them evenly; then place them in a carbonization furnace at 600°C for pretreatment for 6.5 hours, and then transfer them to a vacuum furnace, heat to 1600°C and carbonize them for 10 hours to obtain a precursor carbon material.
[0078] Step 2: Press and grind the precursor carbon material and cut it into 5mm×5mm square precursor carbon sheets with a thickness of about 1.0mm; take another carbon sheet woven and wound by carbon nanotubes, and cut out a number of 20μm×20μm perforations according to a matrix distribution, with a spacing of about 10μm between adjacent perforations to form a grid carbon sheet; cover the upper and lower surfaces of the precursor carbon sheet with a layer of grid carbon sheet, and hot press at 80°C to obtain a composite carbon sheet.
[0079] Step 3: Take 3g of cobalt nitrate hexahydrate, mix, add 1.2g of urea and 420mL of deionized water, stir to dissolve, and obtain a mixed solution; place the composite carbon sheet in the mixed solution, heat to 200°C for hydrothermal reaction for 5h, take out the carbon sheet after the reaction, and place it in a forced air drying oven at 80°C for drying to obtain a doped carbon sheet.
[0080] Step 4: Place the doped carbon sheet in a muffle furnace, heat to 450°C, sinter for 3 hours, and cool to obtain a hard carbon negative electrode sheet.
[0081] Step 5: Take the above-mentioned hard carbon negative electrode sheet and assemble it into a sodium ion button battery according to the positive electrode shell-hard carbon negative electrode sheet-diaphragm (glass fiber)-metal sodium sheet-gasket-spring sheet-negative electrode shell.
[0082] Comparative Example 1
[0083] Step 1: Take corn stalks and cotton stalks of equal mass, rinse them repeatedly with clean water three times, crush them after drying, and mix them evenly; then place them in a carbonization furnace at 600°C for pretreatment for 6.5 hours, and then transfer them to a vacuum furnace, heat to 1600°C and carbonize them for 10 hours to obtain a precursor carbon material.
[0084] Step 2: Press and grind the precursor carbon material, cut it into 5 mm×5 mm square precursor carbon sheets with a thickness of about 1.0 mm, and treat it at 80° C. for 2 min.
[0085] Step 3: Take 1.5g of cobalt chloride hexahydrate and 1.5g of cobalt sulfate heptahydrate, mix them, add 1.2g of urea and 420mL of deionized water, stir to dissolve, and obtain a mixed solution; place the precursor carbon sheet in the mixed solution, heat to 200°C for hydrothermal reaction for 5h, take out the carbon sheet after the reaction is completed, and place it in a forced air drying oven at 80°C for drying to obtain a doped carbon sheet.
[0086] Step 4: Place the doped carbon sheet in a muffle furnace, heat to 450°C, sinter for 3 hours, and cool to obtain a hard carbon negative electrode sheet.
[0087] Step 5: Take the above-mentioned hard carbon negative electrode sheet and assemble it into a sodium ion button battery according to the positive electrode shell-hard carbon negative electrode sheet-diaphragm (glass fiber)-metal sodium sheet-gasket-spring sheet-negative electrode shell.
[0088] Comparative Example 2
[0089] Step 1: Take corn stalks and cotton stalks of equal mass, rinse them repeatedly with clean water three times, crush them after drying, and mix them evenly; then place them in a carbonization furnace at 600°C for pretreatment for 6.5 hours, and then transfer them to a vacuum furnace, heat to 1600°C and carbonize them for 10 hours to obtain a precursor carbon material.
[0090] Step 2: Press and grind the precursor carbon material and cut it into 5mm×5mm square precursor carbon sheets with a thickness of about 1.0mm. Overlap three precursor carbon sheets and hot-press them at 80°C to obtain a composite carbon sheet.
[0091] Step 3: Take 1.5g of cobalt chloride hexahydrate and 1.5g of cobalt sulfate heptahydrate, mix them, add 1.2g of urea and 420mL of deionized water, stir and dissolve to obtain a mixed solution; place the composite carbon sheet in the mixed solution, heat to 200°C for hydrothermal reaction for 5h, take out the carbon sheet after the reaction is completed, and place it in a forced air drying oven at 80°C for drying to obtain a doped carbon sheet.
[0092] Step 4: Place the doped carbon sheet in a muffle furnace, heat to 450°C, sinter for 3 hours, and cool to obtain a hard carbon negative electrode sheet.
[0093] Step 5: Take the above-mentioned hard carbon negative electrode sheet and assemble it into a sodium ion button battery according to the positive electrode shell-hard carbon negative electrode sheet-diaphragm (glass fiber)-metal sodium sheet-gasket-spring sheet-negative electrode shell.
[0094] Test example
[0095] Samples: Examples 1-6, Comparative Examples 1-2 (one)
[0097] The hard carbon negative electrode sheets in Example 1 and Comparative Example 2 were taken respectively, and the surface structures of the hard carbon negative electrode sheets were observed under a scanning electron microscope at magnifications of 200 times and 500 times, respectively. The results are as follows: Figures 2 to 5 shown.
[0098] It can be seen from the SEM images of different samples at different magnifications that the hard carbon negative electrode sheet prepared by the method of Example 1 has uniform surface element distribution, while the hard carbon negative electrode sheet prepared in Comparative Example 1 has surface elements aggregated. This shows that the hard carbon negative electrode sheet and the preparation method thereof provided by the present invention can solve the problem of cobalt element aggregation in the existing cobalt-doped negative electrode sheet. (two)
[0100] The hard carbon negative electrode prepared in Example 1 was taken and subjected to X-ray diffraction analysis to obtain the following Figure 6 The XRD spectrum shown in FIG. 1 is obtained by taking another hard carbon negative electrode sheet prepared in Example 1, and observing the cobalt element form in the sample by transmission electron microscopy. The result is as follows Figure 7 shown. (three)
[0102] The sodium ion button batteries prepared in Examples 1-6 and Comparative Examples 1-2 were respectively taken and subjected to 0.05-2.0V charge and discharge tests at room temperature, wherein the current density was 25 mA / g, thereby obtaining the corresponding electrochemical performance parameters. The results are shown in Table 1 below:
[0103] Table 1 Electrochemical performance test results of different samples
[0104]
[0105] It can be seen from Table 1 above that the sodium ion button batteries prepared by using Examples 1 to 6 have more outstanding charge and discharge performance, and can still maintain better charge and discharge effects after hundreds or thousands of cycles, which means that their cycle performance is more stable. Therefore, the hard carbon negative electrode sheet for sodium ion batteries and the preparation method thereof proposed in the present invention can solve the problem of uneven distribution of doping elements in the prior art, which leads to unstable electrochemical performance.
[0106] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A hard carbon negative electrode material for a sodium ion battery, characterized in that: It comprises a precursor carbon sheet and a grid carbon sheet covered on the surface of the precursor carbon sheet, wherein the grid carbon sheet is penetrated by a plurality of grids; The grid is doped with cobalt material, and the cobalt material is bonded to the precursor carbon sheet or the grid carbon sheet through a covalent bond.
2. The hard carbon negative electrode material for sodium ion battery according to claim 1, characterized in that: The aperture of the grid is 15-50 μm, and the distance between two adjacent grids is 5-20 μm.
3. The hard carbon negative electrode material for sodium ion battery according to claim 1, characterized in that: The grid carbon sheet is prepared by machining nano-carbon materials, and the machining methods include but are not limited to weaving, winding, pressing or cutting.
4. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to any one of claims 1 to 3, characterized in that: The steps include: S1 pretreatment: pre-treating the biomass carbon material by heating and carbonizing it to obtain a precursor carbon material; S2: Slicing the precursor carbon material to make precursor carbon sheets; S3 structural treatment: a grid carbon sheet is coated on the surface of the precursor carbon sheet, and hot pressed to obtain a composite carbon sheet; S4 cobalt doping: placing the composite carbon sheet in a cobalt-doped mixed solution, heating, performing a hydrothermal reaction, and drying to obtain a doped carbon sheet; S5 forming process: sintering the doped carbon sheet to obtain the hard carbon negative electrode material for the sodium ion battery.
5. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 4, characterized in that: In step S1, the pretreatment temperature is 590-620°C and the pretreatment time is 3-10h; The carbonization temperature is 1600-1650°C, and the carbonization time is 5-15h.
6. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 4, characterized in that: In step S4, the cobalt-doped mixed solution includes cobalt salt, urea and water, and the cobalt salt includes one or more of cobalt chloride, cobalt nitrate, cobalt sulfate or cobalt acetate.
7. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 6, characterized in that: The temperature of the hydrothermal reaction is 200-220°C, and the hydrothermal reaction time is 3-10h.
8. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 4, characterized in that: In step S5, the sintering temperature is 440-480° C., and the sintering time is 2-5 hours.
9. A sodium ion battery prepared using the hard carbon negative electrode material for a sodium ion battery according to any one of claims 1 to 3, or a sodium ion battery prepared using the preparation method according to any one of claims 4 to 8.
10. The sodium ion battery according to claim 9, characterized in that: The invention comprises a positive electrode shell, a hard carbon negative electrode material for a sodium ion battery, a diaphragm, a metal sodium sheet, a gasket, a spring sheet and a negative electrode shell which are stacked layer by layer.