Electrolyte for improving high-temperature stability under high voltage and lithium secondary battery

By using a specific ratio of ether-containing spirocyclic compounds and tris(trimethylsilane)phosphate or borate in the lithium-ion battery electrolyte, an organic-inorganic composite interface film is formed, which solves the problem of high temperature problems in lithium-ion batteries under high voltage. The issue of circulation and storage performance has been achieved to reduce the internal resistance of the battery and improve the performance.

CN118782906APending Publication Date: 2024-10-15ZHEJIANG LANTIAN ENVIRONMENTAL PROTECTION HI TECH CO LTD +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202310348589.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

It is difficult with existing technology to simultaneously improve the high-temperature cycle performance and high-temperature storage performance of lithium-ion batteries at high voltages while reducing the internal resistance of the battery.

Method used

An electrolyte is used, which contains a main lithium salt, an organic solvent, a first additive (ether-containing spirocyclic compound) and a second additive (tris(trimethylsilane) phosphate or tris(trimethylsilane) borate). ), by adjusting its proportion in the electrolyte, it forms an organic-inorganic composite interface film of polyether segments and fluorophosphoric acid or borate, inhibiting side reactions, improving the cycle and storage performance of the battery under high temperature and high voltage, and at the same time reducing the battery's Internal resistance.

Benefits of technology

It significantly improves the high-temperature cycle performance and high-temperature storage performance of lithium-ion batteries under high voltage, while reducing the internal resistance of the battery, forming a more stable electrode interface, and enhancing the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782906A_ABST
    Figure CN118782906A_ABST
Patent Text Reader

Abstract

The invention discloses an electrolyte for improving high-temperature stability under high voltage and a lithium secondary battery, the electrolyte comprises a main lithium salt, an organic solvent and a first additive with a structure as shown in the following formula (I): # imgabs0 #, in the formula (I), R1, R2, R3 and R4 are independently selected from hydrogen, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl and cyano-substituted C1-C6 alkyl, and R2, R3 and R4 are independently selected from hydrogen, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl and cyano-substituted C1-C6 alkyl; and a second additive, wherein the second additive is TMSP and / or TMSB; the addition amounts of the first additive and the second additive respectively account for x% and y% of the total mass of the electrolyte, and meet the following relational expression: x / y is more than or equal to 0.2 and less than or equal to 4; 0.2 < = x + y < = 1.5; the organic solvent at least comprises cyclic carbonate, and the dosage of the organic solvent accounts for 10-30wt% of the total mass of the electrolyte. The electrolyte can improve the circulation and storage performance of the lithium ion battery at high temperature and high voltage, and can reduce the internal resistance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a lithium ion battery electrolyte, and in particular to an electrolyte for improving the high temperature stability of a lithium secondary battery under high voltage and a lithium secondary battery comprising the electrolyte. Background Art

[0002] Lithium-ion secondary batteries have a wide range of uses as power sources, especially in recent years as power sources for electric vehicles or consumer electronics, power storage, etc. With the continuous development of the above products, people have put forward higher requirements on the performance of lithium-ion secondary batteries.

[0003] In actual use, factors such as the heat generated by the equipment when working for a long time and the increase in ambient temperature cause lithium-ion secondary batteries to face high temperature conditions. As the temperature increases, the reaction activity of the electrodes and electrolytes increases, and the side reactions intensify, causing serious deterioration in battery performance. Therefore, effective technology is needed to improve the high-temperature stability of the battery under high voltage.

[0004] Literature (DOI: 10.1016 / j.jpowsour.2010.04.040) studies have shown that 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane can form a film on the negative electrode surface, enhance the high temperature stability of SEI, and effectively improve the capacity of the battery after high temperature storage, but the additive significantly increases the internal resistance of the positive and negative electrodes of the battery. At the same time, the present invention has been experimentally verified that ether-containing spiro compounds will significantly deteriorate the battery cycle stability in actual use.

[0005] In response to this problem, patent CN105655640A discloses the use of silicon-based sulfate to reduce the high impedance and cycle attenuation caused by 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane. Patent CN102640344A discloses the use of fluorophosphate or imide salt in combination with 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane to achieve the effect of improving battery cycle and storage performance. However, the present invention has been experimentally verified that as the battery charging cut-off voltage increases, the above scheme has a very limited effect on reducing the internal resistance of the battery.

[0006] Therefore, it is found through research that the above scheme still cannot simultaneously meet the requirements of high-temperature cycle performance, high-temperature storage performance and reducing internal resistance of the battery under high voltage. Summary of the invention

[0007] In order to solve the above technical problems, the present invention discloses an electrolyte and a lithium secondary battery which improve the high temperature cycle performance and high temperature storage performance of the battery under high voltage and reduce the internal resistance of the battery.

[0008] The objective of the present invention is achieved through the following technical solutions:

[0009] An electrolyte for improving high temperature stability under high voltage, comprising a main lithium salt and an organic solvent, the electrolyte further comprising:

[0010] The first additive is an ether-containing spirocyclic compound having a structure shown in the following formula (I):

[0011]

[0012] In formula (I), R1, R2, R3, and R4 are independently selected from hydrogen, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, or C1-C6 alkyl substituted with cyano;

[0013] and a second additive, wherein the second additive is tris(trimethylsilyl)phosphate (TMSP) and / or tris(trimethylsilyl)borate (TMSB);

[0014] The addition amounts of the first additive and the second additive account for x% and y% of the total mass of the electrolyte respectively, and meet the following relationship:

[0015] 0.2≤x / y≤4;

[0016] 0.2≤x+y≤1.5;

[0017] The organic solvent includes cyclic carbonate, and the amount used accounts for 10-30wt% of the total mass of the electrolyte.

[0018] Further, in formula (I), R1, R2, R3, and R4 are independently selected from hydrogen, C1-C3 alkyl, C2-C3 alkenyl, C2-C3 alkynyl, and cyano-substituted C1-C2 alkyl;

[0019] The addition amounts of the first additive and the second additive meet the following relationship:

[0020] 0.05≤x≤1;

[0021] 0.05≤y≤1;

[0022] The cyclic carbonate is selected from at least one of ethylene carbonate, propylene carbonate, butylene carbonate and fluoroethylene carbonate.

[0023] Furthermore, in formula (I), R1, R2, R3, and R4 are independently selected from hydrogen, methyl, ethyl, vinyl, vinylidene, isopropenyl, ethynyl, cyanomethyl, or cyanoethyl;

[0024] The addition amounts of the first additive and the second additive meet the following relationship:

[0025] 0.4≤x / y≤3;

[0026] 0.4≤x+y≤1;

[0027] The cyclic carbonate includes at least one of ethylene carbonate, propylene carbonate or fluoroethylene carbonate.

[0028] More preferably, the addition amounts of the first additive and the second additive conform to the following relationship:

[0029] 0.2≤x≤0.6;

[0030] 0.2≤y≤0.6.

[0031] The first additive is selected from at least one ether-containing spirocyclic compound represented by the following structure:

[0032]

[0033] In the electrolyte of the present invention, by using the first additive and the second additive in combination and adjusting the dosage ratio of the two, a film can be formed at the battery electrode interface, the occurrence of side reactions can be inhibited, the cycle and storage performance of the battery under high temperature and high voltage can be improved, and the internal resistance of the battery can be reduced. When the dosage ratio of the two does not meet the above conditions, the electrochemical performance of the lithium ion battery cannot be effectively improved, and even the battery performance deteriorates.

[0034] It is generally believed that the film-forming mechanism of additives is to have a reduction reaction before the solvent. However, the present invention has found through research that the film-forming mechanism of the first additive and the second additive is different from that of conventional film-forming additives. The additives themselves do not directly participate in the electrochemical reaction, but polymerize on the electrode surface by capturing the free radicals decomposed from the cyclic carbonate solvent. The first additive and the second additive have a competitive relationship in the free radical capture reaction. Although the competitive reaction mechanism is not clear, the ratio of the two additives affects their competitive relationship and thus significantly affects the battery performance.

[0035] After further research and analysis, in the electrolyte of the present invention, the ratio of the content of the first additive to the second additive is between 0.2 and 4, preferably between 0.4 and 3.0. Once the ratio of the content of the first additive to the second additive is too small (such as less than 0.2), the amount of the second additive is much more than the first additive, so that the competitive reaction of the second additive is strong, resulting in the first additive not being able to participate well in the film-forming reaction, and the battery volume expansion increases; once the ratio of the content of the first additive to the second additive is too large (such as greater than 4), the amount of the first additive is much more than the second additive, so that the competitive reaction of the first additive is strong, resulting in the second compound not being able to participate well in the reaction, resulting in an increase in the internal resistance of the battery and deterioration in the cycle performance.

[0036] Under the premise of a reasonable competitive relationship between the first additive and the second additive, the dosage of the first additive and the second additive also has requirements. When the sum of the contents of the first additive and the second additive is between 0.2 and 1.5, preferably between 0.4 and 1.0, the two can form an organic-inorganic composite interface film of polyether segments and fluorophosphate or borate on the surface of the positive and negative electrodes. Once the sum of the contents of the two is too small (such as less than 0.2), the content of the additive participating in the interfacial film-forming reaction is too low, and a good interfacial protective layer cannot be formed, and the battery performance is not significantly improved; once the sum of the contents of the two is too large (such as greater than 1.5), the additive cannot be completely consumed in the initial stage of battery formation, and the additive film-forming reaction that continues to occur during the subsequent charge and discharge cycles causes the interfacial impedance to continue to increase, resulting in a significant deterioration in the battery cycle performance.

[0037] After meeting the above-mentioned specific content ratio between the first additive and the second additive, the respective amounts of the first additive and the second additive must still meet the following requirements, namely:

[0038] 0.05≤x≤1; preferably 0.1≤x≤0.8, more preferably 0.2≤x≤0.6. If the amount of the first additive added is too low (such as less than 0.05), the film-forming effect is poor and the high-temperature performance of the battery cannot be improved; if the amount of the first additive added is too high (such as higher than 1), the internal resistance of the battery increases and the battery performance deteriorates.

[0039] 0.05≤y≤1; preferably 0.1≤y≤0.8, more preferably 0.2≤x≤0.6. If the amount of the second additive added is too low (such as less than 0.05), the internal resistance of the battery cannot be effectively reduced; if the amount of the second additive added is too high (such as greater than 1), the battery volume expands too much and the performance deteriorates.

[0040] According to the electrolyte for improving high temperature stability under high voltage of the present invention, the main lithium salt can be a lithium salt commonly used in the electrolyte. Preferably, the main lithium salt is selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(fluorosulfonyl)imide or lithium bis(trifluoromethylsulfonyl)imide, and the mass concentration in the electrolyte is 8-20%;

[0041] More preferably, the main lithium salt is selected from lithium hexafluorophosphate and / or lithium bis(fluorosulfonyl)imide, and the mass concentration of the main lithium salt in the electrolyte is 10-15%.

[0042] In the electrolyte of the present invention, the organic solvent includes at least cyclic carbonate, especially at least one of ethylene carbonate, propylene carbonate or fluoroethylene carbonate, so as to provide free radicals that can be captured by the first additive and the second additive.

[0043] In addition, the organic solvent further comprises linear carbonate and / or linear carboxylic acid ester, wherein the linear carbonate is selected from at least one of dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl trifluoroethyl carbonate, methyl difluoroethyl carbonate or di(2,2,2-trifluoroethyl) carbonate; preferably at least one of dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate or ethyl propyl carbonate;

[0044] The linear carboxylic acid ester is selected from at least one of methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, propyl propionate, ethyl 2,2-difluoroacetate, ethyl 2,2,2-trifluoroacetate, ethyl 2,2-difluoropropionate or propyl 2,2-difluoropropionate; preferably at least one of methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate or propyl propionate;

[0045] The amount of the linear carbonate and / or linear carboxylate is 50-70 wt % of the total mass of the electrolyte.

[0046] In the actual electrolyte formulation application process, the electrolyte formulation is a complex multi-component system to obtain a lithium secondary battery with more suitable comprehensive performance. Therefore, the electrolyte also includes a basic additive, and the basic additive is selected from a carbon-carbon double bond cyclic carbonate, a sultone compound, a cyclic sulfate, a lithium difluorophosphate, a lithium tetrafluoroborate, a lithium bisoxalate borate, a lithium difluorooxalate borate, a lithium difluorobisoxalate phosphate, a lithium oxalate tetrafluorophosphate, a succinonitrile, a glutaronitrile, adiponectin, trans-butenedinitrile, trans-hexenedinitrile, 1,2-bis(cyanoethoxy)ethane, 1,3,6-hexanetricarbonitrile or 1,2,3-tri(cyanoethoxy)propane. At least one of the addition amount of any basic additive accounts for 0.1 to 5.0 wt% of the total mass of the electrolyte; preferably, the addition amount of any basic additive accounts for 0.2 to 3.0 wt% of the total mass of the electrolyte.

[0047] In a specific embodiment, the basic additive is 1,3-propane sultone and lithium difluorophosphate, and the amount of any one of them is 0.2-3.0wt% of the total mass of the electrolyte. By combining with the first additive and the second additive, the high temperature stability of the lithium secondary battery at high voltage is significantly improved, thereby improving the high temperature cycle performance and high temperature storage performance of the battery, and reducing the internal resistance of the battery.

[0048] In another specific embodiment, the base additive is vinyl sulfate, and its usage accounts for 0.1-5.0wt% of the total mass of the electrolyte, preferably 0.2-3.0wt%. By combining the first additive, the second additive and vinyl sulfate, the rate and low-temperature discharge performance of the battery are further improved.

[0049] The present invention also provides a lithium ion secondary battery, which comprises a positive electrode, a negative electrode, a separator and any one of the above-mentioned electrolytes.

[0050] The active material of the positive electrode is selected from nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, lithium cobalt oxide material or lithium iron phosphate material. The active material of the negative electrode is selected from graphite, silicon carbon, silicon oxide, silicon, tin, metal lithium or a composite material thereof.

[0051] The working voltage of the lithium ion secondary battery is ≥4.3 V, preferably ≥4.35 V. Under the aforementioned high voltage, the electrolyte of the present invention can exert more significant advantages.

[0052] Compared with the prior art, the present invention has the following beneficial effects:

[0053] The electrolyte of the present invention forms an organic-inorganic composite interface film of polyether segments and fluorophosphate borate on the surfaces of the positive and negative electrodes through a competitive relationship between the first additive and the second additive on the basis of a specific ratio and specific respective contents, thereby improving the high-temperature cycle performance and high-temperature storage performance of the lithium secondary battery under high voltage, while reducing the internal resistance of the battery. DETAILED DESCRIPTION

[0054] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited to these specific embodiments. Those skilled in the art should recognize that the present invention covers all possible alternatives, improvements and equivalents within the scope of the claims.

[0055] 1. Preparation of electrolyte

[0056] (1) Preparation of lithium cobalt oxide based electrolyte:

[0057] In a glove box filled with argon (water content <5ppm, oxygen content <10ppm), ethylene carbonate (EC), propylene carbonate (PC), fluoroethylene carbonate (FEC), propyl propionate (PP), and diethyl carbonate (DEC) are mixed in a mass ratio of 10:10:10:40:30 to form an organic solvent. Based on the total mass of the electrolyte, 14% by mass of lithium hexafluorophosphate, 1% by mass of 1,3-propane sultone, and 0.5% by mass of lithium difluorophosphate are added, and the electrolyte is used as a lithium cobalt oxide based electrolyte.

[0058] According to the formula in Table 1 below, the first additive and the second additive are quantitatively added to the basic electrolyte and mixed evenly to form an electrolyte:

[0059] Table 1 Lithium cobalt oxide electrolyte formula

[0060]

[0061]

[0062] Note: After the dosage of additives is adjusted, only the dosage of solvent is adjusted in the basic electrolyte formula, and the distribution ratio of each group in the solvent remains unchanged.

[0063] According to the formula in Table 2 below, vinyl sulfate (DTD), the first additive and the second additive are quantitatively added to the lithium cobalt oxide base electrolyte and mixed evenly to form an electrolyte:

[0064] Table 2 Lithium cobalt oxide electrolyte formula

[0065]

[0066] (2) Preparation of nickel-cobalt-manganese ternary material basic electrolyte:

[0067] In a glove box filled with argon (water content <5ppm, oxygen content <10ppm), ethylene carbonate (EC), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a mass ratio of 25:5:50:20 to form an organic solvent. Based on the total mass of the electrolyte, 14% by mass of lithium hexafluorophosphate, 1% by mass of 1,3-propane sultone, and 0.5% by mass of lithium difluorophosphate are added, and the electrolyte is used as a basic electrolyte for nickel-cobalt-manganese ternary materials.

[0068] According to the formula in Table 3 below, the first additive and the second additive are quantitatively added to the basic electrolyte and mixed evenly to form an electrolyte:

[0069] Table 3 Nickel-cobalt-manganese ternary material electrolyte formula

[0070]

[0071]

[0072] 2. Battery production and performance testing

[0073] The electrolytes prepared in the above embodiments and comparative examples of the present invention are test electrolyte formulas, not commercial battery electrolytes. In the actual lithium secondary battery electrolyte preparation process, corresponding solvents and additives need to be added according to different battery systems. The test electrolyte formula of the present invention maintains the same gain effect on improving the electrochemical performance of the battery in the lithium cobalt oxide-graphite battery system, or the lithium cobalt oxide-silicon carbon battery system, or the nickel cobalt manganese ternary material-graphite system, or the nickel cobalt manganese ternary material-silicon carbon system. The specific operation is as follows:

[0074] The electrolytes obtained in the above examples and comparative examples were respectively made into lithium-ion power batteries with a soft-pack capacity of 1000 mAh, wherein the lithium-ion power batteries comprise a positive electrode sheet, a negative electrode sheet, a separator, an electrolyte and battery auxiliary materials.

[0075] The preparation process is as follows: the positive electrode sheet, the separator and the negative electrode sheet are wound together into a core, which is sealed with an aluminum-plastic film and then baked so that the moisture content of the electrode meets the requirements. After baking, the battery cell is injected with electrolyte, and the finished soft-pack battery cell is obtained through the steps of standing, forming, capacity separation and aging.

[0076] The various properties of the prepared lithium-ion power battery are tested, including:

[0077] (1) Cyclic performance test

[0078] At a specified temperature, charge at a constant current of 1C to the charge cut-off voltage, then charge at a constant voltage until the current drops to 0.1C, then discharge at a constant current of 1C to the cut-off voltage. Repeat this cycle for a specific number of weeks, record the discharge capacity of the first week and the discharge capacity of the last week, and calculate the capacity retention rate of the battery cycle according to the following formula:

[0079] Capacity retention rate = discharge capacity in the last week / discharge capacity in the first week*100%.

[0080] (2) High temperature storage performance test

[0081] At room temperature, the battery was charged at a constant current of 1C to the charge cut-off voltage, and then charged at a constant voltage until the current dropped to 0.1C, and then placed in a 60°C constant temperature oven for 28 days. When the battery after storage cooled to room temperature, the initial volume and the volume after storage were recorded:

[0082] Volume expansion ratio = (volume after storage - volume before storage) / volume before storage * 100%.

[0083] (3) Low temperature discharge performance test

[0084] At room temperature, charge at a constant current of 1C to the charging cut-off voltage, then charge at a constant voltage until the current drops to 0.1C, then discharge at a constant current of 1C to the cut-off voltage V, and record the discharge capacity; repeat the above charging process, then discharge at a constant current of 1C to the cut-off voltage V at low temperature, record the discharge capacity, and calculate the low-temperature discharge performance of the battery according to the following formula:

[0085] Low temperature discharge rate = low temperature discharge capacity / normal temperature discharge capacity * 100%.

[0086] (4) Rate charging performance test

[0087] At room temperature, the battery is charged at a constant current with a specified current to the charging cut-off voltage, and then charged at a constant voltage until the current drops to 0.1C. The total charging capacity and the charging capacity in the constant current stage are recorded, and the constant current charging ratio of the battery is calculated as follows:

[0088] Constant current charging ratio = constant current charging capacity / total charging capacity*100%.

[0089] Finally, the test results were based on the value of comparative example 1 set as 100% to obtain relative values. The specific test results are shown in Table 4, Table 5, and Table 6 below:

[0090] Table 4 LCO / / AG-3.0-4.5V electrochemical test results

[0091]

[0092]

[0093] Table 5 LCO / / AG-3.0-4.5V electrochemical test results

[0094]

[0095] According to the data in Table 4 above, it can be seen from the comparison of Comparative Examples 1 to 5 that the use of the first additive alone can inhibit the volume expansion of the battery under high temperature storage, but it is not good for the high temperature cycle performance and causes the internal resistance of the battery to increase. Comparison of Comparative Examples 1 and 6 to 9 shows that the use of the second additive alone has poor ability to inhibit the volume expansion of the battery under high temperature storage, and its advantage is to reduce the internal resistance of the battery. It can be seen from Examples 1 to 14 and Comparative Examples 1 to 9 that the high temperature performance of the battery under high voltage is effectively improved by the combination of the first additive and the second additive, and the battery has a lower internal resistance.

[0096] Further comparison of Examples 1 to 14 with Comparative Examples 1 and 10 to 13 shows that when 0.2≤x / y≤4; 0.2≤x+y≤1.5; 0.05≤x≤1 and 0.05≤y≤1 are satisfied, the high temperature performance of the battery under high voltage is effectively improved, and the battery has a lower internal resistance; when the above conditions cannot be met at the same time, the above battery performance cannot be improved. It is speculated that the possible reason is that the first additive and the second additive can compete with the free radicals at the negative electrode for polymerization, and the generated interface is composed of fluorophosphate or fluoroborate and polyorthoester, which has good stability, ion permeability and electronic isolation ability, and can inhibit further decomposition of the solvent. As the voltage increases, the first additive and the second additive are oxidized at high voltage before the solvent, generating a composite interface layer with high temperature stability, inhibiting the side reaction of the solvent at the positive electrode, thereby improving the high temperature and high pressure stability of the battery. When the content of the first additive and the second additive is too low, the additives are completely consumed at the negative electrode, resulting in insufficient protection of the positive electrode interface, and the battery's high temperature and high voltage performance cannot be improved; when the content of the first additive and the second additive is too high, the additives continue to decompose at the positive electrode to form a thick interface layer, which increases the internal resistance of the battery and deteriorates the battery cycle performance. In addition, the trimethylsilyl group in the second additive will generate trimethylsilyl fluoride, which is a gas, resulting in increased gas production by the battery. By comparing Examples 1 to 14 with Comparative Examples 1, 14, and 15, it can be seen that when 0.05≤x≤1 or 0.05≤y≤1 is not satisfied, it is impossible to achieve an improvement in the high temperature performance of the battery at high voltage and reduce the internal resistance of the battery.

[0097] According to the data in Table 5 above, by comparing Examples 9 and 26 to 32, it can be seen that the first additive, the second additive and DTD are further used in combination, and the low-temperature discharge performance and rate charging performance of the battery are further improved. It is speculated that the possible reason is that DTD can form an interface layer containing lithium sulfate and lithium sulfate ester, further improving the electronic insulation ability of the negative electrode interface, inhibiting the negative electrode interface side reaction, and improving the interface stability. In addition, lithium sulfate and lithium sulfate ester have good lithium ion conductivity, reducing the resistance to lithium ion migration, thereby achieving the improvement of fast charging and low temperature performance.

[0098] Table 6 NCM622 / / AG-2.8-4.4V electrochemical test results

[0099]

[0100]

[0101] According to the data in Table 6 above, it can be seen that the gain effect brought by the first additive and the second additive of the present invention when satisfying 0.2≤x / y≤4; 0.2≤x+y≤1.5; 0.05≤x≤1 and 0.05≤y≤1 is also applicable to the nickel-cobalt-manganese ternary material NCM622 / / AG system, that is, the electrolyte of the present invention is not limited to the battery material system, and after adjusting the appropriate solvents and additives for different systems, the electrochemical performance of the battery can be improved.

Claims

1. An electrolyte for improving high temperature stability under high voltage, comprising a main lithium salt and an organic solvent, characterized in that: The electrolyte further comprises: The first additive is an ether-containing spirocyclic compound having a structure shown in the following formula (I): In formula (I), R1, R2, R3, and R4 are independently selected from hydrogen, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, or C1-C6 alkyl substituted with cyano; and a second additive, wherein the second additive is tris(trimethylsilyl)phosphate and / or tris(trimethylsilyl)borate; The addition amounts of the first additive and the second additive account for x% and y% of the total mass of the electrolyte respectively, and meet the following relationship: 0.2≤x / y≤4; 0.2≤x+y≤1.5; The organic solvent includes cyclic carbonate, and the amount used accounts for 10-30wt% of the total mass of the electrolyte.

2. The electrolyte according to claim 1, characterized in that: In formula (I), R1, R2, R3, and R4 are independently selected from hydrogen, C1-C3 alkyl, C2-C3 alkenyl, C2-C3 alkynyl, or C1-C3 alkyl substituted with cyano; The addition amounts of the first additive and the second additive meet the following relationship: 0.05≤x≤1; 0.05≤y≤1; The cyclic carbonate is selected from at least one of ethylene carbonate, propylene carbonate, butylene carbonate and fluoroethylene carbonate.

3. The electrolyte according to claim 1 or 2, characterized in that: In formula (I), R1, R2, R3, and R4 are independently selected from hydrogen, methyl, ethyl, vinyl, vinylidene, isopropenyl, ethynyl, cyanomethyl, or cyanoethyl; The addition amounts of the first additive and the second additive meet the following relationship: 0.4≤x / y≤3; 0.4≤x+y≤1; The cyclic carbonate includes at least one of ethylene carbonate, propylene carbonate or fluoroethylene carbonate.

4. The electrolyte according to claim 3, characterized in that: The addition amounts of the first additive and the second additive meet the following relationship: 0.2≤x≤0.6; 0.2≤y≤0.6。 5. The electrolyte according to claim 4, characterized in that: The first additive is selected from at least one ether-containing spiro compound represented by the following structure:

6. The electrolyte according to any one of claims 1 to 5, characterized in that: The main lithium salt is selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethylsulfonyl)imide, and its mass concentration in the electrolyte is 8-20%.

7. The electrolyte according to any one of claims 1 to 5, characterized in that: The organic solvent further comprises a linear carbonate and / or a linear carboxylate, wherein the linear carbonate is selected from at least one of dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl trifluoroethyl carbonate, methyl difluoroethyl carbonate or di(2,2,2-trifluoroethyl) carbonate; The linear carboxylic acid ester is selected from at least one of methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, propyl propionate, ethyl 2,2-difluoroacetate, ethyl 2,2,2-trifluoroacetate, ethyl 2,2-difluoropropionate or propyl 2,2-difluoropropionate; The amount of the linear carbonate and / or linear carboxylate is 50-70 wt % of the total mass of the electrolyte.

8. The electrolyte according to any one of claims 1 to 7, characterized in that: The electrolyte further includes a basic additive, which is selected from at least one of cyclic carbonates with carbon-carbon double bonds, sultone compounds, cyclic sulfates, lithium difluorophosphate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorobis(oxalatophosphate), lithium oxalatetetrafluorophosphate, succinonitrile, glutaronitrile, adiponitrile, trans-butenedinitrile, trans-hexenedinitrile, 1,2-bis(cyanoethoxy)ethane, 1,3,6-hexanetricarbonitrile or 1,2,3-tri(cyanoethoxy)propane, and the addition amount of any basic additive accounts for 0.1 to 5.0 wt% of the total mass of the electrolyte.

9. The electrolyte according to claim 8, characterized in that: The basic additive is selected from at least one of vinylene carbonate, 1,3-propane sultone, lithium difluorophosphate, lithium difluorooxalatoborate or vinyl sulfate, and the amount used accounts for 0.2-3.0wt% of the total mass of the electrolyte.

10. A lithium ion secondary battery comprising a positive electrode, a negative electrode and a separator, characterized in that: The lithium-ion secondary battery further comprises the electrolyte according to any one of claims 1-9.

11. The lithium ion secondary battery according to claim 10, characterized in that: The operating voltage of the lithium-ion secondary battery is ≥4.3V.

Citation Information

Cited By

  • Non-aqueous electrolyte and lithium ion battery

    CN119069810A

  • Non-aqueous electrolyte and lithium ion battery

    CN119069810B

  • Lithium ion battery and electric device thereof

    CN122619945A