Polyolefin-based film, laminate, packaging material, and bale

By optimizing the dynamic viscoelastic properties and heat treatment technology in polyolefin films, the problem of insufficient thermal stability of polypropylene films during heat sterilization is solved, and the effect of improving the thermal stability and barrier properties of the film is achieved.

CN118786033AActive Publication Date: 2024-10-15TORAY INDUSTRIES INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202280092912.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2022-12-19
Publication Date
2024-10-15
Estimated Expiration
2042-12-19

AI Technical Summary

Technical Problem

The existing polypropylene film has insufficient thermal stability during heat sterilization, resulting in pinholes and cracks in the evaporated layer, and reduced water vapor and oxygen barrier properties.

Method used

The storage modulus ratio E'121/E'50 in the main orientation axis direction at 50°C and 121°C obtained by dynamic viscoelasticity measurement at a frequency of 10 Hz is set to exceed 0.25 and not exceed 0.99, and at 150°C The thermal shrinkage rate in the direction of the main orientation axis is controlled between -2% and 10%. The polyolefin film is prepared by combining biaxial stretching and heat treatment technology to improve its thermal stability and barrier properties.

Benefits of technology

It effectively reduces the reduction in structural stability, water vapor and oxygen barrier properties caused by heating, and improves the thermal stability and barrier properties of polyolefin films, making them suitable for high-temperature environments and packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005019021570000451
    Figure BDA0005019021570000451
  • Figure BDA0005019021570000461
    Figure BDA0005019021570000461
  • Figure HDA0005019021580000011
    Figure HDA0005019021580000011
Patent Text Reader

Abstract

The present invention addresses the problem of providing a polyolefin-based film which, for example, has excellent structural stability with respect to heat during vapor deposition when used in packaging applications, and which has good water vapor barrier properties and oxygen barrier properties with respect to heat during heat sterilization treatment. The present invention relates to a polyolefin-based film and a method for manufacturing the same. When the storage moduli in the main orientation axis direction at 50 DEG C and 121 DEG C as determined by dynamic viscoelasticity measurement at a frequency of 10 Hz are E '50 (Pa) and E' 121 (Pa), respectively, E '121 / E' 50 is more than 0.25 and 0.99 or less, the thermal shrinkage in the main orientation axis direction at 150 DEG C is-2% to 10% (inclusive), the tensile elongation in the direction orthogonal to the main orientation axis is 20% to 300% (inclusive), and the tensile elongation in the direction orthogonal to the main orientation axis is 10% to 30% (inclusive). And at least one layer (layer A) containing a cyclic olefin-based resin and a polypropylene-based resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyolefin film, a laminate, a packaging material and a package which are particularly suitable for packaging applications. Background Art

[0002] Since polypropylene film has excellent transparency, mechanical properties, electrical properties, etc., it is used for various purposes such as packaging, tape, cable packaging, and electrical insulation represented by capacitors. Among them, in packaging applications, laminated films formed by evaporating a thin film of aluminum (hereinafter, sometimes referred to as "Al") on a polypropylene film have been widely used. However, the film obtained by Al evaporation is not transparent and is therefore not suitable for applications that require visibility of the contents. In addition, in recent years, people are actively carrying out activities to recycle plastics for packaging, but films containing Al evaporation layers also have the problem of insufficient recyclability.

[0003] According to the above situation, there is a trend to replace the previous Al vapor-deposited layer with a transparent vapor-deposited layer such as aluminum oxide (hereinafter, sometimes referred to as AlOx) or silicon oxide. When these transparent vapor-deposited layers are used, the transparency and recyclability of the packaging material can be improved. However, the transparent vapor-deposited layer is usually thinner and more brittle than the Al vapor-deposited layer, so during the formation of the vapor-deposited layer or in subsequent processes such as bag making, defects such as pinholes and cracks will be generated in the vapor-deposited layer, and there is a problem that the water vapor barrier and oxygen barrier properties are easily damaged. In addition, when polypropylene film is used for food packaging purposes, heat sterilization treatment (boiling, semi-boiling, steaming, etc.) is sometimes implemented, but polypropylene film generally has poor thermal dimensional stability compared with polyester film, so the heat during the heat sterilization treatment will cause the film to deform, and defects such as pinholes and cracks will be generated in the vapor-deposited layer. As a result, there is also a problem that the water vapor barrier and oxygen barrier properties are easily damaged.

[0004] As a film with improved thermal dimensional stability of polypropylene film, a film made by blending a cyclic olefin resin having a glass transition temperature of 120 to 170°C and polypropylene, or a laminated film provided with polypropylene layers on both sides of the cyclic olefin resin layer, has been proposed in the past, thereby improving heat resistance and being suitable for capacitor films that can exhibit withstand voltage even at high temperatures (Patent Documents 1 and 2). Similarly, a film suitable for packaging material use that has high barrier properties, strength suitable for processing, and transparency by providing polypropylene layers on both sides of a resin layer made by blending a cyclic olefin resin and polypropylene has also been proposed (Patent Documents 3 and 4).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application No. 2020-521867

[0008] Patent Document 2: Japanese Patent Application Publication No. 2018-34510

[0009] Patent Document 3: Japanese Patent Application Laid-Open No. 9-272188

[0010] Patent Document 4: Japanese Patent Application No. 2005-535481 Summary of the invention

[0011] Problems to be solved by the invention

[0012] However, the polypropylene film described in Patent Document 1 improves heat resistance by blending cyclic olefin resin with polypropylene resin, but the area stretching ratio during film making is small, the molecular chain of polypropylene resin is insufficiently elongated, and the thermal stability needs to be improved. In addition, the film of Patent Document 2 uses cyclic olefin monomer as the inner layer, so like the polypropylene film described in Patent Document 1, the area stretching ratio during film making is small, the molecular chain of polypropylene resin is insufficiently elongated, and the thermal stability needs to be improved.

[0013] The film of Patent Document 3 suitable for packaging purposes is a film in which a cyclic olefin resin and a polypropylene resin are blended and biaxially stretched, but the cyclic olefin resin in the film is insufficiently thermally fixed after dispersion and stretching, resulting in a problem of poor thermal dimensional stability. The film of Patent Document 4 is a blended film of a cyclic olefin resin and a polypropylene resin, but there is no concept of stretching and the thermal stability is insufficient. Therefore, the films of Patent Documents 3 and 4 have the following problems, that is, the film is deformed due to the heat during the heat sterilization treatment, so that defects such as pinholes and cracks are easily generated in the vapor deposition layer, and the water vapor barrier and oxygen barrier properties are reduced.

[0014] Therefore, an object of the present invention is to provide a polyolefin-based film capable of reducing the decrease in structural stability, water vapor barrier properties, and oxygen barrier properties associated with heating.

[0015] Means of solving the problem

[0016] In order to solve the above-mentioned problems, the present inventors have repeatedly conducted in-depth studies and invented the following first polyolefin film of the present invention and the second polyolefin film of the present invention. The first polyolefin film of the present invention is characterized in that when the storage modulus in the main orientation axis direction at 50°C and 121°C obtained by dynamic viscoelasticity measurement at a frequency of 10 Hz is set to E'50 (Pa) and E'121 (Pa), respectively, E'121 / E'50 exceeds 0.25 and is 0.99 or less, the heat shrinkage in the main orientation axis direction at 150°C is -2% or more and 10% or less, the tensile elongation in the direction orthogonal to the main orientation axis is 20% or more and 300% or less, and has at least one layer (A layer) containing a cyclic olefin resin and a polypropylene resin.

[0017] The second polyolefin film of the present invention has at least one layer (A layer) containing a cyclic olefin resin and a polypropylene resin. When the cross section of the A layer when cut by a plane parallel to the main orientation axis direction and the thickness direction is set as the cross section X, in the rectangle of 1 μm×2 μm size determined in the cross section X in such a way that a pair of short sides are parallel to the thickness direction, there are more than two regions of the cyclic olefin resin passing through the pair of short sides. When the storage modulus in the main orientation axis direction at 50°C and 121°C obtained by the dynamic viscoelasticity measurement at a frequency of 10 Hz is set as E'50 (Pa) and E'121 (Pa), respectively, E'121 / E'50 exceeds 0.20 and is less than 0.99.

[0018] Effects of the Invention

[0019] According to the present invention, a polyolefin-based film can be obtained in which the decrease in structural stability, water vapor barrier properties, and oxygen barrier properties caused by heating can be alleviated. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The schematic diagram shows a rectangle of 1 μm×2 μm defined with a pair of sides parallel to the thickness direction in a cross section X of a polyolefin film according to an embodiment of the present invention, and a region of cyclic olefin resin passing through the pair of sides of the rectangle parallel to the thickness direction.

[0021] Figure 2 This is an enlarged photograph (magnification 2,000 times) of a cross section X of a polyolefin film according to one embodiment (the embodiments of Example 1 and Example 2) of the present invention. DETAILED DESCRIPTION

[0022] Hereinafter, the first and second polyolefin-based films of the present invention are described in detail. Below about preferred range, under the situation of recording upper limit and lower limit respectively, its combination can be arbitrary. In addition, sometimes the first and second polyolefin-based films of the present invention are collectively referred to as the present invention or the polyolefin-based films of the present invention.

[0023] In addition, in this specification, the polyolefin film is sometimes referred to as film below. In addition, in the polyolefin film of the present invention, the "thickness direction" refers to the direction perpendicular to the film surface. The "length direction" refers to the direction corresponding to the flow direction in the film manufacturing process (hereinafter, sometimes referred to as "MD"), and the "width direction" refers to the direction orthogonal to the flow direction in the above-mentioned film manufacturing process in the film surface (hereinafter, sometimes referred to as "TD"). When the film sample is in the shape of a roll, a roller, etc., the film winding direction can be said to be the length direction.

[0024] It should be noted that the polyolefin membrane of the present invention is not a microporous membrane and therefore does not have a large number of pores. That is, the polyolefin membrane of the present invention refers to a polyolefin membrane other than a microporous membrane. Here, the microporous membrane is defined as a membrane having a pore structure, the pore structure penetrating both surfaces of the membrane, and having an air permeability of 5000 seconds / 100 ml or less at 23°C and a relative humidity of 65% in terms of the permeation time of 100 ml of air using a B-type Gurley tester of JIS P 8117 (1998).

[0025] Furthermore, the polyolefin film refers to a sheet-like molded body containing more than 50% by mass and less than 100% by mass of a polyolefin resin when all the components constituting the film are regarded as 100% by mass. It should be noted that, when a plurality of polyolefin resins are included, the content of the polyolefin resin is calculated by adding up all the polyolefin resins.

[0026] The polyolefin resin refers to a resin containing more than 50 mol% and less than 100 mol% of olefin units when all structural units constituting the resin are regarded as 100 mol%. When multiple structural units corresponding to olefin units are contained, all olefin units are summed up as the olefin unit amount.

[0027] The polypropylene-based resin refers to a resin that does not belong to a cyclic olefin-based resin among resins that contain more than 50 mol% and 100 mol% or less of propylene units when all structural units constituting the resin are regarded as 100 mol%.

[0028] Cyclic olefin resin refers to a resin containing more than 10 mol% and less than 100 mol% of cyclic olefin units when all structural units constituting the resin are regarded as 100 mol%. It should be noted that when multiple structural units equivalent to cyclic olefin units are contained, all cyclic olefin units are summed up as the cyclic olefin unit amount.

[0029] In view of thermal stability, the first polyolefin film of the present invention is important in that when the storage modulus in the main orientation axis direction at 50°C and 121°C obtained by dynamic viscoelasticity measurement at a frequency of 10 Hz is set as E'50 (Pa) and E'121 (Pa), respectively, E'121 / E'50 exceeds 0.25 and is 0.99 or less. It should be noted that the method for measuring the storage modulus in the main orientation axis direction is described later.

[0030] The E'121 / E'50 of the polyolefin film is greater than 0.25, which means that the temperature dependence of the storage modulus is small, in other words, it means that the amorphous molecular chains in the film are difficult to move under high temperature environment. By making the E'121 / E'50 of the polyolefin film greater than 0.25, for example, when a layer (hereinafter referred to as the D layer) containing a total of more than 50% by mass and less than 100% by mass of metals and inorganic compounds is vapor-deposited on at least one surface of the film described later, the deformation of the film caused by the heat during vapor deposition and the defects such as pinholes and cracks generated in the D layer can be suppressed, so that the water vapor barrier and oxygen barrier properties of the laminate vapor-deposited with the D layer are good. In addition, the deformation of the film caused by high-temperature treatment such as heat sterilization after bag making can also be suppressed, so the reduction of water vapor barrier and oxygen barrier properties associated with such treatment can also be reduced. On the other hand, when the E'121 / E'50 of the film exceeds 0.99, sometimes the film breaks during film making and other poor productivity situations occur. This is because it is necessary to use a raw material with excessively high crystallinity and to perform biaxial stretching at a high area ratio during film formation.

[0031] From the above viewpoints, the film's E'121 / E'50 is preferably 0.28 or more, more preferably 0.31 or more, further preferably 0.33 or more, and particularly preferably 0.35 or more. On the other hand, the upper limit of E'121 / E'50 is preferably 0.89, more preferably 0.69.

[0032] In addition, in terms of thermal stability, when the storage modulus in the main orientation axis direction at 50°C and 121°C obtained by dynamic viscoelasticity measurement at a frequency of 10 Hz is set as E'50 (Pa) and E'121 (Pa), respectively, it is important that E'121 / E'50 exceeds 0.20 and is 0.99 or less. The E'121 / E'50 of the film is preferably greater than 0.25, more preferably 0.28 or more, further preferably 0.31 or more, further preferably 0.33 or more, and particularly preferably 0.35 or more. On the other hand, the upper limit of E'121 / E'50 is preferably 0.89, and more preferably 0.69.

[0033] In order to control the E'121 / E'50 of the first polyolefin film of the present invention to be more than 0.25 and less than 0.99, and the E'121 / E'50 of the second polyolefin film of the present invention to be more than 0.20 and less than 0.99, for example, a method of controlling the domain structure (sea-island structure) of layer A can be used. More specifically, as a raw material for layer A, it is effective to prepare a composite resin raw material obtained by pre-kneading a cyclic olefin resin and a polypropylene resin, melt-extrude the raw material to form a sheet after controlling the content of the cyclic olefin resin, and make the area stretch ratio 36.0 times or more (preferably 40.0 times or more) and make the preheating temperature before stretching in the width direction in biaxial stretching higher by 5°C to 15°C than the stretching temperature in the width direction.

[0034] It should be noted that, as an effect of pre-preparing the composite resin raw material, an effect of improving stretchability can be expected. This is because, compared with the case of only mixing the resins during film formation, the two resins can be mixed more evenly, so the resin that becomes the island component is finely dispersed in the resin that becomes the sea component. In addition, when the composite resin raw material pre-mixed with a twin-screw extruder in a manner that contains a cyclic olefin resin at a high concentration is diluted and used as a masterbatch, the dispersibility of the cyclic olefin resin becomes higher, so it is preferred.

[0035] The reason why E'121 / E'50 can be adjusted to the preferred range by the above method is considered to be that in the A layer, the peeling of the resin at the sea-island interface of the sea-island structure in which the polypropylene resin is regarded as the sea and the cyclic olefin resin is regarded as the island is suppressed, and the island structure becomes smaller or thinner. As a result, the mobility of the amorphous chains in the film can be suppressed due to the synergistic effect of the high thermal stability of the cyclic olefin resin and the excellent stretchability of the polypropylene resin.

[0036] It is important that the heat shrinkage rate of the first polyolefin film of the present invention in the main orientation axis direction at 150°C is -2% or more and 10% or less. By making the film satisfy the above conditions, for example, when the D layer described later is laminated by vapor deposition, it is possible to suppress defects such as pinholes and cracks in the D layer caused by film shrinkage due to the heat during vapor deposition, and the water vapor barrier and oxygen barrier properties of the laminate laminated with the D layer can be good. In addition, when a high-temperature treatment such as heat sterilization is performed after the bag making process, the film shrinkage can also be suppressed to prevent the water vapor barrier and oxygen barrier properties from being damaged. From the above aspects, the upper limit of the heat shrinkage rate in the main orientation axis direction at 150°C is preferably 8%, more preferably 6%, and further preferably 4%. On the other hand, the lower limit of the heat shrinkage rate in the main orientation axis direction at 150°C is preferably -1%. It should be noted that the heat shrinkage rate in the main orientation axis direction at 150°C can be measured by the method described later.

[0037] The main orientation axis direction in the present invention refers to the direction in which the molecules are most strongly oriented in the polyolefin film plane. Usually, when biaxial stretching is performed in the manufacture of polyolefin films, stretching is performed along the length direction and the width direction, but usually, the side with a larger stretching ratio becomes the main orientation axis direction. When the stretching direction (length direction and width direction) can be determined but the ratio is unknown, the maximum load until fracture can be measured in the tensile test described later, and the direction with a larger measured value is taken as the main orientation axis direction.

[0038] As mentioned above, if the stretching direction and stretching ratio are known, the main orientation axis direction can be easily determined. However, in the case of films where these are unclear, the main orientation axis direction can be determined by the following method. Specifically, prepare a film with any direction facing upward, cut into a rectangle with a length of 150 mm and a width of 10 mm as sample <1>, and define the direction of the long side of sample <1> as 0°. Next, collect sample <2> of the same size in such a way that the long side direction is rotated 15° to the right from the 0° direction. Similarly, rotate the long side direction of the rectangular sample 15° at a time, and collect the sample in the same manner. <3> ~ <12> Next, for each rectangular sample, the maximum load until fracture was measured in a tensile test described later, and the direction in which the measured value was the largest was defined as the main orientation axis direction.

[0039] In the case where a sample with a length of 150 mm and a width of 10 mm cannot be obtained and thus the tensile test described below cannot be performed, the crystal orientation of the α crystal (110) plane based on wide-angle X-rays is measured as follows, and the direction of the main orientation axis is determined based on the following judgment criteria. Specifically, X-rays (CuKα rays) are incident in a direction perpendicular to the film surface, and the crystal peak at 2θ = about 14° (α crystal (110) plane) is scanned in the circumferential direction, and the direction with the highest diffraction intensity in the obtained diffraction intensity distribution is taken as the direction of the main orientation axis.

[0040] There is no particular limitation on the method for making the thermal shrinkage rate of the film in the main orientation axis direction at 150°C satisfy a range of -2% to 10%. For example, it is effective to prepare a composite resin raw material obtained by pre-mixing a cyclic olefin resin and a polypropylene resin as the raw material for layer A, melt-extrude the raw material into sheets while controlling the content of the cyclic olefin resin, and make the preheating temperature before stretching in the width direction higher by 5°C to 15°C than the stretching temperature in the width direction while making the area stretching ratio in biaxial stretching 36.0 times or more (preferably 40.0 times or more).

[0041] It is important that the tensile elongation in the direction perpendicular to the main orientation axis of the first polyolefin film of the present invention is 20% or more and 300% or less. Here, the direction perpendicular to the main orientation axis refers to the direction perpendicular to the main orientation axis in the film surface. If the tensile elongation in the direction perpendicular to the main orientation axis of the film is 20% or more, the polyolefin film can be suppressed from breaking due to the tension during the vapor deposition process and transportation when used for packaging purposes, and the rupture can also be suppressed during the bag making process when the package is made. From the above aspects, the lower limit of the tensile elongation in the direction perpendicular to the main orientation axis is preferably 27%, and more preferably 35%. When the tensile elongation is 300% or less, the polyolefin film can be suppressed from deformation due to the tension during the vapor deposition process and transportation, and the deformation during the bag making process when the package is made can also be suppressed. On the other hand, the upper limit of the tensile elongation in the direction perpendicular to the main orientation axis is preferably 250%, more preferably 200%, further preferably 120%, and particularly preferably 60%. It should be noted that the tensile elongation herein refers to the tensile elongation measured at a tensile speed of 300 mm / min in an environment of 23° C. The tensile elongation can be measured using a known tensile tester, and the detailed procedure is described below.

[0042] There is no particular limitation on the method for making the tensile elongation in the direction perpendicular to the main orientation axis 20% or more and 300% or less, and an example thereof is to make a polyolefin film into a biaxially oriented film. On this basis, as the raw material for the A layer, it is also preferred to prepare a composite resin raw material obtained by pre-mixing a cyclic olefin resin and a polypropylene resin, and to melt extrude the composite resin raw material to form a sheet while controlling the content of the cyclic olefin resin.

[0043] From the perspective of improving thermal stability, it is important that the first and second polyolefin films of the present invention have at least one layer (layer A) containing a cyclic olefin resin and a polypropylene resin. By setting it in this way, the high thermal stability of the cyclic olefin resin and the excellent stretchability of the polypropylene resin are utilized, and the obtained polyolefin film has excellent thermal stability, for example, the laminated body with the vapor-deposited layer D described later has excellent barrier properties.

[0044] It should be noted that the polyolefin film of the present invention may be any of a single film structure consisting of only one A layer, a laminated structure formed by laminating a plurality of A layers in the thickness direction with a total of two or more layers, and a laminated structure formed by laminating an A layer and layers other than the A layer in the thickness direction with a total of two or more layers. However, from the perspective of exhibiting the stretchability of the film, excellent withstand voltage characteristics and reliability in a high temperature environment, and processability, when a layer having a polypropylene resin as a main component, containing more polypropylene resin than the A layer, and having a low content of cyclic olefin resin is used as the B layer, it is preferred to have the B layer.

[0045] As a specific embodiment of the laminated structure of the polyolefin film of the present invention, for example, a 2-layer structure of A layer / B layer, a 3-layer structure of B layer / A layer / B layer, and A layer / B layer / A layer, a 3-layer structure of B layer / A layer / C layer, and a 3-layer structure of A layer / B layer / C layer having a melting point lower than that of A layer and B layer and a melting point of 100°C or more and 150°C or less, and a structure of more than 4 layers with A layer as the inner layer of the film or the outermost layer of both surfaces of the film can be cited. From the perspective of the stability of the stretched film, a structure of B layer / A layer / B layer or B layer / A layer / C layer is preferred. Here, when the overall thickness of the film is regarded as 100%, the lower limit of the thickness of the A layer is preferably 10%, more preferably 35%, further preferably 60%, and particularly preferably 80%. The upper limit is set to 100% including a single layer. By setting the thickness of the A layer to be within the above range, the polyolefin film has a structure that is very stable to the heat during vapor deposition. Therefore, when the vapor-deposited layer and the later-described D layer are laminated to form a laminate, the water vapor barrier property and oxygen barrier property can be improved.

[0046] In addition, when the polyolefin film of the present invention has multiple A layers, the composition may be the same or different. As a laminating method, a feed block method based on coextrusion, a multi-manifold method, a coating method, etc. may be cited, and from the perspective of production efficiency and cost, a laminating method based on coextrusion (e.g., melt coextrusion) is preferred.

[0047] In the polyolefin film of the present invention, the lower limit of the content of cyclic olefin resin in the whole film is preferably 1 mass%, more preferably 2 mass%, and further preferably 3 mass%. On the other hand, the upper limit is preferably 39 mass%, more preferably 25 mass%, more preferably 19 mass%, further preferably 14 mass%, particularly preferably 9 mass%, and most preferably 7.5 mass%. In addition, the lower limit of the content of cyclic olefin resin in film A layer is preferably 1 mass%, more preferably 2 mass%. On the other hand, the upper limit is preferably 39 mass%, more preferably 25 mass%, more preferably 19 mass%, further preferably 14 mass%, particularly preferably 10 mass%, and most preferably 9 mass%. By making the content of cyclic olefin resin in the whole film and film A layer into a preferred range, the area ratio is increased during biaxial stretching, and the water vapor barrier and oxygen barrier properties of the laminate with D layer vapor-deposited on the film can be good.

[0048] In the second polyolefin film of the present invention, when the cross section when the above-mentioned A layer is cut by a surface parallel to the main orientation axis direction and the thickness direction is set as the cross section X, it is important that in the above-mentioned cross section X, in a rectangle of 1 μm×2 μm size determined in a manner that a pair of short sides are parallel to the thickness direction, there are more than 2 regions of the above-mentioned cyclic olefin resin passing through the above-mentioned pair of short sides. In the polyolefin film of the present invention, the region of the cyclic olefin resin passing through a pair of sides parallel to the thickness direction is preferably 4 or more, more preferably 6 or more. The upper limit is not particularly limited and is set to 100. It should be noted that it is preferred that the first polyolefin film of the present invention also satisfies this condition, and the preferred numerical range is the same.

[0049] It is believed that by making the area of ​​the cyclic olefin resin through a pair of sides parallel to the thickness direction more than 2, the cyclic olefin resin becomes a state of being more flat and micro-dispersed in the plane, and the high thermal stability of the cyclic olefin resin and the excellent stretchability of the polypropylene resin can suppress the mobility of the amorphous chain in the film. Therefore, for example, when the D layer described later is laminated by evaporation, the defects such as pinholes and cracks in the D layer caused by the film shrinkage caused by the heat during evaporation can be suppressed, and the water vapor barrier and oxygen barrier properties of the laminated body laminated with the D layer can be good. In addition, when a high temperature treatment such as heat sterilization is performed after the bag making process, the film shrinkage can also be suppressed to prevent the water vapor barrier and oxygen barrier properties from being damaged.

[0050] As a method for making the number of regions of the cyclic olefin resin passing through a pair of sides parallel to the thickness direction in the cross section X to be 2 or more, a method of controlling the regional structure (sea-island structure) of the A layer can be used. For example, as a raw material for the A layer, it is effective to prepare a composite resin raw material by pre-mixing a cyclic olefin resin and a polypropylene resin, melt-extrude it on the basis of controlling the content of the cyclic olefin resin to form a sheet, perform biaxial stretching at an area stretching ratio of 36.0 times or more (preferably 40.0 times or more), and perform heat treatment after biaxial stretching.

[0051] Hereinafter, in the polyolefin film of the present invention, a method for determining a rectangle of 1 μm×2 μm in size with a pair of sides parallel to the thickness direction in a cross section X, and a method for determining the number of regions of cyclic olefin resin with a pair of sides parallel to the thickness direction are described with reference to the accompanying drawings. Figure 1 The schematic diagram shows a rectangle of 1 μm×2 μm defined with a pair of sides parallel to the thickness direction in a cross section X of a polyolefin film according to an embodiment of the present invention, and a region of cyclic olefin resin passing through the pair of sides of the rectangle parallel to the thickness direction. Figure 1Symbols 1 to 5 in the figure respectively represent a part of the cross section X, a sea part, an island part (region), a rectangle of 1 μm×2 μm in cross section X with a pair of sides parallel to the thickness direction, and a pair of sides parallel to the thickness direction. Figure 1 The left figure is a part of the cross section X, and the right figure is an enlarged view of a rectangle indicated by a dotted line of a rectangle of 1 μm×2 μm size determined in a manner that a pair of sides are parallel to the thickness direction in the cross section X. It should be noted that in the polyolefin film of the present invention, the sea portion is a polypropylene resin, and the island portion is a cyclic olefin resin.

[0052] When a rectangle of 1 μm × 2 μm is determined in the section X so that a pair of sides are parallel to the thickness direction, the bottom side of the rectangle is set as the sea part, and when the area is located on the side opposite to the bottom side, it is regarded as no area and is not counted as the number (in Figure 1 In the example above, no such region exists).

[0053] Here, "the region of the cyclic olefin resin passing through a pair of sides parallel to the thickness direction" means the region of the cyclic olefin resin passing through a pair of sides parallel to the thickness direction at the same time. Figure 1 In the example (right figure), the 4th to 7th regions from the top correspond to it, and the 1st to 3rd regions from the top do not correspond to it. Therefore, the number of "regions of cyclic olefin resin passing through a pair of sides parallel to the thickness direction" in this example is 4.

[0054] In the polyolefin film of the present invention, when a layer having a melting point lower than that of the A layer and the B layer and having a melting point of 100°C or more and 150°C or less is set as the C layer, it is preferred that the B layer is located on one outermost surface and the C layer is located on the other outermost surface. Here, the C layer melts at a lower temperature than the A layer and the B layer. Therefore, by melting only the C layer at a temperature lower than the melting point of the A layer and the B layer, the C layer can play the role of a heat-sealing layer. Heat sealing refers to a state (or a process) in which the films are melted and pressed together by heat treatment when the contents are filled and packaged to obtain a bag shape, and heat sealing property refers to the property of the film side that is melted and pressed together by heating.

[0055] From the perspective of making the C layer a heat-sealing layer that functions at a high speed under a lower temperature environment, the C layer preferably contains a polypropylene resin with low crystallinity and a low melting point, and specifically, ethylene-propylene random copolymers, ethylene-propylene-butylene random copolymers, propylene-butylene random copolymers, etc. can be preferably used. From the above aspects, the melting point of the C layer is preferably above 110°C and below 148°C, and more preferably above 120°C and below 145°C. The melting point of the C layer can be read as the peak temperature with the maximum melting heat in the endothermic peak generated by melting when the C layer of the film is analyzed by differential scanning calorimetry (DSC).

[0056] For the polyolefin film of the present invention, when tanδ in the main orientation axis direction at 50°C and 121°C obtained by dynamic viscoelasticity measurement at a frequency of 10 Hz is set to tanδ50 and tanδ121, respectively, tanδ50 / tanδ121 is preferably greater than 0.25 and less than 0.99. Tanδ50 / tanδ121 exceeding 0.25 means that the temperature dependence of the loss tangent (tanδ) is small. That is, the amorphous molecular chains in the film are not easy to move under high temperature environment. For example, when the D layer described later is vapor-deposited, defects such as pinholes and cracks generated in the D layer due to film deformation caused by heat during vapor deposition can be suppressed, so that the water vapor barrier and oxygen barrier properties of the laminate with the D layer vapor-deposited are good. In addition, the deformation of the film caused by high temperature treatment such as heat sterilization after bag making can also be suppressed, so that the reduction of water vapor barrier and oxygen barrier properties associated with such treatment can also be reduced. On the other hand, from the perspective of feasibility, the upper limit of tanδ50 / tanδ121 is set to 0.99 or less. It should be noted that tanδ at each temperature can be obtained from the storage modulus and loss modulus read from the viscoelasticity-temperature curve by the dynamic viscoelasticity method, and its measurement method is described later together with the measurement method of each elastic modulus.

[0057] From the above viewpoints, the lower limit of tan δ50 / tan δ121 of the film is 0.28, preferably 0.31, more preferably 0.33, and further preferably 0.35. On the other hand, the upper limit of tan δ50 / tan δ121 is preferably 0.89, and more preferably 0.69.

[0058] In order to control tanδ50 / tanδ121 to be greater than 0.25 and less than 0.99, for example, it is effective to prepare a composite resin raw material obtained by pre-mixing a cyclic olefin resin and a polypropylene resin as the raw material for layer A, melt-extrude it into a sheet on the basis of controlling the content of the cyclic olefin resin, make the area stretching ratio 36.0 times or more (preferably 40.0 times or more), and make the preheating temperature before stretching in the width direction in biaxial stretching higher than the stretching temperature in the width direction by 5°C or more and less than 15°C.

[0059] In view of being able to impart high barrier properties, the ten-point area height (S10z) of at least one surface of the above-mentioned layer B measured by a three-dimensional non-contact surface shape measuring instrument is preferably 150 nm or more and 900 nm or less. Here, the ten-point area height (S10z) of the surface is a parameter obtained by S5p+S5v as the sum of the five-point peak area height (S5p: the average height of the top of the mountain from the highest to the fifth highest among the tops of the mountain in the reference area) and the five-point valley area depth (S5v: the average height of the valley bottom from the deepest to the fifth deepest among the valley bottoms in the reference area (positive value)) in the evaluation field of view image. That is, the smaller (S10z) is, the smaller the surface difference between the concave and convex is, and conversely, the larger (S10z) is, the larger the surface difference between the concave and convex is.

[0060] For example, the surface of a film without particles has a tendency to have a smaller (S10z), and the surface of a film containing coarse particles has a tendency to have a larger (S10z). Considering the above aspects, the lower limit of the ten-point area height (S10z) of the surface is preferably 180nm, more preferably 200nm. On the other hand, the upper limit is preferably 700nm, more preferably 400nm. In order to control the ten-point area height (S10z) of the surface to be greater than 150nm and less than 900nm, for example, the following structure is effective, even if the B layer described later contains a polypropylene resin and a thermoplastic resin incompatible with the polypropylene resin in an amount of greater than 1% by mass and less than 10% by mass.

[0061] The polyolefin film of the present invention preferably contains at least one of metal particles and inorganic compound particles. In view of being able to impart high barrier properties and smoothness to the film surface, the inorganic compound particles are, for example, any one of aluminum, aluminum oxide (sometimes referred to as alumina), silicon oxide, cerium oxide, calcium oxide, diamond-like carbon film, or a mixture thereof, and particularly preferably contain at least one of aluminum oxide, silicon dioxide, and oxides of aluminum and silicon.

[0062] The type of particles can be determined, for example, by performing energy dispersive X-ray analysis (EDS) and, if necessary, EELS analysis using GATAN GIF "Tridiem". In EELS analysis, the composition of the particles can be identified by comparing the obtained EELS spectrum with the EELS spectrum of a commercially available metal compound or generally disclosed EELS spectrum data. As a measuring device, EDS can use JED-2300F (manufactured by JEOL Ltd., semiconductor detector, Dry SD Extra) and the like, and EELS analysis can use a field emission transmission electron microscope JEM-2100F (manufactured by JEOL Ltd., accelerating voltage 200 kV) and the like.

[0063] In addition, the aspect ratio of the metal particles and inorganic compound particles observed in the cross section when the polyolefin film of the present invention is cut with a plane parallel to the main orientation axis direction and perpendicular to the thickness direction is preferably 2 or more. The more layered the particles are, the higher the barrier properties can be exhibited, so the more preferred aspect ratio is 10 or more, further preferably 30 or more, and particularly preferably 50 or more. The upper limit of the aspect ratio is not particularly limited, and is set to 500.

[0064] As a method for making the aspect ratio of the particles in the film be 2 or more, there is no particular limitation, for example, a method of using a laminate having a polyolefin film layer described later and a layer (D layer) containing a metal and an inorganic compound having a total of more than 50% by mass and less than 100% by mass as a raw material can be cited. At this time, in the melting process of melting the laminate, it is preferably melted with high shear, and the thin layer of the D layer is melted. It should be noted that the aspect ratio of the particle can be calculated as follows, that is, the cross-sectional image of the particle obtained by observation with a SEM (scanning electron microscope) is surrounded by a rectangle with the smallest area, and is calculated as the ratio of the length of its long side to the length of its short side.

[0065] The polyolefin film of the present invention preferably has at least one film surface gloss exceeding 130% and being below 160%. The film surface gloss exceeding 130% means that the light scattering density of the film surface is low, so the surface is smoothed. Therefore, by making the film surface gloss greater than 130%, in the case of a laminate with a D layer deposited thereon, defects such as pinholes and cracks generated in the D layer can be suppressed, so that the water vapor barrier and oxygen barrier properties of the laminate are good. On the other hand, when the film surface gloss exceeds 160%, it means that the surface is excessively smoothed, and sometimes the sliding of the film is extremely easy to reduce. Therefore, by making the film surface gloss below 160%, the deterioration of the operability during the deposition of the D layer and the generation of wrinkles associated therewith can be suppressed, so that the water vapor barrier and oxygen barrier properties of the laminate become good. From the above aspects, the film surface gloss is more preferably 135% or more and 149% or less, and further preferably 140% or more and 148% or less. In addition, the glossiness can be measured according to JISK-7105 (1981), and the details thereof will be described later.

[0066] In order to control the film surface glossiness to be greater than 130% and less than 160% or within the above-mentioned preferred range, it is effective to prepare a composite resin raw material obtained by pre-mixing a cyclic olefin resin and a polypropylene resin as a raw material for layer A, melt-extrude the raw material into sheets while controlling the content of the cyclic olefin resin, prepare a laminated structure having at least layer A and layer B, control the temperature of the molten sheet when it is cooled and solidified to be less than 30°C, and make the area stretching ratio 36.0 times or more (preferably 40.0 times or more).

[0067] The polyolefin film of the present invention is preferably a biaxially oriented film. By making a biaxially oriented film, it is easy to control the storage modulus in the main orientation axis direction at 50°C and 121°C obtained by dynamic viscoelasticity measurement at a frequency of 10 Hz and the tensile elongation in the direction orthogonal to the main orientation axis within the preferred range of the present invention. Here, the biaxially oriented film refers to a film in which the molecular chains are oriented in two orthogonal directions, which is usually obtained by stretching in two orthogonal directions.

[0068] The polyolefin film of the present invention can be widely used for industrial purposes such as packaging, demoulding, tape, and film capacitors. Considering that it is suitable for film capacitors and packaging, the thickness is preferably greater than 0.5 μm and less than 60 μm. By making the thickness greater than 0.5 μm, the relaxation during evaporation processing and transportation can be suppressed, and the film rupture caused by tension can be reduced. Considering the above aspects, the lower limit of the thickness is more preferably 0.8 μm, more preferably 1.2 μm in capacitor applications, and more preferably 10 μm, more preferably 11 μm in packaging applications. On the other hand, by setting the thickness to less than 60 μm, in addition to being able to make the operability good, the manufacturing cost can also be suppressed. Considering the above aspects, the upper limit of the thickness is more preferably 5.5 μm, more preferably 4.0 μm, and particularly preferably 3.2 μm in film capacitor applications, and more preferably 50 μm, more preferably 40 μm, and particularly preferably 19 μm in packaging applications. The film thickness can be determined by measuring the thickness at 10 random locations of the film with a contact micrometer in an atmosphere of 23° C. and 65% RH and calculating the arithmetic mean of all the measured values.

[0069] There is no particular limitation on the method for making the thickness of the polyolefin film greater than 0.5 μm and less than 60 μm or within the above preferred range, and for example, a method of adjusting the discharge amount during melt extrusion of the polyolefin resin composition, a method of adjusting the rotation speed of the casting drum during cooling and solidification of the molten sheet, a method of adjusting the lip gap of the die for discharging the molten sheet, a method of adjusting the stretching ratio in the length direction, a method of adjusting the stretching ratio in the width direction, etc. More specifically, the thickness of the polyolefin film can be reduced by reducing the discharge amount, increasing the rotation speed of the casting drum, reducing the lip gap of the die, and increasing the stretching ratios in the length direction and the width direction.

[0070] Next, the resin preferably used in the polyolefin film of the present invention is described. The A layer of the polyolefin film of the present invention preferably has a polypropylene resin as the main component, and the melting point of the A layer is 135°C or more and 175°C or less, from the perspective of making the storage modulus in the main orientation axis direction at 50°C and 121°C obtained by the dynamic viscoelasticity measurement at a frequency of 10 Hz, the heat shrinkage in the main orientation axis direction at 150°C, and the tensile elongation in the direction orthogonal to the main orientation axis within the above range. From the above aspects, the lower limit of the melting point of the A layer is preferably 140°C, more preferably 145°C, further preferably 150°C, particularly preferably 157°C, and most preferably 163°C. On the other hand, the upper limit of the melting point of the A layer is preferably 173°C, more preferably 171°C, and particularly preferably 169°C. By making the melting point of the A layer in such a range, it is easy to control the E'121 / E'50 of the film and the heat shrinkage in the main orientation axis direction at 150°C to the above preferred range. It should be noted that the melting point of layer A can be read as the peak temperature of the endothermic peak with the largest peak area among the endothermic peaks generated by the second round of melting when layer A of the polyolefin film is analyzed by differential scanning calorimetry (DSC). It should be noted that the detailed method for measuring the melting point is described below.

[0071] The meso pentad fraction of the polypropylene resin used as the main component in the B layer of the polyolefin film of the present invention is preferably 0.900 or more. The lower limit of the meso pentad fraction is preferably 0.930, more preferably 0.960, and further preferably 0.970. The meso pentad fraction is an index of the stereoregularity of the crystalline phase of the polypropylene resin, and is determined by a nuclear magnetic resonance method (NMR method). In the polyolefin film of the present invention, by using a polypropylene resin with a meso pentad fraction of 0.90 or more as the main component of the B layer, the crystallinity of the B layer becomes higher, which has the effect of improving the orientation of the polypropylene film (especially the B layer). As a result, when the polypropylene film is used for packaging purposes, the deformation caused by the heat during vapor deposition can be suppressed, and the D layer described later represented by the vapor-deposited film can be easily and uniformly laminated, and defects such as pinholes and cracks in the D layer can also be suppressed. Therefore, the effect of improving the water vapor barrier and oxygen barrier properties of the laminate laminated with the D layer can be obtained. In addition, from the viewpoint of feasibility and improvement of the adhesion between the layer B and the layer D, the upper limit of the meso pentad fraction is preferably 0.99, more preferably 0.98.

[0072] The polypropylene resin used in the B layer of the polyolefin film of the present invention may be one kind or a mixture of two or more kinds. However, from the perspective of reducing deformation caused by heat during vapor deposition when the film is made, the melting point of the polypropylene resin as the main component is preferably above 151°C, more preferably above 153°C, further preferably above 155°C, particularly preferably above 158°C, and most preferably above 160°C. By making the melting point of the polypropylene resin as the main component of the B layer above 151°C, the B layer can maintain high crystallinity, so the deformation of the polypropylene film caused by heat during vapor deposition is reduced. That is, when the D layer described later is laminated by vapor deposition, defects such as pinholes and cracks in the D layer are reduced, and the water vapor barrier and oxygen barrier properties of the laminate laminated with the D layer become higher.

[0073] When two or more polypropylene resins are used in the B layer of the polyolefin film of the present invention, as the polypropylene resin other than the main component, a modified polypropylene resin is preferably used. By using the above resin, the content of nitrogen and oxygen elements on the surface of the B layer increases, and when the D layer described later is laminated, the adhesion between the B layer and the D layer can be improved. As modified polypropylene resins, for example, the "Admer" (registered trademark) series (unsaturated carboxylic acid modified polypropylene) of Mitsui Chemicals (Co., Ltd.) and the "Yumax" (registered trademark) series (acid-modified low molecular weight polypropylene resin) of Sanyo Chemical Industries (Co., Ltd.) can be cited. From the perspective of maintaining the crystallinity of the B layer at a high level, when the resin of the B layer as a whole is regarded as 100% by mass, the content of the modified polypropylene resin in the B layer is preferably 40% by mass or less, more preferably 30% by mass or less, and further preferably 20% by mass or less.

[0074] In addition, in the B layer of the polyolefin film of the present invention, from the perspective of imparting smoothness to the surface layer, an incompatible resin incompatible with the polypropylene resin may be added within a range that does not hinder the effect of the present invention. When the total amount of resin constituting the B layer is regarded as 100% by mass, the amount of incompatible resin incompatible with the polypropylene resin is preferably 1% by mass or more and 10% by mass or less. From the perspective of imparting smoothness to the surface layer of the polyolefin film, the incompatible resin incompatible with the polypropylene resin is preferably 2% by mass or more, more preferably 3% by mass or more, and the upper limit is preferably 9% by mass, more preferably 8% by mass.

[0075] Here, as the incompatible resin, polymethylpentene resin is particularly preferably used from the viewpoint of high affinity with polypropylene resin and ability to reduce the domain size. In addition, the melting point of polymethylpentene resin is preferably 185°C to 240°C, more preferably 220°C to 240°C, from the viewpoint of extrusion stability when blended with polypropylene and surface concavity and convexity imparted by utilizing the regional sea island structure. Based on these characteristics, in the polypropylene film of the present invention, it is preferred that the polymer in which the structural unit derived from 4-methylpentene-1 is 80 mol% or more and 100 mol% or less in 100 mol% of all structural units is used, for example, the "TPX" (registered trademark) MX series, "TPX" (registered trademark) DX series, "TPX" (registered trademark) RT series, etc. sold as the "TPX" (registered trademark) series by Mitsui Chemicals (Strain) can be preferably used. Specifically, "TPX" (registered trademark) MX002, MX004, DX310, DX845, and RT31 are preferred because they have high affinity with polypropylene resins and can reduce the domain size.

[0076] The cyclic olefin resin used in the polyolefin film of the present invention is described below. The cyclic olefin resin is obtained by, for example, mainly polymerizing a cyclic olefin monomer.

[0077] Examples of the cyclic olefin monomer include monocyclic olefins such as cyclobutene, cyclopentene, cycloheptene, cyclooctene, cyclopentadiene, and 1,3-cyclohexadiene, bicyclo[2,2,1]hept-2-ene, 5-methyl-bicyclo[2,2,1]hept-2-ene, 5,5-dimethyl-bicyclo[2,2,1]hept-2-ene, 5-ethyl-bicyclo[2,2,1]hept-2-ene, 5-butyl-bicyclo[2,2,1]hept-2-ene, 5-ethyl-bicyclo[2,2,1]hept-2-ene, 5-hexyl-bicyclo[2,2,1]hept-2-ene, 5-octyl-bicyclo[2,2,1]hept-2-ene, 5-octadecyl-bicyclo[2,2,1]hept-2-ene, and 5-methylene-bicyclo[2,2 ,1]hept-2-ene, 5-vinyl-bicyclo[2,2,1]hept-2-ene, bicyclic olefins such as 5-propenyl-bicyclo[2,2,1]hept-2-ene, tricyclo[4,3,0,12.5]dec-3,7-diene, tricyclo[4,3,0,12.5]dec-3-ene, tricyclo[4,3,0,12.5]undec-3,7-diene, tricyclo[4,3,0,12.5]undec-3,8-diene, tricyclo[4,3,0,12.5]undec-3-ene, 5-cyclopentyl-bicyclo[2,2,1]hept-2-ene, 5-cyclohexyl-bicyclo[2,2,1]hept-2-ene, 5-cyclohexenylbicyclo[2,2,1]hept-2-ene, 5-phenyl-bicyclo[2 ,2,1]hept-2-ene, tetracyclo[4,4,0,12.5,17.10]dodec-3-ene, 8-methyltetracyclo[4,4,0,12.5,17.10]dodec-3-ene, 8-ethyltetracyclo[4,4,0,12.5,17.10]dodec-3-ene, 8-methylenetetracyclo[4,4,0,12.5,17.10]dodec-3-ene, 8-ethyltetracyclo[4,4,0,12.5,17.10]dodec-3-ene, 8-vinyltetracyclo[4,4,0,12.5,17.10]dodec-3-ene, 8-propenyl-tetracyclo[4,4,0,12.5,17.10]dodec-3-ene, etc. olefins, and 8-cyclopentyl-tetracyclo[4,4,0,12.5,17.10]dodec-3-ene, 8-cyclohexyl-tetracyclo[4,4,0,12.5,17.10]dodec-3-ene, 8-cyclohexenyl-tetracyclo[4,4,0,12.5,17.10]dodec-3-ene, 8-phenyl-cyclopentyl-tetracyclo[4,4,0,12.5,17.10]dodec-3-ene, tetracyclo[7,4,13.6,01.9,02.7]tetradec-4,9,11,13-tetraene, tetracyclo[8,4,14.7,01.10,03.8]pentadeca-5,10,12,14-tetraene, pentacyclo[6,6,13.6,02.7,09.14〕-4-hexadecene, pentacyclo[6,5,1,13.6,02.7,09.13]-4-pentadecaene, pentacyclo[7,4,0,02.7,13.6,110.13]-4-pentadecaene, heptacyclo[8,7,0,12.9,14.7,111.17,03.8,012.16]-5-eicosene, heptacyclo[8,7,0,12.9,03.8,14.7,012.17,113.16]-14-eicosene, cyclopentadiene tetramer and other polycyclic olefins. These cyclic olefin monomers can be used alone or in combination of two or more. .

[0078] As the cyclic olefin monomer, among the above, from the viewpoint of productivity and surface properties, it is preferred to use a tricyclic olefin having 10 carbon atoms such as bicyclo[2,2,1]hept-2-ene (hereinafter referred to as norbornene), a tricyclic olefin having 10 carbon atoms such as tricyclo[4,3,0,12.5]dec-3-ene (hereinafter referred to as tricyclodecene), a tetracyclic olefin having 12 carbon atoms such as tetracyclo[4,4,0,12.5,17.10]dodec-3-ene (hereinafter referred to as tetracyclododecene), cyclopentadiene, or 1,3-cyclohexadiene.

[0079] If the total amount of structural units derived from cyclic olefin monomers in 100 mol% of the polymer exceeds 20 mol% and is 100 mol% or less, the cyclic olefin resin is preferably a resin formed by polymerizing only the above-mentioned cyclic olefin monomers (hereinafter, sometimes referred to as COP) or a resin formed by copolymerizing the above-mentioned cyclic olefin monomers with chain olefin monomers (hereinafter, sometimes referred to as COC), or both may be mixed.

[0080] As a method for producing COP, known methods such as addition polymerization or ring-opening polymerization of cyclic olefin monomers can be cited, for example, a method of subjecting norbornene, tricyclodecene, tetracyclodecene and derivatives thereof to ring-opening metathesis polymerization and then hydrogenating them, a method of subjecting norbornene and derivatives thereof to addition polymerization, a method of subjecting cyclopentadiene and cyclohexadiene to 1,2- or 1,4-addition polymerization and then hydrogenating them, etc. Among these methods, a method of subjecting norbornene, tricyclodecene, tetracyclodecene and derivatives thereof to ring-opening metathesis polymerization and then hydrogenating them is more preferred in terms of productivity and moldability.

[0081] In the case of COC, as the preferred chain olefin monomers for copolymerization, ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, etc. can be listed. Among them, ethylene can be particularly preferably used from the perspective of productivity and cost. In addition, as a method for manufacturing a resin formed by copolymerizing a cyclic olefin monomer and a chain olefin monomer, known methods such as addition polymerization of a cyclic olefin monomer and a chain olefin monomer can be listed, and for example, a method of addition polymerization of norbornene and its derivatives with ethylene can be listed. Among them, from the viewpoint of productivity and moldability, a binary or ternary copolymer containing norbornene or tricyclodecene as a cyclic olefin monomer and ethylene and / or propylene as a chain olefin monomer is more preferred.

[0082] The cyclic olefin resin used in the polyolefin film of the present invention is preferably amorphous. In addition, regarding the glass transition temperature of the amorphous cyclic olefin resin, from the perspective of controlling the E'121 / E'50 of the polyolefin film and the thermal shrinkage rate in the main orientation axis direction at 150°C within the above-mentioned preferred range, it is preferably above 125°C, more preferably above 130°C, and further preferably above 135°C. By making the glass transition temperature above 125°C, the thermal stability when forming the film is improved. Although there is no particular upper limit, it is set to 200°C from the perspective of film forming properties. It should be noted that the cyclic olefin resin in the polyolefin film of the present invention is amorphous and is defined as: the melting peak temperature (Tm) obtained when the cyclic olefin resin is heated from 30°C to 260°C at 20°C / min cannot be observed using a differential scanning calorimeter DSC.

[0083] The polyolefin film of the present invention, even when the polypropylene resin is the main component, can also include resins other than polypropylene resin and cyclic olefin resin within the scope of not damaging the purpose of the present invention. As specific resins, vinyl polymer resins, polyester resins, polyamide resins, polyphenylene sulfide resins, polyimide resins, polycarbonate resins, etc., including various polyolefin resins can be cited, and polymethylpentene, syndiotactic polystyrene, etc. are particularly preferably exemplified. When the resin components constituting the polyolefin film are regarded as 100% by mass as a whole, the content of resins other than polypropylene resin and cyclic olefin resin is preferably less than 3% by mass, more preferably less than 2% by mass, and further preferably less than 1% by mass. When the content of resins other than polypropylene resin and cyclic olefin resin is more than 3% by mass, the influence of the regional interface becomes larger, so sometimes the stretchability is reduced, or the water vapor barrier and oxygen barrier of the laminated body laminated with the D layer are reduced. It should be noted that the layer containing these components is not particularly limited.

[0084] The polyolefin film of the present invention can be widely used for industrial purposes such as packaging, demoulding, tape, film capacitors, etc. For example, when used for packaging, it can be suitably used as a polyolefin film with excellent structural stability against heat during vapor deposition, and good water vapor barrier properties and oxygen barrier properties against heat during heat sterilization.

[0085] <Laminate>

[0086] Next, the laminate of the present invention is described. As the laminate of the present invention, a layer (D layer) containing a metal and an inorganic compound with a total content of more than 50% by mass and less than 100% by mass is provided on at least one surface of the polyolefin film of the present invention. Here, "a layer containing a metal and an inorganic compound with a total content of more than 50% by mass and less than 100% by mass" means that when all the components constituting the layer are regarded as 100% by mass, a layer containing only more than 50% by mass of metal, a layer containing only more than 50% by mass of inorganic compounds, and a layer containing any one of metal and inorganic compounds and a total content of more than 50% by mass. As the metal and / or inorganic compound of the D layer, from the perspective of improving the adhesion with the film, improving the gas barrier properties when laminated to the film, and reducing the environmental load, for example, any one of aluminum, aluminum oxide, silicon oxide, cerium oxide, calcium oxide, diamond-like carbon film, or a mixture thereof is preferably used.

[0087] Here, in the case where the polyolefin film is a laminated structure, the average height (Spk) of the protruding peaks on the surface of the D layer measured by a three-dimensional non-contact surface roughness meter is preferably greater than 10nm and less than 400nm. By setting Spk to more than 10nm, moderate smoothness can be imparted, and the film transportability and high water vapor barrier and oxygen barrier properties of the vapor deposition process can be achieved. On the other hand, by setting Spk to less than 400nm, the formation of steep protrusions can be suppressed, and therefore, the reduction in water vapor barrier and oxygen barrier properties caused by defects such as pinholes and cracks in the D layer caused by the protrusions can be reduced. From the above aspects, the lower limit of Spk is preferably 20nm, more preferably 30nm, and further preferably 40nm. On the other hand, the upper limit of Spk is preferably 350nm, more preferably 250nm, further preferably 150nm, and particularly preferably 130nm.

[0088] In order to control the Spk of the laminate to the above-mentioned preferred range, it is effective to prepare a composite resin raw material obtained by pre-mixing a cyclic olefin resin and a polypropylene resin as the raw material for layer A, melt-extrude it into sheets on the basis of controlling the content of the cyclic olefin resin, prepare a laminated structure, control the cooling temperature of the molten sheet to a relatively low level (preferably below 30°C) when cooling and solidifying, and perform biaxial stretching with an area stretching ratio of 36.0 times or more (preferably 40.0 times or more).

[0089] The thickness of the D layer in the laminate of the present invention is preferably 200 nm or less from the perspectives of obtaining the recyclability of the laminate as a resin or film, improving the barrier properties by being less prone to rupture, and visibility of the contents when made into a packaging material. From the above perspectives, it is more preferably 110 nm or less, further preferably 50 nm or less, and further preferably 30 nm or less. The lower limit is not particularly limited, but is set to 1 nm from the perspective of expressing barrier properties.

[0090] In addition, in the laminate of the present invention, a resin layer with a thickness of 1 μm or less may be provided between the D layer and the surface of the polyolefin film by coating or the like. By providing the resin layer, effects such as improving the adhesion between the D layer and the polyolefin film may be obtained in some cases. However, from the perspective of manufacturing cost and recyclability, a method without the resin layer (i.e., a method in which the D layer is directly laminated on the outermost surface of the polyolefin film) is preferred, and a method in which the D layer is provided on the surface of the B layer of the polyolefin film is more preferred.

[0091] As a method for forming a D layer on the polyolefin film of the present invention to form a laminate, coating, vapor deposition, lamination, etc. can be cited. Vacuum deposition is particularly preferred because it is independent of humidity and can exhibit excellent gas barrier properties in a thin film. As a vapor deposition method, physical vapor deposition methods such as vacuum vapor deposition, EB vapor deposition, sputtering, and ion plating, and various chemical vapor deposition methods such as plasma CVD can be used. From the perspective of productivity, vacuum vapor deposition is particularly preferred.

[0092] In addition, from the perspective of improving the oxygen permeability of the laminate of the present invention, for example, a top coat layer containing an organic-inorganic mixture may be laminated on the surface of layer D. A preferred example of the top coat layer is a mixture of an alkoxide containing a metal or silicon atom and / or a polycondensate thereof and a water-soluble polymer.

[0093] <Packaging materials, packages>

[0094] The packaging material and the package of the present invention are described below. The packaging material of the present invention is characterized by comprising at least one of the polyolefin film of the present invention and the laminate of the present invention. The packaging material of the present invention has excellent structural stability against heat during vapor deposition, and particularly has good water vapor barrier properties and oxygen barrier properties when a transparent vapor-deposited layer is laminated. Therefore, although it is easily degraded by water vapor and oxygen, it can be suitably used for packaging.

[0095] The package of the present invention is characterized in that the contents are packaged using the packaging material of the present invention. The contents are not particularly limited, but from the perspective of the excellent transparency, water vapor barrier property, and oxygen barrier property of the packaging material of the present invention, visibility from the outside is required, and substances that are easily degraded by water vapor and oxygen are preferred. It should be noted that the package of the present invention is obtained by covering the contents with the packaging material of the present invention, and its form is not particularly limited. For example, a package obtained by processing the packaging material of the present invention into a bag shape by heat sealing and placing the contents therein can be cited. Specific examples of such a package include retort pouch foods and the like.

[0096] <Manufacturing method>

[0097] The polyolefin film of the present invention can be obtained by biaxial stretching, heat treatment and relaxation treatment using raw materials that can impart the above-mentioned properties. As a biaxial stretching method, it can be obtained by a blowing simultaneous biaxial stretching method, a tenter simultaneous biaxial stretching method, and a tenter sequential biaxial stretching method. Among them, from the perspective of improving the film forming stability, crystalline / amorphous structure, surface properties of the film, and especially improving the stretching ratio of the present invention while controlling mechanical properties and thermal dimensional stability, it is preferred to use a tenter sequential biaxial stretching method and a tenter simultaneous biaxial stretching method.

[0098] Next, the method for producing the polyolefin film of the present invention is described by way of example. First, a composite resin raw material premixed with a cyclic olefin resin and a polypropylene resin is diluted or directly melt-extruded onto a support to form an unstretched film. The unstretched film is stretched in the length direction and then stretched in the width direction to perform biaxial stretching in sequence. Thereafter, a heat treatment and a relaxation treatment are performed to produce a biaxially oriented polyolefin film. The following is described in more detail, but the present invention is not necessarily to be construed as being limited thereto.

[0099] First, for the polyolefin film of the present invention, the dispersion state of the cyclic olefin resin and the polypropylene resin (A) is improved, and E'121 / E'50 is controlled to be more than 0.25 and less than 0.99, so that a film with a small temperature dependence of the storage modulus is obtained. Therefore, in particular, from the perspective of suppressing the film deformation caused by heat when the D layer is vapor-deposited on the film and improving the water vapor barrier and oxygen barrier properties of the laminated body laminated with the D layer, it is preferred to mix the cyclic olefin resin, the polypropylene resin and the antioxidant in advance to form a composite. The composite can be made using a short-axis extruder, a twin-axis extruder, etc., and from the perspective of obtaining a good dispersion state and high thermal stability, a twin-axis extruder is particularly preferred.

[0100] The amount of the antioxidant is preferably 0.2 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.4 parts by mass or more, based on 100 parts by mass of the composite resin component. The upper limit is set to 1.0 parts by mass.

[0101] Next, a resin raw material formed by mixing a cyclic olefin resin and a polypropylene resin is supplied to a single screw extruder for layer A, and a polypropylene resin or a polypropylene resin composition as a raw material for layer B and a polypropylene resin or a polypropylene resin composition as a raw material for layer C are supplied to a single screw extruder for layer B and a single screw extruder for layer C, respectively. Melt extrusion is performed from a single screw extruder of each of layer A, layer B, and layer C, with the extrusion temperature set at 220°C to 280°C, preferably 230°C to 270°C, and foreign matter is removed by passing through a filter. Next, these molten resins are merged in a laminating device such as a feed block in a manner to form a desired layer structure (when the unstretched layer A is set as layer a, the unstretched layer B is set as layer b, and the unstretched layer C is set as layer c, for example, layer b / layer a / layer c). Then, extrusion is performed from a slit die at a temperature of 200°C to 260°C.

[0102] Here, from the perspective of fully melting the resin during melt extrusion and preventing the molecular chains from being cut due to shearing caused by the screw rotation, so that the film structure will not relax even at high temperatures and can be stable, it is preferred to set the temperature before the filter to a high temperature, set the temperature after passing through the filter to a lower temperature than before the filter, and set the die temperature just before discharge to a multi-stage low-temperature setting that can achieve further low temperatures. In addition, the oxygen concentration in the raw material feeding hopper is preferably 1% or less (volume basis, the same below), more preferably 0.1% or less, and further preferably 0.05% or less. By setting the oxygen concentration in the raw material feeding hopper to 1% or less, the oxidative degradation of the polypropylene resin can be suppressed, and E'121 / E'50 can be easily controlled to the preferred range of the present invention.

[0103] Next, the molten resin sheet extruded from the slit die is cooled and solidified on a casting drum (cooling drum) whose surface temperature is controlled to be 10° C. to 40° C. to obtain an unstretched film. At this time, when co-extrusion lamination is performed in such a manner that the drum surface side that the molten sheet extruded from the die first contacts becomes the B layer, it is easy to control the roughness parameter of the D layer formed on the surface of the B layer within a desired range, so it is preferred.

[0104] As a method for bonding the molten sheet to the casting drum, any of the methods of electrostatic application, bonding using the surface tension of water, air knife method, pressure roller method, underwater casting method, air chamber method, etc. can be used. In addition, a combination of multiple methods is also possible, and the air knife method is preferably used because it can make the film planarity good and can control the surface roughness. In addition, when the air knife method is used, in order to prevent the vibration of the film, it is preferred to appropriately adjust the position of the air knife in a manner that air flows on the downstream side of the film.

[0105] From the viewpoint of making the surface of the obtained polypropylene film smooth and achieving the improvement of the thickness uniformity and adhesion of the D layer formed by the vapor-deposited film, the surface temperature of the casting drum is preferably 10° C. to 35° C., more preferably 10° C. to 30° C., and particularly preferably 10° C. to 25° C. By setting the temperature in such a range, the mesophase fraction of the surface layer part of the unstretched film, especially the roll surface side (the surface side that becomes the B layer after stretching), can be increased, so that the unstretched film has a mesophase structure.

[0106] Mesophase refers to the middle phase of crystallization and amorphous, and is specifically generated when solidified from a molten state at a very fast cooling rate. It is generally known that if polypropylene is cooled and solidified, crystallization is carried out and spherulites grow, but it is believed that if the unstretched film that produces spherulites in this way is stretched, the tensile stress is different between the crystallization and amorphous inside the spherulites, between the spherulites, etc., and local stretching is uneven, resulting in uneven thickness and uneven structure. On the other hand, the mesophase does not take the form of spherulites, so uneven stretching is not produced, and the stretching uniformity becomes high, so the thickness uniformity when the film is made is high, and the surface roughness is also small and easy to become uniform.

[0107] Next, the unstretched film is biaxially stretched to be biaxially oriented. More specifically, the unstretched film is maintained at a temperature of preferably 100 to 170° C., more preferably 120 to 165° C., stretched in the longitudinal direction to preferably 2.0 to 12 times, more preferably 3.0 to 11 times, further preferably 4.0 to 10 times, particularly preferably 4.5 to 10 times, and most preferably 5.0 to 9.0 times, and then cooled to room temperature.

[0108] Next, the film is introduced into a tenter while the two ends in the width direction of the film that has been uniaxially stretched in the length direction are clamped by a clamp. Here, in the present invention, by setting the temperature of the preheating process immediately before stretching in the width direction to the stretching temperature in the width direction + 5 to the stretching temperature in the width direction + 15°C, the fibril structure with high orientation in the length direction can be further strengthened by uniaxial stretching, so the temperature dependence of the storage modulus of the film can be reduced, and E'121 / E'50 can be easily controlled within the above-mentioned preferred range. In addition, from the perspective of being able to improve thermal dimensional stability, it is preferred to stabilize the insufficiently oriented molecular chains by high-temperature preheating after uniaxial stretching. From the above-mentioned aspects, the upper limit of the temperature of the preheating process immediately before stretching in the width direction is preferably the stretching temperature in the width direction + 12°C, and more preferably the stretching temperature in the width direction + 10°C.

[0109] Next, the film is stretched in the width direction while being clamped at both ends thereof. From the viewpoint of controlling E'121 / E'50 to be within the above-mentioned preferred range, the stretching temperature in the width direction is preferably 150 to 175°C, more preferably 155 to 175°C.

[0110] From the perspective of reducing the temperature dependence of the storage modulus of the film and making it easier to control E'121 / E'50 within the above-mentioned preferred range, the stretching ratio in the width direction is preferably 6.0 to 20.0 times, more preferably 8.1 to 17.0 times, and even more preferably 9.1 to 15.0 times. By setting the stretching ratio in the width direction to 6.0 times or more, the orientation contribution of the fibril structure that is highly oriented in the length direction by uniaxial stretching is mitigated, so that the deformation of the film caused by the heat when the D layer is vapor-deposited on the film is reduced, and the water vapor barrier and oxygen barrier properties of the laminate laminated with the D layer are maintained. In addition, increasing the stretching ratio in the width direction compared to the length direction can impart orientation in the width direction while maintaining a high orientation state in the length direction, so that the molecular chain tension in the plane is increased, thereby particularly improving the temperature dependence of the storage modulus.

[0111] Here, the area stretching ratio is preferably 36.0 times or more. By making the area stretching ratio 36.0 times or more, the molecular chain tension in the film surface is increased, and the regional structure becomes smaller or thinner, so the temperature dependence of the storage modulus when the film is made can be reduced, the thermal dimensional stability can be improved, and the elongation at break can be improved. As a result, for the obtained film, the deformation caused by the heat when the D layer is evaporated on the film is suppressed, and the water vapor barrier and oxygen barrier properties of the laminated body laminated with the D layer are excellent. In the present invention, the area stretching ratio refers to the value obtained by multiplying the stretching ratio in the length direction by the stretching ratio in the width direction. From the above aspects, the area stretching ratio is more preferably 38.0 times or more, further preferably 40.0 times or more, and particularly preferably 44.0 times or more. The upper limit of the area stretching ratio is not particularly limited. From the perspective of feasibility, it is 90.0 times in the case of sequential biaxial stretching and 150 times in the case of simultaneous biaxial stretching.

[0112] It is important for the polyolefin film of the present invention to set a high area stretch ratio while reducing the temperature dependence of the storage modulus and the heat shrinkage rate in the main orientation axis direction at 150°C, and to increase the tensile elongation in the direction perpendicular to the main orientation axis. That is, in the present invention, it is preferred to increase the dispersibility of the cyclic olefin resin region dispersed in the polypropylene resin, and to set the preheating temperature during biaxial stretching and further stretching in the width direction to a temperature higher than the stretching temperature.

[0113] In the manufacture of the polypropylene film of the present invention, in the subsequent heat treatment and relaxation treatment process, while the two ends in the width direction are tightened and clamped by a clamp, a heat treatment of 145°C or more and 170°C or less is performed while giving 2 to 20% relaxation in the width direction. This is preferred from the perspective of removing the residual strain of the film and improving the thermal dimensional stability. Through such a treatment, it is particularly possible to suppress the deformation of the film caused by the heat when the D layer is evaporated on the film, so that the water vapor barrier and oxygen barrier properties of the laminated body laminated with the D layer are good. From the above-mentioned aspects, the lower limit of the heat treatment temperature is preferably 150°C, more preferably 155°C, and further preferably 160°C. In the relaxation treatment, from the perspective of improving the structural stability of the film to heat, the lower limit of the relaxation rate is preferably 5%, more preferably 8%, and further preferably 11%. On the other hand, the upper limit is preferably 18%, and more preferably 17%.

[0114] After the above-mentioned heat treatment and relaxation treatment steps, the film is guided to the outside of the tenter, the clamps at both ends of the film in the width direction are released at room temperature, and the blank portions on both sides of the film in the width direction are cut in the winding machine step.

[0115] Next, in order to improve the peeling force of the D layer, it is preferred to perform an online surface modification treatment on the surface (usually the surface on the side in contact with the casting drum) of the layer (D layer) containing a total of more than 50% by mass and less than 100% by mass of metal and inorganic compounds. Examples of the online surface modification treatment include, for example, corona discharge treatment in the air or in an atmosphere gas of oxygen, nitrogen, hydrogen, argon, carbon dioxide, silane gas or a mixture thereof, or plasma treatment, ion beam treatment, and the like.

[0116] In particular, corona discharge treatment is effective in an atmosphere gas having an oxygen concentration of 10% or less, preferably 5% or less, and more preferably 1% or less. As a specific embodiment of an atmosphere gas having an oxygen concentration of 1% or less, nitrogen, carbon dioxide or a mixture thereof is preferably selected, and a mixture of nitrogen and carbon dioxide is particularly effective. In addition, a method of combining the corona discharge treatment in the above-mentioned atmosphere gas with a plasma treatment or an ion beam treatment is also effective. By treating in this atmosphere, the generation of low molecular weight substances associated with the severance of the molecular chains of polypropylene can be suppressed on the film surface, and hydrophilic functional groups can be effectively introduced, so that the peeling force of the D layer from the polyolefin film can be easily improved. The film thus obtained is wound into a roll to obtain the polyolefin film of the present invention.

[0117] It should be noted that, in order to obtain the polyolefin film of the present invention, if the manufacturing conditions of interest are specifically listed, they are described as follows as examples. It should be noted that it is preferred that all of these manufacturing conditions are satisfied, but it is not necessarily set as an embodiment in which all of them are possessed, and appropriate combinations may also be made. For example, for "in sequential biaxial stretching, the preheating temperature before stretching in the width direction is the stretching temperature in the width direction + 5 to the stretching temperature in the width direction + 15°C", simultaneous biaxial stretching may also be used instead.

[0118] · Premix the cyclic olefin resin and the polypropylene resin.

[0119] The extrusion conditions were set such that the temperature before the filter was high, the temperature after the filter was low compared to that before the filter, and the die temperature immediately before discharge was even lower (multi-stage low temperature reduction).

[0120] ·The oxygen concentration in the raw material supply hopper is kept below 1%.

[0121] The above-mentioned premixed resin raw material is used for the A layer, and a laminate structure is prepared with the A layer as the inner layer.

[0122] The area stretching ratio of the biaxial stretching is 36.0 times or more.

[0123] In the sequential biaxial stretching, the preheating temperature before the stretching in the width direction is the stretching temperature in the width direction + 5 to the stretching temperature in the width direction + 15°C.

[0124] After biaxial stretching, the film is relaxed by 2 to 20% in the width direction and heat treated at 145° C. to 170° C.

[0125] <Metal film laminate film, thin film capacitor formed using the same, and methods for producing the same>

[0126] The metal film laminated film of the present invention has a metal film on at least one surface of the polyolefin film of the present invention. The metal film laminated film can be obtained by providing a metal film on at least one surface of the polypropylene film of the present invention.

[0127] In the present invention, the method of imparting the metal film is not particularly limited. For example, it is preferred to use a method in which aluminum or an alloy of aluminum and zinc is vapor-deposited on at least one side of a polyolefin film to form a vapor-deposited film or other metal film that serves as an internal electrode of a film capacitor. At this time, other metal components such as nickel, copper, gold, silver, and chromium may also be vapor-deposited simultaneously or sequentially with aluminum. In addition, a protective layer may be provided on the vapor-deposited film using oil or the like. In the case where the surface roughness of the polyolefin film is different on the surface and the back, it is preferred to provide a metal film on the surface side with a smooth roughness to form a metal film laminate film from the perspective of improving the withstand voltage.

[0128] In the present invention, after forming the metal film, the metal film laminate can be annealed or heat treated at a specific temperature as needed. In addition, for insulation or other purposes, a resin such as polyphenylene ether can be applied on at least one surface of the metal film laminate.

[0129] The film capacitor of the present invention is formed using the metal film laminate film of the present invention. That is, the film capacitor of the present invention has the metal film laminate film of the present invention.

[0130] For example, the film capacitor of the present invention can be obtained by laminating or winding the metal film laminate film of the present invention described above by various methods. The preferred method for producing a wound film capacitor is as follows.

[0131] Aluminum is deposited on one side of a polyolefin film under reduced pressure. At this time, the film is deposited in stripes with blank portions extending in the length direction. Next, a knife is inserted into the center of each deposited portion and each blank portion on the surface to cut the film, thereby producing a strip-shaped roll with a blank portion on one side of the surface. For a strip-shaped roll with a blank portion on the left or right, two rolls with a blank portion on the left and right are stacked and wound in such a way that the deposited portion extends from the blank portion in the width direction, thereby producing a wound body.

[0132] When vapor deposition is performed on both sides, the vapor deposition is performed in a stripe shape with a blank portion extending in the length direction of one side, and the vapor deposition is performed in a stripe shape on the other side in such a way that the blank portion in the length direction is located in the center of the vapor deposition portion on the back side. Next, a blade is inserted into the center of the blank portion of each of the front and back sides to cut, and a strip-shaped roll is produced with blanks on one side of each side (for example, if there is a blank on the right side of the front side, there is a blank on the left side of the back side). The obtained roll and the undeposited laminated film are stacked and wound in such a way that the metallized film protrudes from the laminated film in the width direction to obtain a wound body.

[0133] As a method for obtaining the film capacitor of the present invention from the metal layer laminate film of the present invention, for example, a method of pulling out a core material from the wound body prepared as above and pressing it, spraying a metal spray film on both end surfaces to form an external electrode, and welding a lead wire on the metal spray film to form a wound film capacitor can be cited. The uses of film capacitors involve electric vehicles, hybrid vehicles, fuel cell vehicles and other electric vehicles, power control units of electric aircraft such as drones, railway vehicles, solar power generation and wind power generation, and general household appliances. The film capacitor of the present invention can also be applied to these uses.

[0134] The power control unit, electric vehicle, and electric aircraft of the present invention are described below. The power control unit of the present invention has the film capacitor of the present invention. The power control unit is a system for managing power in an electric vehicle, electric aircraft, etc. having a mechanism driven by electricity. By installing the film capacitor of the present invention in the power control unit, the power control unit itself can be miniaturized, heat-resistant, and efficient, and as a result, fuel efficiency is improved.

[0135] The electric vehicle of the present invention has the power control unit of the present invention. Here, the electric bicycle refers to a vehicle having a mechanism for driving using electricity, such as an electric vehicle, a hybrid vehicle, and a fuel cell vehicle. As described above, the power control unit of the present invention is not only miniaturized, but also has excellent heat resistance and efficiency. Therefore, by providing the electric vehicle with the power control unit of the present invention, it is possible to achieve improved fuel efficiency, etc.

[0136] Example

[0137] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to the following embodiments. It should be noted that the evaluation of each item was performed by the following method.

[0138] <Methods for measuring characteristic values ​​and evaluating effects>

[0139] The method for measuring the characteristic values ​​and the method for evaluating the effects in the present invention are as follows.

[0140] (1) Determination of the main orientation axis direction

[0141] Prepare a polyolefin film, cut it into a rectangle with a length of 150 mm and a width of 10 mm with the longitudinal direction facing upward, and use it as sample <1>. At this time, the direction of the long side of the rectangular sample <1> is defined as 0°. Next, collect a sample <2> of the same size in such a way that the long side direction is rotated 15° to the right from the 0° direction. Similarly, the long side direction of the rectangular sample is rotated 15° at a time, and the samples are collected in the same way. <3> ~ <12> . Next, for each rectangular sample, install it on a tensile testing machine ("Tensilon" (registered trademark) UCT-100 manufactured by Orientec) in such a way that the long side direction becomes the stretching direction and the initial distance between chucks is 20 mm, and set the stretching speed to 300 mm / min for tensile test in an atmosphere of 23°C. Read the maximum load until the sample breaks at this time, and divide it by the cross-sectional area of ​​the sample before the test (film thickness × width) to calculate the stress of the maximum point strength. Perform the same measurement 5 times for each sample, and calculate the average value of the stress of the maximum point strength. The long side direction of the sample with the largest average value is taken as the main orientation axis direction of the polyolefin film, and the direction orthogonal to it in the film surface is taken as the direction orthogonal to the main orientation axis of the polyolefin film.

[0142] (2) Film thickness

[0143] The thickness of the polyolefin film was measured at 10 random locations using a contact electronic micrometer (K-312A model) manufactured by Anritsu Co., Ltd. in an atmosphere of 23°C and 65% RH. The arithmetic mean of the thickness at the 10 locations was defined as the film thickness (unit: μm).

[0144] (3) Ratio of storage modulus in the main orientation axis direction: E'121 / E'50

[0145] Under the device and conditions shown below, a rectangular polyolefin film (width (short side) 10 mm × length (long side) 20 mm) cut with the main orientation axis as the long side direction is installed in the chuck part of the device at 23°C and placed in a furnace. The atmosphere in the furnace where the film is placed is cooled with liquid nitrogen, and the temperature is raised from -100°C to 180°C for measurement. The viscoelasticity-temperature curve is drawn by dynamic viscoelasticity measurement, and the storage modulus (E'50) at 50°C is read. It should be noted that the number of measurement tests is n=3, and the average value of the storage modulus (E'50) is calculated. Similarly, the number of measurement tests is set to n=3, and the storage modulus (E'121) at 121°C is read from the viscoelasticity-temperature curve to obtain its average value. The average value of the obtained E'121 is divided by the average value of the obtained E'50 to obtain E'121 / E'50 (unit; dimensionless).

[0146] <Equipment and conditions>

[0147] Device: EXSTAR DMS6100 (manufactured by Seiko Instruments)

[0148] Test mode: tensile mode

[0149] Distance between chucks: 20mm

[0150] Frequency: 10Hz

[0151] Strain amplitude: 20.0μm

[0152] Gain: 1.5

[0153] Initial force amplitude: 490mN

[0154] Temperature range: -100~180℃

[0155] Heating rate: 5℃ / min

[0156] Measurement atmosphere: air

[0157] Measurement of thickness: The film thickness in (2) above was used.

[0158] (4) Heat shrinkage in the main orientation axis direction at 150°C (%)

[0159] In the main orientation axis direction of the polyolefin film, 5 samples with a width of 10 mm and a length of 150 mm (measurement direction) were cut out and marked at 5 mm from both ends to make the test length 100 mm (l0). Next, the test piece was sandwiched between paper and heated in an oven kept at 150°C for 10 minutes while maintaining a horizontal state. After being taken out, the size (l1) was measured and calculated using the following formula. The average value of the 5 pieces was taken as the thermal shrinkage rate in each direction. Thermal shrinkage rate = {(l0-l1) / l0}×100(%).

[0160] (5) Tensile elongation in the direction perpendicular to the main orientation axis (%)

[0161] A rectangular polyolefin film or laminate (width (short side) 10 mm × length (long side) 150 mm) cut out with the film test length direction (the direction orthogonal to the main orientation axis determined as described above) as the long side direction is used as the test sample. Next, the initial distance between the chucks is set to 20 mm on the sample tensile testing machine ("Tensilon" (registered trademark) UCT-100 manufactured by Oeience Tech) and the tensile test of the film is performed at 23°C with the tensile speed set to 300 mm / min. At this time, the position of the long side direction of the sample is adjusted so that the center of the sample comes to the vicinity of the center between the chucks. The elongation (unit: %) at the moment of sample rupture is obtained by measurement. The measurement is performed 5 times, and the tensile elongation of the polyolefin film or laminate in the direction orthogonal to the main orientation axis is calculated as the average value of the elongation at the breaking point.

[0162] (6) Ratio of tanδ in the main orientation axis direction: tanδ50 / tanδ121

[0163] Under the same apparatus and conditions as those in (3) above, the viscoelasticity-temperature curve is plotted by the dynamic viscoelasticity method, and the storage modulus (E'50) at 50°C and the loss modulus (E"50) at 50°C are read. It should be noted that the measurement test number n=3 is carried out, and the average values ​​of the storage modulus (E'50) and the loss modulus (E"50) are calculated, and the loss tangent (tanδ50) at 50°C in the direction of the main orientation axis of the film is calculated by the following formula.

[0164] Formula: tanδ50=E”50 / E'50

[0165] Similarly, according to the measurement test number n=3, the storage modulus (E'121) at 121°C and the loss modulus (E"121) at 121°C are read from the viscoelasticity-temperature curve, and their average values ​​are calculated. The loss tangent (tanδ121) at 121°C in the direction of the main orientation axis of the film is calculated by the following formula.

[0166] Formula: tanδ121=E”121 / E’121

[0167] The obtained value of tan δ50 is divided by the obtained value of tan δ121 to obtain tan δ50 / tan δ121 (unit: dimensionless).

[0168] (7) Glossiness

[0169] According to JIS K-7105 (1981), the film surface on the casting drum contact side was measured using a digital variable angle gloss meter UGV-5D manufactured by Suga Test Instruments Co., Ltd. at an incident angle of 60° and a light receiving angle of 60°, and the average value of the data obtained at 5 points was taken as the gloss (%).

[0170] (8) Melting point (Tm) of the raw resin composition and the resin composition of each layer of the film

[0171] As samples, the raw resin composition used in the polyolefin resin film of the present invention (in the case of mixing multiple raw materials, a resin composition obtained by mixing them in a specified ratio) and the material formed by cutting each layer of the polyolefin film are used. Using a differential scanning calorimeter (EXSTAR DSC6220 manufactured by Seiko Instruments), 3 mg of a polyolefin resin sample is heated from 30°C to 260°C at 20°C / min in a nitrogen atmosphere. Then, after keeping at 260°C for 5 minutes, the temperature is lowered to 30°C at 20°C / min. Furthermore, after keeping at 30°C for 5 minutes, the temperature is raised from 30°C to 260°C at 20°C / min. The peak temperature of the endothermic curve obtained during the temperature increase is taken as the melting point of the raw resin composition and each layer of the film. In this embodiment, (Tm) is calculated from the average value of measurements performed for n=3. It should be noted that when two or more peak temperatures are observed in the range of more than 130°C and less than 260°C, or when a peak temperature can be observed in a multi-stage DSC graph called a shoulder peak (observed in the case of a graph in which two or more peaks overlap), in this embodiment, the temperature of the peak with the largest absolute value of the heat flow (unit: mW) on the vertical axis of the DSC graph is taken as the melting point (Tm) (°C).

[0172] (9) The number of cyclic olefin resin regions in a 1 μm × 2 μm rectangle in layer A that passes through a pair of sides parallel to the thickness direction (number / 2 μm) 2 )

[0173] The A layer of the polyolefin film is cut with a plane parallel to the main orientation axis direction and the thickness direction by a microtome method to form a polypropylene film sheet having a cut surface. The above-mentioned cross section is stained with RuO4, and the stained surface is cut to collect an ultrathin section having a cross section X. The collected ultrathin section is observed under the following conditions using a transmission electron microscope (TEM). It should be noted that at this time, the cyclic olefin resin is stained darker than the polypropylene resin.

[0174] · Equipment: Transmission electron microscope (TEM) HT7700 manufactured by Hitachi, Ltd.

[0175] Accelerating voltage: 100 kV

[0176] Observation magnification: 2,000 times

[0177] In the image collected during the above observation, a 2 μm 2A square rectangle is defined by making a pair of sides 1 μm in the thickness direction and 2 μm in the direction perpendicular to the thickness direction, and the number of regions of cyclic olefin resin passing through a pair of sides parallel to the thickness direction in the rectangle is counted. The same measurement is repeated 10 times in total by changing the position of the rectangle in the image, and the average value of the obtained number of regions is calculated. The value obtained by rounding off the value to one decimal place is calculated as the number of regions of cyclic olefin resin passing through a pair of sides parallel to the thickness direction in layer A (number / 2 μm 2 ). It should be noted that, when a rectangle with a pair of sides of 1 μm in the thickness direction and 2 μm in the direction perpendicular to the thickness direction is determined in the cross section X, the bottom side of the rectangle is set as the sea part, and when the region is located on the side opposite to the bottom side, it is regarded as there is no such region and is not counted as the number. In addition, the region with a constricted portion is also regarded as a cyclic olefin resin region that is more densely dyed than the polypropylene resin part of the sea part and is treated as a connecting region.

[0178] (10) Ten-point area height of the surface measured by a three-dimensional non-contact surface shape measuring instrument (S10z)

[0179] The S10z value is measured using the scanning white interference microscope VS1540 manufactured by Hitachi HiTech Science, a three-dimensional non-contact surface shape measuring instrument. In addition, during the analysis, the captured image is corrected by a fourth-order polynomial approximation using the attached analysis software to remove the fluctuation component, and then processed using a median (3×3) filter, followed by interpolation processing (for pixels for which height data cannot be obtained, compensation is performed using height data calculated from surrounding pixels). The measurement conditions are as follows. It should be noted that when the B layer is located on both surfaces, both surfaces are measured and the lower value is used.

[0180] Manufacturer: Hitachi High-tech Co., Ltd.

[0181] Device name: Scanning white interference microscope VS1540

[0182] ·Measurement conditions: Objective lens 10×

[0183] Lens tube 1×

[0184] Zoom lens 1×

[0185] Wavelength filter 530nm white

[0186] Measurement mode: Wave

[0187] Measurement software: VS-Measure Version 10.0.4.0

[0188] · Analysis software: VS-Viewer version 10.0.3.0

[0189] · Analysis condition: S-Filter = 5 μm

[0190] · Measured area: 0.561 × 0.561 [mm 2 .

[0191] (11) Heat sealability

[0192] Superpose the C-layer surface of the film (in the case of no C-layer, the surface opposite to the vapor deposition side) on a stretched PET film with a thickness of 12 μm, and perform heat sealing under the following conditions using a flat heat sealer to produce a laminate. Use "Tensilon" (registered trademark) manufactured by Orientec Co., Ltd. to conduct a T-shaped peel test on the interface between the polyolefin film of the present invention and the stretched PET film, and measure the heat seal strength. It should be noted that the laminate for the peel test is sampled in a short strip shape with a width of 20 mm × a length of 150 mm, and the heat seal strength is measured at a stretching speed of 300 mm / min. This measurement is performed 3 times, and the average value of the obtained values is calculated, and the obtained value is used as the heat seal strength (N / 25.4 mm). When the heat seal strength can reach 2 N / 25.4 mm or more, it is determined that the heat sealability is qualified (A), and if it is lower than 2 N / 25.4 mm, it is determined that the heat sealability is unqualified (B).

[0193] <Heat seal conditions>

[0194] · Pressing pressure: 0.4 N / mm 2

[0195] · Pressing time: 1 second

[0196] · Heater temperature: 120 °C.

[0197] (12) Water vapor barrier property after Al vapor deposition or AlOx vapor deposition

[0198] <Method of Al vapor deposition>

[0199] Install a film roller in a vacuum vapor deposition apparatus equipped with a film moving device, form a high vacuum state of 1.00 × 10 -2 Pa, and while heating and evaporating aluminum metal on a cooling metal drum at 20 °C, move the film to form a vapor deposition thin film layer on the B layer. At this time, control it so that the thickness of the vapor deposition film becomes 100 nm. After vapor deposition, return the inside of the vacuum vapor deposition apparatus to normal pressure, unwind the wound film, and cure it at a temperature of 40 °C for 2 days to obtain a laminate with a vapor deposition layer of Al (aluminum) laminated on the film.

[0200] <Method of AlOx vapor deposition>

[0201] A film roller was set in a vacuum deposition device equipped with a film conveying device to form a 1.00×10 -2 Pa, on a cooling metal drum at 20°C, oxygen was introduced while AlOx was reacted and evaporated, and the film was advanced to form a vapor-deposited layer on the surface previously treated with corona discharge. At this time, the thickness of the vapor-deposited layer was controlled to 20 nm. After vapor deposition, the vacuum vapor deposition device was restored to normal pressure, the wound film was rewound, and aged at 40°C for 2 days to obtain a laminate having a vapor-deposited layer of AlOx (aluminum oxide) laminated on the film.

[0202] <Evaluation method of water vapor barrier properties>

[0203] For the laminated body subjected to Al vapor deposition or AlOx vapor deposition, the water vapor transmission rate was measured using a water vapor transmission rate measuring device "PERMATRAN-W" (registered trademark) 3 / 30 manufactured by MOCON / Modern Controls, under the conditions of temperature 40°C and humidity 90% RH. The measurement was performed 5 times for each sample, and the average value of the obtained values ​​was calculated as the water vapor transmission rate of the film (unit: g / m 2 Based on the obtained water vapor permeability, the water vapor barrier property of the laminate was determined according to the following criteria. B or higher was considered to have good water vapor barrier property, and C was considered to have no practical problem.

[0204] S: 0.3g / m 2 / day or less.

[0205] A: more than 0.3g / m 2 / day and 0.5g / m 2 / day or less.

[0206] B: more than 0.5g / m 2 / day and 1.0g / m 2 / day or less.

[0207] C: more than 1.0g / m 2 / day and 2.0g / m 2 / day or less.

[0208] D: more than 2.0g / m 2 / day, or the film may break during the vapor deposition process.

[0209] (13) Oxygen barrier properties after Al vapor deposition or AlOx vapor deposition

[0210] By the method described in (12), a laminated body having an Al vapor-deposited layer or an AlOx vapor-deposited layer is obtained. For each laminated body, the oxygen permeability is measured at a temperature of 23°C and a humidity of 0% RH using an oxygen permeability measuring device "OX-TRAN" (registered trademark) 2 / 20 manufactured by MOCON / Modern Controls. The measurement is performed 5 times for each sample, and the average value of the obtained values ​​is calculated and used as the oxygen permeability of the film (unit: cc / m 2 Based on the obtained oxygen permeability, the oxygen barrier property of the laminate was determined according to the following criteria. B or higher was considered to have good oxygen barrier property, and C was considered to have no practical problem.

[0211] S: 1.5cc / m 2 / day or less.

[0212] A: greater than 1.5cc / m 2 / day and 2.0cc / m 2 / day or less.

[0213] B: greater than 2.0cc / m 2 / day and 10cc / m 2 / day or less.

[0214] C: greater than 10cc / m 2 / day and 100cc / m 2 / day or less.

[0215] D: more than 100cc / m 2 / day, or film breakage occurred during the vapor deposition process.

[0216] (14) Thickness of D layer

[0217] The thickness of the D layer constituting the laminate of the present invention is measured by cross-sectional observation using a transmission electron microscope (TEM). A sample for cross-sectional observation is prepared using a microsampling system (FB-2000A manufactured by Hitachi, Ltd.) by the FIB method (specifically, based on the method described in "Polymer Surface Processing" (written by Akira Iwamori) p. 118-119). Next, a transmission electron microscope (H-9000UHRII manufactured by Hitachi, Ltd.) is used to set the acceleration voltage to 300 kV, and the cross-section of the observation sample is observed, and the thickness of the D layer is confirmed at any 10 locations using the length measurement function of the transmission electron microscope. The arithmetic mean value thereof is taken as the thickness of the D layer (unit: nm).

[0218] (15) Average height of the protruding peaks on the D layer surface (Spk)

[0219] The Spk value was measured using a scanning white interference microscope VS1540 from Hitachi HiTech Science, a three-dimensional non-contact surface shape measuring instrument. In addition, during the analysis, the accompanying analysis software was used to remove the fluctuation component by performing a polynomial 4th-order approximate surface correction on the captured image, and then the image was processed using a median (3×3) filter and then interpolated (for pixels for which height data could not be obtained, the height data calculated from the surrounding pixels was used for compensation). The measurement conditions are as follows.

[0220] Manufacturer: Hitachi High-tech Co., Ltd.

[0221] Device name: Scanning white interference microscope VS1540

[0222] ·Measurement conditions: Objective lens 10×

[0223] Lens tube 1×

[0224] Zoom lens 1×

[0225] Wavelength filter 530nm white

[0226] Measurement mode: Wave

[0227] Measurement software: VS-Measure Version 10.0.4.0

[0228] Analysis software: VS-Viewer version 10.0.3.0

[0229] ·Measurement area: 0.561×0.561[mm 2 ].

[0230] (16) Evaluation of film capacitor characteristics (withstand voltage and reliability at 135°C)

[0231] On one side of the film (it should be noted that when the wetting tension is different between the front and back sides, the side with higher wetting tension) a vapor-deposited film A and a vapor-deposited film B were prepared respectively. The vapor-deposited film A was obtained by vapor-depositing aluminum with a film resistance of 10Ω / sq and a so-called T-shaped blank (using masking oil, a longitudinal pitch (period) of 17mm, and a fuse width of 0.5mm) in a direction perpendicular to the longitudinal direction with blank portions provided using a vacuum vapor deposition machine manufactured by Albuck Co., Ltd. The vapor-deposited film B was a vapor-deposited film without a vapor-deposited pattern having a T-shaped blank. The vapor-deposited films A and B were cut separately to obtain vapor-deposited rolls A and B with a film width of 50mm (blank width at the end was 2mm). Next, the capacitor element was wound by a component winding machine (KAW-4NHB) manufactured by Kaito Seisakusho Co., Ltd. in such a way that the component capacity after forming the capacitor element was 10μF, with the vapor deposition reels A and B alternately stacked, and metal spraying was performed, and then heat treatment was performed for 12 hours at a temperature of 128°C under reduced pressure, and leads were installed to form capacitor elements. Using 10 capacitor elements obtained in this way, a voltage of 150VDC was applied to the capacitor elements at a high temperature of 135°C, and after 10 minutes at this voltage, the applied voltage was slowly increased in steps at 50VDC / 1 minute, and the so-called step-up voltage test was repeated in which the above operation was repeated.

[0232] <Evaluation of Withstand Voltage>

[0233] In the step voltage test, the change in electrostatic capacitance is measured and plotted on a graph, and the voltage resistance is calculated by dividing the voltage at which the capacitance becomes 70% of the initial value by the film thickness (above (1)). The average value of 10 capacitor elements is calculated and evaluated according to the following standards: A means that it can be used, and B means that the performance is poor in practical use.

[0234] A: 320V / μm or more

[0235] B: Less than 320V / μm.

[0236] <Reliability Evaluation>

[0237] After the voltage was increased until the electrostatic capacitance decreased to 12% or less relative to the initial value, the capacitor element with the highest increase in withstand voltage among the 10 capacitor elements was disassembled, the state of damage was examined, and the reliability was evaluated as follows: A means usable, and B means poor performance in practical use.

[0238] A: No change in device shape, and through-type damage is observed in 1 or more layers and 10 or more layers. Or no change in device shape or through-type damage is observed.

[0239] B: Changes in device shape were observed, or penetration damage of more than 10 layers was observed.

[0240] [Resin, etc.]

[0241] In the production of the polyolefin-based films in the respective Examples and Comparative Examples, the following resins and the like were used.

[0242] (Polypropylene resin for A layer)

[0243] A1: Homopolypropylene resin (manufactured by Prime Polymer Co., Ltd., “F133A”) (meso-pentad fraction: 0.973, melting point: 165° C., MFR=3.0 g / 10 min)

[0244] A2: Homopolypropylene resin (manufactured by Prime Polymer Co., Ltd., “F113G”) (meso-pentad fraction: 0.940, melting point: 162° C., MFR: 2.9 g / 10 min)

[0245] (Polypropylene resin for B layer)

[0246] B1: Homopolypropylene resin (manufactured by Prime Polymer Co., Ltd., “F113G”) (meso pentad fraction: 0.940, melting point: 162° C., MFR: 2.9 g / 10 min)

[0247] B2: Homopolypropylene resin (manufactured by Prime Polymer Co., Ltd., “F133A”) (meso pentad fraction: 0.973, melting point: 165° C., MFR=3.0 g / 10 min)

[0248] (Polypropylene resin for C layer)

[0249] C1: ethylene-propylene random copolymer ("WFW4M" manufactured by Nippon Polypro Co., Ltd., melting point: 135°C, MFR = 7.0 g / min).

[0250] <Components other than polypropylene resin>

[0251] Cyclic olefin resins:

[0252] COC1: "TOPAS" (registered trademark) 6013F-04 manufactured by Polyplastics (resin (COC) obtained by copolymerizing ethylene and norbornene, glass transition temperature: 138°C)

[0253] COC2: APEL (registered trademark) 5014CL manufactured by Mitsui Chemicals (resin (COC) obtained by copolymerizing ethylene and a norbornadiene derivative, glass transition temperature of 136°C)

[0254] Antioxidants:

[0255] "IRGANOX" (registered trademark) 1010 manufactured by Ciba Specialty Chemicals.

[0256] <Thermoplastic resins incompatible with polypropylene resins>

[0257] Polymethylpentene resin (PMP):

[0258] Mitsui Chemicals, Inc. "TPX" (registered trademark) (RT31, melting point: 232°C, MFR: 9 g / 10 min@260°C)

[0259] <Masterbatch for layer A>

[0260] Polyolefin resin raw materials (AM1):

[0261] The components were mixed so that the polypropylene resin (A1) was 69.5 parts by mass, the cyclic olefin resin (COC1) was 30 parts by mass, and the antioxidant was 0.5 parts by mass. After kneading and extrusion using a twin-screw extruder set at 260° C., the strands were water-cooled and fragmented to prepare a polyolefin resin raw material (AM1).

[0262] Polyolefin resin raw materials (AM2):

[0263] The components were mixed so that the polypropylene resin (A2) was 69.5 parts by mass, the cyclic olefin resin (COC1) was 30 parts by mass, and the antioxidant was 0.5 parts by mass. After kneading and extrusion using a twin-screw extruder set at 260° C., the strands were water-cooled and fragmented to prepare a polyolefin resin raw material (AM2).

[0264] Polyolefin resin raw materials (AM3):

[0265] The components were mixed so that the polypropylene resin (A1) was 69.5 parts by mass, the cyclic olefin resin (COC2) was 30 parts by mass, and the antioxidant was 0.5 parts by mass. After kneading and extrusion using a twin-screw extruder set at 260° C., the strands were water-cooled and fragmented to prepare a polyolefin resin raw material (AM3).

[0266] <Masterbatch for layer B>

[0267] Polyolefin resin raw materials (BM1)

[0268] The components were mixed so that the polypropylene resin (B1) was 69.5 parts by mass, the polymethylpentene resin (PMP) was 30 parts by mass, and the antioxidant was 0.5 parts by mass. After kneading and extrusion using a twin-screw extruder set at 260° C., the strands were water-cooled and fragmented to prepare a polyolefin resin raw material (BM1).

[0269] (Example 1)

[0270] The components were mixed so that the polyolefin resin raw material (AM1) was 32 parts by mass, the polypropylene resin (A1) was 67.6 parts by mass, and the antioxidant was 0.4 parts by mass, and the mixture was supplied to the single screw melt extruder for the A layer, the polypropylene resin B1 was supplied to the single screw melt extruder for the B layer, and the polypropylene resin C1 was supplied to the single screw melt extruder for the C layer. Here, the oxygen concentration in the feed hopper of each extruder was controlled to 0.05%, and after melt extrusion was performed at a temperature of 260° C. by each extruder, foreign matter was removed from the extruded molten resin using a sintered filter with a cutoff of 80 μm. Then, a three-layer structure with a layer structure of b / a / c was formed at a temperature of 250° C. using a dispenser (the compositions for the B layer, A layer, and C layer in a molten state are designated as b, a, and c, respectively). The lamination ratio is 1 / 10 / 1 (the cyclic olefin resin contained in the A layer is 9.6% by mass, and the thickness ratio of the A layer relative to the entire film is about 83%, so the cyclic olefin resin contained in the entire film is 8.0% by mass). At this time, the adjustment of the lamination ratio is carried out by adjusting the extrusion amount from each extruder. Furthermore, the laminated molten resin is introduced into the T die head and discharged into a sheet at a temperature of 240°C. The discharged molten sheet is cooled and solidified on a casting drum maintained at 21°C to obtain an unstretched sheet. It should be noted that at this time, b is brought into contact with the casting drum, and air controlled to 40°C is blown from the air knife so that the molten sheet is in close contact with the casting drum.

[0271] Next, the unstretched polyolefin film is preheated to 145°C in stages using a plurality of roller groups, and then stretched to 5.2 times in the length direction by passing between rollers maintained at a temperature of 155°C and having a peripheral speed difference. Next, the stretched film is cooled by passing between rollers maintained at 70°C, and then cooled to room temperature to obtain a uniaxially oriented film. Furthermore, the obtained uniaxially oriented film is introduced into a tenter, preheated to 165°C while clamping both ends in the width direction with clamps, stretched to 9.2 times at 158°C in the width direction, and then heat treated at 162°C while giving 12% relaxation in the width direction. Then, while continuing to tighten the both ends in the width direction with clamps, the film is guided to the outside of the tenter after a cooling process at 140°C, and the clamps at both ends in the width direction are released. Next, the film surface (the B layer side that becomes the contact surface of the casting drum) is subjected to a 25W·min / m 2The polyolefin film was subjected to corona discharge treatment in a mixed gas atmosphere of carbon dioxide and nitrogen at a volume ratio of 15:85 (an environment with an oxygen concentration of 0.8% by volume) with a treatment intensity of 15:85, and then wound into a roll. Next, the polyolefin film was unrolled from the roll, and Al was vapor-deposited on the surface subjected to corona discharge treatment by the above method to obtain a laminate having an Al vapor-deposited layer (D layer). The properties of the obtained polyolefin film and laminate are shown in Table 1.

[0272] (Example 2)

[0273] The polyolefin film and the laminate were prepared in the same manner as in Example 1, except that AlOx was deposited instead of Al to prepare a laminate having an AlOx layer (D layer). The properties of the obtained polyolefin film and the laminate having the D layer deposited thereon are shown in Table 1. It should be noted that the deposition of AlOx was performed by the aforementioned method.

[0274] (Example 3)

[0275] The polyolefin film prepared in Example 2 was crushed and compressed by a crusher, and was put into an extruder in which the oxygen concentration in the hopper was controlled to 0.05% and the temperature was set to 240°C for kneading and extrusion. The strands were water-cooled and fragmented to obtain recycled pellets (AR1). Next, A1, AM1, and AR1, which are polyolefin resin raw materials for layer A, were mixed in a mass ratio of 53:27:20 and supplied to a single screw melt extruder for layer A, polypropylene resin B1 was supplied to a single screw melt extruder for layer B, and polypropylene resin C1 was supplied to a single screw melt extruder for layer C. Here, the oxygen concentration in the feed hopper of each extruder was controlled to 0.05%, and each extruder was used for melt extrusion at a temperature of 260° C., and the film forming conditions were set as shown in Table 1 (the cyclic olefin content contained in the A layer was 9.7% by mass, and the thickness ratio of the A layer to the entire film was 83%, so the cyclic olefin content contained in the entire film was 8.1% by mass). Except for this, a polyolefin film and a laminate having a D layer deposited thereon were prepared in the same manner as in Example 2. The properties of the obtained polyolefin film and the laminate having a D layer deposited thereon are shown in Table 1.

[0276] (Example 4)

[0277] The same operation as in Example 2 was performed except that the layer structure was set to B / A / B, the polypropylene resin B2 was used for the B layer, and the film forming conditions were set as shown in Table 1, to produce a polyolefin film and a laminate having a D layer deposited thereon. The properties of the obtained polyolefin film and the laminate having a D layer deposited thereon are shown in Table 1. It should be noted that the deposition was performed on the B layer side in contact with the casting drum.

[0278] (Example 5)

[0279] The layer structure was set to B / A / B, and the components were mixed so that the polyolefin resin raw material (AM2) was 63 parts by mass, the polypropylene resin (A1) was 36.6 parts by mass, and the antioxidant was 0.4 parts by mass, and the components were supplied to the single screw melt extruder for the A layer. The lamination ratio and film forming conditions were set as shown in Table 1. A polyolefin film and a laminated body with a D layer deposited thereon were prepared in the same manner as in Example 2. The properties of the obtained polyolefin film and the laminated body with a D layer deposited thereon are shown in Table 1. It should be noted that the vapor deposition was performed on the B layer side in contact with the casting drum.

[0280] (Example 6)

[0281] The layer structure was made into a single A layer, and the components were mixed so that the polyolefin resin raw material (AM1) was 66.7 parts by mass, the polypropylene resin (A1) was 32.6 parts by mass, and the antioxidant was 0.4 parts by mass, and the components were supplied to a single screw melt extruder for the A layer. The film forming conditions were as shown in Table 1. Except for this, a polyolefin film and a laminated body with a D layer deposited thereon were prepared in the same manner as in Example 2. The properties of the obtained polyolefin film and the laminated body with a D layer deposited thereon are shown in Table 1. It should be noted that the deposition was performed on the surface in contact with the casting drum.

[0282] (Example 7)

[0283] As the B layer of Example 2, the components were mixed so that the polyolefin resin raw material (B1) was 95.6 parts by mass, the polyolefin resin raw material (BM1) was 4 parts by mass, and the antioxidant was 0.4 parts by mass, and the components were supplied to a single screw melt extruder for the B layer. As the A layer, the components were mixed so that the polyolefin resin raw material (AM1) was 28.6 parts by mass, the polypropylene resin (A1) was 67.6 parts by mass, and the antioxidant was 0.4 parts by mass, and the components were supplied to a single screw melt extruder for the A layer (the cyclic olefin resin contained in the A layer was 8.6% by mass, and the thickness ratio of the A layer to the entire film was about 83%, so the cyclic olefin resin contained in the entire film was 7.1% by mass). Except that the film forming conditions were set as shown in Table 1, a polyolefin film and a laminated body on which the D layer was vapor-deposited were prepared in the same manner as in Example 2. The properties of the obtained polyolefin film and the laminated body on which the D layer was vapor-deposited are shown in Table 1. It should be noted that the vapor deposition is performed on the surface in contact with the casting drum.

[0284] (Example 8)

[0285] As the B layer of Example 2, the components were mixed so that the polyolefin resin raw material (B1) was 87.6 parts by mass, the polyolefin resin raw material (BM1) was 12 parts by mass, and the antioxidant was 0.4 parts by mass, and the components were supplied to the single screw melt extruder for the B layer. As the A layer, the components were mixed so that the polyolefin resin raw material (AM1) was 28.6 parts by mass, the polypropylene resin (A1) was 67.6 parts by mass, and the antioxidant was 0.4 parts by mass, and the components were supplied to the single screw melt extruder for the A layer. Except that the film forming conditions were set as shown in Table 1, a polyolefin film and a laminated body on which the D layer was vapor-deposited were prepared in the same manner as in Example 2. The properties of the obtained polyolefin film and the laminated body on which the D layer was vapor-deposited are shown in Table 1. It should be noted that the vapor deposition was performed on the surface in contact with the casting drum.

[0286] (Example 9)

[0287] A polyolefin resin raw material (AM3) was used as the A layer of Example 8, and the film forming conditions were set as shown in Table 1. A polyolefin film and a laminate having a D layer deposited thereon were prepared in the same manner as in Example 8. The properties of the obtained polyolefin film and the laminate having a D layer deposited thereon are shown in Table 1. It should be noted that the vapor deposition was performed on the surface in contact with the casting drum.

[0288] (Example 10)

[0289] The film thickness was 3.1 μm, and the components were mixed so that the polyolefin resin raw material (AM1) as the A layer was 28.6 parts by mass, the polypropylene resin (A1) was 67.6 parts by mass, and the antioxidant was 0.4 parts by mass, and the mixture was supplied to a single screw melt extruder for the A layer, and the film forming conditions were as shown in Table 1. A polyolefin film was produced in the same manner as in Example 4, except that the film forming conditions were as shown in Table 1. The capacitor properties of the produced film are shown in Table 1.

[0290] (Example 11)

[0291] A polyolefin film was produced in the same manner as in Example 10 except that a polyolefin resin raw material (AM3) was used as the A layer of Example 10 and the film production conditions were set as shown in Table 1. Table 1 shows the capacitor properties of the produced film.

[0292] (Comparative Example 1)

[0293] A polyolefin film and a laminate having a D layer deposited thereon were prepared in the same manner as in Example 2 except that only the polypropylene resin A1 was used in the A layer without using a masterbatch and the film forming conditions were set as shown in Table 2. The properties of the obtained polyolefin film and the laminate having a D layer deposited thereon are shown in Table 2.

[0294] (Comparative Example 2)

[0295] The layer structure was set to B / A / B, no masterbatch was used for the A layer, the components were mixed so that the polypropylene resin A1 was 90 parts by mass, the cyclic olefin resin was 9.6 parts by mass, and the antioxidant was 0.4 parts by mass, and the components were supplied to the single screw melt extruder for the A layer, and the polypropylene resin B2 was used for the B layer, and the film forming conditions were set as shown in Table 2. A polyolefin film and a laminated body with a D layer deposited thereon were prepared in the same manner as in Example 2. The properties of the obtained polyolefin film and the laminated body with a D layer deposited thereon are shown in Table 2. It should be noted that the deposition was performed on the B layer side in contact with the casting drum.

[0296] (Comparative Example 3)

[0297] A laminate of a polyolefin film and a D layer deposited thereon was prepared in the same manner as in Example 2 except that the film forming conditions and the lamination ratio were set as shown in Table 2. Table 2 shows the properties of the obtained laminate of a polyolefin film and a D layer deposited thereon.

[0298] (Comparative Example 4)

[0299] The oxygen concentration in the raw material feeding hopper was set to 10%, the temperature condition during extrusion was set to 260°C instead of the multi-stage low temperature in which the temperature was gradually lowered from the extruder to the T-die, and the film forming conditions were set as shown in Table 2. A polyolefin film and a laminate having a D layer deposited thereon were prepared in the same manner as in Example 4. The properties of the obtained polyolefin film and the laminate having a D layer deposited thereon are shown in Table 2. It should be noted that the deposition was performed on the B layer side in contact with the casting drum.

[0300] (Comparative Example 5)

[0301] The laminate structure was set to B / A / B, the laminate thickness ratio was set to 1 / 8 / 1, and the components were mixed so that the polyolefin resin raw material (AM2) was 63 parts by mass, the polypropylene resin (A1) was 36.6 parts by mass, and the antioxidant was 0.4 parts by mass for the A layer, and the components were supplied to the single screw melt extruder for the A layer. The film forming conditions without biaxial stretching were shown in Table 2. Except for this, a polyolefin film and a laminated body with a D layer deposited thereon were prepared in the same manner as in Example 4. The properties of the obtained polyolefin film and the laminated body with a D layer deposited thereon are shown in Table 2. It should be noted that the deposition was performed on the B layer side in contact with the casting drum.

[0302] (Comparative Example 6)

[0303] A polyolefin film was produced in the same manner as in Example 4 except that the film thickness was set to 3.1 μm and the film production conditions were set as shown in Table 2. Table 2 shows the produced polyolefin film and film capacitor properties.

[0304] (Comparative Example 7)

[0305] A polyolefin-based film was produced in the same manner as in Comparative Example 2 except that the film thickness was set to 3.1 μm and the film production conditions were set as shown in Table 2. Table 2 shows the capacitor properties of the produced film.

[0306]

[0307]

[0308] Industrial Applicability

[0309] According to the present invention, a polyolefin film can be provided, which can reduce the reduction of structural stability, water vapor barrier properties and oxygen barrier properties associated with heating. Since the polyolefin film of the present invention has the above characteristics, it is suitable for packaging films that are easily degraded by water vapor and oxygen.

[0310] Explanation of symbols

[0311] 1 Part of section X

[0312] 2 Sea part

[0313] 3 island parts (areas)

[0314] 4A rectangle with a size of 1 μm × 2 μm in section X with one pair of sides parallel to the thickness direction

[0315] 5 A pair of sides parallel to the thickness direction

Claims

1. A polyolefin film, characterized in that: When the storage modulus in the main orientation axis direction at 50°C and 121°C obtained by dynamic viscoelasticity measurement at a frequency of 10 Hz is set to E'50 (Pa) and E'121 (Pa), respectively, E'121 / E'50 exceeds 0.25 and is less than 0.99, the heat shrinkage in the main orientation axis direction at 150°C is greater than -2% and less than 10%, the tensile elongation in the direction orthogonal to the main orientation axis is greater than 20% and less than 300%, and there is at least one layer comprising cyclic olefin resin and polypropylene resin, namely, layer A.

2. A polyolefin film comprising at least one layer comprising a cyclic olefin resin and a polypropylene resin, namely, layer A; when the cross section of layer A when cut by a plane parallel to the main orientation axis direction and the thickness direction is set as section X, in a rectangle of 1 μm×2 μm in size determined in section X with a pair of short sides parallel to the thickness direction, there are two or more regions of the cyclic olefin resin passing through the pair of short sides; when the storage modulus in the main orientation axis direction at 50°C and 121°C obtained by dynamic viscoelasticity measurement at a frequency of 10 Hz is set as E'50 (Pa) and E'121 (Pa), respectively, E'121 / E'50 exceeds 0.20 and is not more than 0.

99.

3. The polyolefin film according to claim 1 or 2, wherein tan δ50 / tan δ121 exceeds 0.25 and is not more than 0.99 when tan δ in the main orientation axis direction at 50°C and 121°C obtained by dynamic viscoelasticity measurement at a frequency of 10 Hz is defined as tan δ50 and tan δ121, respectively. The polyolefin film according to any one of claims 1 to 3, wherein when the layer B is a layer mainly composed of a polypropylene resin and having a lower content of a cyclic olefin resin than the layer A, the layer B is provided on at least one surface of the layer A.

5. The polyolefin film according to claim 4, wherein when a layer having a lower melting point than the A layer and the B layer and a melting point of 100°C to 150°C is set as the C layer, the B layer is located on one outermost surface and the C layer is located on the other outermost surface. The polyolefin film according to claim 4 or 5, wherein a ten-point region height S10z of at least one surface of the layer B measured by three-dimensional non-contact surface profilometry is 150 nm to 900 nm. 7 . The polyolefin-based film according to claim 4 , wherein the layer B contains 1% by mass or more and 10% by mass or less of a thermoplastic resin incompatible with the polypropylene-based resin. 8 . The polyolefin-based film according to claim 1 , comprising at least one of metal particles and inorganic compound particles. 9 . The polyolefin-based film according to claim 8 , wherein the inorganic compound particles include at least one of aluminum oxide, silicon dioxide, and oxides of aluminum and silicon. 10 . The polyolefin-based film according to claim 1 , comprising a polypropylene-based resin as a main component. 11 . The polyolefin film according to claim 1 , wherein the glossiness of at least one film surface exceeds 130% and is 160% or less. 12 . The polyolefin-based film according to claim 1 , which is a biaxially oriented film. 13 . A laminate comprising the polyolefin-based film according to claim 1 , and a layer D which is a layer containing a metal and an inorganic compound in a total amount of more than 50% by mass and not more than 100% by mass. 14 . The laminate according to claim 13 , wherein an average height Spk of protruding peaks on the surface of the D layer measured by a three-dimensional non-contact surface roughness meter is 10 nm to 400 nm. 15 . A packaging material comprising at least one of the polyolefin film according to claim 1 and the laminate according to claim 13 or 14 .

16. A package body formed by packaging contents with the packaging material according to claim 15. 17 . A metal film laminated film comprising a polyolefin film according to claim 1 , wherein a metal film is provided on at least one surface of the polyolefin film.

18. A thin film capacitor formed by using the metal film laminate film according to claim 17.

19. A power control unit comprising the film capacitor according to claim 18.

20. An electric vehicle comprising the power control unit according to claim 19.

21. An electric aircraft comprising the power control unit according to claim 19.

Citation Information

Patent Citations

  • Laminated film

    CN104661813A

  • Polypropylene film, metallized film, and film capacitor

    CN111051400A

  • Heat-shrinkable polyolefin laminated film

    JP2005014428A

  • Readily tearable co-extruded multilayer barrier film and packaging material

    WO2020050258A1