Spherical silica powder

By controlling the particle size grade and sphericity of the spherical silica powder and optimizing the particle size distribution, the problem of insufficient fluidity of molten spherical silica in the existing technology is solved, and better fluidity and molding performance are achieved.

CN118786089APending Publication Date: 2024-10-15DENKA CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380020957.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-09
Filing Date
2023-02-06
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing fused spherical silica has insufficient fluidity to meet the needs of certain applications.

Method used

By controlling the particle size grade and sphericity of the spherical silica powder, in particular, a sphericity S1 with a particle size of 5 μm or more and less than 10 μm, a sphericity S2 with a particle size of 10 μm or more and less than 20 μm, a particle size of 20 μm or more and less than 20 μm are set. Less than 30μm The sphericity S3 and the sphericity S4 with a particle size of 30 μm or more and less than 45 μm have a sphericity of 0.74 or more, and the average sphericity SAVE is calculated, combined with the particle size distribution and packing density measured by the wet laser diffraction and scattering method, and the particle size distribution is optimized to improve Liquidity.

Benefits of technology

Significantly improves the fluidity and moldability of spherical silica powder, enhances the mixability with resin and molding performance, and reduces the occurrence of molding defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786089A_ABST
    Figure CN118786089A_ABST
Patent Text Reader

Abstract

A spherical silica powder according to the present invention is configured such that, as measured using a wet flow image analyzer, the sphericity degree of a particle diameter of 5 [mu] m or more and less than 10 [mu] m is S1, the sphericity degree of a particle diameter of 10 [mu] m or more and less than 20 [mu] m is S2, and the sphericity degree of a particle diameter of 20 [mu] m or more and less than 30 [mu] m is S3; when a sphericity degree for a particle size of 30 [mu] m or more and less than 45 [mu] m is set as S4 and a sphericity degree for a particle size of 45 [mu] m or more is set as S5, at least two or more of S1, S2, S3, S4 and S5 are 0.74 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to spherical silicon dioxide powder. Background Art

[0002] Various developments have been made on spherical silica. As such a technique, for example, the technique described in Patent Document 1 is known. Patent Document 1 describes a method of obtaining molten spherical silica by spraying a siliceous raw material powder into a flame to melt the powder.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2001-261328 Summary of the invention

[0006] However, as a result of the investigation by the present inventors, it has been found that the fused spherical silica described in Patent Document 1 has room for improvement in terms of fluidity.

[0007] The present inventors have further studied and found that the flowability can be improved by appropriately controlling the sphericity of spherical silica powders of each particle size class, thereby completing the present invention.

[0008] According to one aspect of the present invention, the following spherical silica powder is provided.

[0009] 1. A spherical silica powder, wherein the sphericity of the particle size of 5 μm or more and less than 10 μm measured by a wet flow image analyzer is S1, the sphericity of the particle size of 10 μm or more and less than 20 μm is S2, the sphericity of the particle size of 20 μm or more and less than 30 μm is S3, the sphericity of the particle size of 30 μm or more and less than 45 μm is S4, and the sphericity of the particle size of 45 μm or more is S5,

[0010] At least two or more of S1, S2, S3, S4 and S5 are 0.74 or more.

[0011] 2. The spherical silicon dioxide powder according to 1., wherein

[0012] The average sphericity obtained by averaging the five values ​​of S1, S2, S3, S4, and S5 (excluding the value of 0) is defined as S. AVE When S AVE It is above 0.77.

[0013] 3. The spherical silicon dioxide powder according to 2., which is composed of:

[0014] In the volume frequency particle size distribution of the spherical silica powder measured by a wet laser diffraction scattering method, the particle diameter at which the cumulative value is 50% is defined as D 50 hour,

[0015] S AVE and D 50 Satisfy 0.01≤S AVE / D 50 ≤0.1.

[0016] 4. The spherical silica powder according to any one of 1. to 3.,

[0017] The tapped bulk density measured according to step B below is 1.2 g / cm 3 ~1.6g / cm 3 .

[0018] (Step B)

[0019] The spherical silica powder was naturally dropped from a height of 25 cm at a rate of 5 to 10 g per minute. 3 The inside of the measuring cup is filled with water until it overflows from the cup to prepare a full cup in the shape of a mountain.

[0020] Next, the portion of the cup that is filled in a mountain shape is scraped off without shaking it, and the mass (g) of the spherical silica powder filled in the cup is measured to calculate the loose bulk density (g / cm 3 ).

[0021] On the other hand, for the cup filled with a mountain shape, after vibrating 180 times in the up and down direction (stroke length 2 cm, 1 second / time), the part exceeding the upper surface of the cup was scraped off, and the mass (g) of the spherical silica powder filled in the cup was measured, and the tapped bulk density (g / cm 3 ).

[0022] 5. The spherical silicon dioxide powder according to 1. to 4.,

[0023] When the loose bulk density measured in step B is defined as A and the tapped bulk density is defined as P,

[0024] The degree of compression calculated based on ((P-A) / P)×100 is 15% to 50%.

[0025] 6. The spherical silicon dioxide powder according to any one of 1. to 5.,

[0026] In the volume frequency particle size distribution measured by the laser diffraction scattering method based on the wet method, the particle diameter at which the cumulative value is 10% is defined as D 10 The particle size with a cumulative value of 50% is set as D 50The particle size with a cumulative value of 97% is set as D 97 hour,

[0027] (D 97 -D 10 ) / D 50 It is 1.0~10.0.

[0028] 7. The spherical silicon dioxide powder according to any one of 1. to 6.,

[0029] In the volume frequency particle size distribution measured by the laser diffraction scattering method based on the wet method, the particle diameter at which the cumulative value is 50% is defined as D 50 The particle size with a cumulative value of 97% is set as D 97 hour,

[0030] D 97 / D 50 It is 2.0~30.0.

[0031] According to the present invention, a spherical silica powder having excellent fluidity is provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a schematic cross-sectional view showing the structure of a thermal spraying device for producing spherical silica powder. DETAILED DESCRIPTION

[0033] The outline of the spherical silica powder according to the present embodiment will be described.

[0034] The spherical silica powder of the present embodiment is constituted such that when the sphericity of the particle size of 5 μm or more and less than 10 μm measured using a wet flow image analyzer is set to S1, the sphericity of the particle size of 10 μm or more and less than 20 μm is set to S2, the sphericity of the particle size of 20 μm or more and less than 30 μm is set to S3, the sphericity of the particle size of 30 μm or more and less than 45 μm is set to S4, and the sphericity of the particle size of 45 μm or more is set to S5, at least two or more of S1, S2, S3, S4 and S5 are greater than 0.74.

[0035] At least two of S1, S2, S3, S4 and S5 are 0.74 or more, preferably 0.80 or more, and more preferably 0.84 or more. This can improve fluidity.

[0036] In addition, at least two, preferably three or more, and more preferably four or more of S1, S2, S3, S4, and S5 satisfy 0.74 or more. This can improve fluidity.

[0037] The average sphericity obtained by averaging the five values ​​of S1, S2, S3, S4, and S5 (excluding the value of 0) is defined as S.AVE The median diameter of the spherical silica powder measured by a wet flow image analyzer is defined as S 50 (μm).

[0038] S AVE The lower limit of S is, for example, 0.77 or more, preferably 0.82 or more, and more preferably 0.87 or more. This can improve fluidity. AVE The upper limit of may be, for example, 0.99 or less.

[0039] The sphericity of the spherical silica powder can be measured by following the following procedure A at room temperature of 25°C and humidity of 60%.

[0040] For the obtained spherical silica powder, a wet flow image analyzer (FPIA-3000 manufactured by Sysmex Corporation) was used to measure the sphericity (S1) of a particle size of 5 μm or more and less than 10 μm, the sphericity (S2) of a particle size of 10 μm or more and less than 20 μm, the sphericity (S3) of a particle size of 20 μm or more and less than 30 μm, the sphericity (S4) of a particle size of 30 μm or more and less than 45 μm, and the sphericity (S5) of a particle size of 45 μm or more.

[0041] The sphericity of each particle size class is the square value of the circularity of each particle size class.

[0042] In this embodiment, for example, by appropriately selecting the raw material components of the spherical silica powder, the method for producing the spherical silica powder, etc., the sphericity, S AVE and S 50 Among them, for example, the sphericity, S of each particle size grade of the above-mentioned S1, S2, S3, S4 and S5 can be adjusted by appropriately controlling the raw material supply amount, raw material particle size, flame temperature, combustible gas, combustion-supporting gas, dispersion gas and other melting flame conditions. AVE and S 50 The factors for setting the sphericity to the desired numerical range include (i) if the raw material supply amount is reduced, the sphericity increases, and if it is increased, the sphericity decreases; (ii) if the particle sizes of multiple raw materials are close to the average particle size, the sphericity increases, and the more it deviates from the average particle size, the lower the sphericity; (iii) the higher the flame temperature, the higher the sphericity, and if it is low, the sphericity decreases; (iv) the higher the temperature of the combustible gas, the higher the sphericity, and if it is low, the sphericity decreases; (v) the closer the combustion-supporting gas is to the theoretical ratio, the higher the sphericity, and the more it deviates from the theoretical ratio, the lower the sphericity; (vi) by appropriately introducing a dispersed gas, agglomeration is reduced and the sphericity is improved.

[0043] The spherical silica powder of the present embodiment can be configured such that, when the loose bulk density measured in the following step B is A and the tapped bulk density is P, the compression degree calculated based on ((P-A) / P))×100 is, for example, 15% to 50%.

[0044] The upper limit of the compression degree is, for example, 50% or less, preferably 40% or less, and more preferably 30% or less. This can improve fluidity.

[0045] The lower limit of the tapped bulk density (P) is, for example, 1.2 g / cm 3 Above, preferably 1.25 g / cm 3 More preferably, 1.3 g / cm 3 As a result, operability can be improved.

[0046] The upper limit of the tapped bulk density (P) is, for example, 1.6 g / cm 3 Below, preferably 1.5 g / cm 3 Below, more preferably 1.4 g / cm 3 Thereby, the miscibility with the resin can be improved.

[0047] The loose bulk density, tapped bulk density and compression of the spherical silicon dioxide powder can be measured at room temperature of 25° C. and humidity of 55% according to the following step B.

[0048] First, spherical silica powder was naturally dropped from a height of 25 cm at a rate of 5 to 10 g per minute. 3 The inside of the measuring cup is filled with water until it overflows from the cup to prepare a full cup in the shape of a mountain.

[0049] Next, the portion of the cup that is filled in a mountain shape is scraped off without shaking it, and the mass (g) of the spherical silica powder filled in the cup is measured to calculate the loose bulk density (g / cm 3 ).

[0050] On the other hand, for the cup filled with a mountain shape, after vibrating 180 times in the up and down direction (stroke length 2 cm, 1 second / time), the part exceeding the upper surface of the cup was scraped off, and the mass (g) of the spherical silica powder filled in the cup was measured, and the tapped bulk density (g / cm 3 ).

[0051] The volume frequency particle size distribution of the spherical silica powder was measured by a laser diffraction scattering method based on a wet method. In the volume frequency particle size distribution, the particle size at which the cumulative value was 10% was defined as D. 10 The particle size with a cumulative value of 50% is set as D 50 The particle size with a cumulative value of 97% is set as D97 .

[0052] Can be constructed as S AVE and D 50 Satisfy 0.01≤S AVE / D 50 ≤0.1.

[0053] S AVE / D 50 The lower limit of is, for example, 0.01 or more, preferably 0.015 or more, and more preferably 0.023 or more. This can improve the fluidity.

[0054] S AVE / D 50 The upper limit is, for example, 0.1 or less, preferably 0.75 or less, and more preferably 0.5 or less. This can improve fluidity.

[0055] (D 97 -D 10 ) / D 50 The upper limit of is, for example, 10.0 or less, preferably 7.0 or less, and more preferably 5.0 or less. This makes the width of the particle size distribution sharper and improves the fluidity.

[0056] On the other hand, (D 97 -D 10 ) / D 50 The lower limit of is, for example, 1.0 or more, preferably 1.1 or more, and more preferably 2.0 or more. Thus, the particle size distribution has a certain width, and the moldability can be improved.

[0057] D 97 / D 50 The upper limit of is, for example, 30.0 or less, preferably 20.0 or less, and more preferably 15.0 or less. Thus, the particle size of the coarse particles becomes sharp, and molding defects of the resin molded product caused by the coarse particles can be suppressed.

[0058] On the other hand, D 97 / D 50 The lower limit of is, for example, 2.0 or more, preferably 3.0 or more, and more preferably 5.0 or more. Thus, the particle size distribution has a certain width, and the fluidity and moldability can be improved.

[0059] The particle size distribution of spherical silica powder is a value based on particle size measurement using a laser diffraction light scattering method, and can be measured, for example, using "Model LS-13-230" (manufactured by Beckman Coulter) as a particle size distribution measuring machine. During the measurement, water is used as a solvent, and as a pretreatment, a homogenizer can be used to apply a 200W output for dispersion treatment for 1 minute. In addition, it is prepared so that the PIDS (Polarization Intensity Differential Scattering) concentration is 45-55%. It should be noted that the refractive index of water is 1.33, and the refractive index of the powder takes into account the refractive index of the material of the powder. For example, amorphous silica is measured with a refractive index of 1.50.

[0060] The method for producing the spherical silica powder according to the present embodiment will be described.

[0061] Spherical silica powder is also called molten spherical particles, which are produced by feeding silica raw material powder into a high-temperature flame formed by the combustion reaction of a combustible gas and a combustion-supporting gas, and melting and spheroidizing the powder above its melting point. If necessary, the molten spherical particles thus obtained can also be classified and sieved.

[0062] An example of a schematic diagram of a thermal spraying apparatus for producing spherical silica powder is shown in FIG. Figure 1 .

[0063] Figure 1 The thermal spraying device 100 is composed of a melting furnace 2 provided with a burner 1, cyclone separators 4, 6 for classifying molten spherical particles generated by high-temperature exhaust gas of the flame through suction by a blower 9, and a bag filter 8 for recovering fine powder that cannot be captured by the cyclone separators 4, 6.

[0064] The melting furnace 2 is constituted by a vertical furnace body, but is not limited thereto, and may be a so-called horizontal furnace or a tilted furnace which is placed horizontally and ejects flames in the horizontal direction.

[0065] The high-temperature exhaust gas is cooled by passing through pipes 3, 5, and 7 having water-cooling jackets.

[0066] The blower 9 may be connected to a suction gas amount control valve and a gas exhaust port (not shown).

[0067] A collected powder extraction device (not shown) may be connected to the lower portion of the melting furnace 2, the cyclone separators 4, 6, and the bag filter 8.

[0068] The classification can be performed using known equipment such as a gravity settling chamber, a cyclone separator, a classifier having rotary blades, etc. The classification operation can be incorporated into the conveying process of the molten spheroidized product, or can be performed in another pipeline after collectively capturing the molten spheroidized product.

[0069] As the combustible gas, for example, one or more of acetylene, propane, butane, etc. can be used, but propane, butane, or a mixed gas thereof having a relatively low calorific value is preferred.

[0070] As the combustion-supporting gas, for example, a gas containing oxygen can be used. Generally speaking, it is cheap and most preferred to use pure oxygen of more than 99 weight %. In order to reduce the calorific value of the gas, an inert gas such as air or argon can also be mixed into the combustion-supporting gas.

[0071] The spherical silicon dioxide powder may be amorphous and / or crystalline.

[0072] The amorphous rate of the spherical silica powder, for example, measured by the following method, is preferably 95% or more, and more preferably 97% or more. The amorphous rate is determined by the intensity ratio of a specific diffraction peak by using a powder X-ray diffraction device (e.g., RIGAKU company trade name "Model MiniFlex"), and performing X-ray diffraction analysis in the range of 26° to 27.5° of CuKα rays. In the case of siliceous powder, crystalline silica has a main peak at 26.7°, but there is no peak in amorphous silica. When amorphous silica and crystalline silica are mixed, a peak height of 26.7° corresponding to the proportion of crystalline silica can be obtained. Therefore, the crystalline silica mixing ratio is calculated based on the ratio of the X-ray intensity of the sample to the X-ray intensity of the crystalline silica standard sample (X-ray diffraction intensity of the sample / X-ray diffraction intensity of crystalline silica), and the amorphous rate is calculated by the formula Amorphous rate (%) = (1-crystalline silica mixing ratio) × 100.

[0073] The spherical silica powder preferably has a specific surface area S measured by the BET method. B The theoretical specific surface area S calculated from the particle size distribution C The ratio (S B / S C ) is, for example, 2.5 or less. This ratio is large, which means that it contains many ultrafine particles that cannot be detected by a particle size distribution measuring machine such as a laser diffraction method. From the viewpoint of suppressing the increase in viscosity when the spherical silica particles are added to the resin composition, the above S B / S C The value of is more preferably 2.5 or less, particularly 2.0 or less.

[0074] Specific surface area S BThis is a value based on the BET method and can be measured using, for example, "Model 4-SORBU2" (manufactured by YUASA IONICS Co., Ltd.) as a specific surface area measuring device.

[0075] For the theoretical specific surface area S C , can also be automatically calculated using the particle size distribution measuring machine mentioned above. The principle of the measuring machine is based on the formula S C =6 / (ρ·D). Where D is the area average particle size (μm), ρ is the density of the spherical silica powder (g / cm 3 ). For example, if the powder is amorphous silicon dioxide, it is 2.21.

[0076] It should be noted that D is obtained by the formula D = Σ(ni·ai·di) / Σ(ni·ai). This means that in one powder group, there are n1, n2, ···ni, ··nk particles having particle sizes from small to large d1, d2, ···di, ··dk, respectively. In addition, when the surface area of ​​each particle is set to a1, a2, ···ai, ··ak, respectively, D is obtained by D = (n1·a1·d1+n2·a2·d2+···+ni·ai·di+···+nk·ak·dk) / (n1·a1·+n2·a2+···+ni·ai+···+nk·ak).

[0077] It is preferred that the spherical silica powder does not substantially contain particles smaller than 50 nm, because this can suppress an increase in viscosity when mixed with a resin composition.

[0078] Substantially containing no particles smaller than 50 nm means that the number of particles smaller than 50 nm in any 100 photographs taken with an electron microscope at a magnification of 50,000 times is counted and the average value per photograph is less than 50. The number of particles smaller than 50 nm is preferably small.

[0079] Electron microscope photographs can be taken using a field emission scanning electron microscope (model "FE-SEM, JSM-6301F" manufactured by JEOL Ltd.) at an acceleration voltage of 15 kV and an irradiation current of 3×10-11 A. As a pre-treatment for photographing, carbon is evaporated on the spherical silica powder for 2 seconds using a vacuum evaporation device (model "JEE-4X" manufactured by JEOL Ltd.) and then gold-palladium is evaporated for 60 seconds.

[0080] A material obtained by blending the spherical silica powder of the present invention with a resin composition can be suitably used as a resin molding material.

[0081] Next, the resin composition according to the present embodiment will be described.

[0082] The resin composition contains a resin, a known resin additive, and the like in addition to the spherical silica powder of the present invention.

[0083] In the resin composition, the spherical silica powder can be used alone or mixed with other fillers. The resin composition can contain 10 to 99% by mass of spherical silica powder, or can also contain 10 to 99% by mass of a mixed inorganic powder containing spherical silica powder and other fillers. In addition, in the mixed inorganic powder, the content of other fillers is, for example, 1 to 20% by mass, or 3 to 15% by mass relative to 100% by mass of the spherical silica powder.

[0084] In addition, in this specification, unless otherwise specified, "to" means that the upper limit value and the lower limit value are included.

[0085] Examples of other fillers include alumina, titanium dioxide, silicon nitride, aluminum nitride, silicon carbide, talc, calcium carbonate, etc. The other fillers have an average particle size of about 5 to 100 μm, and their particle size composition and shape are not particularly limited.

[0086] Examples of the resin include epoxy resins, silicone resins, phenolic resins, melamine resins, urea-formaldehyde resins, unsaturated polyesters, fluororesins, polyamides such as polyimide, polyamide-imide, and polyether-imide, polyesters such as polybutylene terephthalate and polyethylene terephthalate, polyphenylene sulfide, fully aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS resins, AAS (acrylonitrile acrylic rubber styrene) resins, and AES (acrylonitrile, ethylene, propylene, diene rubber-styrene) resins, etc. These resins may be used alone or in combination of two or more thereof.

[0087] The resin composition can be produced by, for example, mixing the raw material components in a predetermined quantitative ratio using a mixer, Henschel mixer or the like, kneading the mixture using a heating roll, a kneader, a single-screw or twin-screw extruder or the like, and then pulverizing the mixture after cooling.

[0088] The embodiments of the present invention have been described above, but these are examples of the present invention, and various configurations other than the above can be adopted. In addition, the present invention is not limited to the above embodiments, and modifications and improvements within the scope of achieving the purpose of the present invention are included in the present invention.

[0089] Example

[0090] Hereinafter, the present invention will be described in detail with reference to Examples, but the present invention is not limited at all to the description of these Examples.

[0091] <Manufacturing of spherical silica powder>

[0092] use Figure 1 The thermal spraying device 100 shown is used to produce spherical silicon dioxide powder. The thermal spraying device has a burner 1 disposed on the upper part of a melting furnace 2, and a collection system pipeline composed of cyclone separators 4 and 6 and a bag filter 8 is directly connected to the lower part.

[0093] The burner 1 has a double-tube structure capable of forming an inner flame and an outer flame, and is disposed on the top of the melting furnace 2, and is connected to a combustible gas supply pipe 11, a combustion-supporting gas supply pipe 12, and a raw material supply pipe 13 respectively.

[0094] In the melting furnace 2, the silicon dioxide raw material powder is supplied to the high temperature flame from the raw material supply pipe 13 to be melted, and spheroidized molten spherical particles can be formed. The molten spherical particles passing through the melting furnace 2 are sucked by the blower 9 together with the combustion exhaust gas, move with the air in the pipes 3, 5, 7, and are classified and captured by the cyclone separators 4, 6 or the bag filter 8.

[0095] (Examples 1 to 12, Comparative Examples 1 to 2)

[0096] Using the thermal spraying device 100, LPG as a combustible gas is supplied from the combustible gas supply pipe 11, and oxygen as a combustion-supporting gas is supplied from the combustion-supporting gas supply pipe 12. In the burner 1, a high-temperature flame is formed by the combustion of LPG and oxygen. The carrier gas as a raw material is set to 20 Nm 3 / hr, and the supply rate of combustible gas to the burner is set to 8Nm 3 / hr, and the supply rate of combustion-supporting gas is set to 20Nm 3 / hr. Natural silica powder (average particle size 5 μm to 50 μm) was supplied to the flame formed as described above to obtain spherical amorphous silicon dioxide powder. The obtained powder was classified and the classified powders were mixed to obtain powders of Examples 1 to 12.

[0097] (Comparative Examples 1-2)

[0098] Spherical silica powder was obtained in the same manner as in the above-mentioned Example except for the powder supply amount and the flame forming conditions.

[0099] Comparative Example 1 The powder supply amount was set to 2.0 times that of Example 1, and the carrier gas as the raw material was set to 20 Nm 3 / hr, and the supply rate of combustible gas to the burner is set to 5Nm 3 / hr, and set the supply rate of combustion-supporting gas to 15Nm 3 / hr.

[0100] Comparative Example 2 The powder supply amount was set to 3.3 times that of Example 1, and the carrier gas as the raw material was set to 15 Nm 3 / hr, and the supply rate of combustible gas to the burner is set to 4Nm3 / hr, and set the supply rate of combustion-supporting gas to 15Nm 3 / hr.

[0101]

[0102] <Sphericity>

[0103] The sphericity of the spherical silica powder was determined as follows under the conditions of room temperature of 25° C. and humidity of 60%.

[0104] For the obtained spherical silica powder, a wet flow image analyzer (FPIA-3000 manufactured by Sysmex Corporation) was used to measure the sphericity (S1) of a particle size of 5 μm or more and less than 10 μm, the sphericity (S2) of a particle size of 10 μm or more and less than 20 μm, the sphericity (S3) of a particle size of 20 μm or more and less than 30 μm, the sphericity (S4) of a particle size of 30 μm or more and less than 45 μm, and the sphericity (S5) of a particle size of 45 μm or more.

[0105] [Measurement Procedure]

[0106] The measurement sample used in the above-mentioned wet flow image analysis apparatus was prepared as follows.

[0107] 0.05 g of spherical silica powder sample was weighed in a 20 ml glass beaker container, 10 ml of 25 mass % aqueous solution of propylene glycol was added, and then dispersed for 3 minutes using an ultrasonic disperser (ASU-10M manufactured by AS ONE). All of it was placed in FPIA-3000 and measured in LPF mode / quantitative counting (total count number 100, repeated measurement number 1).

[0108] The wet flow image analyzer is used to analyze the circumference of a particle projection image and the circumference of a circle corresponding to the area of ​​the particle projection image, and the circularity is calculated using the following formula.

[0109] Circularity = (circumference of particle projection image) / (circumference of the circle equivalent to the area of ​​particle projection image)

[0110] The sphericity and circularity are average values ​​of particles within the range of each particle size class.

[0111] Sphericity is the square of the circularity of each particle size class.

[0112] In addition, the average sphericity (S1, S3, S4 and S5) is calculated from the average of the four values ​​(excluding those with a value of 0). AVE ).

[0113] <Loose bulk density, tapped bulk density, compression>

[0114] Under the conditions of room temperature of 25° C. and humidity of 60%, the loose bulk density, tapped bulk density and degree of compression of the spherical silica powder were determined as follows.

[0115] The obtained spherical silica powder was naturally dropped from a height of 25 cm at a rate of 5 to 10 g per minute. 3 The inside of the measuring cup is filled with water until it overflows from the cup to prepare a full cup in the shape of a mountain.

[0116] Next, the portion of the cup that is filled in a mountain shape is scraped off without shaking it, and the mass (g) of the spherical silica powder filled in the cup is measured to calculate the loose bulk density (g / cm 3 ).

[0117] On the other hand, for the cup filled with a mountain shape, after vibrating 180 times in the up and down direction (stroke length 2 cm, 1 second / time), the part exceeding the upper surface of the cup was scraped off, and the mass (g) of the spherical silica powder filled in the cup was measured, and the tapped bulk density (g / cm 3 ).

[0118] When the loose bulk density obtained by the above-mentioned procedure is defined as A and the tapped bulk density is defined as P, the compression degree (%) is determined based on the formula: ((P-A) / P)×100.

[0119] <Particle size distribution>

[0120] The obtained spherical silica powder was measured by a particle size distribution measuring device (LS-13-230 manufactured by Beckman Coulter) using a laser diffraction scattering method based on a wet method to determine the volume frequency particle size distribution. Water was used as a solvent, and as a pretreatment, a homogenizer was used to apply an output of 200 W for 1 minute for dispersion treatment. In addition, the PIDS (Polarization Intensity Differential Scattering) concentration was prepared and measured at 45 to 55%.

[0121] Based on the obtained volume frequency particle size distribution, calculate the particle size D with a cumulative value of X%. X .

[0122] <Flowability of resin composition>

[0123] 90 parts by mass of the obtained silica powder and biphenyl epoxy resin (Japan Epoxy 5.5 parts by mass of phenolic resin (YX-4000HK manufactured by Resin Co., Ltd.), 4.8 parts by mass of phenolic resin (phenol aralkyl resin, MEHC-7800S manufactured by Meiwa Chemicals Co., Ltd.), 0.15 parts by mass of triphenylphosphine (manufactured by Hokuko Chemical Industry Co., Ltd.: TPP) and 0.35 parts by mass of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.: KBM-573) were mixed under the conditions of room temperature and a rotation speed of 2000 rpm, and the obtained mixture was heated and kneaded in a co-rotating intermeshing twin-screw extruder (screw diameter D = 25 mm, L / D = 10.2, blade rotation speed 50 to 120 rpm, ejection amount 3.0 kg / Hr, kneaded material temperature 98 to 100°C) to obtain a resin composition.

[0124] The obtained resin composition was used and molded using a spiral flow mold according to EMMI-1-66 (Epoxy Molding Material Institute; Society of Plastic Industry) at a mold temperature of 175° C., a molding pressure of 7.4 MPa, and a holding time of 90 seconds.

[0125] The resin composition with a spiral flow of 120 cm or more was evaluated as good, and the resin composition with a spiral flow of less than 120 cm was evaluated as poor.

[0126] <Moldability of resin composition>

[0127] Using the resin composition obtained in the evaluation of the above <Flowability of the resin composition>, a 48-pin TSOP sealed with an analog component was produced using a transfer molding machine using a mold with a resin thickness of 70 μm above and below the chip, and visual inspection was performed to see if there were any appearance defects such as lack of filling. The evaluation of no appearance defects was good, and the evaluation of appearance defects was poor.

[0128] The mold temperature was 175° C., the molding pressure was 7.4 MPa, and the holding time was 120 seconds. After molding, post-curing was performed at 155° C. for 6 hours.

[0129] The spherical silica powders of Examples 1 to 12 showed a result that the flowability was improved compared with Comparative Example 1, and a result that the moldability was improved compared with Comparative Example 2.

[0130] This application claims the benefit of priority based on Japanese patent application No. 2022-018509, filed on February 9, 2022, the disclosure of which is incorporated herein in its entirety.

[0131] Explanation of symbols

[0132] 1 Burner

[0133] 2 Melting furnace

[0134] 3Piping

[0135] 4 Cyclone separator

[0136] 5 piping

[0137] 6 Cyclone separator

[0138] 7Piping

[0139] 8-Bag Filter

[0140] 9 Blower

[0141] 11 Combustible gas supply pipe

[0142] 12 Combustion-supporting gas supply pipe

[0143] 13Raw material supply pipe

[0144] 100 Thermal Spraying Equipment

Claims

1. A spherical silica powder, wherein the sphericity of the particle size of 5 μm or more and less than 10 μm measured by a wet flow image analyzer is S1, the sphericity of the particle size of 10 μm or more and less than 20 μm is S2, the sphericity of the particle size of 20 μm or more and less than 30 μm is S3, the sphericity of the particle size of 30 μm or more and less than 45 μm is S4, and the sphericity of the particle size of 45 μm or more is S5, At least two or more of S1, S2, S3, S4 and S5 are 0.74 or more.

2. The spherical silicon dioxide powder according to claim 1, The average sphericity obtained from the average of S1, S2, S3, S4, and S5 is defined as S. AVE When S AVE is above 0.77, among which, When calculating the average value, exclude S1, S2, S3, S4, and S5 whose values ​​are 0.

3. The spherical silicon dioxide powder according to claim 2, wherein: In the volume frequency particle size distribution of the spherical silica powder measured by a wet laser diffraction scattering method, the particle diameter at which the cumulative value is 50% is defined as D 50 hour, S AVE and D 50 Satisfy 0.01≤S AVE / D 50 ≤0.

1.

4. The spherical silicon dioxide powder according to any one of claims 1 to 3, The tapped bulk density measured according to step B below is 1.2 g / cm 3 ~1.6g / cm 3 ; Step B: The spherical silica powder was naturally dropped from a height of 25 cm at a rate of 5 to 10 g per minute. 3 The inside of the measuring cup is filled with water until it overflows from the cup, and a full cup is prepared; Next, for the cup filled with a mountain shape, the part that exceeds the upper surface of the cup is scraped off without shaking it, and the mass of the spherical silica powder filled in the cup is measured in g, and the loose bulk density is calculated in g / cm 3 ; On the other hand, for the cup filled with a mountain shape, after vibrating 180 times in the up and down direction with a stroke length of 2 cm and 1 second per time, the part exceeding the upper surface of the cup was scraped off, and then the mass of the spherical silica powder filled in the cup was measured in g, and the tapped bulk density was calculated in g / cm 3 .

5. The spherical silicon dioxide powder according to claim 4, When the loose bulk density measured in step B is defined as A and the tapped bulk density is defined as P, The degree of compression calculated based on ((P-A) / P)×100 is 15% to 50%.

6. The spherical silicon dioxide powder according to any one of claims 1 to 5, In the volume frequency particle size distribution measured by the laser diffraction scattering method based on the wet method, the particle diameter at which the cumulative value is 10% is defined as D 10 The particle size with a cumulative value of 50% is set as D 50 The particle size with a cumulative value of 97% is set as D 97 hour, (D 97 -D 10 ) / D 50 It is 1.0~10.

0.

7. The spherical silicon dioxide powder according to any one of claims 1 to 6, In the volume frequency particle size distribution measured by the laser diffraction scattering method based on the wet method, the particle diameter at which the cumulative value is 50% is defined as D 50 The particle size with a cumulative value of 97% is set as D 97 hour, D 97 / D 50 It is 2.0~30.0.

Citation Information

Patent Citations

  • Silica powder and use thereof

    WO2007108437A1