Method for producing tempered glass, and tempered glass

By forming a compressive stress layer on the surface of chemically strengthened glass, and using polyvalent metal ions containing molten salt to adjust the stress distribution, the problem of deformation defects and uneven stress distribution in thin glass during chemical strengthening treatment is solved, and the shape of the strengthened glass is realized. Improved and strengthened protective glass for foldable devices.

CN118786102APending Publication Date: 2024-10-15NIPPON ELECTRIC GLASS CO LTD

Patent Information

Application Number
CN202280092855.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-18
Filing Date
2022-12-15
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Thin chemically strengthened glass is prone to deformation defects and uneven stress distribution during the chemical strengthening process of molten salt, resulting in poor shape problems.

Method used

A tempered glass manufacturing method that forms a compressive stress layer on the surface layer. A plate-like or film-like chemically strengthened glass of 0.2 mm or less is brought into contact with a molten salt containing polyvalent metal ions to adjust the stress distribution. It is preferable to use a molten salt containing alkaline earth metal nitrates. Salt, control immersion time and temperature, inhibit unnecessary ion exchange and stress changes.

Benefits of technology

Effectively eliminates deformation defects, improves the shape and strength characteristics of strengthened glass, is suitable for protective glass of foldable devices, and improves productivity and product flatness and strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786102A_ABST
    Figure CN118786102A_ABST
Patent Text Reader

Abstract

Provided is a method for producing tempered glass, which eliminates the defect of deformation caused by ion exchange in thin tempered glass and improves the shape of the tempered glass. This method for producing tempered glass obtains tempered glass having a compressive stress layer on the surface layer thereof, and is provided with: a preparation step for preparing plate-like or film-like chemically tempered glass having a thickness of 0.2 mm or less as processing glass; and an adjustment step in which, after the preparation step, the surface of the glass for treatment is brought into contact with an adjustment molten salt containing polyvalent metal ions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to strengthened glass, in particular to thin chemically strengthened glass. Background Art

[0002] In recent years, chemically strengthened glass with a thickness of about 0.4 mm to 1.0 mm has been often used as cover glass for various electronic terminals and display devices. So-called foldable smartphones and tablet PCs have been developed, which can fold the display surface of the display. In order to make the cover glass used in such devices bendable, the thickness is made thinner than before. For example, the technology of Patent Document 1 studies an extremely thin size of 0.5 mm or less.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application No. 2016-508954 Summary of the invention

[0006] Problems to be solved by the invention

[0007] However, the extremely thin glass described above is easily deformed compared to the thicker conventional glass, and therefore, when the chemical strengthening treatment using molten salt is performed, defects such as undulating deformation of the glass surface and wrinkle-like defects may occur. Such defects are considered to be caused, for example, by the following reasons: the degree of ion exchange is deviated due to the deviation of the adhesion state of the molten salt to the glass surface, resulting in deviation of the ion concentration distribution and stress distribution in the main surface direction of the glass.

[0008] An object of the present invention is to provide a method for producing tempered glass which eliminates deformation defects caused by ion exchange in thin tempered glass and improves the shape of the tempered glass, and to provide tempered glass improved by the method.

[0009] Means for solving problems

[0010] The method for producing tempered glass of the present invention is characterized in that it is a method for producing tempered glass having a compressive stress layer on the surface layer, and comprises the following steps: a preparation step of preparing a plate-shaped or film-shaped chemically tempered glass having a thickness of 0.2 mm or less as a treatment glass; and a conditioning step of bringing the surface of the treatment glass into contact with a conditioning molten salt containing polyvalent metal ions after the preparation step.

[0011] In the method for producing a tempered glass of the present invention, it is preferable that, in the adjusting step, stress distribution in a direction along the main surface of the process glass is adjusted.

[0012] In the method for producing tempered glass of the present invention, it is preferred that the adjusting molten salt used in the adjusting step contains alkaline earth metal nitrate, and the concentration of the total amount of alkaline earth metal nitrate R(NO3)2 in the adjusting molten salt is 0.1 mass % to 100 mass %.

[0013] With such a configuration, unnecessary ion exchange of the processing glass can be suppressed, and variation in stress characteristics of the tempered glass in the adjustment step can be appropriately suppressed.

[0014] In the method for producing tempered glass of the present invention, it is preferable that the thickness of the process glass is 0.06 mm or less.

[0015] With such a structure, it is possible to obtain tempered glass that is particularly suitable for foldable devices.

[0016] In the method for producing a tempered glass of the present invention, it is preferred that, in the adjustment step, the time for immersing the treatment glass in the adjustment molten salt is 10 seconds to 600 seconds.

[0017] With such a configuration, it is possible to prevent the deformation defect from being eliminated due to the processing time of the adjustment step being too short, and the stress characteristics of the tempered glass from being deteriorated due to the processing time of the adjustment step being too long.

[0018] In the method for producing tempered glass of the present invention, it is preferable that the temperature of the adjusting molten salt is 350°C to 565°C.

[0019] With such a configuration, it is possible to suppress the occurrence of defects due to the molten residue of the adjusting molten salt in the adjusting step, and the decomposition of the molten salt and the generation of gas due to excessive heating.

[0020] In the method for producing tempered glass of the present invention, it is preferred that the adjusting molten salt used in the adjusting step contains, by mass%, 0.5% to 45% of Ca(NO3)2 and 55% to 99.5% of KNO3+NaNO3 (the total amount of KNO3 and NaNO3).

[0021] With such a configuration, the adjustment molten salt can be obtained using a material that is easy to manage and low in cost.

[0022] In the method for producing tempered glass of the present invention, it is preferred that the content of LiNO 3 in the adjusting molten salt used in the adjusting step is less than 5 mass %.

[0023] With such a configuration, it is possible to suppress the excessive release of alkali metal ions from the processing glass, and appropriately suppress the variation in the stress characteristics of the tempered glass in the adjustment step.

[0024] In the method for manufacturing tempered glass of the present invention, it is preferred that the adjustment step is adjusted so that the ratio CS2 / CS1 of the outermost compressive stress value CS2 of the compressive stress layer of the tempered glass after the adjustment step to the outermost compressive stress value CS1 of the compressive stress layer of the treatment glass before the adjustment step becomes 0.8 to 1.

[0025] With such a configuration, it is possible to suppress the variation in stress characteristics before and after the adjustment step to be small.

[0026] In the method for producing the tempered glass of the present invention, it is preferable to adjust the adjustment step so that the compressive stress value CS2 of the outermost surface of the compressive stress layer of the tempered glass after the adjustment step becomes 400 MPa or more.

[0027] With such a configuration, the obtained tempered glass can have strength characteristics required as cover glass for devices such as smartphones and tablet PCs.

[0028] In the method for manufacturing tempered glass of the present invention, it is preferred that the adjustment step is adjusted so that the ratio DOL2 / DOL1 of the stress depth DOL2 of the compressive stress layer of the tempered glass after the adjustment step to the stress depth DOL1 of the compressive stress layer of the process glass before the adjustment step is 0.9 to 1.2.

[0029] With such a configuration, it is possible to suppress the variation in stress characteristics before and after the adjustment step to be small.

[0030] In the method for producing tempered glass of the present invention, it is preferable to adjust the adjustment step so that when the thickness of the tempered glass after the adjustment step is t2, the stress depth DOL2 of the compressive stress layer of the tempered glass becomes greater than or equal to 0.1·t2.

[0031] With such a configuration, the obtained tempered glass can have strength characteristics required as cover glass for smartphones, touch panel devices, and the like.

[0032] In the method for producing a tempered glass of the present invention, it is preferable that the warpage of the tempered glass after the adjustment step is 0.2 mm or less.

[0033] With such a configuration, the obtained tempered glass can have the flatness required as a cover glass for smartphones, touch panel devices, and the like.

[0034] In the method for producing tempered glass of the present invention, it is preferred that the tempered glass after the adjustment step contains, in mol %, 50% to 80% SiO2, 5% to 25% Al2O3, 0% to 15% B2O3, 0% to 15% Li2O, 1% to 20% Na2O, and 0% to 10% K2O as a glass composition.

[0035] Another embodiment of the method for manufacturing tempered glass of the present invention is characterized in that it is a method for manufacturing tempered glass having a compressive stress layer on the surface, and comprises the following steps: a preparation step of preparing a plate-shaped or film-shaped chemically tempered glass with a thickness of 0.2 mm or less into which alkali ions are introduced as a treatment glass; and an adjustment step of immersing the treatment glass in an adjustment molten salt after the preparation step; the adjustment molten salt contains 0.5% to 60% of Ca(NO3)2 and 40% to 99.5% of KNO3+NaNO3 as a composition in mass%.

[0036] The tempered glass of the present invention is characterized in that it is a plate-shaped or film-shaped tempered glass having a compressive stress layer with a thickness of 0.2 mm or less on the surface, the compressive stress value CS2 of the outermost surface of the compressive stress layer is 400 MPa or more, and the Ca ion concentration in the surface portion is higher than that in the interior. Here, the "surface portion" refers to a portion within 3 μm from the surface of the tempered glass.

[0037] Effects of the Invention

[0038] According to the present invention, shape defects of tempered glass caused by ion exchange can be corrected, and the productivity of tempered glass can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a flowchart showing a method for producing tempered glass according to an embodiment of the present invention.

[0040] Figure 2 This is an image obtained by observing the shape of the main surface of the tempered glass of Example No. 12 using a scanning white light interference microscope.

[0041] Figure 3 This is an image obtained by observing the shape of the main surface of the tempered glass of Example No. 5 using a scanning white light interference microscope.

[0042] Figure 4 This is an image obtained by observing the shape of the main surface of the tempered glass of Comparative Example No. 14 using a scanning white light interference microscope. DETAILED DESCRIPTION

[0043] Hereinafter, a method for producing tempered glass according to an embodiment of the present invention will be described.

[0044] <Method for producing tempered glass>

[0045] Figure 1 FIG. 1 is a flow chart showing a method for manufacturing tempered glass according to an embodiment of the present invention. Figure 1 As shown, the method for producing tempered glass of the present invention includes a preparation step S1, a first inspection step S2, an adjustment step S3, a cleaning / drying step S4, a second inspection step S5, and a packaging / shipping step S6.

[0046] The tempered glass of the present invention is obtained by carrying out the adjustment step S3 of bringing the treatment glass into contact with a polyvalent metal molten salt.

[0047] First, in the preparation step S1, a treatment glass is prepared. The treatment glass is a plate-shaped or film-shaped chemically strengthened glass having a uniform thickness of 0.2 mm or less that has been chemically strengthened in advance by ion exchange. Here, the film-shaped glass refers to, for example, a thin glass having a degree of flexibility that can be rolled into a roll or can be bent.

[0048] The process glass is produced by preparing a plate-shaped or film-shaped glass (hereinafter referred to as chemically strengthened glass) containing an alkali metal oxide as a composition in the preparation step S1 and subjecting the chemically strengthened glass to a chemical strengthening treatment.

[0049] In the present embodiment, the preparation step S1 includes a forming step S11 and a chemical strengthening step S12 .

[0050] The forming step 11 is a step of forming the chemically strengthened glass and processing it as needed. In the forming step S11, the chemically strengthened glass is obtained by cutting and processing a plate-shaped or film-shaped mother glass obtained by a forming method such as an overflow down-draw method, a slit down-draw method, a float method, or a redraw method into small pieces of glass. In order to obtain a smooth surface, the overflow down-draw method is preferably used as a forming method.

[0051] The end faces of the chemically strengthened glass are preferably chamfered and treated to improve strength by grinding, heat treatment, etching, etc. The main surface of the chemically strengthened glass can be ground, but for example, when the main surface is pre-smoothed by the overflow down-draw method, and the thickness is uniform and the precision is good, the main surface may not be ground, that is, it is used in a non-ground state. It should be noted that when the overflow down-draw method is formed and no grinding is performed, the main surface of the chemically strengthened glass becomes a fire-polished surface. The chemically strengthened glass can be further subjected to a thinning treatment to reduce the thickness by etching. It should be noted that in the present invention, the main surface refers to the surface and the back surface of the entire plate-like or sheet-like glass surface except the end face.

[0052] The chemically strengthened glass is preferably formed so that the treatment glass has a shape described below. The shape of the chemically strengthened glass is, for example, a rectangular shape having a thickness of 0.2 mm or less and long and short sides in a plan view.

[0053] The chemically strengthened glass preferably contains, by mol%, 50% to 80% SiO2, 5% to 25% A12O3, 0% to 15% B2O3, 0% to 15% Li2O, 1% to 20% Na2O, and 0 to 10% K2O as a glass composition.

[0054] The reasons why the above composition is preferred are shown below. In the description of the content range of each component, unless otherwise specified, % means mole %.

[0055] SiO2 is a component that forms a glass network. If the content of SiO2 is too little, it is difficult to vitrify. In addition, the thermal expansion coefficient becomes too high and the thermal shock resistance is easily reduced. Therefore, the suitable lower limit range of SiO2 is more than 50%, more than 55%, more than 57%, more than 59%, and especially more than 61%. On the other hand, if the content of SiO2 is too much, the solubility and formability are easily reduced. In addition, the thermal expansion coefficient becomes too low and it is difficult to match the thermal expansion coefficient of the surrounding materials. Therefore, the suitable upper limit range of SiO2 is less than 80%, less than 75%, less than 70%, less than 68%, less than 67.5%, and especially less than 67%.

[0056] A12O3 is a component that improves ion exchange performance, and is a component that improves strain point, Young's modulus, fracture toughness, and Vickers hardness. Therefore, the suitable lower limit range of A12O3 is more than 5%, more than 8%, more than 10%, more than 11%, and more than 11.2%. On the other hand, if the content of A12O3 is too much, the high-temperature viscosity rises, and the melting property and formability are easily reduced. In addition, devitrified crystals are easily precipitated on the glass, and it is difficult to utilize the overflow down-drawing method to form it into a plate shape. In particular, when using alumina-based refractory as a forming body refractory, when utilizing the overflow down-drawing method to form a glass sheet, devitrified crystals of spinel are easily precipitated at the interface with the alumina-based refractory. In addition, acid resistance is also reduced, and it is difficult to be applied to the acid treatment process. Therefore, the upper limit range of the suitable Al2O3 is 25% or less, 21% or less, 20.5% or less, 20% or less, 19.9% ​​or less, 19.5% or less, 19.0% or less, and particularly 18.9% or less. If the content of Al2O3, which has a great influence on the ion exchange performance, is set to a suitable range, it is easy to design CS / DOL to a high value even in 0.2 mm glass.

[0057] B2O3 is a component that reduces high temperature viscosity and density, stabilizes glass and makes it difficult for crystals to precipitate, and reduces the liquidus temperature. In addition, it is a component that suppresses Young's modulus, improves bending strength and crack resistance. However, if the content of B2O3 is too much, there is a tendency for surface coloring called color spots (Japanese: ヤケ) to occur through chemical strengthening treatment, or water resistance to decrease, or the compressive stress value of the compressive stress layer to decrease. Therefore, the suitable lower limit range of B2O3 is more than 0%, more than 0.01%, more than 0.02%, more than 0.1%, more than 0.3%, and the suitable upper limit range is less than 35%, less than 30%, less than 25%, less than 22%, less than 20%, and especially less than 15%. It should be noted that from the viewpoint of giving priority to improving CS, the content of B2O3 can be further preferably 0.2% to 5%, 0.3% to 1%. In addition, from the viewpoint of improving chemical durability for the purpose of suppressing defects during etching, the upper limit of the content of B2O3 may be preferably 1% or more, 1.5% or more, or 2% or more, and the lower limit may be 5% or less, 4.5% or less, 4% or less, or 3% or less. On the other hand, from the viewpoint of preferentially suppressing Young's modulus, the content of B2O3 may be further preferably 10% to 25%, 15% to 23%, or 18% to 22%.

[0058] Li2O is an ion exchange component, in particular, a component that makes the Li ions contained in the glass exchange with the K ions in the molten salt to obtain a high surface compressive stress value. In addition, Li2O is a component that reduces high temperature viscosity and improves solubility and formability. Therefore, the suitable lower limit range of Li2O is more than 0%, more than 0.01%, more than 0.5%, more than 1%, more than 3%, more than 4%, more than 4.2%, more than 5%, more than 5.5%, more than 6.5%, more than 7%, more than 7.3%, more than 7.5%, more than 7.8%, and especially more than 8%. Therefore, the suitable upper limit range of Li2O is less than 20%, less than 15%, less than 13%, less than 12%, less than 11.5%, less than 11%, less than 10.5%, less than 10%, especially less than 9.9%, less than 9%, and less than 8.9%.

[0059] Na2O is an ion exchange component, and is a component that reduces high temperature viscosity, improves solubility and formability. In addition, Na2O is also a component that improves devitrification resistance and reaction devitrification with formed body refractory, especially alumina refractory. If the content of Na2O is too little, the solubility is reduced, or the thermal expansion coefficient is excessively reduced, or the ion exchange rate is easily reduced. Therefore, the suitable lower limit range of Na2O is 5% or more, 7% or more, 8% or more, 8.5% or more, 9% or more, 9.5% or more, 10% or more, 11% or more, 12% or more, and especially 12.5% ​​or more. On the other hand, if the content of Na2O is too much, the phase separation produces viscosity and acid resistance is easily reduced. In addition, sometimes the component balance of the glass composition is lacking, and the devitrification resistance is reduced instead. Therefore, the suitable upper limit range of Na2O is 20% or less, 19.5% or less, 19% or less, 18% or less, 17% or less, 16.5% or less, 16% or less, 15.5% or less, and particularly 15% or less.

[0060] K2O is a component that reduces high temperature viscosity and improves solubility and formability. In addition, it is also a component that improves resistance to devitrification and increases Vickers hardness. However, if the content of K2O is too much, phase separation will cause viscosity and acid resistance will be easily reduced. In addition, sometimes the component balance of the glass composition is lacking, and the resistance to devitrification is reduced. Therefore, the suitable lower limit range of K2O is more than 0%, more than 0.01%, more than 0.02%, more than 0.1%, more than 0.5%, more than 1%, more than 1.5%, more than 2%, more than 2.5%, more than 3%, and especially more than 3.5%, and the suitable upper limit range is less than 10%, less than 5.5%, less than 5%, and especially less than 4.5%.

[0061] Li2O and Na2O are components that exchange ions with K ions in molten salt to obtain high surface compressive stress values. Therefore, the suitable lower limit range of Li2O+Na2O is 1% or more, 3% or more, 4% or more, 5% or more, 6% or more, 7% or more, 8% or more, 9% or more, 10% or more, 11% or more, 12% or more, 13% or more, 14% or more, 15% or more, 16% or more, 17% or more, 18% or more, and especially 18.5% or more in terms of mole %. On the other hand, if the content of Li2O+Na2O is too much, the thermal expansion coefficient becomes too high, and the thermal shock resistance is easily reduced. In addition, sometimes the component balance of the glass composition is destroyed, but the resistance to devitrification is reduced. Therefore, the suitable upper limit range of Li2O+Na2O is less than 20%, especially less than 19%.

[0062] In addition to the above components, the chemically strengthened glass may contain, for example, the following components as a glass composition.

[0063] MgO is a component that reduces high temperature viscosity, improves solubility, formability, strain point and Young's modulus, and is a component that has the greatest effect of improving ion exchange performance among alkaline earth metal oxides. However, if the content of MgO is too much, the density and thermal expansion coefficient are likely to increase, and the glass is likely to lose clarity. Therefore, the upper limit range of MgO is preferably below 12%, below 10%, below 8%, below 6%, and particularly below 5%. It should be noted that when MgO is introduced into the glass composition, the lower limit range of MgO is preferably above 0.1%, above 0.5%, above 1%, and particularly above 2%.

[0064] Compared with other components, CaO has a greater effect of reducing high temperature viscosity, improving solubility, formability, strain point, and Young's modulus without reducing devitrification resistance. The content of CaO is preferably 0% to 10%. However, if the content of CaO is too much, the density and thermal expansion coefficient become high, and the component balance of the glass composition is lacking, and the devitrification resistance and ion exchange performance of the glass are easily reduced. Therefore, the suitable content of CaO is 0% to 5%, 0.01% to 4%, 0.1% to 3%, and especially 1% to 2.5%.

[0065] SrO is a component that reduces high temperature viscosity without reducing devitrification resistance, and improves solubility, formability, strain point, and Young's modulus. However, if the SrO content is too high, the density and thermal expansion coefficient become higher, or the ion exchange performance decreases, or the glass composition lacks a balance of components, and the glass is prone to devitrification. The suitable content range of SrO is 0% to 5%, 0% to 3%, 0% to 1%, and particularly 0% to less than 0.1%.

[0066] BaO is a component that reduces high temperature viscosity without decreasing devitrification resistance, and improves solubility, formability, strain point, and Young's modulus. However, if the BaO content is too high, the density and thermal expansion coefficient become higher, or the ion exchange performance decreases, or the glass composition lacks a balance of components, and the glass is prone to devitrification. The suitable content range of BaO is 0% to 5%, 0% to 3%, 0% to 1%, and particularly 0% to less than 0.1%.

[0067] ZnO is a component that improves ion exchange performance, and is particularly effective in increasing the compressive stress value. In addition, it is a component that does not reduce low-temperature viscosity but reduces high-temperature viscosity. However, if the ZnO content is too much, there is a tendency for glass phase separation, reduced devitrification resistance, increased density, or reduced stress depth of the compressive stress layer. Therefore, the ZnO content is preferably 0% to 6%, 0% to 5%, 0% to 1%, 0% to 0.5%, and particularly 0% to less than 0.1%.

[0068] ZrO2 is a component that significantly improves the ion exchange performance, and is a component that improves the viscosity and strain point near the liquidus viscosity, but if its content is too much, the resistance to devitrification may be significantly reduced, and the density may become too high. Therefore, the suitable upper limit range of ZrO2 is less than 10%, less than 8%, less than 6%, and especially less than 5%. It should be noted that when it is desired to improve the ion exchange performance, it is preferred to introduce ZrO2 into the glass composition. In this case, the suitable lower limit range of ZrO2 is more than 0.001%, more than 0.01%, 0.5%, and especially more than 1%.

[0069] P2O5 is a component that improves ion exchange performance, and in particular, increases the stress depth of the compressive stress layer. In addition, it is a component that suppresses the Young's modulus to a low level. However, if the content of P2O5 is too much, the glass is prone to phase separation. Therefore, the content of P2O5 is preferably 0% to 10%, 0% to 8%, 0% to 6%, 0% to 4%, 0% to 2%, 0% to 1%, and particularly preferably 0% to less than 0.1%.

[0070] As a clarifier, 0ppm to 30000ppm (3%) of one or more selected from the group consisting of As2O3, Sb2O3, SnO2, F, Cl, SO3 (preferably the group consisting of SnO2, Cl, SO3) can be introduced. From the viewpoint of reliably enjoying the clarification effect, the content of SnO2+SO3+Cl is preferably 0ppm to 10000ppm, 50ppm to 5000ppm, 80ppm to 4000ppm, 100ppm to 3000ppm, and particularly preferably 300ppm to 3000ppm. Here, "SnO2+SO3+Cl" refers to the total amount of SnO2, SO3 and Cl.

[0071] The suitable content range of SnO2 is 0ppm to 10000ppm, 0ppm to 7000ppm, and particularly 50ppm to 6000ppm. The suitable content range of Cl is 0ppm to 1500ppm, 0ppm to 1200ppm, 0ppm to 800ppm, 0ppm to 500ppm, and particularly 50ppm to 300ppm. The suitable content range of SO3 is 0ppm to 1000ppm, 0ppm to 800ppm, and particularly 10ppm to 500ppm.

[0072] Rare earth oxides such as Nd2O3 and La2O3 are components that increase the Young's modulus. In addition, if a complementary color is added, the color is reduced and the color tone of the glass can be controlled. However, the cost of the raw materials themselves is high, and if a large amount is introduced, the resistance to devitrification is easily reduced. Therefore, the content of rare earth oxides is preferably 0% to 4%, 0% to 3%, 0% to 2%, 0% to 1%, and particularly preferably 0% to 0.5%.

[0073] In the present invention, from the perspective of environmental considerations, it is preferred that As2O3, F, PbO, and Bi2O3 are substantially not contained. Here, "substantially containing no As2O3" means that although As2O3 is not actively added as a glass component, it is allowed to be mixed at an impurity level. Specifically, it means that the content of As2O3 is less than 500ppm. "Substantially containing no F" means that although F is not actively added as a glass component, it is allowed to be mixed at an impurity level. Specifically, it means that the content of F is less than 500ppm. "Substantially containing no PbO" means that although PbO is not actively added as a glass component, it is allowed to be mixed at an impurity level. Specifically, it means that the content of PbO is less than 500ppm. "Substantially containing no Bi2O3" means that although Bi2O3 is not actively added as a glass component, it is allowed to be mixed at an impurity level. Specifically, it means that the content of Bi2O3 is less than 500ppm.

[0074] As an example, the chemically strengthened glass may not contain B2O3 as a glass composition, or contain a very small amount of B2O3, and limit its content. That is, the chemically strengthened glass may contain 50% to 80% SiO2, 5% to 25% Al2O3, 0% to 1% B2O3, 0% to 20% Li2O, 1% to 20% Na2O, and 0% to 10% K2O as a glass composition in mol%.

[0075] As another example, as a glass composition, the chemically strengthened glass may contain B2O3 as an essential component. That is, the chemically strengthened glass may contain 50% to 80% of SiO2, 5% to 25% of Al2O3, 1% to 5% of B2O3, 0% to 20% of Li2O, 1% to 20% of Na2O, and 0% to 10% of K2O as a glass composition in mol%.

[0076] Note that when chemically strengthened glass contains B2O3 as an essential component in its glass composition, there is a concern that the formability of the glass may decrease. Therefore, in order to achieve a balance, for example, the content of other components such as Al2O3 can be restricted. That is, the chemically strengthened glass can contain, in mol%, 50% to 80% of SiO2, 5% to 10% of Al2O3, 1% to 5% of B2O3, 0% to 20% of Li2O, 1% to 20% of Na2O, and 0% to 10% of K2O as the glass composition.

[0077] Note that the composition of the above-mentioned chemically strengthened glass is an example, and as long as chemical strengthening can be performed by ion exchange, chemically strengthened glass with a known composition can be used. In addition, for the treated glass obtained by chemically strengthening the above-mentioned chemically strengthened glass (i.e., the chemical strengthening step S12) and the strengthened glass obtained after the adjustment step S3, in the part where ion exchange has not been performed, it becomes the same composition as that of the chemically strengthened glass before chemical strengthening.

[0078] The chemically strengthened glass obtained in the forming step S11 is chemically strengthened in the chemical strengthening step S12. The chemical strengthening step S12 is a step of chemically strengthening the chemically strengthened glass by immersing it in an alkali metal molten salt (Japanese original text: アル力リ溶融 ). In the present embodiment, the case where the chemically strengthened glass is chemically strengthened by one-time chemical strengthening treatment is exemplified.

[0079] The above-mentioned alkali metal molten salt is a salt containing alkali metal ions capable of ion-exchanging with the components in the chemically strengthened glass, typically alkali metal nitrates (Japanese original text: アル力リ硝酸 ). Examples of the alkali metal nitrates include NaNO3, KNO3, LiNO3, etc., and they can be used alone (100% by mass) or in combination of multiple kinds. The mixing ratio when mixing multiple alkali metal nitrates can be determined arbitrarily. For example, in mass%, it can be 5% to 95% of NaNO3 and 5% to 95% of KNO3, preferably 30% to 80% of NaNO3 and 20% to 70% of KNO3, more preferably 50% to 70% of NaNO3 and 30% to 50% of KNO3.

[0080] The conditions such as the temperature of the molten salt and the immersion time in the chemical strengthening treatment can be set according to the composition, etc. within the range where the above-mentioned stress characteristics can be obtained. The temperature of the molten salt is, for example, 350°C to 500°C, preferably 355°C to 470°C, 360°C to 450°C, 365°C to 430°C, 370°C to 410°C. In addition, the immersion time is, for example, 3 minutes to 300 minutes, preferably 5 minutes to 120 minutes, more preferably 7 minutes to 100 minutes.

[0081] The chemically strengthened glass immersed in the alkali metal molten salt may be preheated to the temperature of the strengthening molten salt in the chemical strengthening step S12, or may be immersed in the strengthening molten salt while being kept at room temperature (eg, 1° C. to 40° C.).

[0082] After the chemical strengthening step S12, the processing glass is obtained. After the chemical strengthening step S12, the processing glass is preferably cleaned and dried. By cleaning, the attached matter attached to the processing glass can be removed. In addition, by drying the processing glass after cleaning, the alkali metal ions can be prevented from flowing into the attached water.

[0083] It should be noted that the content of the above-mentioned preparation step S1 of the treatment glass is an example, and it can be modified as follows. Specifically, it is also possible to obtain a pre-formed ion exchange glass, that is, to omit the forming step S11 and perform the treatment in the chemical strengthening step S12. In addition, it is also possible to prepare the treatment glass by obtaining a treatment glass that has been processed (formed and ion exchanged) in advance in a manner having the above-mentioned composition and characteristics, thereby omitting the forming step S11 and the chemical strengthening step S12.

[0084] The process glass prepared in the preparation step S1 is inspected in the first inspection step S2.

[0085] The first inspection step S2 is a step of inspecting whether the shape of the process glass prepared in the preparation step S1 is good. Specifically, the process glass is inspected by the operator's visual inspection, using an image inspection device, etc., to see whether it has deformation defects such as undulating shapes and wrinkled shapes. In the first inspection step S2, if a deformation defect is found in the process glass, the next adjustment step S3 is performed on the process glass. On the other hand, if no deformation defect is found and it meets the standards as a product, the process glass is not subjected to the adjustment step S3 and is subjected to the packaging / shipping step S5 as a tempered glass product.

[0086] The adjustment step S3 is a step of correcting the deformation of the processing glass in which the deformation defect was found in the first inspection step S2 to flatten the shape of the glass. Specifically, the processing glass is immersed in a molten salt for adjustment containing polyvalent metal ions to adjust the stress distribution along the main surface.

[0087] The polyvalent metal salt contains a component that hinders the introduction of alkali metal ions to the surface of the processing glass. On the surface of the processing glass having deformation defects, there are excess and insufficient alkali metal ions introduced by chemical strengthening. By performing the adjustment step S3 of bringing the polyvalent metal molten salt into contact with the processing glass, the excess alkali metal ions are exchanged with the polyvalent metal ions, and the insufficient alkali metal ions are filled with alkali metal ions. Therefore, it is possible to obtain a strengthened glass in which the stress distribution along the main surface direction is adjusted.

[0088] The polyvalent metal salt is typically an alkaline earth nitrate. As alkaline earth nitrates, Ca(NO3)2, Mg(NO3)2, Sr(NO3)2, Ba(NO3)2, etc. can be cited, and they can be used alone or in a mixture. The suitable lower limit range of the total amount of alkaline earth metal nitrate R(NO3)2 in the adjustment molten salt is 0.1% or more, 0.5% or more, 1% or more, 3% or more, and particularly 5% or more in terms of mass %. The suitable upper limit range is 100% or less, 90% or less, 80% or less, 75% or less, 70% or less, 65% or less, 60% or less, 55% or less, 50% or less, 45% or less, and particularly 40% or less. If the concentration of R(NO3)2 is too high, the melting point becomes too high and difficult to melt. On the other hand, if the concentration of R(NO3)2 is too low, the effect of hindering the introduction of alkali metal ions into the surface of the treatment glass cannot be obtained.

[0089] It should be noted that, from the viewpoint of reducing the raw material cost of the molten salt, preventing the generation of nitrogen oxide gas and precipitation due to thermal decomposition, Ca (NO3) 2 is particularly preferably used as a polyvalent metal salt. The suitable lower limit range of the concentration of Ca (NO3) 2 in the molten salt for adjustment is 0.1% or more, 0.5% or more, 1% or more, 3% or more, and especially 5% or more in terms of mass %. The suitable upper limit range is 100% or less, 90% or less, 80% or less, 75% or less, 70% or less, 65% or less, 60% or less, 55% or less, 50% or less, 45% or less, and especially 40% or less. If the concentration of Ca (NO3) 2 in the molten salt for adjustment is too low, it is difficult to obtain the effect of hindering the introduction of alkali metal ions to the surface of the treatment glass. On the other hand, if the concentration of Ca (NO3) 2 in the molten salt for adjustment is too high, the melting point becomes too high and melting becomes difficult, and it is possible that the residual Ca (NO3) 2 in the melt adheres to the tempered glass and becomes a bad cause. In addition, there is a possibility that thermal decomposition of Ca(NO 3 ) 2 may occur, and inhalation of the generated nitrogen oxide gas may cause health damage, and precipitation of CaO generated in the molten salt may adhere to the tempered glass and cause defects.

[0090] The remainder other than the polyvalent metal salt in the adjustment molten salt is preferably an alkali metal nitrate. As alkali metal nitrate, NaNO3, KNO3, LiNO3, etc. can be cited. In particular, when using NaNO3 and KNO3, the suitable lower limit range of the concentration of NaNO3+KNO3 is more than 0%, more than 10%, more than 20%, more than 30%, more than 40%, more than 45%, more than 50%, more than 55%, especially more than 60%. The suitable upper limit range is less than 99.9%, less than 99.5%, less than 99%, less than 97%, less than 95%, less than 90%, less than 80%, especially less than 70%. If the concentration of NaNO3+KNO3 is too low, the melting point becomes too high and difficult to melt. On the other hand, if the concentration of NaNO3+KNO3 is too high, the ion exchange of the alkali metal ion is carried out, so that the stress characteristics of the strengthened glass change, which may deviate from the desired range. It should be noted that in order to prevent the increase in the raw material cost of the molten salt and the excessive release of the alkali metal ions introduced into the treatment glass in the chemical strengthening step S12, the concentration of LiNO3 in the molten salt is preferably 0 to less than 5%, 0 to 3%, and particularly preferably 0 to 1% in terms of mass%.

[0091] The preferred lower limit range of the temperature of the adjustment molten salt in the adjustment step S3 is 350°C or more, 355°C or more, 360°C or more, 365°C or more, and particularly 370°C or more. The preferred upper limit range is 565°C or less, 550°C or less, 530°C or less, 520°C or less, 500°C or less, 480°C or less, 460°C or less, and particularly 440°C or less. If the temperature of the adjustment molten salt is too low, the polyvalent metal salt is difficult to melt, and the polyvalent metal salt remaining after melting may adhere to the tempered glass and cause a defect. On the other hand, if the temperature of the adjustment molten salt is too high, the polyvalent metal salt may be thermally decomposed, generating nitrogen oxide gas and precipitation of polyvalent metal oxides, which may adhere to the tempered glass and cause a defect.

[0092] The preferred lower limit range of the immersion time in the molten salt for adjustment is more than 10 seconds, more than 15 seconds, more than 20 seconds, more than 25 seconds, and particularly more than 30 seconds. The preferred upper limit range is less than 600 seconds, less than 500 seconds, less than 400 seconds, less than 300 seconds, less than 240 seconds, less than 180 seconds, and particularly less than 120 seconds. If the immersion time in the molten salt for adjustment is too short, the effect of hindering the introduction of alkali metal ions into the surface of the treatment glass cannot be obtained. If the immersion time in the molten salt for adjustment is too long, it is possible that the ion exchange of the alkali metal ions is carried out, and the stress characteristics of the tempered glass vary and deviate from the desired range. In addition, the warping of the tempered glass may deteriorate.

[0093] The processing glass immersed in the adjusting molten salt may be preheated to the temperature of the adjusting molten salt in the adjusting step S3, or may be immersed in the adjusting molten salt while being kept at room temperature (eg, 1° C. to 40° C.).

[0094] In addition, the tempered glass can be further ground after the adjustment step S3. In the case where the size, shape, and surface state of the tempered glass change due to chemical strengthening and immersion in a polyvalent metal salt, they can be corrected by performing a grinding process. On the other hand, since the increase of unnecessary microcracks due to the grinding process is also considered, as described above, when the chemically strengthened glass is an unground product formed by an overflow down-draw method, etc., and the main surface of the treatment glass after the chemical strengthening step S12 and the main surface of the tempered glass after the adjustment step S3 are also smooth non-ground surfaces (fire-polished surfaces), it is preferred not to perform a grinding process. It should be noted that when the chemically strengthened glass, the treatment glass, and the tempered glass are formed by the overflow down-draw method, they have a forming converging surface inside.

[0095] In addition, the tempered glass may also be subjected to an etching treatment after the adjustment step S3. Specifically, the entire tempered glass is immersed in a liquid etching medium, and the entire surface of the tempered glass is wet-etched. By such a treatment, the entire glass can be etched uniformly, so that the thickness deviation caused by the etching treatment can be suppressed. When such an etching treatment is performed, the surface of the tempered glass is composed of an etched surface.

[0096] As an etching medium, an acidic or alkaline aqueous solution capable of etching glass can be used. As an acidic etching medium, for example, an acidic aqueous solution containing HF can be used. In addition, as an alkaline etching medium, for example, an alkaline water solution containing NaOH or KOH can be used.

[0097] The etching medium is preferably used to perform etching in such a manner that the etching amount (thickness reduction caused by etching) of one surface of the tempered glass is, for example, 0.25 μm to 3 μm. By setting the etching amount to such a range, the variation of the compressive stress and the depth of the compressive stress on the outermost surface before and after etching is reduced, making it easier to control.

[0098] According to the tempered glass described above, by appropriately controlling its stress characteristics and thickness dimension and further reducing surface defects by etching, it is possible to simultaneously achieve high bending performance, bending strength, and suppression of shattering when broken.

[0099] The tempered glass after the conditioning step S3 is preferably cleaned and dried in the cleaning / drying step S4. By cleaning, the attached matter attached to the tempered glass can be removed. In addition, by drying the tempered glass after cleaning, the alkali metal ions can be prevented from flowing into the attached water.

[0100] The tempered glass that has passed through the cleaning / drying step S4 is inspected again in the second inspection step S5 to see if it is good (whether there are foreign matter defects, deformation defects such as unevenness, etc.). Specifically, the tempered glass is inspected by the operator's visual inspection or by using an image inspection device to check whether it has defects and whether it meets the standards as a product. If no defects are found and it meets the standards as a product, the treated glass is packaged / shipped as a product in the step S5. It should be noted that if some defects are observed in the tempered glass or it does not meet the standards as a product, it is preferably crushed and discarded, or reused as a raw material for chemically strengthened glass.

[0101] The tempered glass is preferably protected by affixing a protective film in the packaging / shipping step S5. As the protective film, a self-adhesive protective film or a protective film having a slightly adhesive adhesive is preferably used in order to obtain a high surface cleanliness without residual adhesive after peeling.

[0102] <Glass for treatment>

[0103] The process glass according to the embodiment of the present invention obtained through the above-mentioned preparation step S1 has the following characteristics.

[0104] The upper limit range suitable for the thickness t1 of the processing glass is below 0.2mm, below 0.15mm, below 0.1mm, below 0.08mm, below 0.06mm, particularly below 0.05mm, and the lower limit range suitable for is above 0.02mm, above 0.025mm, particularly above 0.03mm. If the processing glass is too thick, the above-mentioned processing glass may be damaged when bent. In addition, if the processing glass is too thin, it is difficult to ensure strength. In addition, if the glass is made too thin, it is difficult to improve the compressive stress value on the surface, which may damage flexibility instead.

[0105] The processing glass of the present invention is preferably a rectangular shape (rectangle) having long sides and short sides when viewed from above. The size of the above-mentioned tempered glass can be determined arbitrarily, and the length of the long side is preferably 40mm to 550mm, 50mm to 500mm, 60mm to 450mm, 65mm to 400mm, 70mm to 300mm, 75mm to 200mm, and particularly 80mm to 160mm. The length of the short side of the above-mentioned tempered glass is preferably 30mm to 400, 40mm to 350mm, 45mm to 300mm, 50mm to 200mm, 55mm to 120mm, and particularly 60mm to 80mm.

[0106] The processing glass has a compressive stress layer on the surface and a tensile stress layer inside. The suitable lower limit range of the outermost compressive stress CS1 of the compressive stress layer (compressive stress layer before the adjustment process) of the processing glass is 400MPa or more, 450MPa or more, 500MPa or more, 550MPa or more, and especially 600MPa or more. The suitable upper limit range is below 1100MPa, below 1000MPa, below 950MPa, below 900MPa, and especially below 880MPa. The larger the compressive stress CS1 of the outermost surface of the processing glass, the easier it is to prevent breakage caused by the tensile stress generated in the curved portion of the protective glass when the flexible display is bent. On the other hand, if a very large compressive stress is formed on the surface, the tensile stress existing inside the strengthened glass becomes extremely high, which may easily cause an increase in the dimensional change before and after the chemical strengthening treatment and explosive scattering when broken. Therefore, the suitable upper limit of the compressive stress CS1 of the outermost surface of the processing glass is 1300 MPa or less, 1100 MPa or less, 900 MPa or less, and particularly 800 MPa or less.

[0107] Regarding the depth DOL1 of the compressive stress layer of the processing glass (the compressive stress layer before the adjustment process), when the thickness of the processing glass is set to t1, the suitable lower limit range of DOL1 is 0.1·t1 or more, 0.12·t1 or more, 0.15·t1 or more, 0.18·t1 or more, and especially 0.2·t1 or more. The greater the depth DOL1 of the compressive stress layer of the processing glass, the less likely the processing glass and the tempered glass will break even if they are deeply damaged, and the deviation of the mechanical strength becomes smaller. On the other hand, if the depth DOL1 of the compressive stress layer of the processing glass is too large, the dimensional change before and after the chemical strengthening treatment may become larger. Therefore, the dimensional change before and after the chemical strengthening treatment may become larger. The suitable upper limit range of DOL1 is below 0.5·t1, below 0.45·t1, below 0.4·t1, and especially below 0.35·t1.

[0108] The tensile stress CT1 inside the process glass is, for example, 10 MPa to 1000 MPa.

[0109] It should be noted that the stress-related values ​​such as the outermost compressive stress (CS1, CS2), the depth of the compressive stress layer (DOL1, DOL2), and the tensile stress value (CT1, CT2) in the present invention can be measured using a measuring device such as FSM-6000 and SLP-1000 manufactured by Orihara Manufacturing Co., Ltd.

[0110] In addition, when the processing glass is a chemically strengthened glass strengthened by a one-step ion exchange, the internal tensile stress can also be estimated by calculating the value by the following formula (1).

[0111] CT1=(CS1×DOL1) / (t1-2×DOL1)...(1)

[0112] <Tempered glass>

[0113] The tempered glass according to the embodiment of the present invention obtained through the adjustment step S3 has the following characteristics.

[0114] The suitable upper limit range of the thickness t2 of the tempered glass is 0.2 mm or less, 0.15 mm or less, 0.1 mm or less, 0.08 mm or less, 0.06 mm or less, and particularly 0.05 mm or less, and the suitable lower limit range is 0.02 mm or more, 0.025 mm or more, and particularly 0.03 mm or more. If the tempered glass is too thick, the above-mentioned treatment glass may be broken when bent. In addition, if the tempered glass is too thin, it is difficult to ensure strength, and if the glass is too thin, it may be difficult to increase the surface compressive stress value.

[0115] The size of the tempered glass of the present invention is about the same as the size of the process glass used to obtain the tempered glass, and the preferred size range is also the same as the size of the process glass. That is, before and after the adjustment step S3, although the shape of the process glass due to the deformation defect changes, the size of the tempered glass obtained does not change significantly relative to the process glass. The change rate of the long side and the short side of the glass before and after the adjustment step S3 is, for example, 5% or less.

[0116] The suitable lower limit range of the outermost compressive stress CS2 of the compressive stress layer of the tempered glass (the compressive stress layer after the adjustment step S3) is 400MPa or more, 450MPa or more, 500MPa or more, 550MPa or more, and especially 600MPa or more. The larger the outermost compressive stress CS2 of the processing glass is, the easier it is to prevent the breakage caused by the tensile stress generated in the curved portion of the protective glass when the flexible display is bent. On the other hand, if a very large compressive stress is formed on the surface, it is possible that the tensile stress existing inside the tempered glass becomes extremely high, and the dimensional change before and after the chemical strengthening treatment is large. Therefore, the suitable upper limit range of the outermost compressive stress CS2 of the processing glass is below 1100MPa, below 1000MPa, below 950MPa, below 900MPa, and especially below 880MPa.

[0117] Regarding the depth DOL2 of the compressive stress layer of the tempered glass (the compressive stress layer after the adjustment step S3), when the thickness of the tempered glass is set to t2, the suitable lower limit range of DOL2 is 0.1·t2 or more, 0.12·t2 or more, 0.15·t2 or more, 0.18·t2 or more, and especially 0.2·t2 or more. The greater the depth DOL2 of the compressive stress layer of the tempered glass, the less likely the tempered glass is to break even if the tempered glass is deeply damaged, and the deviation of the mechanical strength becomes smaller. On the other hand, if the depth DOL2 of the compressive stress layer of the tempered glass is too large, the dimensional change before and after the chemical strengthening treatment may become larger. Therefore, the dimensional change before and after the chemical strengthening treatment may become larger. The suitable upper limit range is 0.5·t2 or less, 0.45·t2 or less, 0.4·t2 or less, and especially 0.35·t2 or less.

[0118] The tensile stress CT2 inside the tempered glass is, for example, 10 MPa to 1000 MPa. It should be noted that the tensile stress value CT2 can also be estimated by replacing the compressive stress CS1 with CS2, the depth of the compressive stress layer DOL1 with DOL2, and the thickness of the glass t1 with t2 in the above formula (1).

[0119] The ratio CS2 / CS1 of the outermost compressive stress value CS2 of the compressive stress layer of the tempered glass after the adjustment step S3 to the outermost compressive stress value CS1 of the compressive stress layer of the treatment glass before the adjustment step S3 is preferably 0.8 to 1, 0.85 to 1, 0.9 to 1, and particularly preferably 0.95 to 1. If CS2 / CS1 is too small, the bending strength of the tempered glass may be reduced relative to the treatment glass.

[0120] The suitable lower limit range of the ratio DOL2 / DOL1 of the stress depth DOL2 of the compressive stress layer of the tempered glass after the adjustment process to the stress depth DOL1 of the compressive stress layer of the processing glass before the adjustment process S3 is 0.9 or more, 0.92 or more, and particularly 0.95 or more. The suitable upper limit range is 1.2 or less, 1.15 or less, and particularly 1.1 or less. If DOL2 / DOL1 is too small, the bending strength of the tempered glass may be reduced relative to the processing glass. On the other hand, when DOL2 / DOL1 is too large, sometimes the surface CS2 decreases as the ion diffusion proceeds, in which case the bending strength of the tempered glass may be reduced relative to the processing glass.

[0121] The ratio CT2 / CT1 of the tensile stress value CT2 inside the tempered glass after the adjustment step S3 to the tensile stress value CT1 inside the treatment glass before the adjustment step S3 is, for example, 0.9 to 1.2. If CT2 / CT1 is too large, the tempered glass may explode when broken.

[0122] The warpage of the tempered glass is preferably 0 mm to 0.3 mm, 0 mm to 0.2 mm, and particularly preferably 0 mm to 0.15 mm. The warpage of the tempered glass is obtained by placing the tempered glass on a horizontal surface such as a platform with the convex surface facing downward and measuring the maximum height of the tempered glass from the horizontal surface.

[0123] The alkaline earth metal concentration, especially the Ca concentration, of the surface of the tempered glass is preferably higher than that of the interior of the tempered glass. By increasing the alkaline earth metal concentration of the surface, a tempered glass having a sufficiently adjusted stress distribution along the main surface can be obtained.

[0124] (Variation Example)

[0125] In the above-mentioned embodiments, the shape of the chemically strengthened glass, the processing glass, and the tempered glass is a rectangle when viewed from above, but the present invention is not limited to this. The shape of the chemically strengthened glass, the processing glass, and the tempered glass when viewed from above can be, for example, a square, a circle, an ellipse, or the like.

[0126] In addition, in the above-mentioned embodiments, the chemically strengthened glass, the treatment glass, and the tempered glass are exemplified as having a thin thickness of 0.2 mm or less as a whole, but the present invention is not limited thereto. The chemically strengthened glass, the treatment glass, and the tempered glass of the present invention may also have a thick portion in part. If the thick portion is set as the touch surface of the foldable device, the touch surface can be protected when the foldable device is folded.

[0127] In the manufacturing method of the tempered glass of the present invention, the case where the chemically tempered glass, the treatment glass, and the tempered glass are in the form of a flat plate is exemplified, but the present invention is not limited thereto. In the manufacturing method of the tempered glass of the present invention, the chemically tempered glass, the treatment glass, and the tempered glass may be subjected to three-dimensional bending processing as required to give a three-dimensional shape. For example, by preliminarily subjecting the chemically tempered glass to three-dimensional bending processing in whole or in part, the treatment glass and the tempered glass after the adjustment step S3 may be given a three-dimensional curved shape.

[0128] In the above embodiment, the case where the treatment glass is glass that has been subjected to one chemical strengthening treatment in the chemical strengthening step S12 is exemplified, but in the method for manufacturing the tempered glass of the present invention, the treatment glass may be glass that has been subjected to two or three or more chemical strengthening treatments. In addition, a heat treatment may be performed before and after the ion exchange. By performing a heat treatment, stress can be relaxed, ion diffusion can be promoted, and the depth of the compressive stress layer can be controlled.

[0129] In the method for producing tempered glass of the present invention, the adjustment step S3 may be performed without going through the inspection step S2. That is, all the glass prepared in the preparation step S1 may be used as treatment glass in the steps after the adjustment step S3.

[0130] In the method for producing tempered glass of the present invention, when alkaline earth nitrate is used as the adjusting molten salt, the adjusting step S3 may be performed after the chemical strengthening step S12 without washing and drying the treatment glass.

[0131] In the method for producing tempered glass of the present invention, the cleaning / drying step S4, the second inspection step S5, and the packaging / shipping step S6 may be omitted.

[0132] In the method for producing tempered glass of the present invention, the tempered glass can be laminated with any plate-shaped or sheet-shaped resin material, or a transparent material such as a metal material or glass via an adhesive or the like to be used as a laminate.

[0133] Example

[0134] Hereinafter, the method for producing a tempered glass and the tempered glass of the present invention will be described based on examples. It should be noted that the following examples are merely illustrative, and the present invention is not limited to the following examples at all.

[0135] The sample was prepared as follows: First, a chemically strengthened glass having a glass composition of 66.3% SiO2, 11.4% Al2O3, 0.5% B2O3, 1.4% K2O, 15.2% Na2O, 0.2% Li2O, 4.8% MgO, and 0.2% SnO2 was prepared.

[0136] Specifically, glass raw materials were prepared to have the above composition and melted at 1600° C. for 21 hours using a platinum pot. The resulting molten glass was then formed by flowing down from a refractory forming body using an overflow down-draw method, and formed and processed into the dimensions listed in Table 1 to obtain chemically strengthened glass.

[0137] Next, the chemically strengthened glass was immersed in a strengthening molten salt of 100% KNO3 at 430°C for 600 seconds to obtain a treated glass.

[0138] Furthermore, the treatment glasses Nos. 1 to 3 and 5 to 13 were immersed in a molten salt for adjustment under the treatment conditions (molten salt composition, temperature, time) described in Table 1 to obtain tempered glasses.

[0139] In Table 1, Nos. 1 to 3 and 5 to 13 are examples of the present invention, and Nos. 4 and 14 are comparative examples.

[0140] [Table 1]

[0141]

[0142] The outermost compressive stress (CS1, CS2) and the depth of compressive stress (DOL1, DOL2) in Table 1 are values ​​measured at the thin part of each sample using a surface stress meter FSM-6000LE manufactured by Orihara Manufacturing Co., Ltd. More specifically, DOL is DOL_zero measured using FSM-6000LE. In addition, the tensile stress values ​​(CT1, CT2) are values ​​calculated using the above calculation formula.

[0143] The surface shape was evaluated according to the following points.

[0144] First, a scanning white light interference microscope (VertScan, manufactured by Ryoka Systems Co., Ltd.) was used to measure the shape z (x, y) of the main surface of each sample. The measurement was performed in WAVE mode, using a 530nm white filter and a 2.5x magnification objective lens, with a measurement area of ​​5409.70μm×7208.58μm and a resolution of 640 pixels×480 pixels. The obtained measurement image was synthesized using the analysis software VS-Viewer. The measurement area after the synthesis of the field of view is 10007.95μm×25590.47μm. In order to remove the long-period ripples of the measured sample, the synthesized data was corrected using VS-Viewer, and band decomposition processing was performed in a manner to extract the case where the period length λ of the surface unevenness is 0.2mm<λ<1.0mm. The shape z (x, y) of the main surface is obtained from the image after band decomposition.

[0145] Next, the images showing the surface shape of the tempered glass obtained as described above are evaluated in three grades: a, b, and c. Specifically, a means that no deformation defect is observed on the surface, b means that deformation defect is observed in a relatively narrow range on the surface (occupying less than 10% of the area in the observation area), and c means that deformation defect is observed in a relatively wide range on the surface (occupying more than 10% of the area in the observation area). Examples of the images of the surface shape in each evaluation are shown in FIG. Figures 2 to 4 Specifically, Figure 2 , the surface shape of the glass of Example No. 12 is shown as an example of glass evaluated at level a. Figure 3 , the surface shape of the glass of Example No. 5 is shown as an example of glass evaluated in the b-level. Figure 4 In FIG. 14, the surface shape of the glass of Comparative Example No. 14 is shown as an example of glass evaluated at level c. In addition, the deformation defect means a portion displayed in a darker color than the surrounding area.

[0146] The warpage of each sample was obtained by placing the sample on a horizontal surface such as a platform with the convex surface facing downward and measuring the maximum height of the tempered glass from the horizontal surface.

[0147] In addition, the surface Ca ion concentration and the internal Ca ion concentration were measured according to the following procedures.

[0148] For chemically strengthened glass, Ca concentration was measured using an Electron Probe MicroAnalyzer (EPMA). The sample was cut perpendicularly to the main surface, and the thickness of the main surface of the glass plate and the center of the cut surface were measured. The measurement was performed using JXA-8100 manufactured by JEOL Ltd., with an acceleration voltage of 15 kV, a probe current of 500 nA, and a spectroscopic crystal PETH (Ca Kα ray, peak position: 107.57 mm) to obtain a curve of characteristic X-ray counts of Ca.

[0149] According to the results of the above-mentioned surface shape evaluation, it was confirmed that in No. 1 to 3, 5 to 13, the surface state of the sample was improved by immersing in the adjustment molten salt containing Ca (NO3) 2 compared with No. 4 and 14 which were not immersed. In addition, in No. 1 to 3, when the temperature of the adjustment molten salt was high, a higher improvement effect was obtained. In addition, in No. 5 to 12, when the concentration of Ca (NO3) 2 in the adjustment molten salt was high, a higher improvement effect was obtained.

[0150] Furthermore, it was confirmed that Ca ions were not detected from the inside of the tempered glass of No. 12, but Ca ions were detected from the surface. Therefore, it was found that Ca ion concentration was introduced into the surface of the tempered glass subjected to the adjustment step S3.

[0151] Industrial Applicability

[0152] The tempered glass of the present invention can be used, for example, for smartphones, mobile phones, tablet computers, personal computers, digital cameras, touch panel displays, cover glasses of other display devices, vehicle-mounted display devices, and vehicle-mounted panels.

[0153] Description of Reference Numerals

[0154] S1 Preparation process

[0155] S11 Forming process

[0156] S12 Chemical Strengthening Process

[0157] S2 1st inspection process

[0158] S3 Adjustment Process

[0159] S4 cleaning / drying process

[0160] S5 2nd inspection process

[0161] S6 Packaging / Factory Process

Claims

1. A method for manufacturing tempered glass, It is characterized in that A method for producing tempered glass for obtaining tempered glass having a compressive stress layer on the surface layer, comprising the following steps: a preparation step of preparing a plate-shaped or film-shaped chemically strengthened glass having a thickness of 0.2 mm or less as treatment glass; and The conditioning step is a step of contacting the surface of the treatment glass with a conditioning molten salt containing polyvalent metal ions after the preparation step.

2. The method for producing tempered glass according to claim 1, in, In the adjustment step, stress distribution in a direction along the main surface of the process glass is adjusted.

3. The method for producing tempered glass according to claim 1 or 2, in, The adjustment molten salt used in the adjustment step includes an alkaline earth metal nitrate. The total amount of alkaline earth metal nitrates R(NO 3 ) 2 The concentration of the adjusting molten salt is 0.1% by mass to 100% by mass.

4. The method for producing tempered glass according to any one of claims 1 to 3, in, The thickness of the processing glass is 0.06 mm or less.

5. The method for producing tempered glass according to any one of claims 1 to 4, in, In the adjustment step, the treatment glass is immersed in the adjustment molten salt for a period of 10 to 600 seconds.

6. The method for producing tempered glass according to any one of claims 1 to 5, in, The temperature of the adjusting molten salt is 350°C to 565°C.

7. The method for producing tempered glass according to any one of claims 1 to 6, in, The adjusting molten salt contains 0.5% to 45% of Ca(NO 3 ) 2 , 55% ~ 99.5% KNO 3 +NaNO 3 .

8. The method for producing tempered glass according to any one of claims 1 to 7, in, The LiNO in the adjusting molten salt 3 The content is less than 5% by mass.

9. The method for producing tempered glass according to any one of claims 1 to 8, in, The adjustment step is adjusted so that the compressive stress value CS of the outermost surface of the compressive stress layer of the tempered glass after the adjustment step is 2 Relative to the compressive stress value CS of the outermost surface of the compressive stress layer of the processing glass before the adjustment step 1 CS 2 / CS 1 Become 0.8~1.

10. The method for producing tempered glass according to any one of claims 1 to 9, in, The adjustment step is adjusted so that the compressive stress value CS of the outermost surface of the compressive stress layer of the tempered glass after the adjustment step is 2 Become 400MPa or more.

11. The method for producing tempered glass according to any one of claims 1 to 10, in, The adjustment step is adjusted so that the stress depth DOL of the compressive stress layer of the tempered glass after the adjustment step is 2 The stress depth DOL of the compressive stress layer of the processing glass before the adjustment step is 1 DOL 2 / DOL 1 Become 0.9~1.

2.

12. The method for producing tempered glass according to any one of claims 1 to 11, in, The adjustment step is adjusted so that the thickness of the tempered glass after the adjustment step is set to t 2 In the case of the tempered glass, the stress depth DOL of the compressive stress layer is 2 becomes 0.1·t 2 above.

13. The method for producing tempered glass according to any one of claims 1 to 12, in, The warping of the tempered glass after the adjustment step is 0.2 mm or less.

14. The method for producing tempered glass according to any one of claims 1 to 13, in, The tempered glass after the adjustment step contains 50% to 80% SiO in mol%. 2 5%~25%Al 2 O 3 , 0% to 15% B 2 O 3 , 0%~15%Li 2 O, 1% ~ 20% Na 2 O, 0% to 10% K 2 O as a glass composition.

15. A tempered glass, It is characterized in that It is a plate-shaped or film-shaped tempered glass with a compressive stress layer of less than 0.2 mm thickness on the surface. The compressive stress value CS of the outermost surface of the compressive stress layer 2 The pressure is 400 MPa or more, and the Ca ion concentration on the surface is higher than that in the interior.

Citation Information

Patent Citations

  • High-strength chemically-strengthened glass and glass strengthening method

    CN105837031A

  • Low temperature chemical strengthening process for glass

    CN107873021A

  • Chemically strengthened glass sheet and its production method

    JP2019210195A

Cited By

  • Processing control method and device for arched morphology structure of glass key

    CN122261027A