Refractory for continuous casting and refractory member

By limiting the magnesium oxide content and optimizing the carbon composition and particle size composition of the refractory for continuous casting, a roughly continuous void layer is formed, which solves the problems of insufficient corrosion resistance and reduced thermal shock resistance of the refractory to acidic inclusion steels. Achieving high durability and low expansion without preheating.

CN118786103AActive Publication Date: 2024-10-15KROSAKI HARIMA CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202380024112.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-02
Filing Date
2023-02-17
Publication Date
2024-10-15
Estimated Expiration
2043-02-17

AI Technical Summary

Technical Problem

Existing refractories for continuous casting have insufficient corrosion resistance to acidic inclusion steels when the magnesium oxide content is high, and the thermal shock resistance decreases due to the magnesium oxide-carbon reaction during repeated use, especially during preheating. Poor performance in an inadequate state.

Method used

Control densification and pore morphology in the refractory by limiting the magnesium oxide content to less than 40%, using a free carbon content of 10% to 30%, and forming a roughly continuous layer of voids around the refractory particles, optimizing the particle size composition and carbon matrix structure to improve corrosion resistance and thermal shock resistance.

Benefits of technology

Significantly improves the corrosion resistance and thermal shock resistance of refractories and refractory components, ensuring excellent durability even without preheating, reducing thermal expansion, and balancing strength and wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786103A_ABST
    Figure CN118786103A_ABST
Patent Text Reader

Abstract

The present invention improves the corrosion resistance and thermal shock resistance of a refractory for continuous casting and a refractory component. Specifically, this refractory contains 10-30 mass% of a free carbon component, the remainder being composed of one or more substances selected from corundum, spinel, and periclase, the periclase content being less than 40 mass%, and the total content of a silica component and a silicon carbide component being less than 15 mass%. Refractory particles having a particle diameter of more than 0.3 mm are 20 vol% or more and refractory particles having a particle diameter of 0.045 mm or less are 3-30 vol% (inclusive) when the content of the refractory particles excluding the constituent comprising a free carbon component from the constituent of the refractory is taken as 100 vol%. A substantially continuous void layer having a shape similar to that of a coarse particle is present around at least the coarse particle having the largest particle size. The refractory has an apparent porosity of 16% or less and a maximum coefficient of thermal expansion of 0.6% or less at 1500 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a refractory for continuous casting and a refractory component such as a nozzle for continuous casting using the refractory. Background Art

[0002] The present inventors disclosed in Patent Document 1 a refractory for continuous casting having both excellent corrosion resistance and thermal shock resistance.

[0003] Patent Literature Patent Document 1: Japanese Patent No. 6027676 Summary of the invention

[0004] The present inventors have found that further improvement in corrosion resistance and thermal shock resistance is desirable when they have produced a refractory component using the refractory disclosed in Patent Document 1 and repeated tests. That is, since the refractory disclosed in Patent Document 1 contains more than 40% by mass of magnesium oxide (periclite), it has excellent corrosion resistance to steels containing basic inclusions such as CaO and MnO, but on the contrary, it has insufficient corrosion resistance to steels containing acidic inclusions such as SiO2. In addition, it is known that the refractory disclosed in Patent Document 1 will cause magnesium oxide-carbon reaction (the reaction of (1) below) when used, and especially when used repeatedly, the structure will be deteriorated, and high elastic modulus will occur, resulting in a decrease in thermal shock resistance. MgO(solid)+C(solid)→Mg(gas)+CO(gas)(1) In recent years, since continuous casting nozzles and refractory parts for continuous casting are increasingly used in a state where preheating is insufficient or not performed, further improvement in thermal shock resistance has been desired.

[0005] The technical problem to be solved by the present invention is to improve the corrosion resistance and thermal shock resistance of refractory and refractory parts used for continuous casting.

[0006] The inventors are based on the above-mentioned defects caused by containing more magnesium oxide (periclite), and the content of magnesium oxide (periclite) is limited to less than 40% by mass. On this basis, in order to improve corrosion resistance and thermal shock resistance, it is found that controlling the pore morphology inside the refractory while achieving densification of the refractory is the key. Moreover, it is found that the particle size composition (volume ratio) of the refractory particles in the refractory is one of the important control factors, so that the present invention is completed.

[0007] That is, according to one aspect of the present invention, the following refractory for continuous casting can be provided. A refractory for continuous casting, comprising 10% to 30% by mass of free carbon components, the remaining main mineral phase is composed of one or more selected from corundum, spinel and periclase, the content of periclase is less than 40% by mass, and the total content of silicon dioxide and silicon carbide components is less than 15% by mass, characterized in that: When the portion of the constituent consisting of the free carbon component is removed from the constituent of the refractory as 100% by volume, the refractory particles having a particle size exceeding 0.3 mm account for more than 20% by volume, and the refractory particles having a particle size of less than 0.045 mm account for more than 3% by volume and less than 30% by volume, Among the refractory particles in the refractory, at least around the coarse particles of the largest particle size, there is a substantially continuous void layer similar in shape to the coarse particles, and in the substantially continuous void layer, the total thickness of the void layer existing at the interface between the matrix structure containing carbon at both ends and the coarse particles is 0.3% or more and 3.0% or less relative to the particle size of the coarse particles, Furthermore, the apparent porosity is 16% or less, and the maximum thermal expansion coefficient up to 1500° C. is 0.6% or less.

[0008] According to another aspect of the present invention, there is provided a refractory component for continuous casting, wherein the refractory for continuous casting of the present invention is disposed partially or entirely on a portion in contact with molten steel.

[0009] According to the present invention, the corrosion resistance and thermal shock resistance of the refractory and refractory parts for continuous casting can be improved, thereby achieving excellent durability even in an environment where the refractory is used without preheating. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 Schematic diagrams showing the structure of refractory particles and their surroundings as aggregates in the refractory of the present invention, (a) is a case where there is a void layer with a shape similar to the particle outline around the refractory particles and the particles are approximately located in the center (a typical example of the present invention), and (b) is a case where there is a void layer with a shape similar to the particle outline around the refractory particles and the particles are located on either side of the inner wall surface of the void layer (an example of the distribution produced when preparing a sample for microscopic observation). Figure 2 This is a cross-sectional view showing an example of an immersion nozzle which is one aspect of a refractory component to which the refractory of the present invention is applied. Figure 3 This is a cross-sectional view showing another example of an immersion nozzle which is one aspect of a refractory component to which the refractory of the present invention is applied. Figure 4This is an example of a continuous casting facility for steel and is an explanatory diagram showing an example of installation of refractory parts for continuous casting. Figure 5 This is a cross-sectional view showing an example of a long nozzle which is one form of a refractory component to which the refractory of the present invention is applied. Figure 6 This is a cross-sectional view showing an example of a lower nozzle which is one aspect of a refractory component to which the refractory of the present invention is applied. Figure 7 This is a cross-sectional view showing another example of a long nozzle which is one aspect of a refractory component to which the refractory of the present invention is applied. Figure 8 This is a cross-sectional view showing an example of a long stopper rod which is one aspect of a refractory component to which the refractory of the present invention is applied. Explanation of symbols 20-refractory of the present invention; 21-powder line material (refractory on the back side); 22-difficult to adhere material; 22G-refractory for ventilation; 22S-space (gas passage path, pressure storage chamber); A-upper nozzle; B-sliding nozzle plate; C-lower nozzle; D-long nozzle; E-long plug rod; F-immersion nozzle; G-refractory for lining. DETAILED DESCRIPTION

[0011] As mentioned above, in order to solve the above-mentioned problems, it is important to realize the densification of refractory and control the pore morphology inside refractory at the same time.Therefore, the inventors take the following refractory organization as the target, that is, in the matrix organization (hereinafter referred to as "carbonaceous matrix") containing 3-dimensional continuous carbon, there are refractory particles with a particle size exceeding 0.3mm as aggregate in a discontinuous manner, and at the same time, among these refractory particles, there is a refractory organization of a roughly continuous void layer similar to the shape of the coarse particles at least around the coarse particles of the maximum particle size.That is, by adopting such a refractory organization, the thermal expansion of the coarse particles that have a greater contribution to the thermal expansion of the refractory can be absorbed by the roughly continuous void layer around the particles, and the result can obtain the effect of making the thermal expansion of the coarse particles disappear in appearance.That is, in the heating process, during the period when there is a void layer around the coarse particles, the thermal expansion of the refractory is mainly based on the thermal expansion of the 3-dimensional continuous carbonaceous matrix part, thereby reducing the thermal expansion of the refractory. And, in the present invention, by limiting the volume ratio of the refractory particles (hereinafter referred to as "coarse-grained refractory particles") with a particle size exceeding 0.3mm and the refractory particles (hereinafter referred to as "micro-particle refractory particles") with a particle size below 0.045mm, the densification of the refractory can be achieved, and the control of the pore morphology inside the refractory as described above can be achieved, thereby the improvement of the corrosion resistance and thermal shock resistance of the refractory and refractory parts used for continuous casting can be achieved. Specific description is given below.

[0012] The refractory of the present invention contains a free carbon component of more than 10% by mass and less than 30% by mass. Here, "free carbon component" refers to a carbon component consisting of a carbon component monomer other than compounds such as carbides such as B4C and SiC, except for inevitable impurities, and refers to amorphous or quasi-crystalline such as graphite generated by various organic binders, pitch, tar, and carbon black by being heated, and in addition, all carbon components present in the refractory organization in a particle shape (including fibrous shape) or a shape or structure that is present in the refractory organization in a continuous or discontinuous state without forming a specific shape. When the content of free carbon component is less than 10 mass %, then 3-dimensional continuous carbonaceous matrix will not be formed in refractory structure, and enough low expansion effect cannot be obtained.In addition, when exceeding 30 mass %, then the damage of carbonaceous matrix caused by molten steel, slag etc. can become fierce, and the melting loss amount of refractory can be caused to increase and corrosion resistance decrease.In addition, when using graphite etc. as free carbon component source in a large number, formability can decrease and the compactness of refractory can be impaired, and from this point on, corrosion resistance also can decrease.Preferably the content of free carbon component is more than 15 mass % and less than 25 mass %.

[0013] The main mineral phase of refractory of the present invention is made of one or more than two kinds selected from corundum, spinel and periclase.But the content of periclase is limited to less than 40 mass %.This is because, when the content of periclase (magnesium oxide) is more than 40 mass %, defects as mentioned above will be produced.In addition, the content of preferred periclase is below 35 mass %. Here, in the present invention, "main mineral phase" refers to the most mineral phase among the mineral phases in the refractory, and when there are more than two most mineral phases, they are all the main mineral phases. In addition, when refractory particles containing multiple mineral phases are included, the multiple mineral phases included by the refractory particles are respectively combined with the same mineral phases included by other refractory particles to determine the "main mineral phase".

[0014] In the refractory of the present invention, the content of the silicon dioxide component and the silicon carbide component is limited to less than 15% by mass. This is because, when the content of the silicon dioxide component and the silicon carbide component is more than 15% by mass, the corrosion resistance will be significantly reduced. In addition, since there is a function of suppressing the oxidation of free carbon components, etc. on the silicon carbide component, it can be appropriately contained within a range of less than 15% by mass, for example, if it is less than 5% by mass, it can play an oxidation inhibition function and will not substantially reduce the corrosion resistance.

[0015] Next, one of the characteristics of the present invention, that is, the particle size composition (volume ratio) of the refractory particles in the refractory will be described. In the present invention, the particle size composition (volume ratio) of the refractory particles in the refractory is characterized in that, when the portion of the constituent composed of free carbon components is removed from the constituent of the refractory as 100 volume %, the coarse-grained refractory particles are more than 20 volume %, and the fine-grained refractory particles are more than 3 volume % and less than 30 volume %. Since when the coarse refractory particles are less than 20% by volume, the volume ratio of the refractory particles of the microparticles or the medium particles described later will increase relatively, so the number of refractory particles in the refractory will increase. As a result, the refractory structure in which the refractory particles are continuously present will become high expansion. Therefore, the thermal shock resistance will decrease. Although the upper limit of the volume ratio of the coarse refractory particles is not particularly limited, from the viewpoint of stably ensuring the necessary characteristics such as the strength and corrosion resistance required as the refractory for continuous casting, for example, it can be less than 60% by volume. The volume ratio of the coarse refractory particles is preferably more than 30% by volume, more preferably more than 40% by volume and less than 60% by volume. In addition, although the upper limit of the particle size of the coarse refractory particles is not particularly limited, it is also preferably less than 3mm, more preferably less than 1mm, from the viewpoint of stably ensuring the necessary characteristics such as the strength and corrosion resistance required as the refractory for continuous casting. That is, as coarse-grained refractory particles, in addition to particle sizes exceeding 0.3 mm and being less than 1 mm, the refractory of the present invention may also include particle sizes exceeding 1 mm and being less than 3 mm, but the volume proportion of the particle sizes exceeding 1 mm and being less than 3 mm is preferably 15 volume % or less, when the portion other than the constituent material consisting of free carbon components removed from the constituent material of the refractory is taken as 100 volume %, and more preferably 0 volume %, i.e., refractory particles having a particle size exceeding 1 mm and being less than 3 mm are not included.

[0016] In addition, when the volume ratio of the refractory particles of microparticles is less than 3 volume %, it is impossible to obtain a dense refractory and corrosion resistance decreases. On the other hand, because when the volume ratio of the refractory particles of microparticles exceeds 30 volume %, the number of the refractory particles in the refractory will increase, so the refractory structure of the continuous existence of refractory particles will become high expansion. Therefore, thermal shock resistance will decrease. The volume ratio of the refractory particles of the preferred microparticles is more than 5 volume % and less than 15 volume %. In addition, in the refractory of the present invention, the refractory particles of the microparticles are substantially present in the carbonaceous matrix.

[0017] Above, although the volume ratio of the refractory particles of coarse grain (particle diameter exceeds 0.3mm) and microparticle (particle diameter 0.045mm or less) is described, refractory of the present invention suitably comprises the refractory particles of medium grain (particle diameter exceeds 0.045mm and is 0.3mm or less).Its volume ratio is, when the part of the constituent consisting of free carbon component is removed from the constituent of refractory as 100 volume %, the remainder of the volume ratio of the refractory particles of coarse grain and the volume ratio of the refractory particles of microparticle, specifically, is preferably 10 volume % or more and 77 volume % or less, more preferably 30 volume % or more and 70 volume % or less.

[0018] Here, in the present invention, the particle size of refractory particles refers to the size of the mesh when the refractory particles are screened with a sieve. For example, refractory particles with a particle size of less than 0.045 mm refer to refractory particles that pass through a sieve with a mesh of 0.045 mm, and refractory particles with a particle size exceeding 0.3 mm refer to refractory particles that do not pass through a sieve with a mesh of 0.3 mm.

[0019] Next, the organization of the refractory of the present invention is described in detail. As described above, the basic organizational form of the refractory of the present invention is the following refractory organization, in a 3-dimensional continuous carbonaceous matrix, there are refractory particles with a particle size of more than 0.3mm as aggregates in a discontinuous manner, and at the same time, among these refractory particles, there is a refractory organization of a roughly continuous void layer similar to the shape of the coarse particles at least around the coarse particles of the maximum particle size. Specifically, in the roughly continuous void layer, the total thickness of the void layer on the interface between the carbonaceous matrix at both ends and the coarse particles is, relative to the particle size of the coarse particles, a refractory organization of more than 0.3% and less than 3.0%.

[0020] Here, the term "substantially continuous void layer" means that, under cross-sectional observation of a microscope around the refractory particles as aggregate, the voids have an enlarged shape that is substantially similar to the shape of the particle cross-sectional shape, and the particles are present inside the voids like a bell ball (see Figure 1(a)). That is, there is no structure in which a structure such as carbon that hinders the thermal expansion of the refractory particles exists in the void layer, and the void layer is not uniform or does not have voids, and there are random portions where the refractory particles are in direct contact with each other or the refractory particles and the carbonaceous matrix. In addition, in the refractory of the present invention, a void layer exists in the whole surrounding of the refractory particles as aggregate, that is, in a "continuous state", but when the void layer is verified by microscopic observation, it can be said that the refractory particles exist in a floating manner without being fixed in the space, so when the sample is made from the refractory, a part of the surface of the refractory particles may also be generated that is in contact with other refractory particles and the carbonaceous matrix around them (refer to Figure 1 (b)). Therefore, considering the actual situation in the verification, the expression "substantially continuous" is used. In fact, although there is a void layer around the refractory particles as a whole, for example, when verifying the sample under microscope observation, even if there is a part that contacts other refractory particles or carbonaceous matrix, the part is not in a state of "bonding or bonding" to the extent that the refractory particles are fixed. That is, through such a "substantially continuous void layer", the thermal expansion of the refractory particles can be absorbed, thereby achieving low expansion of the refractory.

[0021] From the viewpoint of reducing the thermal expansion of refractory, the thickness of the interstitial layer around the refractory particles is as thick as possible, and preferably there is the interstitial layer around all refractory particles as aggregate. However, since the interstitial layer around the refractory particles can become the reason for the strength reduction of the refractory, it is necessary to obtain the balance of thermal expansion and strength, damage, etc. while adjusting the thickness of the interstitial layer.

[0022] The ratio of the void layer thickness to the particle size (void layer thickness rate of each particle: MS value (micro space value)) is that the larger the particle, the smaller its ratio is, and the smaller the particle, the larger its ratio is. Therefore, the MS value of the coarse particle with the maximum particle size among the specific refractory particles refers to the lower limit value of the void layer thickness rate of each particle in the refractory structure being specified, and the heat shock resistance of the general refractory can be evaluated.

[0023] Here, the MS value refers to the ratio of the thickness L of the void layer between the coarse particle and the carbonaceous matrix (the total thickness of the void layer on both sides of the particle is taken as L) to the coarse particle diameter D, and can be obtained by the following formula. MS value = (L / D) × 100 (%)

[0024] Specifically, in the present invention, the MS value (%) is calculated by the following method. In the microscopic organization observation of refractory, 10 coarse particles are selected in the order of the size of the particle diameter, and in the face of each particle, the largest circle that contacts with its outline and is enclosed is outlined, and an arbitrary line through the center is drawn. And, based on this line, 3 lines of 45 ° spacing through the center of the above-mentioned circle are drawn again, and a total of 4 lines are drawn for each particle. Thereafter, on the above-mentioned lines of the particle, the length between the contour points at the two ends of the particle is used as D1, D2, D3, D4, and the total of the interstitial layer thickness of the particle interface present on each line at both ends is measured as L1, L2, L3, L4 respectively. Use the numerical value obtained by these 4 lines, calculate MS1, MS2, MS3, MS4 calculated by the above formula respectively, and calculate the average value of these numerical values ​​as the interstitial layer thickness rate of 1 coarse particle, i.e., MS value. Utilize the above-mentioned method to calculate the MS values ​​of 10 coarse particles selected in advance respectively, and average them as the MS value of this refractory organization.

[0025] In addition, the reason for evaluating the MS value of the refractory structure by using the coarse particles of the maximum particle size, i.e., 10 coarse particles selected in the order of the size of the particle size in the microscopic organization observation of the refractory, is that the larger the particle size, the greater the change in volume and length caused by its expansion, and the greater the impact on the thermal shock resistance of the refractory. Therefore, as an index for adjusting and evaluating the MS value of thermal shock resistance, it is necessary to calculate the coarse particles of the maximum particle size in the refractory structure. In addition, from the same viewpoint, in the present invention, the above-mentioned "roughly continuous void layer" needs to be present at least around the coarse particles of the maximum particle size, i.e., 10 coarse particles selected in the order of large to small particle size in the microscopic organization observation of the refractory.

[0026] The inventors have confirmed that in a refractory in which the main mineral phase is composed of one or more of corundum, spinel and periclase, and the content of periclase is less than 40% by mass, there is a low expansion effect, and the thickness of the void layer around the refractory particles that can be balanced in terms of strength, corrosion resistance and wear resistance is, based on the MS value calculated for the coarse particles of the maximum particle size, 0.3% to 3.0%. That is, when the above-mentioned MS value is less than 0.3%, sufficient low expansion effect cannot be obtained. In addition, when the above-mentioned MS value exceeds 3.0%, the strength decreases, and the corrosion resistance and wear resistance also decrease. Thus, in the present invention, by forming the following refractory structure, that is, among the refractory particles in the refractory, there is a roughly continuous void layer similar to the shape of the coarse particles at least around the coarse particles of the maximum particle size, and in the roughly continuous void layer, the total thickness of the void layer on the interface between the carbon-containing matrix structure at both ends and the coarse particles is a refractory structure of not less than 0.3% and not more than 3.0% relative to the particle size of the coarse particles, thereby being able to provide a refractory that can significantly improve thermal shock resistance and achieve a balance in strength, corrosion resistance and wear resistance.

[0027] The MS value control method is to form a substantially continuous void layer having a shape similar to that of at least the largest coarse particles among the refractory particles in the refractory and to control the thickness of the void layer, for example, as follows. Although the control of MS value is synonymous with the control of thermal expansion coefficient, due to the fact that in the process of heat treatment, the larger the refractory particles (coarse particles), the larger the thermal expansion amount, and the more significant the thermal expansion difference with the carbonaceous matrix, the more easily a substantially continuous void layer (hereinafter also referred to as "MS") similar to its shape is generated around the coarse particles, and the smaller the refractory particles, the smaller the thermal expansion amount becomes, and it is difficult to generate a clear MS. Therefore, by controlling the particle size composition (volume ratio) of the refractory particles in the refractory, it is possible to achieve the control of MS value, that is, the control of thermal expansion coefficient. In the present invention, when the part of the constituent composed of free carbon components is removed as 100% by volume, by making the refractory particles with a particle size exceeding 0.3mm be more than 20% by volume, making the refractory particles with a particle size of less than 0.045mm be more than 3% by volume and less than 30% by volume, it is possible to achieve low expansion and its control. For example, when lower expansion is desired, the generation of MS can be promoted by reducing the volume ratio of refractory particles with a particle size of less than 0.045 mm within the above-mentioned particle size composition (volume ratio) to cut off the continuity of the refractory particles in the refractory structure, and increasing the volume ratio of refractory particles with a particle size exceeding 0.3 mm.

[0028] By combining the above-mentioned constitution (chemical composition, main mineral phase, granularity constitution (volume ratio) of refractory particles and refractory organization), the refractory of the present invention can stably coexist with a compactness of an apparent porosity of less than 16% and a low expansion property of less than 0.6% of the maximum thermal expansion coefficient up to 1500°C. Thus, the corrosion resistance and thermal shock resistance of the refractory and refractory parts for continuous casting can be improved, and excellent durability can be exerted even in an environment of use without preheating.

[0029] Here, in the present invention, the chemical composition, refractory structure, apparent porosity, thermal expansion coefficient, etc. of the refractory are basically evaluated for the sample "after heating in a non-oxidizing atmosphere at 1000°C". The reason is to achieve the removal of components such as moisture, organic matter, water and matter, carbon oxides, etc. in the refractory, and to stabilize the chemical composition of the refractory by carbonization of the organic binder component to improve the analysis accuracy. From this point of view, the heating time is set to the period until the weight change caused by heating disappears. However, when the refractory has been heat-treated at a temperature above 1000°C in the manufacturing process, or when it has been heat-treated at a temperature above 800°C according to the type of volatile components, the chemical composition, refractory structure, apparent porosity, thermal expansion coefficient, etc. can be evaluated in the product state after its production.

[0030] Preferably, the refractory of the present invention comprises a boron component of 0.1 mass % or more and 3.0 mass % or less in terms of B2O3 conversion value. The boron component generates fibrous aluminum borates etc. in a carbonaceous matrix when the refractory is heated. Thus, the densification and strengthening of the carbonaceous matrix can be achieved and the strength of the refractory can be improved.

[0031] In addition, the refractory of the present invention can also include carbon fiber in the carbonaceous matrix. Carbon fiber can fill the defective parts such as cracks produced by the shrinkage of the carbonaceous matrix, and the shrinkage of the carbonaceous matrix is ​​caused by the carbonization of the organic binder component during the heating of the refractory. Thus, the densification and strengthening of the carbonaceous matrix can be achieved, and the strength of the refractory is improved. From the viewpoint of giving full play to the strength improvement effect of this refractory, the aspect ratio of the preferred carbon fiber is more than 15 and less than 200, and preferably its content is less than 5% by mass.

[0032] Similar to the preparation of the samples in the examples described later, the refractory of the present invention can be prepared by the same method as the preparation method of general refractory having one or more mineral phases selected from corundum, spinel and periclase as the main mineral phase. For example, a binder is added to the raw material mixture including refractory particles constituting the main mineral phase, the kneaded clay is adjusted to a state suitable for forming, and then the clay is formed by CIP (Cold Isostatic Pressing), dried at a temperature below about 300°C, and then heat treated in a non-oxidizing atmosphere at about 800°C to about 1200°C.

[0033] Next, a refractory component for continuous casting using the refractory of the present invention will be described. Figure 2 In FIG. 1 , a submerged nozzle, which is one form of a refractory component for continuous casting, is shown in longitudinal section. exist Figure 2 (a) shows an example of an immersion nozzle in which the refractory material 20 of the present invention is arranged as a single layer from the surface in contact with the molten steel to the back side in a part of the area in contact with the molten steel. Figure 2 In (a), if the refractory 20 of the present invention is also arranged on the powder line material 21 part, it can be an immersion nozzle in which the refractory of the present invention is arranged as a single layer in the entire area of ​​the part in contact with the molten steel, from the surface in contact with the molten steel to the back side. In the case of a nozzle with a single-layer structure, the danger of fracturing, etc. can be reduced, and a simple method can also be used in the production. In the production of such a nozzle with a single-layer structure, it is only necessary to fill the refractory of the present invention with clay as a single layer in the target area in the CIP forming mold based on the above-mentioned production method. In addition, although Figure 2 (a) shows an example of a cylindrical shape, but the nozzle such as the immersion nozzle of the refractory material to which the present invention is applied is not limited to such a cylindrical shape, for example, Figure 2 The shapes of the nozzles shown in (b) are flat, elliptical, funnel-shaped (funnel-shaped with a larger diameter at the top) and other shapes, which are mainly used for casting thin plates, and can be applied to nozzles of various shapes. In addition, Figure 2 (c) shows that there is Figure 2 (a) is an example of an immersion nozzle having the function of blowing gas into molten steel from a part of the inner hole portion (inner hole wall surface) of the immersion nozzle. In this example, a highly permeable refractory (hereinafter referred to as "ventilation refractory") 20G is arranged on a part of the inner hole portion. The material of the ventilation refractory 20G can be a general alumina-graphite ventilation refractory. In addition, it can also be a material that can improve the porosity and permeability while maintaining the refractory composition of the present invention. In addition, Figure 2 The symbol 20S in (c) is a space, which is the passage path of the gas and also the pressure storage chamber of the gas.

[0034] exist Figure 3In the figure, there is shown an example of an immersion nozzle in which a refractory 20 of the present invention is arranged on a part or the whole of the part in contact with molten steel, and a layer composed of a refractory (difficult to adhere material 22) composed of a composition different from the refractory 20 of the present invention is arranged inside the refractory 20 of the present invention, thereby forming a plurality of layers, and the plurality of layers form an integral structure in a state of direct contact with each other. In the production of such a nozzle composed of multiple layers, it is only necessary to separate a gap for clay injection at a position of a specified thickness in the radial direction from the surface in contact with molten steel in the target area in the CIP forming mold based on the above-mentioned production method, fill the inside (core rod side) with clay for refractory different from the refractory of the present invention, and fill the back side with clay for refractory of the present invention. Thereafter, before forming, it is only necessary to remove the clamp such as the plate used for separation and perform press forming.

[0035] Examples of nozzles for continuous casting of refractory materials to which the present invention can be applied or suitably include, in addition to immersion nozzles, pouring nozzles (including upper nozzles, open nozzles, etc.), intermediate nozzles, and flow rate control nozzles (especially inner holes, etc.). exist Figure 4 In the figure, there is shown an example of the structure of a continuous casting device for steel, and on the left side of the same figure, there is shown an example in which a nozzle portion serving as a flow path for the molten steel when discharging the molten steel from the molten steel container is a structure composed of a plurality of nozzles, and in the structure, an immersion nozzle F is an externally mounted example. The refractory material 20 of the present invention can be applied not only to the immersion nozzle F, but also to a part or the whole of the portion in contact with the molten steel of various nozzles such as the upper nozzle A, the sliding nozzle plate B, the lower nozzle C, and the long nozzle D of such a structure composed of a plurality of nozzles for continuous casting. In addition, it can also be applied to a so-called inserted immersion nozzle ( Figure 4 The right side of the nozzle is not immersed in the molten steel, and the so-called open nozzle is not immersed in the molten steel. In addition, it can also be used as a stopper rod E located above the nozzle part to control the flow rate of the molten steel or open and close it, or a refractory G for lining the molten steel container.

[0036] exist Figure 5 and Figure 6 , there is shown an example in which a long nozzle and a lower nozzle are respectively provided with a refractory material 20 of the present invention on a part or the whole of the part in contact with molten steel. Figure 5 and Figure 6 In the embodiment, either or both of the inner refractory layer and the back side refractory layer may be the refractory 20 of the present invention. In addition, Figure 7 In the example, the refractory material 20 of the present invention is used to form a long nozzle other than the powder line material 21. Figure 7 In the embodiment, the refractory material 20 of the present invention may be arranged on the powder line material 21 portion.

[0037] exist Figure 8 , there is shown an example of a long stopper rod in which the refractory material 20 of the present invention is arranged on a part or the whole of the part in contact with the molten steel. Figure 8 In the embodiment, either or both of the tip end portion and the base end portion other than the tip end portion of the long stopper rod may be the refractory 20 of the present invention. Example

[0038] The raw material matching and evaluation results of the embodiments of the present invention and the comparative example are shown in Tables 1 to 6 below. In addition, in each table, "the volume ratio of refractory particles" is the volume ratio calculated based on the raw material matching, but the volume ratio is also maintained in the refractory made. That is, the "volume ratio of refractory particles" represented in each table is the same as the volume ratio of refractory particles of each particle size when the part of the constituent consisting of the free carbon component is removed from the constituent of the refractory as 100% by volume. In addition, in each table, "mineral phase" is represented as the refractory raw material in the raw material matching, but the mineral phase constituting these refractory raw materials will also be maintained in the refractory made. And, in each table, "additive" refers to the boron component source, and the addition amount is represented as the addition amount of the external doping of 100% by mass of the raw material matching relative to the "additive" other than the raw material.

[0039] An organic binder, namely a phenolic resin, is added to the raw material mix of each example shown in each table, and the kneaded clay is adjusted to a state suitable for forming. After the clay is formed by CIP, it is cured and dried at 300°C, and then heat-treated at 1000°C in a non-oxidizing atmosphere to obtain a refractory of each example.

[0040] The chemical composition of the obtained refractory was analyzed, the structural state was observed, and the refractory was subjected to evaluation tests. The chemical composition analysis was carried out according to the method of Japanese Industrial Standard JIS R2216. In the observation of the structural state, after the resin was impregnated into the refractory structure, a mirror surface was polished by mechanical grinding, and the MS value was obtained by the above-mentioned method under microscope observation, and the continuity of the void layer was observed. As evaluations of the refractory, the apparent porosity, the maximum thermal expansion coefficient up to 1500° C., the corrosion resistance, and the thermal shock resistance were evaluated, and a comprehensive evaluation was performed based on these evaluation results.

[0041] The apparent porosity is measured according to the method of Japanese Industrial Standard JIS R2205. The thermal expansion coefficient was measured up to 1500°C according to the method of Japanese Industrial Standard JIS R2207-3, and the maximum thermal expansion coefficient up to 1500°C was evaluated.

[0042] The corrosion resistance is evaluated by immersing the prism sample (20×20×180mm) of the refractory of each example in a crucible in which about 30mm of synthetic slag with a CaO / SiO2 mass ratio adjusted to 1.0 floats on the surface of low-carbon steel melted at 1550°C for 60 minutes. After being lifted up, the melting loss at the interface of the molten steel-molten slag is measured, and the degree is compared. Specifically, the melting loss of the refractory of each example is converted into a melting loss index with the melting loss of Comparative Example 2 as 100, and the situation where the melting loss index is less than 100 is recognized as the effect of solving the problem. More specifically, the situation where the melting loss index is less than 90 is evaluated as 0 (excellent), the situation where it exceeds 90 and is less than 100 is evaluated as △ (good), and the situation where it is more than 100 is evaluated as × (poor).

[0043] The evaluation of heat shock resistance is carried out by injecting molten iron at 1600°C into the inner hole of the sample at room temperature using a cylindrical sample (outer diameter / inner diameter (inner bore diameter) / height = 130 / 55 / 300mm), and applying heat shock to the refractory of the sample. After the test, the horizontal section is cut at 50mm intervals and checked for cracks. Then, the situation where no cracks are observed is evaluated as ○ (excellent), the situation where microcracks are confirmed is evaluated as △ (good), and the situation where cracks are confirmed is evaluated as × (poor).

[0044] The comprehensive evaluation was that the case where the MS value in the organizational state was within the range of the present invention (0.3% to 3.0%), the continuity of the void layer was approximately continuous, the apparent porosity was within the range of the present invention (16% to 1500°C), and the maximum thermal expansion coefficient to 1500°C was within the range of the present invention (0.6% to 0), the corrosion resistance was evaluated as 0, and the thermal shock resistance was evaluated as 0 was evaluated as ○ (excellent). The case where the MS value in the organizational state was within the range of the present invention (0.3% to 3.0%), the continuity of the void layer was approximately continuous, the apparent porosity was within the range of the present invention (16% to 1500°C), and the maximum thermal expansion coefficient to 1500°C was within the range of the present invention (0.6% to 0), and either the corrosion resistance or the thermal shock resistance was evaluated as △ was evaluated as △ (good). The case where the continuity of the void layer in the organizational state was partially continuous, the apparent porosity exceeded 16%, the maximum thermal expansion coefficient to 1500°C exceeded 0.6%, and the corrosion resistance was evaluated as × or the thermal shock resistance was evaluated as × was evaluated as × (poor).

[0045] (Table 1)

[0046] In Table 1, Examples 1 to 5 are examples in which the content of the free carbon component (hereinafter referred to as "FC") in the refractory is different, but within the scope of the present invention, the apparent porosity is low and the corrosion resistance is also excellent, and the thermal shock resistance is also excellent, and the comprehensive evaluation is ○ (excellent) or △ (good), and good results can be obtained. Among them, the comprehensive evaluation of Examples 2 to 4 in which the content of FC is within the preferred range of 15 mass % or more and 25 mass % or less is ○ (excellent), and particularly good results can be obtained. In contrast, Comparative Example 1 is an example in which the FC content is lower than the lower limit of the present invention, and a three-dimensional continuous carbonaceous matrix is ​​not formed in the refractory structure, and the continuity of the void layer around the coarse particles is damaged and becomes "partially continuous". Therefore, a sufficient low expansion effect is not obtained, and high expansion is achieved, and the thermal shock resistance decreases. On the other hand, Comparative Example 2 is an example in which the FC content exceeds the upper limit of the present invention, and the corrosion resistance decreases.

[0047] (Table 2)

[0048] In Table 2, Example 6 to Example 9 are different examples of the volume ratio of coarse refractory particles, but within the scope of the present invention, the comprehensive evaluation is ○ (excellent) or △ (good), and good results can be obtained. In addition, Example 6 is an example in which the volume ratio of coarse refractory particles is the lower limit of the present invention, i.e., 20% by volume. If the volume ratio of coarse refractory particles is 30% by volume, i.e., Example 7, it becomes high expansion, resulting in poor thermal shock resistance. In addition, Example 8 is an example in which the upper limit of the particle size of coarse refractory particles is 3mm, but if compared with Example 9 in which the upper limit of the particle size of coarse refractory particles is 1mm, the apparent porosity increases, resulting in poor corrosion resistance. On the other hand, Comparative Example 3 is an example in which the volume ratio of coarse-grained refractory particles is lower than the lower limit of the present invention, and as a result, the number of refractory particles in the refractory increases, becoming a refractory structure in which refractory particles exist continuously. Therefore, it becomes high expansion, and thermal shock resistance decreases.

[0049] Similarly in Table 2, embodiment 10, embodiment 11, embodiment 3, embodiment 12 and embodiment 13 are different examples of the volume ratio of the refractory particles of microparticles, but within the scope of the present invention, the comprehensive evaluation is ○ (excellent) or △ (good), and good results can be obtained. Wherein, the comprehensive evaluation of embodiment 11, embodiment 3 and embodiment 12 in the preferred range of the volume ratio of the refractory particles of microparticles above 5 mass % and below 15 mass % is ○ (excellent), and particularly good results can be obtained. On the contrary, Comparative Example 4 is an example in which the volume ratio of the refractory particles of microparticles is lower than the lower limit of the present invention, and a dense refractory cannot be obtained, and corrosion resistance decreases. On the other hand, Comparative Example 5 is an example in which the volume ratio of the refractory particles of microparticles exceeds the upper limit of the present invention, and as a result, the number of the refractory particles in the refractory increases, and becomes a refractory structure in which the refractory particles continuously exist. Therefore, it becomes high expansion, and thermal shock resistance decreases.

[0050] (Table 3)

[0051] In Table 3, Examples 3 and Examples 14 to 19 are examples in which the main mineral phases are different, but good results can be obtained within the scope of the present invention. In addition, in Example 15, the most abundant mineral phases are two kinds of corundum and spinel, so the main mineral phases are two kinds of corundum and spinel. In addition, in Example 17, the most abundant mineral phases are three kinds of corundum, spinel and periclase, so the main mineral phases are three kinds of corundum, spinel and periclase. On the other hand, in Comparative Example 6, the main mineral phase is periclase, but the periclase content exceeds the upper limit of the present invention, resulting in decreased corrosion resistance.

[0052] Likewise in Table 3, Embodiment 20 to Embodiment 22 are examples of refractory raw materials (refractory particles) comprising a plurality of mineral phases, but within the scope of the present invention, good results can be obtained. In addition, in Table 3, as refractory raw materials comprising a plurality of mineral phases, alumina zirconium oxide raw materials, zirconium mullite raw materials and mullite raw materials were used, but the content of the mineral phase of each raw material is as follows. Alumina zirconia raw materials: corundum 60 mass%, zirconium oxide 40 mass% Zirconium mullite raw materials: 50% by mass of zirconium oxide, 35% by mass of corundum, 15% by mass of silicon dioxide Mullite raw materials: 60% by mass of corundum, 40% by mass of silicon dioxide As described above, in the present invention, in the case of refractory particles containing multiple mineral phases, the multiple mineral phases contained in the refractory particles are respectively combined with the same mineral phases contained in other refractory particles to determine the "main mineral phase". For example, in Example 21, 65% by mass of zirconium mullite raw material contains 65×0.35=22.75% by mass of corundum, and if it is combined with 11.2% by mass of corundum in the corundum raw material, it is 33.95% by mass in the raw material combination. In addition, although 65% by mass of zirconium mullite raw material contains 65×0.5=32.5% by mass of zirconium oxide, since the content of zirconium oxide in the raw material combination is less than the content of the above-mentioned corundum, the main mineral phase of Example 21 is corundum.

[0053] On the other hand, in Table 3, the main mineral phase of Comparative Example 7 is zirconium oxide contained in the zirconium mullite raw material, which is outside the scope of the present invention. In addition, in Comparative Example 7, the content (total) of the silicon dioxide component and the silicon carbide component in the refractory exceeds the upper limit of the present invention. Therefore, the corrosion resistance decreases. In addition, although the main mineral phase of Comparative Example 8 is corundum, which is within the scope of the present invention, the contents (total) of silicon dioxide and silicon carbide in the refractory exceed the upper limit of the present invention, and thus the corrosion resistance is reduced.

[0054] (Table 4)

[0055] In Table 4, Embodiment 3, Embodiment 23 and Embodiment 24 are different examples of the content (total) of the silicon dioxide component and the silicon carbide component in the refractory, but within the scope of the present invention, comprehensive evaluation is ○ (excellent) or △ (good), and good results can be obtained. On the other hand, Comparative Example 9 is an example that the content (total) of the silicon dioxide component and the silicon carbide component in the refractory exceeds the upper limit value of the present invention, and the corrosion resistance decreases. In addition, by comparing Example 3 with Examples 23 and 24, it is preferred that the content (total) of the silicon dioxide component and the silicon carbide component in the refractory is 5% by mass or less, and it is particularly preferred to reduce the content of the silicon dioxide component.

[0056] (Table 5)

[0057] The examples shown in Table 5 are examples of different amounts and types of additives, but within the scope of the present invention, the comprehensive evaluation is ○ (excellent) or △ (good), and good results can be obtained. Among them, Example 26, Example 3, and Example 27 to Example 30, which contain 0.1 mass % or more and 3.0 mass % of boron components in terms of B2O3 conversion value, are comprehensively evaluated as ○ (excellent), and particularly good results can be obtained.

[0058] (Table 6)

[0059] The examples shown in Table 6 are examples of different aspect ratios and contents of carbon fibers, but within the scope of the present invention, the comprehensive evaluation is ○ (excellent) or △ (good), and good results can be obtained. Among them, the comprehensive evaluation of Example 32, Example 3, and Example 33, in which the aspect ratio of the carbon fibers is 15 to 200 and the content of the carbon fibers is limited to 5% by mass or less, is ○ (excellent), and particularly good results can be obtained.

Claims

1. A refractory for continuous casting, comprising 10 mass % or more and 30 mass % or less of free carbon components, the remaining main mineral phase is composed of one or more selected from corundum, spinel and periclase, the content of periclase is less than 40 mass %, and the total content of silicon dioxide and silicon carbide components is less than 15 mass %, characterized in that: When the portion of the constituent consisting of the free carbon component is removed from the constituent of the refractory as 100% by volume, the refractory particles having a particle size exceeding 0.3 mm account for more than 20% by volume, and the refractory particles having a particle size of less than 0.045 mm account for more than 3% by volume and less than 30% by volume, Among the refractory particles in the refractory, at least around the coarse particles of the largest particle size, there is a substantially continuous void layer similar in shape to the coarse particles, and in the substantially continuous void layer, the total thickness of the void layer existing at the interface between the matrix structure containing carbon at both ends and the coarse particles is 0.3% or more and 3.0% or less relative to the particle size of the coarse particles, Furthermore, the apparent porosity is 16% or less, and the maximum thermal expansion coefficient up to 1500° C. is 0.6% or less.

2. The refractory for continuous casting according to claim 1, characterized in that: The refractory particles having a particle size exceeding 0.3 mm account for 30% by volume or more, and the refractory particles having a particle size of 0.045 mm or less account for 5% by volume or more and 15% by volume or less.

3. The refractory for continuous casting according to claim 1 or 2, characterized in that: The boron component is contained in an amount of not less than 0.1 mass % and not more than 3.0 mass % in terms of B2O3 conversion value.

4. The refractory for continuous casting according to any one of claims 1 to 3, characterized in that: The matrix structure contains carbon fibers having an aspect ratio of 15 to 200, and the content of the carbon fibers is 5% by mass or less.

5. A refractory component for continuous casting, characterized in that: The refractory for continuous casting according to any one of claims 1 to 4 is arranged on a part or the whole of a portion in contact with molten steel.

Citation Information

Patent Citations

  • Refractory for nozzle used in continuous casting and nozzle for continuous casting

    CN102164695A

  • Manufacture of sliding nozzle plate

    JP1985096567A

  • Carbon-containing refractory

    JP1989176266A

  • Refractory for continuous casting and nozzle for continuous casting

    JP2013035040A

  • Refractory for casting, nozzle for casting using the same and plate for sliding nozzle

    JP2015193511A