Polyimide precursor for display substrate, polyimide film for display substrate, and display substrate

By containing acidic groups in the polyimide film, it extends the charging half-life and reduces the attenuation rate, solving the problem of charge charging at the interface of the polyimide film and achieving high adhesion and charge suppression.

CN118786164APending Publication Date: 2024-10-15UBE CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380024310.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-03
Filing Date
2023-03-03
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

When a polyimide film is used as a display substrate, it is easy to accumulate charges at the interface, causing the problem of residual images in the display.

Method used

By containing acidic groups in the polyimide film, the charge half-life is extended and the charge decay rate after 120 seconds is reduced, thereby suppressing charge accumulation and charging and achieving high adhesion.

Benefits of technology

It effectively suppresses the charging of charges on the display substrate, reduces the occurrence of residual images, and improves the adhesion of the polyimide film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786164A_ABST
    Figure CN118786164A_ABST
Patent Text Reader

Abstract

The present invention provides a polyimide precursor for display substrates, which has a structural unit represented by general formula (1), and which contains an acidic group-containing group as at least some of the group represented by X1 in general formula (1), the group represented by Y1 in general formula (1), and the terminal group. The content of the acidic group is 15 * 10 <-3 > or more. (In general formula (1), X1 is a tetravalent aromatic group or aliphatic group, Y1 is a divalent aromatic group, and R1 and R2 are each independently a hydrogen atom, an alkyl group having 1-6 carbon atoms, or an alkylsilyl group having 3-9 carbon atoms. > # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyimide precursor for a display substrate which has a long charging half-life, a low charging decay rate after 120 seconds based on the charging half-life measurement, can contribute to the suppression of charge up, and can achieve high adhesion, and a polyimide film for a display substrate and a display substrate obtained using the polyimide precursor. Background Art

[0002] Polyimide is widely used in electrical and electronic equipment such as flexible wiring boards and TAB (Tape Automated Bonding) tapes due to its excellent heat resistance, solvent resistance (chemical resistance), mechanical properties, and electrical properties. For example, polyimide obtained from aromatic tetracarboxylic dianhydride and aromatic diamine, particularly polyimide obtained from 3,3',4,4'-biphenyltetracarboxylic dianhydride and p-phenylenediamine, is preferably used.

[0003] In addition, polyimide is being studied as a substitute for glass substrates in the field of display devices. By replacing the glass substrates used in various display devices with plastic substrates made of polyimide, it is possible to provide lightweight and highly flexible displays that can be bent or rolled.

[0004] For example, Patent Document 1 proposes a method of using a polyimide precursor including a specific unit structure as a polyimide precursor applicable to display substrates.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2012-41531 Summary of the invention

[0008] Problems to be solved by the invention

[0009] When a polyimide film is used for a display substrate, in order to obtain sufficient gas barrier properties, a SiO x On the other hand, when the polyimide film is used as a display substrate, electric charges are accumulated at the interface between the polyimide film and the inorganic gas barrier layer. Due to the occurrence of charging, a small amount of current flows through the switching element, etc., which causes a residual image on the display.

[0010] Means for solving problems

[0011] In this regard, the inventors conducted in-depth research and found that by making the polyimide film contain acidic groups in a specified proportion, the charge half-life is long, and the charge decay rate after 120 seconds based on the charge half-life measurement can be reduced, thereby promoting the elimination of charge accumulation at the interface between the polyimide film and the inorganic gas barrier layer, thereby helping to suppress charging, thereby completing the present invention.

[0012] Furthermore, the present inventors have conducted intensive studies and have found that high adhesion can be achieved by adopting the above-mentioned configuration.

[0013] That is, the present invention provides the following [1] to [8].

[0014] [1] A polyimide precursor for a display substrate, which is a polyimide precursor for a display substrate having a structural unit represented by the following general formula (1), wherein X in the general formula (1) is 1 The group shown, Y in the above general formula (1) 1 At least a part of the groups shown in the formula (a) and the terminal groups includes a group containing an acidic group,

[0015] The content of the above acidic groups is 15×10 -3 above.

[0016] [Chemistry 1]

[0017]

[0018] (In the above general formula (1), X 1 is a tetravalent aromatic group or aliphatic group, Y 1 is a divalent aromatic group, R 1 , R 2 Each is independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkylsilyl group having 3 to 9 carbon atoms.

[0019] [2] The polyimide precursor for a display substrate according to [1], wherein the group containing an acidic group is at least one selected from a group containing a carboxyl group and a group containing a sulfonic acid group.

[0020] [3] The polyimide precursor for a display substrate according to [2], wherein the carboxyl group-containing group is a group derived from at least one selected from 3,5-diaminobenzoic acid, 5,5'-methylenebis(2-aminobenzoic acid), mellitic acid and mellitic anhydride, and trimellitic anhydride.

[0021] [4] The polyimide precursor for a display substrate according to [3], wherein the carboxyl group-containing group is a group derived from at least one selected from 3,5-diaminobenzoic acid, mellitic acid and mellitic anhydride, and trimellitic anhydride.

[0022] [5] The polyimide precursor for a display substrate as described in any one of [2] to [4], wherein the group containing a sulfonic acid group is a group derived from at least one selected from 1,4-phenylenediamine-2-sulfonic acid, 1,3-phenylenediamine-4-sulfonic acid, 3,5-diamino-2,4,6-trimethylbenzenesulfonic acid and 4,4'-diaminostilbene-2,2'-disulfonic acid.

[0023] [6] The polyimide precursor for a display substrate according to [5], wherein the group containing a sulfonic acid group is a group derived from at least one selected from 1,4-phenylenediamine-2-sulfonic acid and 1,3-phenylenediamine-4-sulfonic acid.

[0024] [7] A polyimide film for a display substrate, obtained using the polyimide precursor for a display substrate according to any one of [1] to [6].

[0025] [8] A display substrate comprising the polyimide film for a display substrate according to [7].

[0026] Effects of the Invention

[0027] According to the present invention, a polyimide precursor for a display substrate can be provided which has a long charging half-life, has a low charging decay rate after 120 seconds based on charging half-life measurement, can contribute to suppressing charging, and can achieve high adhesion. DETAILED DESCRIPTION

[0028] <Polyimide precursor for display substrate>

[0029] The polyimide precursor for display substrates of the present invention is a polyimide precursor for forming a polyimide film for display substrates, and is a polyimide precursor having a structural unit represented by the following general formula (1), wherein X in the general formula (1) is 1 The group shown, Y in the above general formula (1) 1 At least a part of the groups shown in the formula (a) and the terminal groups includes a group containing an acidic group,

[0030] The content of the above acidic groups is 15×10 -3 above.

[0031] [Chemistry 2]

[0032]

[0033] (In the above general formula (1), X 1 is a tetravalent aromatic group or aliphatic group, Y 1 is a divalent aromatic group, R 1 , R2 Each is independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkylsilyl group having 3 to 9 carbon atoms.

[0034] In the above general formula (1), X 1 Y is the residue after removing four COOH groups from tetracarboxylic acid (i.e., the residue after removing two carboxylic anhydride groups (CO)2O from tetracarboxylic dianhydride), 1 It is the residue after removing two NH2 groups from a diamine. 1 , R 2 A hydrogen atom or an alkylsilyl group having 3 to 9 carbon atoms is preferred, and a hydrogen atom is more preferred.

[0035] As the structural unit represented by the general formula (1), there can be mentioned a structural unit obtained by reacting a tetracarboxylic acid component and a diamine component to form an amide bond (—CONH—).

[0036] As a tetracarboxylic acid component, aromatic tetracarboxylic dianhydride, aliphatic tetracarboxylic dianhydride, etc. are mentioned, for example.

[0037] Specific examples of the aromatic tetracarboxylic dianhydride include 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), pyromellitic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, diphenylsulfone-3,4,3',4'-tetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl)sulfide dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride (also known as 4,4'-(hexafluoroisopropylidene)diphthalic anhydride), 2,3,3',4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, 2 ,2-bis(3,4-dicarboxyphenyl)propane dianhydride, p-phenylenebis(trimellitic acid monoester anhydride), p-biphenylenebis(trimellitic acid monoester anhydride), m-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, p-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)phthalic dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)phthalic dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)biphenyl dianhydride, 2,2-bis[(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, 2,3,6,7-naphthalenetetracarboxylic acid dianhydride, 1,4,5,8-naphthalenetetracarboxylic acid dianhydride, 4,4'-(2,2-hexafluoroisopropylidene)diphthalic acid dianhydride, etc. These may be used alone or in combination of two or more.

[0038] As the aliphatic tetracarboxylic dianhydride, alicyclic tetracarboxylic dianhydride can be preferably used. Specific examples of alicyclic tetracarboxylic dianhydride include (1S, 2R, 4S, 5R)-cyclohexanetetracarboxylic dianhydride, cis, cis, cis-1,2,4,5-cyclohexanetetracarboxylic dianhydride, (1S, 2S, 4R, 5R)-cyclohexanetetracarboxylic dianhydride, (1R, 2S, 4S, 5R)-cyclohexanetetracarboxylic dianhydride, bicyclo [2.2.2] octane-2,3,5,6-tetracarboxylic dianhydride, bicyclo [2.2.2] oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, 4-(2,5-dioxo-tetrahydrofuran)-1,2,4,5-cyclohexane ... 1,2-dihydronaphthalene-1,2-dicarboxylic anhydride, tetrahydrofuran-2,3,4,5-tetracarboxylic dianhydride, bicyclo-3,3',4,4'-tetracarboxylic dianhydride, 1,2,3,4-cyclopentanetetracarboxylic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride (hereinafter sometimes referred to as "CBDA"), 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,4-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2,3,4-cyclohexanetetracarboxylic dianhydride, pentacyclic [8.2.1.1 4,7 .0 2,9 .0 3,8 ]tetradecane-5,6,11,12-tetracarboxylic dianhydride, 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic dianhydride, cyclohex-1-ene-2,3,5,6-tetracarboxylic dianhydride, bicyclo[2.2.1]heptane-2,3,5,6-tetracarboxylic dianhydride, etc. These may be used alone or in combination of two or more.

[0039] The tetracarboxylic acid compound as the tetracarboxylic acid component is preferably an acid dianhydride selected from 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), pyromellitic dianhydride (PMDA), 4,4'-oxydiphthalic dianhydride (ODPA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), 1,2,3,4-cyclobutanetetracarboxylic dianhydride (CBDA), 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride (6FDA), and 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride (DSDA), and 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride (s-BPDA) is more preferred.

[0040] Examples of the diamine compound as the diamine component include 4,4'-diaminodiphenyl ether, 2,2'-dimethylbenzidine, 4,4'-diaminodiphenylmethane, 4,4'-diamino-1,2-diphenylethane, p-phenylenediamine (PPD), m-phenylenediamine, 2,4-diaminotoluene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, m-phenylenediamine, p-phenylenediamine, 2,2 -Aromatic diamines having an aromatic group, such as bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-methylenebis(2,6-xylidine), α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene, 2,2'-dimethyl-4,4'-aminobiphenyl, 3,3'-dimethyl-4,4'-aminobiphenyl, and 2,2'-ethylenediphenylamine; 1,4-diaminocyclohexane, 1,4-diamino-2-methylcyclohexane, 1,4-diamino-2-ethylcyclohexane cyclohexane, 1,4-diamino-2-n-propylcyclohexane, 1,4-diamino-2-isopropylcyclohexane, 1,4-diamino-2-n-butylcyclohexane, 1,4-diamino-2-isobutylcyclohexane, 1,4-diamino-2-sec-butylcyclohexane, 1,4-diamino-2-tert-butylcyclohexane, 1,2-diaminocyclohexane, 1,3-diaminocyclobutane, 1,4-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, diaminobicycloheptane, diaminomethyl Alicyclic diamines having an alicyclic structure such as bicycloheptane, diaminooxybicycloheptane, diaminomethyloxybicycloheptane, isophoronediamine, diaminotricyclodecane, diaminomethyltricyclodecane, bis(aminocyclohexyl)methane, bis(aminocyclohexyl)isopropylidene, 6,6'-bis(3-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirobiindane, and 6,6'-bis(4-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirobiindane;2,2'-Bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 2,3,5,6-tetrafluoro-1,4-diaminobenzene, 2,4,5,6-tetrafluoro-1,3-diaminobenzene, 2,3,5,6-tetrafluoro-1,4-benzene(dimethylamine), 2,2'-difluoro-(1,1'-biphenyl)-4,4'-diamine, 2,2',6,6'-tetrafluoro-(1,1'-biphenyl)-4,4'-diamine, 4,4'-diaminooctafluorobiphenyl, 2,2-bis(4-aminophenyl)hexafluoropropane, 4,4'-oxy Fluorine-containing diamines such as bis(2,3,5,6-tetrafluoroaniline), 3,3'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 4,4'-diamino-2,2'-bis(trifluoromethyl)diphenyl ether, 1,4-bis[4-amino-2-(trifluoromethyl)phenoxy]benzene, 2,2-bis[4-[4-amino-2-(trifluoromethyl)phenoxy]hexafluoropropane, 3,5-diaminotrifluorinated benzene, 4,4-diamino-2-(trifluoromethyl)diphenyl ether; diamines containing ester bonds such as 4-aminobenzoic acid 4-aminophenyl ester and bis(4-aminophenyl)terephthalate; etc. These may be used alone or in combination of two or more. ;

[0041] The diamine compound as the diamine component is preferably 4,4'-diaminodiphenyl ether, 2,2'-dimethylbenzidine, 4,4'-diaminodiphenylmethane, 4,4'-diamino-1,2-diphenylethane, p-phenylenediamine (PPD), and 2,2-bis[4-(4-aminophenoxy)phenyl]propane, and more preferably p-phenylenediamine (PPD).

[0042] The polyimide precursor of the present invention contains an acidic group-containing group as X in the above general formula (1). 1 The group shown, Y in the above general formula (1) 1 The groups shown in the figure and at least a part of the terminal groups, and the acidic group content is 15×10 -3 The acid group content is preferably 16×10 -3 More preferably 18×10 -3 More preferably, 20×10 -3 By including the acidic groups in such a content, the polyimide film obtained from the polyimide precursor of the present invention can contain a predetermined amount of acidic groups, thereby making the charge half-life long, and further, the charge decay rate after 120 seconds can be suppressed to a low level, thereby contributing to the suppression of charging, and further achieving high adhesion. It should be noted that the charge half-life and the charge decay rate after 120 seconds can be measured by the charge half-life measurement according to JIS L 1094A.

[0043] The acidic group content can be calculated from the following formula.

[0044] Acidic group content = {(number of moles of the acidic group-containing monomer used to form the polyimide precursor) × (number of acidic groups per molecule of the acidic group-containing monomer)} ÷ (number of moles of all monomers forming the polyimide precursor)

[0045] Here, in the case of using a plurality of monomers containing acidic groups with different numbers of acidic groups per molecule, according to their usage ratio, the content of the acidic group is calculated according to the above formula and used. In addition, with respect to tetracarboxylic acid, it is assumed that 4 carboxylic acids in the acidic group in 1 molecule react with diamine during polymerization, and do not remain as acidic groups when polyimide is made, and the number of acidic groups when the amount of acidic groups is calculated is calculated using the number obtained by subtracting 4 from the number of acidic groups (including anhydride groups) in 1 molecule of tetracarboxylic acid. That is, based on the number of free carboxyl groups that do not contribute to the generation of imide bonds, the content of the acidic group is calculated. For example, 3,3',4,4'-biphenyltetracarboxylic dianhydride has only 4 carboxyl groups, all of which contribute to the generation of imide bonds, so in the calculation of the content of the above-mentioned acidic groups, the number of acidic groups is zero. In addition, regarding mellitic acid, there are mixed states of a state with no acid anhydride group, a state with one acid anhydride group, and a state with two acid anhydride groups. On the other hand, 4 of the 6 carboxyl groups constituting mellitic acid are used to form an imide bond, and after forming a polyimide precursor or a polyimide film, there are usually 2 free carboxyl groups. Therefore, regarding mellitic acid, the number of carboxyl groups as acidic groups is 2, and the content of acidic groups can be calculated based on this.

[0046] As the acidic group, there is no particular limitation, and carboxyl (-COOH), sulfonic acid (-SO3H), phosphonic acid (-PO3H2), etc. can be cited. Among these, carboxyl and sulfonic acid are preferred because they can make the charged half-life longer and can suppress the charged decay rate after 120 seconds to a lower level, thereby achieving a higher suppression effect on charging. It should be noted that, here, as the acidic group, it can be a group that provides an acidic group such as unesterified by hydrolysis.

[0047] As X in the above general formula (1) 1 The method of containing a group containing an acidic group is not particularly limited, and examples thereof include a method of using a specific tetracarboxylic acid compound as at least a part of the tetracarboxylic acid component. Examples of such specific tetracarboxylic acid compounds include -COOR 1 、-COOR 2In addition to the carboxyl group having two amide bonds (-CONH-), a compound having an acidic group such as a carboxyl group (hereinafter referred to as a tetracarboxylic acid compound having an acidic group). That is, the tetracarboxylic acid compound having an acidic group is a compound containing an acidic group that does not contribute to the imidization reaction in addition to the tetracarboxylic acid structure that contributes to the imidization reaction.

[0048] As the specific example of the tetracarboxylic acid compound with an acidic group, as the compound with carboxyl as the acidic group, for example mellitic acid, mellitic anhydride, methyl mellitic acid, dimethyl mellitic acid, trimethyl mellitic acid, ethyl mellitic acid, diethyl mellitic acid, triethyl mellitic acid, propyl mellitic acid, dipropyl mellitic acid, tripropyl mellitic acid, butyl mellitic acid, dibutyl mellitic acid, tributyl mellitic acid, phenyl mellitic acid, diphenyl mellitic acid, triphenyl mellitic acid etc. can be enumerated. They can be used alone, or two or more kinds can be used in combination. Among these, preferred mellitic acid and mellitic anhydride are.

[0049] The amount of the tetracarboxylic acid compound having an acidic group used may be appropriately selected according to the amount of the acidic group contained in the polyimide precursor, and is preferably 1 mol% or more, more preferably 2 mol% or more, preferably 70 mol% or less, more preferably 60 mol% or less, further preferably 50 mol% or less, still more preferably 10 mol% or less, and particularly preferably 6 mol% or less, based on 100 mol% of the total amount of the tetracarboxylic acid component.

[0050] In addition, as the Y in the above general formula (1) 1The method of containing a group containing an acidic group in the group shown is not particularly limited, and for example, a method of using a diamine compound containing an acidic group as at least a part of the diamine component can be mentioned. Such a diamine compound containing an acidic group can be any compound having an acidic group such as a carboxyl group in addition to a diamine structure, and as a compound having a carboxyl group as an acidic group, for example, 3,5-diaminobenzoic acid (3,5-DABA), 5,5'-methylenebis(2-aminobenzoic acid), 3,3'-diamino-4,4'-dicarboxybiphenyl, 4,4'-diamino-3,3'-dicarboxydiphenylmethane, 3,3'-diamino-4,4'-dicarboxydiphenylmethane, 2,2-bis[4-(4-amino-3-carboxyphenyl)phenyl]propane, etc. can be mentioned. In addition, as the compound having sulfonic acid group as acidic group, 1,4-phenylenediamine-2-sulfonic acid, 1,3-phenylenediamine-2-sulfonic acid, 3,5-diamino-2,4,6-trimethylbenzenesulfonic acid and 4,4'-diaminobenzene-2,2'-disulfonic acid, 4,4'-bis(4-aminophenoxy)biphenyl-3,3'-disulfonic acid etc. can be cited. They can be used alone or two or more kinds can be mixed and used. Among these, as the compound having carboxyl group as acidic group, 3,5-diaminobenzoic acid (3,5-DABA) is preferred, and as the compound having sulfonic acid group as acidic group, 1,4-phenylenediamine-2-sulfonic acid and 1,3-phenylenediamine-2-sulfonic acid are preferred.

[0051] The amount of the acidic group-containing diamine compound used can be appropriately selected according to the amount of the acidic group contained in the polyimide precursor, and is preferably 2 mol% or more, more preferably 3 mol% or more, and further preferably 4 mol% or more, and is preferably 70 mol% or less, more preferably 60 mol% or less, further preferably 50 mol% or less, further more preferably 10 mol% or less, and particularly preferably 6 mol% or less, based on 100 mol% of the total amount of the diamine component.

[0052] Alternatively, as a method for making the terminal group contain a group containing an acidic group, there is no particular limitation, and for example, a method of replacing a part of the tetracarboxylic acid component with a dicarboxylic acid compound having an acidic group or a dicarboxylic acid compound anhydride having an acidic group can be cited. The dicarboxylic acid compound having an acidic group is a compound having an acidic group other than the carboxyl group constituting the dicarboxylic acid structure and not contributing to the imidization reaction in addition to the dicarboxylic acid structure that contributes to the imidization reaction. In addition, the dicarboxylic acid compound anhydride having an acidic group is a compound having an acidic group other than the carboxyl group constituting the dicarboxylic acid structure and not contributing to the imidization reaction in addition to the dicarboxylic anhydride structure that contributes to the imidization reaction.

[0053] As the dicarboxylic acid compound with an acidic group or the dicarboxylic acid compound anhydride with an acidic group, as the compound with carboxyl as the acidic group, for example, trimellitic acid, trimellitic anhydride, trimellitic acid, trimellitic anhydride, etc. can be mentioned. In addition, as the compound with sulfonic acid group as the acidic group, 3-sulfophthalic acid, 4-sulfophthalic acid, 3-sulfophthalic anhydride, 4-sulfophthalic anhydride, etc. can be mentioned. They can be used alone or two or more can be mixed and used. Among these, preferably there is a compound with carboxyl as the acidic group, preferably trimellitic anhydride.

[0054] The amount of the dicarboxylic acid compound having an acidic group or the anhydride of the dicarboxylic acid compound having an acidic group used may be appropriately selected depending on the amount of the acidic group contained in the polyimide precursor, and is preferably 1 mol% or more, more preferably 1.5 mol% or more, and even more preferably 2 mol% or more, in terms of tetracarboxylic acid conversion, in the total of 100 mol% of the tetracarboxylic acid component, the dicarboxylic acid compound having an acidic group and the anhydride of the dicarboxylic acid compound having an acidic group, and is preferably 35 mol% or less, more preferably 30 mol% or less, even more preferably 25 mol% or less, and particularly preferably 5 mol% or less, and is preferably 2 mol% or more, more preferably 3 mol% or more, and even more preferably 4 mol% or more, and is preferably 70 mol% or less, more preferably 60 mol% or less, even more preferably 50 mol% or less, still more preferably 10 mol% or less, and particularly preferably 6 mol% or less, in terms of the compound conversion. The dicarboxylic acid compound having an acidic group and the anhydrous dicarboxylic acid compound having an acidic group contain a dicarboxylic acid structure rather than a tetracarboxylic acid structure as a structure contributing to the imidization reaction, and therefore the amount added in terms of tetracarboxylic acid is usually half of the amount added in terms of the compound.

[0055] In addition, as Y in the above general formula (1), 1 The group represented by may include a group represented by the following general formula (2).

[0056] [Chemistry 3]

[0057]

[0058] (In the above general formula (2), R 3 , R 4 , R 5 , R 6 Each is independently a hydrogen atom, an alkyl group having 1 to 12 carbon atoms which may have a substituent, or an aryl group having 6 to 12 carbon atoms which may have a substituent.)

[0059] By containing the group represented by the general formula (2), the charging half-life can be made longer and the charging decay rate after 120 seconds can be suppressed to a lower level, thereby further improving the effect of suppressing charging.

[0060] As a group represented by the above general formula (2) as Y in the above general formula (1) 1 The method of using a group represented by the following formula (3) as at least a part of the diamine component includes, for example, a method of using a diamine compound containing a triazine structure represented by the following general formula (3).

[0061] [Chemistry 4]

[0062]

[0063] (In the above general formula (3), R 3 , R 4 , R 5 , R 6 Same as the above general formula (2).

[0064] In the above general formula (2) and the above general formula (3), R 3 , R 4 , R 5 Each is independently a hydrogen atom, an alkyl group having 1 to 12 carbon atoms which may be substituted, or an aryl group having 6 to 12 carbon atoms which may be substituted, preferably a hydrogen atom, an alkyl group having 1 to 12 carbon atoms which may not be substituted, or an aryl group having 6 to 12 carbon atoms which may not be substituted, more preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms which may not be substituted, and still more preferably a hydrogen atom.

[0065] In the above general formula (2) and the above general formula (3), R 6 It is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms which may have a substituent, or an aryl group having 6 to 12 carbon atoms which may have a substituent, preferably a hydrogen atom, an alkyl group having 1 to 12 carbon atoms which may not have a substituent, or an aryl group having 6 to 12 carbon atoms which may not have a substituent, more preferably a hydrogen atom or an aryl group having 6 to 12 carbon atoms which may not have a substituent, and further preferably a phenyl group.

[0066] Specific examples of the triazine structure-containing diamine compound represented by the general formula (3) include 2,4-bis(3-aminoanilino)-6-anilino-1,3,5-triazine (p-ATDA), 2,4-bis(3-aminoanilino)-6-benzylamino-1,3,5-triazine, 2,4-bis(3-aminoanilino)-6-naphthylamino-1,3,5-triazine, 2,4-bis(3-aminoanilino)-6-biphenylamino-1,3,5-triazine, 2,4-bis(3-aminoanilino)-6-diphenylamino-1,3,5-triazine, 2,4-bis(3-aminoanilino)-6-dibenzylamino-1,3,5-triazine, and 2,4-bis(3-aminoanilino)-6-dinaphthylamino-1,3,5-triazine. , 2,4-bis(3-aminoanilino)-6-N-methylanilino-1,3,5-triazine, 2,4-bis(3-aminoanilino)-6-N-methylnaphthylamino-1,3,5-triazine, 2,4-bis(3-aminoanilino)-6-methylamino-1,3,5-triazine, 2,4-bis(3-aminoanilino)-6-ethylamino-1,3,5-triazine, 2,4-bis(3-aminoanilino)-6-dimethylamino-1,3,5-triazine, 2,4-bis(3-aminoanilino)-6-diethylamino-1,3,5-triazine, 2,4-bis(3-aminoanilino)-6-dibutylamino-1,3,5-triazine, 2,4-bis(3-aminoanilino)-6-amino-1,3,5-triazine, etc. These may be used alone or in combination of two or more. Among these, 2,4-bis(3-aminoanilino)-6-anilino-1,3,5-triazine (p-ATDA) is preferred. By using 2,4-bis(3-aminoanilino)-6-anilino-1,3,5-triazine (p-ATDA), a group represented by the following formula (4) can be introduced as Y in the above general formula (1). 1 .

[0067] [Chemistry 5]

[0068]

[0069] The amount of the triazine structure-containing diamine compound represented by the general formula (3) is preferably 50 to 100 mol%, more preferably 70 to 100 mol%, and even more preferably 90 to 100 mol%, based on 100 mol% of the total amount of the diamine component. 1 The ratio of the structural unit containing the group represented by the general formula (2) in 100 mol % of the groups represented by the general formula (2) is preferably 50 to 100 mol %, more preferably 70 to 100 mol %, and even more preferably 90 to 100 mol %.

[0070] The polyimide precursor of the present invention can be easily prepared using, for example, a conventionally known method. The preparation method of the polyimide precursor of the present invention is not particularly limited. For example, by reacting approximately equimolar tetracarboxylic acid components and diamine components in a solvent at a relatively low temperature of 100°C or below, preferably 80°C or below, in a manner such that the imidization reaction does not proceed or does not proceed excessively, the polyimide precursor can be obtained in a state where the polyimide precursor is dissolved in the solvent, i.e., in a state of a polyimide precursor solution. It should be noted that in the polyimide precursor solution thus obtained, in addition to the polyamic acid as the polyimide precursor, a polyimide precursor or polyimide partially or completely imidized and formed by the imidization reaction may also be included.

[0071] The polymerization temperature when obtaining the polyimide precursor of the present invention is preferably 25°C to 100°C, more preferably 40°C to 80°C, and further preferably 50°C to 80°C. The polymerization time is preferably 0.1 hours to 24 hours, and more preferably 2 hours to 12 hours. By making the polymerization temperature and the polymerization time within the above range, a high molecular weight polyimide precursor can be easily obtained with good production efficiency. The polymerization can also be carried out in an air atmosphere, usually in an inert gas, preferably nitrogen atmosphere. The molar ratio of the tetracarboxylic acid component and the diamine component is approximately equimolar, specifically, 0.90 to 1.10, preferably 0.95 to 1.05, more preferably more than 0.98 and less than 1.04, and more preferably more than 0.98 and less than 1.03. In addition, in this specification, "substantially equimolar" means that the above-mentioned molar ratio exceeds the range of 0.99 to 1.01, and "equimolar" means a significant figure of 1.00 for the molar ratio.

[0072] When making a tetracarboxylic acid component and a diamine component react, the following method can be usually preferably adopted: adding a diamine component to a polymerization apparatus filled with a solvent, confirming that the diamine component is dissolved, and then adding a tetracarboxylic acid component.

[0073] As the solvent used when making tetracarboxylic acid component and diamine component react, as long as can make polyimide precursor polymerization and can dissolve polyimide precursor, can be any solvent, can be aqueous solvent, can be organic solvent.Solvent can be a mixture of 2 or more kinds, can also use the mixed solvent of 2 or more kinds of organic solvents or the mixed solvent of water and 1 or more kinds of organic solvents. The organic solvent is not particularly limited, and examples thereof include N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, N-methylcaprolactam, hexamethylphosphoric triamide, 1,2-dimethoxyethane, bis(2-methoxyethyl)ether, 1,2-bis(2-methoxyethoxy)ethane, tetrahydrofuran, bis[2-(2-methoxyethoxy)ethyl]ether, 1,4-dioxane, dimethyl sulfoxide, dimethyl sulfone, diphenyl ether, cyclopentane, diphenyl sulfone, tetramethyl urea, anisole, m-cresol, phenol, γ-butyrolactone, etc. It should be noted that in the present invention, the solvent used when polymerizing the polyimide precursor can be directly used as the solvent of the polyimide precursor solution when manufacturing the polyimide film for display substrates.

[0074] The polyimide precursor solution is not particularly limited, and the solid content concentration of the polyimide precursor is preferably 5% by mass or more and 45% by mass or less relative to the total amount of the polyimide precursor and the solvent, more preferably 5% by mass or more and 40% by mass or less, and further preferably more than 10% by mass and less than 30% by mass. If the solid content concentration is lower than 5% by mass, it is sometimes time-consuming to thicken the thickness of the film, and if it is higher than 45% by mass, the solution viscosity sometimes becomes too high, and a special film manufacturing device is sometimes required.

[0075] The viscosity of the polyimide precursor solution at 30° C. is not limited, but is preferably 1000 Pa·sec or less, more preferably 0.5 Pa·sec to 500 Pa·sec, further preferably 1 Pa·sec to 300 Pa·sec, and particularly preferably 2 Pa·sec to 200 Pa·sec for ease of handling.

[0076] To the polyimide precursor solution, known additives such as amine compounds, dehydrating agents and other additives for accelerating imidization reaction, organic phosphorus-containing compounds, the above-mentioned fillers, surfactants, silane coupling agents, leveling materials and the like may be added as needed.

[0077] As the amine compound, there can be mentioned substituted or unsubstituted nitrogen-containing heterocyclic compounds, N-oxide compounds of the nitrogen-containing heterocyclic compounds, substituted or unsubstituted amino acid compounds, aromatic hydrocarbon compounds or aromatic heterocyclic compounds having hydroxyl groups, etc. As specific examples of the imidization catalyst, there can be mentioned imidazole derivatives such as 1,2-dimethylimidazole, N-methylimidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, 5-methylbenzimidazole, N-benzyl-2-methylimidazole, isoquinoline, 3,5-lutidine, 3,4-lutidine, 2,5-lutidine, 2,4-lutidine, 4-n-propylpyridine, etc. The amount of the imidization catalyst used is preferably 0.01 times or more and 2 times or less, and particularly preferably 0.02 times or more and 1 times or less relative to the amic acid unit of the polyamic acid. By using an imidization catalyst, the physical properties of the obtained polyimide film, particularly the elongation and edge tear resistance, may be improved.

[0078] Examples of other amine compounds include aliphatic tertiary amines such as trimethylamine and triethylenediamine, aromatic tertiary amines such as dimethylaniline, and heterocyclic tertiary amines such as isoquinoline, pyridine, α-picoline, and β-picoline, and they can be added as needed.

[0079] Examples of the dehydrating agent include aliphatic carboxylic anhydrides such as acetic anhydride, propionic anhydride, and butyric anhydride, and aromatic carboxylic anhydrides such as benzoic anhydride.

[0080] Examples of the organic phosphorus-containing compound include phosphoric acid esters such as monocaproyl phosphate, monooctyl phosphate, monolauryl phosphate, monomyristyl phosphate, monocetyl phosphate, monostearyl phosphate, monophosphate of triethylene glycol monotridecyl ether, monophosphate of tetraethylene glycol monolauryl ether, monophosphate of diethylene glycol monostearyl ether, dicaproyl phosphate, dioctyl phosphate, didecanoyl phosphate, dilauryl phosphate, dimyristyl phosphate, dicetyl phosphate, distearyl phosphate, diphosphate of tetraethylene glycol mononeopentyl ether, diphosphate of triethylene glycol monotridecyl ether, diphosphate of tetraethylene glycol monolauryl ether, and diphosphate of diethylene glycol monostearyl ether, and amine salts of these phosphoric acid esters. Examples of the amine include ammonia, monomethylamine, monoethylamine, monopropylamine, monobutylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, trimethylamine, triethylamine, tripropylamine, tributylamine, monoethanolamine, diethanolamine, and triethanolamine.

[0081] <Polyimide film for display substrate>

[0082] The polyimide film for display substrates of the present invention is obtained by using the above-mentioned polyimide precursor for display substrates.

[0083] The polyimide film for display substrates of the present invention can be produced by a known method using, for example, the above-mentioned polyimide precursor solution (a solution containing the polyimide precursor for display substrates of the present invention, also referred to as “display substrate forming solution”).

[0084] The polyimide film for the display substrate of the present invention can be manufactured, for example, by the following methods: a method in which a polyimide precursor solution is applied to a support and dried, and the obtained laminate of the support and the polyimide precursor film is chemically imidized / or thermally imidized; a method in which a polyimide precursor solution is applied to a support and dried, and the obtained laminate of the support and the polyimide precursor film is chemically imidized / or thermally imidized, and then the polyimide film is peeled off from the support; or a method in which a polyimide precursor solution is applied to a support and dried, and then the polyimide precursor film is peeled off from the support to obtain a self-supporting film, and then the self-supporting film is fixed and chemically imidized / or thermally imidized.

[0085] The method for coating the polyimide precursor solution on the support is not particularly limited as long as it is a method that can form a desired coating film, and known methods such as spin coating, screen printing, rod coating, electrodeposition, casting, extrusion molding, etc. can be appropriately used. Considering the subsequent drying, heating, etc. until the polyimide film is formed, for example, the thickness of the coating film can be formed to about 1 μm to 500 μm.

[0086] The drying conditions are not particularly limited, and the drying temperature can be set to a temperature range of, for example, 20°C to 200°C, preferably 180°C to 180°C, and more preferably 30°C to 150°C. The drying time varies according to the heating temperature, for example, 1 minute to 60 minutes, preferably 30 minutes to 20 minutes. The heating means is hot air, infrared rays, etc., and the means are not particularly limited, and can be performed multiple times or staged. The drying conditions can be selected, for example, in an atmosphere of an inert gas such as vacuum, nitrogen, or air, etc., taking into account the characteristics of the polyimide film.

[0087] The support on which the polyimide precursor solution is applied is not particularly limited as long as the polyimide precursor solution can be applied and does not affect subsequent formation of a polyimide precursor film by drying and heating, chemical imidization, or thermal imidization reaction, but glass, metal, plastic substrates, etc. are preferably used.

[0088] In the present invention, chemical imidization and / or thermal imidization can be carried out by heat treatment. If thermal imidization is used as an example, the maximum heating temperature in the heat treatment is usually above 300°C, preferably above 350°C, more preferably above 450°C, and further preferably above 470°C. The upper limit of the heat treatment temperature is preferably below 600°C, more preferably below 550°C, and further preferably below 520°C, as long as the properties of the polyimide film are not reduced. It should be noted that the heat treatment can also be carried out in an air atmosphere, usually in an inert gas, preferably in a nitrogen atmosphere. Chemical imidization depends on the type of additives such as a chemical imidization catalyst, and milder heat treatment conditions than thermal imidization can be applied. For example, the heat treatment may be performed in a temperature range of usually 100°C or higher, preferably 120°C or higher, more preferably 150°C or higher, further preferably 200°C or higher, and usually 360°C or lower, preferably 300°C or lower, more preferably 250°C or lower, further preferably 220°C or lower.

[0089] The heat treatment of chemical imidization and / or thermal imidization can be carried out in stages. For example, it is preferred to carry out the first heat treatment at a relatively low temperature of 100°C to 170°C for about 0.5 minutes to 30 minutes, followed by a second heat treatment at a temperature of more than 170°C and less than 220°C for about 0.5 minutes to 30 minutes, and then, at a high temperature of more than 220°C and less than 350°C, a third heat treatment is carried out for about 0.5 minutes to 30 minutes, and then a fourth high-temperature heat treatment can be carried out from more than 350°C to the highest heating temperature. The heat treatment is preferably carried out continuously. For example, it is preferred to carry out the heat treatment from a relatively low temperature of 100°C to 170°C to the highest heating temperature. There is no particular restriction on the heating rate, and it is preferably more than 1°C / minute and less than 30°C / minute, and particularly preferably more than 2°C / minute and less than 20°C / minute. If it is in the above range, the foaming caused by the rapid temperature increase can be suppressed, so it is preferred.

[0090] The polyimide film for display substrates of the present invention is obtained using the polyimide precursor for display substrates, and therefore has a long charging half-life, a low charging decay rate after 120 seconds based on the charging half-life measurement, can contribute to the suppression of charging, and can achieve high adhesion.

[0091] Specifically, the charged half-life measured based on the charged half-life according to JIS L 1094A is preferably 48 seconds or more, more preferably 50 seconds or more, and further preferably 52 seconds or more. The charged half-life measured based on the charged half-life is the time from when the polyimide film for display substrate of the present invention is charged by corona discharge to when the polyimide film is charged to half the amount of charge.

[0092] The charging half-life can be measured, for example, as follows: Specifically, the polyimide film for a display substrate of the present invention is charged by corona discharge in accordance with JIS L 1094A, and the charging half-life is measured.

[0093] In addition, the charge decay rate of the polyimide film for display substrate of the present invention after 120 seconds measured based on the charge half-life according to JIS L 1094A is preferably 63% or less, more preferably 61% or less. In addition, the lower limit of the charge decay rate after 120 seconds is preferably 30% or more. The charge decay rate after 120 seconds measured based on the charge half-life is the ratio of the reduction in the charge amount after 120 seconds after the polyimide film for display substrate of the present invention is charged by corona discharge to the charge amount just after being charged. That is, it is calculated by the charge decay rate after 120 seconds (%) = {(charge amount just after being charged - charge amount after 120 seconds) ÷ charge amount just after being charged} × 100.

[0094] The measurement of the charge decay rate after 120 seconds can be performed, for example, as follows. That is, the polyimide film for display substrate of the present invention is charged by corona discharge according to JIS L 1094A, and thus can be performed by measuring the charge amount just after charging and the charge amount after 120 seconds, and in this case, it can be performed simultaneously with the measurement of the charge half-life.

[0095] In addition, in the present invention, from the perspective of more appropriately suppressing charging, it is preferred that when used for display substrates, the charging half-life or the charging decay rate after 120 seconds shows a value close to that of the inorganic material forming the inorganic layer as the gas barrier layer stacked on the polyimide film for display substrates. In particular, SiO is preferably used as the inorganic material forming the inorganic layer. X , SiO X The charge half-life of inorganic materials such as SiO is relatively long, and the charge decay rate after 120 seconds is relatively small. Therefore, as described above, by making the charge half-life longer and the charge decay rate after 120 seconds lower, it is possible to get closer to SiO X The charged half-life of the inorganic material forming the inorganic layer and the charged decay rate after 120 seconds can be obtained by measuring the charged half-life according to JIS L 1094A and the charged decay rate after 120 seconds in the same manner as described above.

[0096] In addition, the 90-degree peel strength of the polyimide film for display substrates of the present invention is preferably 15 mN / mm or more, more preferably 20 mN / mm or more. The 90-degree peel strength can be measured by forming the polyimide film for display substrates of the present invention on the surface of glass and performing a 90-degree peel test on the formed polyimide film.

[0097] <Display Substrate>

[0098] The polyimide film for a display substrate of the present invention is suitable for use in display substrates such as displays and touch panels.

[0099] The display substrate is formed, for example, as follows. That is, first, an inorganic gas barrier layer is formed on the surface of the polyimide film for the display substrate of the present invention by sputtering, vapor deposition, gel-sol method, etc., as a gas barrier layer for water vapor, oxygen, etc. The inorganic gas barrier layer is, for example, made of SiO x Then, a conductive layer of a conductive material (metal or metal oxide, conductive organic matter, conductive carbon, etc.) is formed thereon to form a display substrate. The conductive layer is formed in a predetermined circuit pattern by photolithography, various printing methods, inkjet method, etc. After that, components such as elements and semiconductors for constituting a display may be additionally formed.

[0100] The display substrate of the present invention can be manufactured by the following steps: forming an inorganic gas barrier layer on the surface of a polyimide film obtained using a polyimide precursor for a display substrate of the present invention, forming a conductive layer thereon in a circuit pattern, and then peeling the polyimide film having the inorganic gas barrier layer and the conductive layer formed on the surface from the support. The peeling method is not particularly limited, and can be performed, for example, by laser peeling in which peeling is performed by irradiating a laser from the support side, or by mechanical peeling in which peeling is performed mechanically.

[0101] The display substrate of the present invention thus obtained is formed by forming an inorganic gas barrier layer on the surface of the polyimide film for display substrate obtained using the polyimide precursor for display substrate of the present invention, and forming a conductive layer thereon in the form of a circuit pattern. In addition, the display substrate of the present invention comprises a polyimide film for display substrate obtained using the polyimide precursor for display substrate of the present invention, and the polyimide film for display substrate of the present invention has a long charging half-life, and therefore is effective in eliminating charge accumulation at the interface with the inorganic gas barrier layer, thereby contributing to the suppression of charging.

[0102] Example

[0103] Hereinafter, the present invention will be described in more detail with reference to Examples, Comparative Examples and Reference Examples, but the present invention is not limited to these Examples.

[0104] The measurement methods used in the following examples are shown.

[0105] [Content of acidic groups]

[0106] First, the total amount of acidic groups contained in the polyimide film is calculated by the following formula for each raw material of the acid dianhydride, diamine, tetracarboxylic acid, and end-capping agent. In the case of tetracarboxylic acid, it is assumed that 4 carboxylic acids among the acidic groups in one molecule react with diamine during polymerization and do not remain as acidic groups during film formation. The number of acidic groups when calculating the amount of acidic groups is calculated by subtracting 4 from the number of acidic groups (including anhydride groups) in one molecule of tetracarboxylic acid.

[0107] Acidic group amount contained in raw material (mol) = Amount of raw material (mol) × (Number of acidic groups in one molecule of raw material)

[0108] Next, the total molar number of the acid dianhydride, diamine, tetracarboxylic acid, and end-capping agent excluding the catalyst was taken as the total amount (mol) of monomers added, and the content of acidic groups (-COOH group, -SO3H group) contained in the polyimide film was calculated by the following formula.

[0109] Content of acidic groups in the film = Total amount of acidic groups in the raw materials (mol) / Total amount of monomers added (mol)

[0110] [Charge half-life based on charge half-life measurement, charge decay rate after 120 seconds]

[0111] The polyimide film was cut into 55 mm in length and width to prepare a test piece. The test piece was subjected to a charge half-life measurement in a corona charging mode using a Static Honestmeter manufactured by Shishido Electrostatic Ltd. under the conditions of 23±2°C, 50% RH, applied voltage: -10 kV, applied time: 30 s, and maximum measurement time: 120 s in accordance with JIS L1094A. The charge half-life and charge decay rate after 120 seconds were measured.

[0112] [90 degree peel strength]

[0113] The 90-degree peel strength is measured according to the following method. A glass plate formed with a polyimide film is cut into a width of 25 mm to make a test piece. With respect to the test piece, after the head is exposed for fixing the test piece, the test piece is fixed to the Tensilon RTF-1350 peel test measuring fixture, and a tensile tester is used to peel more than 50 mm at a speed of 50 mm / min, and the load therebetween is measured. The value obtained by dividing the peel load by the peel width (mm) of the test piece is obtained as the 90-degree peel strength.

[0114] The abbreviations of the compounds used in the following examples are as follows.

[0115] s-BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride

[0116] PPD: p-phenylenediamine

[0117] 3,5-DABA: 3,5-diaminobenzoic acid

[0118] MPD: Metaphenylenediamine

[0119] HAB: 3,3'-dihydroxybenzidine

[0120] DATP: 4,4"-diaminoterphenyl

[0121] [Example 1]

[0122] Into a reaction container equipped with a stirrer and a nitrogen inlet tube, 34.4734 g of NMP (N-methylpyrrolidone), 1.4340 g of PPD, and 0.0842 g of 3,5-DABA were added, and stirred at 50° C. for 30 minutes under a nitrogen atmosphere, and then 3.9820 g of s-BPDA was added and reacted to obtain a polyimide precursor solution (polyamic acid solution). At this time, s-BPDA:PPD:3,5-DABA (molar ratio) = 100:96:4.

[0123] Next, the polyamic acid solution prepared in the synthesis example was spin-coated on an alkali-free glass wafer, and heated at 120°C, 150°C, 200°C, and 250°C for 10 minutes each, and at 450°C for 5 minutes to remove the solvent and imidize the film, thereby obtaining a polyimide film having a thickness of 10 μm. The evaluation results are shown in Table 1.

[0124] [Example 2]

[0125] A polyimide precursor solution was obtained in the same manner as in Example 1 except that the amount of the diamine component and the tetracarboxylic acid component used was s-BPDA:trimellitic anhydride:PPD (molar ratio) = 98:4:100, and then the solvent was removed, imidization was performed, etc., to obtain a polyimide film. The evaluation results are shown in Table 1.

[0126] [Example 3]

[0127] A polyimide precursor solution was obtained in the same manner as in Example 1 except that the amounts of the diamine component and the tetracarboxylic acid component used were s-BPDA:mellitable acid:PPD (molar ratio) = 98:2:100, and then the solvent was removed, imidization was performed, etc., to obtain a polyimide film. The evaluation results are shown in Table 1.

[0128] It should be noted that, regarding the mellitic acid used in Example 3, the acidic groups that finally remained in the film were assumed to be two carboxylic acids obtained by removing four carboxylic acids of the tetracarboxylic acid component from six carboxylic acids as the number of acidic groups of mellitic acid, and when calculating the content of the acidic groups (the number of acidic groups per 1 molecule of the raw material), it was calculated to be 2.

[0129] [Example 4]

[0130] A polyimide precursor solution was obtained in the same manner as in Example 1 except that the amount of the diamine component and the tetracarboxylic acid component used was s-BPDA:PPD:1,4-phenylenediamine-2-sulfonic acid (molar ratio) = 100:96:4, and then the solvent was removed, imidization was performed, etc., to obtain a polyimide film. The evaluation results are shown in Table 1.

[0131] [Comparative Example 1]

[0132] A polyimide precursor solution was obtained in the same manner as in Example 1 except that the used amounts of the diamine component and the tetracarboxylic acid component were s-BPDA:PPD=100:100, and then the solvent was removed, imidization was performed, and a polyimide film was obtained.

[0133] [Comparative Example 2]

[0134] A polyimide precursor solution was obtained in the same manner as in Example 1 except that the usage amounts of the diamine component and the tetracarboxylic acid component were s-BPDA:PPD:MPD=100:96:4, and then the solvent was removed, imidization was performed, etc., to obtain a polyimide film.

[0135] [Comparative Example 3]

[0136] A polyimide precursor solution was obtained in the same manner as in Example 1 except that the usage amounts of the diamine component and the tetracarboxylic acid component were s-BPDA:PPD:HAB=100:96:4, and then the solvent was removed, imidization was performed, etc., to obtain a polyimide film.

[0137] [Comparative Example 4]

[0138] A polyimide precursor solution was obtained in the same manner as in Example 1 except that the used amounts of the diamine component and the tetracarboxylic acid component were s-BPDA:DATP=100:100, and then the solvent was removed, imidization was performed, etc., to obtain a polyimide film.

[0139]

[0140] As shown in Table 1, by making the polyimide precursor contain an acidic group at a predetermined ratio, a polyimide film having a charge half-life of 48 seconds or more and a charge decay rate of 63% or less after 120 seconds can be obtained. Since the polyimide film obtained in this way has a long charge half-life and a low charge decay rate after 120 seconds, it can contribute to the suppression of charging by being used as a polyimide film for a display substrate (Examples 1 to 4). In addition, regarding the 90° peel strength, the peel strength in Example 1 was 25 mN / mm, which was higher than the peel strength in Comparative Example 1, i.e., 13 mN / mm. It was confirmed that in Example 2, the more difficult the peeling operation of the film set in the jig for peel strength measurement was, the higher the adhesion was.

[0141] Industrial Applicability

[0142] The polyimide precursor for a display substrate of the present invention is suitably used for a display substrate.

Claims

1. A polyimide precursor for a display substrate, which is a polyimide precursor for a display substrate having a structural unit represented by the following general formula (1), wherein: As X in the general formula (1) 1 The group shown, Y in the general formula (1) 1 At least a part of the groups shown in the formula (a) and the terminal groups includes a group containing an acidic group, The acid group content is 15×10 -3 above, [Chemistry 6] In the general formula (1), X 1 is a tetravalent aromatic group or aliphatic group, Y 1 is a divalent aromatic group, R 1 , R 2 Each is independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkylsilyl group having 3 to 9 carbon atoms.

2. The polyimide precursor for a display substrate according to claim 1, wherein The group containing an acidic group is at least one selected from a group containing a carboxyl group and a group containing a sulfonic acid group.

3. The polyimide precursor for a display substrate according to claim 2, wherein The carboxyl group-containing group is a group derived from at least one selected from 3,5-diaminobenzoic acid, 5,5′-methylenebis(2-aminobenzoic acid), mellitic acid and mellitic anhydride, and trimellitic anhydride.

4. The polyimide precursor for a display substrate according to claim 3, wherein The carboxyl group-containing group is a group derived from at least one selected from 3,5-diaminobenzoic acid, mellitic acid and mellitic anhydride, and trimellitic anhydride.

5. The polyimide precursor for a display substrate according to claim 2, wherein The group containing a sulfonic acid group is a group derived from at least one selected from 1,4-phenylenediamine-2-sulfonic acid, 1,3-phenylenediamine-4-sulfonic acid, 3,5-diamino-2,4,6-trimethylbenzenesulfonic acid, and 4,4′-diaminostilbene-2,2′-disulfonic acid.

6. The polyimide precursor for a display substrate according to claim 5, wherein The group containing a sulfonic acid group is a group derived from at least one selected from 1,4-phenylenediamine-2-sulfonic acid and 1,3-phenylenediamine-4-sulfonic acid. 7 . A polyimide film for a display substrate, obtained by using the polyimide precursor for a display substrate according to claim 1 . 8 . A display substrate comprising the polyimide film for a display substrate according to claim 7 .