Catalysts and methods for depolymerizing polymer waste material

By using acidic compounds and catalysts deposited by coating agents for pyrolysis in polymer waste materials, the problem of heating control in the chemical recycling of polymer waste materials is solved, efficient depolymerization and the generation of low-carbon purity products are achieved, and the cost is reduced Energy consumption and CO2 emissions.

CN118786172APending Publication Date: 2024-10-15BASELL POLIOLEFINE ITALIA SRL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380024344.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-30
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the existing chemical recycling process of polymer waste materials, the mixing of different types of polymers makes heating control difficult, resulting in high energy costs and poor product quality, and it is difficult for existing technologies to effectively depolymerize multiple polymer waste materials.

Method used

Acidic compounds are used as active components and are deposited on a granular non-porous carrier with the help of a coating agent to form a catalyst, which is used for pyrolysis with polymer waste materials to generate high-content gaseous fractions and low-carbon purity depolymerization products.

Benefits of technology

Efficient depolymerization of polymer waste materials is achieved to generate depolymerization products with high gaseous content and low carbon purity, and the catalyst can be used multiple times, reducing energy consumption and CO2 emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005017159370000171
    Figure BDA0005017159370000171
  • Figure BDA0005017159370000211
    Figure BDA0005017159370000211
  • Figure BDA0005017159370000231
    Figure BDA0005017159370000231
Patent Text Reader

Abstract

A catalyst for depolymerizing a polymer waste material comprising an acidic component deposited on a solid support by means of a coating agent, and a method of depolymerizing a polymer waste material using the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] not applicable. Technical Field

[0003] The present disclosure relates to depolymerization of polymer waste materials. More specifically, the present disclosure relates to a catalyst for depolymerization of polymer waste materials, the catalyst comprising an acidic component deposited on a solid support by means of a coating agent, and to a catalytic method for depolymerizing polymer waste materials using the catalyst. Background Art

[0004] Plastics include a wide range of synthetic and semi-synthetic materials that use polymers as their main components. Their plasticity allows plastics to be molded, extruded or pressed into solid objects of various shapes. This adaptability, combined with a wide range of other properties (such as light weight, durability and low production cost), has led to their widespread use. The production of plastics has increased dramatically over the past few decades. At the same time, the increase in the amount of plastics causes environmental problems because most plastics are resistant to natural degradation processes. As a result, the material can last for centuries or more, filling landfills and even appearing in the food chain as microplastics.

[0005] Therefore, increasing efforts are being made to improve the recycling of polymer waste materials. Current recycling procedures rely mainly on mechanical recycling and chemical recycling. For mechanical recycling, plastics are mechanically transformed without changing their chemical structure so that they can be used to produce new materials. Typical mechanical recycling steps include collecting polymer waste materials, sorting polymer waste materials into different types of plastics and colors, packaging plastic waste materials by pressing or grinding, washing and drying polymer waste materials, and reprocessing polymer waste materials into pellets by agglomerating, extruding and cooling the plastics to obtain recycled raw materials, which can then be formed into new articles.

[0006] During chemical recycling, plastics are reprocessed and their structure and chemical properties are modified so that they can be used as raw materials for different industries or as basic input or feedstock for manufacturing new polymer products. Chemical recycling generally involves the following steps: collecting plastic waste materials and then heating the plastic waste materials to break down the polymers to obtain monomers which are then used to remake polymers or used to produce other synthetic chemicals.

[0007] In practice, different types of polymer waste materials are often collected together, which makes chemical recycling particularly troublesome because the mixture of different polymers makes it difficult to control the heating process, resulting in high energy costs and poor yield and quality of the resulting products.

[0008] In this regard, considerable efforts have been made to improve the depolymerization process of polymers.

[0009] The beginning of chemical recycling of polymer waste materials can be traced back to the 1970s. US 3,984,288 describes a method for treating rubber and plastic wastes, which comprises the following series of steps: (i) heating and melting rubber and plastic wastes at a temperature T1 in an extruder to knead and melt the wastes, and extruding the molten wastes in a molten state into a decomposition zone, (ii) heating the molten wastes in the decomposition zone at a temperature T2 in the extruder to form decomposition products and conveying the decomposition products to a retorting zone, (iii) heating the decomposition products in the retorting zone at a temperature lower than the heating temperature T2 in the decomposition zone to gasify the products by retorting, and (iv) conveying the retorting products to a cooling zone to cool the retorting products to separate liquid materials from gaseous materials.

[0010] DE 198 22 568 relates to a process for utilizing plastic polymers, in which the plastic polymers are brought into contact with a catalyst at elevated temperature and the reaction products resulting from the gas phase obtained are at least partially condensed.

[0011] US2021 / 0054161 provides a technology involving polymer depolymerization, particularly methods and systems for de-crosslinking polyacrylic acid salt-based polymers and other polymers, and compositions made from de-crosslinked polyacrylic acid salt-based polymers and other polymers to produce polyacrylic acid (PAA) from superabsorbent polymers (SAP) by ultrasonic treatment of aqueous SAP hydrogels.

[0012] WO 2021 / 048185 introduces a method for depolymerizing plastics, which comprises the following steps: a) introducing a raw material containing plastics; b) mixing the raw material containing plastics with a catalyst to obtain a reactant mixture; and c) heating the reaction mixture to obtain a product, wherein the catalyst is halloysite.

[0013] WO 2020 / 061521 relates to a method for depolymerizing plastics, which comprises a) mixing solid plastic particles with a solvent to produce a heterogeneous reaction mixture, b) conveying the heterogeneous reaction mixture through a first section of a first heat exchanger to preheat the heterogeneous reaction mixture, c) conveying the preheated heterogeneous reaction mixture to a heating zone of a heating chamber; d) heating the heterogeneous mixture in the heating zone of the heating chamber to a reaction temperature sufficient to initiate conversion of the heterogeneous reaction mixture into a homogeneous reaction solution comprising a liquefied reaction product, e) conveying the homogeneous reaction solution through a second section of the first heat exchanger to cool the homogeneous reaction solution, and f) conveying the homogeneous reaction solution to a settling tank to allow the liquefied reaction product to be converted into a solid reaction product and precipitate from the cooled homogeneous reaction solution.

[0014] In view of the above and the growing demand for polymers, there remains a need for efficient recycling of polymer waste materials. The present disclosure addresses this need by providing a catalyst for depolymerizing polymer waste materials and a method for recycling polymer waste materials by depolymerization using the catalyst. Summary of the invention

[0015] In one aspect, the present disclosure provides a catalyst for depolymerizing polymer waste materials, the catalyst comprising an acidic compound as an active component, the acidic compound being deposited on a particulate non-porous support with the aid of a coating agent.

[0016] In one embodiment, the particulate non-porous support is selected from the group consisting of sand, glass beads and metal particles.

[0017] In one embodiment, the acidic compound is selected from the group consisting of Al / Si mixed oxides, Al2O3, aluminosilicates, silica and zeolites.

[0018] In one embodiment, the coating agent is selected from oil, inorganic hydrogel or a combination thereof.

[0019] In one embodiment, the active compound is contained in the catalyst in an amount of 0.5 to 6.0 wt%, preferably 1.0 to 4.0 wt%, based on the total weight of the catalyst.

[0020] In another aspect, the present disclosure provides a method for depolymerizing polymer waste materials, the method comprising the steps of: (a) providing a feedstock of polymer waste materials; (b) mixing the feedstock with a catalyst of the present disclosure; (c) pyrolyzing the mixture; (d) collecting a gaseous fraction produced during the pyrolysis; and (e) separating the collected gaseous fraction to obtain gaseous and liquid depolymerization products.

[0021] In one embodiment, the process further comprises the step of distilling the liquid depolymerization product.

[0022] In one embodiment, the polymer waste material is a polymer waste material consisting of or comprising a plastic material, wherein the plastic material is selected from the group consisting of polyethylene (PE), polypropylene (PP), polystyrene (PS), polyethylene terephthalate (PET), polyvinyl chloride (PVC), polyamide (PA), polyurethane (PU), polyacrylonitrile (PAN) and polybutylene (PB) and mixtures thereof or consists thereof.

[0023] In one embodiment, the gas content in the depolymerization product after step (e) is preferably greater than 30 wt%, more preferably greater than 50 wt%, especially greater than 70 wt%, based on the combined weight of gas and depolymerization product and liquid depolymerization product.

[0024] In one embodiment, based on the total weight of the gaseous depolymerization product after step (e) of the process of the present disclosure, the gaseous depolymerization product of the general formula C n H 2n The content of the compound is at least 50 wt%, preferably at least 60 wt%, in particular at least 65 wt%, wherein n=2-4.

[0025] In one embodiment, the liquid depolymerization product obtained has an olefinic compound content expressed as a bromine number (g bromine / 100 g sample) of less than 150, preferably from 10 to 100, more preferably from 15 to 80, even more preferably from 20 to 70, in particular from 25 to 100, determined according to ASTM D1159-01, and / or the 1H-NMR spectrum of the liquid depolymerization product obtained shows less than 10 mol %, preferably less than 5 mol %, in particular not more than 3 mol % of olefinic protons.

[0026] In one embodiment, the content of aromatic compounds in the obtained liquid depolymerization product is less than 10 mol%, preferably less than 5 mol%, in particular not more than 3 mol%, the content of aromatic components being measured as the content of aromatic protons in mol% determined by 1H-NMR spectroscopy.

[0027] In a preferred aspect, the polymer waste material feedstock for depolymerization is characterized by: (a) a polyolefin content, in particular a total content of polypropylene (PP) and polyethylene (PE) of more than 50 wt%, preferably more than 60 wt%, more preferably more than 70 wt%, in particular more than 80 wt%, in particular more than 90 wt%, based on the total weight of the polymer waste material feedstock; (b) a total ash content of less than 15 wt%, preferably less than 10 wt%, more preferably less than 5 wt%, most preferably less than 3 wt%, the total ash content being determined as the residue after heating the polymer waste material feedstock at 800° C. in air for 120 hours; (c) a bulk density of 70 g / l to 500 g / l, preferably 100 g / l to 450 g / l, for the polymer waste material feedstock in comminuted form, or of 300 g / l to 700 g / l for the polymer waste material feedstock in granular form, the bulk densities being respectively determined according to DIN EN 6001-2:2003. 53466 determined; and (d) a total volatile content (TV) of less than 5%, preferably less than 3%, measured as the weight loss of a 10 g sample at 100° C. at 200 mbar for 2 hours. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Hereinafter, certain embodiments of the present disclosure will be described with reference to the accompanying drawings, wherein the same reference numerals represent the same elements. However, it should be understood that the accompanying drawings illustrate various embodiments described herein and are not intended to limit the scope of the various technologies described herein.

[0029] Figure 1 is a flowchart depicting a general process according to an embodiment of the present disclosure; and

[0030] Figure 2 is a flowchart illustrating an operation example according to an embodiment of the present disclosure. DETAILED DESCRIPTION

[0031] The disclosure herein generally relates to catalysts and methods for depolymerization of plastic waste materials.

[0032] Depolymerization catalyst

[0033] In one aspect, the present disclosure provides a catalyst for depolymerizing polymer waste materials, the catalyst comprising an acidic compound as an active component, the acidic compound being deposited on a particulate non-porous support with the aid of a coating agent.

[0034] Surprisingly it was found that the catalyst of the present disclosure allows the production of high purity depolymerization products with high content of gaseous fractions and low char production. Furthermore, it was found that the catalyst of the present disclosure can be easily separated from any solid residues of the depolymerization process, thus allowing multiple uses.

[0035] Without wishing to be bound by theory, the above performance may be due to the fact that the catalyst effectively supports the transfer of heat generated during the pyrolysis of the polymer waste material.

[0036] In order to facilitate the effective pyrolysis and depolymerization of polymer waste materials, the catalyst of the present disclosure is in granular form. Preferably, a granular non-porous support is selected from sand, glass beads and metal particles. The granular non-porous support can have any shape, such as spherical, cylindrical or any non-uniform shape. In addition to being granular, the support used in the catalyst of the present invention is also non-porous. Within the meaning of the present disclosure, non-porous should be understood as impermeable to gases (such as air) or liquids (such as water). In order to make the catalyst of the present disclosure specifically designed to be mixed with polymer waste materials undergoing depolymerization, the support preferably has an average particle size D50 of 0.2 mm to 20 mm, preferably 0.5 mm to 10 mm, more preferably 1 mm to 8 mm, most preferably 1 mm to 6 mm determined according to sieve analysis according to ISO3310-1 / ASTM E11. With a wire mesh screen The Retsch test sieve apparatus is an example of a useful sieving device.

[0037] Sand is a preferred type of non-porous particulate carrier and preferably has the following particle size distribution:

[0038] Minimum maximum <3000μm 70% 90% >1400μm 40% 80% >1000μm 50% 80% <1000μm 0% 20%

[0039] The acidic compound of the catalyst of the present disclosure is preferably selected from the group consisting of: Al / Si mixed oxide, Al2O3, aluminosilicate, silica and zeolite. The Al / Si mixed oxide particularly preferred in the present disclosure refers to a material having a neutral structure containing a mixture of Al2O3 and SiO2.

[0040] Zeolites as referred to in this disclosure are understood to be crystalline microporous aluminosilicates consisting of zeolites having the general structure M n +x / n[AlO2]-x(SiO2) y ]+zH2O corner-sharing SiO4- and AlO4- tetrahedra, wherein n is the charge of the cation M, which is usually an alkali metal or alkaline earth metal or a hydrogen ion, preferably selected from H + 、Na + , Ca2 + , K + and Mg2 + ions, and z defines the number of water molecules incorporated into the crystal structure. Zeolites differ from mixed Al / Si oxides in that they define pore structures and ionic properties. In a particularly preferred embodiment, the zeolite used as an acidic compound is selected from zeolite Y, zeolite β, zeolite A, zeolite X, zeolite L and mixtures thereof, particularly zeolite Y and zeolite β. The zeolites listed are well known and commercially available. Particularly preferred are zeolites in which the metal ion M is replaced by hydrogen. Other specific examples of suitable zeolite-type components for the present disclosure include, but are not limited to, ZSM-5, ZSM-11, ZSM-22, ZSM-23, ZSM-35, ZSM-48, ZSM-50, TS-1, TS-2, SSZ-46, MCM-22, MCM-49, FU-9, PSH-3, ITQ-1, EU-1, NU-10, silicalite-1, silicalite-2, boronite-C, boronite-D, BCA and mixtures thereof.

[0041] In a particularly preferred embodiment, the acidic compound is an Al / Si mixed oxide. The composition of the Al / Si mixed oxide used as a carrier can be adjusted as required. However, the result of depolymerization is particularly good when the acidic compound contains a specific amount of Al O and SiO. Therefore, in a preferred embodiment, the Al O contained in the acidic compound in an amount of 20-99wt%, preferably 30-80wt%, especially 40-70wt%, based on the gross weight of the acidic compound. In addition, the acidic compound preferably contains 1-80wt%, preferably 20-70wt%, especially 30-60wt% SiO based on the gross weight of the acidic compound.

[0042] Surprisingly, it has been found that the result of the depolymerization process can be improved even further if the acidic compound contains an excess of Al2O3 relative to SiO2. Therefore, in a preferred embodiment, the acidic compound comprises an excess of Al2O3 relative to SiO2. Further preferred are embodiments in which the weight ratio of Al2O3 to SiO2 in the acidic compound is from 99:1 to 30:70, preferably from 9:1 to 3:2, in particular from 4:1 to 3:2.

[0043] The SiO2 and Al2O3 contents of the acidic compound can be determined by atomic emission spectrometry using inductively coupled plasma (ICP-AES).

[0044] The coating agent used in the catalyst of the present disclosure is preferably selected from oil, inorganic hydrogel or a combination thereof. As inorganic hydrogel, silica hydrogel is preferred. As for the oil used as coating agent, aromatic-free white mineral oil, preferably based on isoparaffin, is preferred. In a preferred embodiment, the kinematic viscosity of the oil used at 20° C. is 140-180 mm 2 / s, preferably 150-170mm 2 / s, and / or a kinematic viscosity of 40-80 mm at 40°C 2 / s, preferably 50-70mm 2 / s, and / or a kinematic viscosity of 5-15 mm at 100°C 2 / s, preferably 7-10mm 2 / s. The kinematic viscosity can be determined according to ISO 3104.

[0045] The preferred amount of coating agent is 1-300%, preferably 2-150 wt%, more preferably 5-100 wt%, most preferably 10-80 wt%, based on the amount of acidic compound.For hydrogels, the amount to be employed refers to dry weight.

[0046] In another preferred embodiment, the active compound is included in the catalyst of the present disclosure in an amount of 0.5 to 6 wt %, preferably 2 to 4 wt %, based on the total weight of the catalyst.

[0047] The catalyst of the present disclosure is preferably obtained by mixing a granular non-porous support and a coating agent, and then adding an acidic compound in powder form to the resulting mixture. The mixture may optionally be heat treated to obtain the catalyst. The heat treatment may be carried out, for example, at a temperature of 100 to 600° C. In a preferred embodiment, the granular non-porous support undergoes a drying step before mixing with the coating agent.

[0048] In a preferred embodiment, the present disclosure therefore relates to a catalyst obtained by a process comprising the steps of: (a) mixing a particulate non-porous support and a coating agent; and (b) adding an acidic compound in powder form to the mixture of step (a).

[0049] In a particularly preferred embodiment, the catalyst features the following: (a) sand as a granular nonporous support; (b) an Al / Si mixed oxide or a zeolite as an acidic compound; and (c) mineral oil or a silica hydrogel as a coating agent.

[0050] The catalyst of the present disclosure and preferably those catalysts in which component (c) is selected from hydrogel can surprisingly be reactivated by heating, thereby allowing multiple uses and saving resources. In a preferred embodiment, the catalyst can therefore be reactivated by heat treatment. The heat treatment is preferably carried out at a temperature of 500-900°C, particularly 550-900°C, most preferably 600-850°C. In some embodiments of the present disclosure, the heat treatment preferably occurs in an oxidizing atmosphere such as air or oxygen. The treatment time can be selected by experimental studies to find the best balance between catalyst activity and energy consumption. In this regard, the concentration of carbon residues on the catalyst is a parameter to be considered. Preferably, the carbon residue of the regenerated catalyst is less than 20wt% of the catalyst, preferably less than 15wt%, more preferably less than 10wt%, and most preferably less than 5wt%. Without excluding other treatment times, a treatment time of 0.5 to 100 hours, preferably 1 to 20 hours, more preferably 2 to 10 hours is possible.

[0051] Depolymerization

[0052] On the other hand, the present disclosure provides a method for depolymerizing plastic waste materials, the method comprising the steps of: (a) providing a raw material of plastic waste materials; (b) mixing the raw material with a catalyst of the present disclosure; (c) pyrolyzing the mixture; (d) collecting gaseous fractions produced during pyrolysis; and (e) separating the collected gaseous fractions to obtain gaseous and liquid depolymerization products.

[0053] As already explained, the used catalyst is preferably separated from any solid content remaining after the depolymerization process and reintroduced into the process.

[0054] The collected gaseous fraction can be separated into liquid and gaseous depolymerization products by condensation. Thus, the liquid depolymerization product and the gaseous depolymerization product can be further processed.

[0055] The process of the present disclosure may produce little to no char. Thus, in a preferred embodiment, the residue of the depolymerization process of the present disclosure has a char content of less than 5 wt%, preferably less than 2 wt%, based on the total weight of the product.

[0056] The obtained liquid depolymerization product may be further separated. Therefore, the method of the present disclosure may further include a step of distilling the liquid depolymerization product.

[0057] Surprisingly, it has been found that the process of the present disclosure can produce a depolymerization product having a high gas content. In a preferred embodiment, the gas content in the depolymerization product after step (e) is preferably greater than 30 wt%, more preferably greater than 50 wt%, and especially greater than 70 wt%, based on the combined weight of the gas and the depolymerization product and the liquid depolymerization product.

[0058] The gaseous fraction of depolymerization product is also characterized by the high content of monomer olefinic C2-C4 compound, and described monomer olefinic C2-C4 compound is particularly useful for further processing, for example, for the production of polymkeric substance.Owing to produce a large amount of this compound in depolymerization process, gaseous depolymerization product can be directly used as the raw material in cracking method and subsequent polymerization.The gaseous product comprising light olefins and light alkanes can for example be transferred to downstream cracker to produce polymerization grade monomer stream by baking oven.Other by-products such as ethane, propane and butanes will be cracked in baking oven.Therefore can bypass the product obtained after the processing depolymerization that usually needs to obtain the step of required monomer, saved valuable energy and reduced CO2 output.

[0059] Polymer waste materials raw materials

[0060] It is found that the method of the present disclosure is suitable for recycling various polymer waste materials, particularly plastic waste materials. The polymer waste material raw materials used in the method of the present disclosure can include substantially all polymer materials, particularly those materials formed by synthetic polymers. Non-limiting examples include polyolefins, such as polyethylene, polypropylene, etc., polystyrene, polyethylene terephthalate (PET), polyvinyl chloride (PVC), polyamide, polycarbonate, polyurethane, polyester, natural and synthetic rubber, tires, filled polymers, composite materials and plastic alloys, plastics dissolved in solvents, etc. In the process of developing the method of the present disclosure, it is surprisingly found that other hydrocarbon materials can also be used as polymer waste material raw materials. These hydrocarbons can include biomass, bio-oil, petroleum, etc. Therefore, although this specification mainly relates to the depolymerization of polymer raw materials, it should be understood that the method of the present disclosure is also applicable to and covers the use of other hydrocarbons. When it is necessary to produce light gas olefins, it can be preferred that the plastic raw materials mainly composed of polyolefins or containing a considerable portion of polyolefins. Mixtures of various different plastics and hydrocarbon materials can be used without restriction.

[0061] The polymer waste material feedstock may consist of one type of polymer waste material, or may be a mixture of two or more different polymer waste materials. The polymer waste material feedstock may be provided in a variety of different forms. In smaller scale operations, the polymer waste material feedstock may be in powder form. In larger scale operations, the polymer waste material feedstock may be in the form of particles, such as particles having a particle size of 1 to 20 mm, preferably 2 to 10 mm, more preferably 2 to 8 mm, or in the form of chopped flakes and / or small pieces of film, preferably with a particle size of 1 to 20 mm. In the context of the present disclosure, having a particle size within a defined range means that 90 wt % of the particles have a particle size within a defined range. The particle size may be determined by sieving or by using a Beckman Coulters LS13320 laser diffraction particle size analyzer.

[0062] The polymer waste material consists mainly of plastic materials and is usually named after the type of polymer that forms the major component of the polymer waste material. Preferably, the polymer waste material used as a feedstock in the process of the present disclosure contains more than 25 wt%, preferably more than 40 wt% and more preferably more than 50 wt% of polymer material based on its total weight. Other components in the polymer waste material feedstock may be, for example, additives such as fillers, reinforcing materials, processing aids, plasticizers, pigments, light stabilizers, lubricants, impact modifiers, antistatic agents, inks, antioxidants, etc.

[0063] The polymer waste material used in the method of the present disclosure preferably comprises polyolefins and polystyrenes, such as high density polyethylene (HDPE), linear low density polyethylene (LLDPE), low density polyethylene (LDPE), ethylene-propylene-diene monomer (EPDM), polypropylene (PP) and polystyrene (PS). Particularly preferred is a polymer waste material comprising a mixture of polyolefins and polystyrenes.

[0064] Other polymer waste materials, such as polyvinyl chloride, polyvinylidene chloride, polyethylene terephthalate, polyurethane (PU), acrylonitrile-butadiene-styrene (ABS), nylon and fluorinated polymers can also be used in the process of the present disclosure. If present in the polymer waste material, these polymers are preferably present in an amount of less than 50 wt%, preferably less than 30 wt%, more preferably less than 20 wt%, and even more preferably less than 10 wt% of the total weight of the polymer waste material feedstock dry weight.

[0065] Preferably, the polymer waste material comprises one or more thermoplastic polymers and is substantially free of thermosetting polymers. In this regard, substantially free is intended to mean that the content of thermosetting polymers is less than 15 wt %, preferably less than 10 wt %, even more preferably less than 5 wt % of the polymer waste material feedstock.

[0066] The polymer waste material used in the process of the present disclosure is preferably selected from the group consisting of: single plastic waste, qualified or unqualified single virgin plastic, mixed plastic waste, rubber waste, cracker residue, used oil, biomass or mixtures thereof. Single plastic waste, unqualified single virgin plastic, mixed plastic waste, rubber waste or mixtures thereof are preferred. Unqualified single virgin plastic, mixed plastic waste or mixtures thereof are particularly preferred.

[0067] The polymer waste material may also contain limited amounts of non-pyrolyzable components, such as water, glass, stone, metals, etc. as contaminants. "Limited amounts" preferably refers to an amount less than 50 wt%, preferably less than 20 wt%, more preferably less than 10 wt% of the total weight of the dry polymer waste material feedstock.

[0068] The polymer waste material may optionally be extruded prior to use as a feedstock in the process of the present disclosure. In a preferred embodiment, the polymer waste material is pelletized and the pellets are used as a feedstock in the process of the present disclosure. In other preferred embodiments, the polymer waste material is used in a molten state, for example at a temperature of 200° C. to 300° C.

[0069] Particularly preferred types of polymer waste materials for use as feedstock in the process of the present disclosure are characterized by the following features:

[0070] i) a total volatile content (IV) of less than 5%, preferably less than 3%, more preferably less than 2%, in particular less than 1%, measured as the weight loss of a 10 g sample after 2 hours at 100° C. and a pressure of 200 mbar;

[0071] ii) the polymer waste material is shredded and optionally compacted polymer waste having a bulk density of 70 g / l to 500 g / l, preferably 100 g / l to 450 g / l, or the polymer waste material is in granular form and has a bulk density of 300 g / l to 700 g / l, the bulk density being determined according to DIN 53466;

[0072] iii) the content of polyolefins, in particular polypropylene (PP) and / or polyethylene (PE), in the polymer waste material is greater than 50 wt%, preferably greater than 60 wt%, more preferably greater than 70 wt%, in particular greater than 80 wt%, in particular greater than 90 wt%, based on the total weight of the polymer waste material feedstock;

[0073] iv) the amount of polar polymer contaminants in the polymer waste material is less than 10 wt%, preferably less than 5 wt%, more preferably less than 3 wt%, based on the total weight of the polymer waste material;

[0074] v) the amount of cellulose, wood and / or paper in the polymer waste material is less than 10 wt%, preferably less than 5 wt%, and more preferably less than 3%, based on the total weight of the polymer waste material;

[0075] vi) a total chlorine content of less than 1.0 wt%, preferably less than 0.5 wt%, more preferably less than 0.1 wt%, based on the total weight of the polymer waste material;

[0076] vii) the total ash content of the polymer waste material feedstock is less than 15 wt%, preferably less than 10 wt%, more preferably less than 5 wt%, and most preferably less than 3 wt%, as determined as the residue after heating the polymer waste material at 800°C in air for 120 hours. In other preferred embodiments, the ash content is 0.01-2 wt%, preferably 0.02-1.5 wt%, more preferably 0.05-1.0 wt%.

[0077] In a preferred embodiment of the present disclosure, the polymer waste material used as a feedstock in the process of the present disclosure is limited by an upper limit of the secondary components, ingredients or impurities expressed as a weight percentage. The lower limit of the amount of these components, ingredients or impurities in the preferred polymer waste material is preferably below the detection limit, or the lower limit is 0.001 wt% or 0.01 wt% or 0.1 wt%, respectively.

[0078] A variety of techniques are known for separating materials in polymer waste material streams. Moving beds, drums and screens, and air separators are used to differentiate materials by size, weight, and density. Advanced sorting of plastic waste by spectroscopic techniques (MIR, NIR [near infrared]), X-ray, or fluorescence spectroscopy provides a high quality plastic waste stream with a high polyolefin content.

[0079] Automatic separation technologies for waste plastics include dry sorting technology, electrostatic sorting technology, mechanical sorting methods (involving centrifugal force, specific gravity, elasticity, particle shape, selective cutting and mechanical properties), as well as wet sorting technology (such as sink-float sorting method) and chemical sorting methods.

[0080] Suitable feedstocks for use in the methods of the present disclosure may be obtained by applying any known sorting techniques, for example as summarized in B. Ruj et al.: Sorting of plastic waste for effective recycling, Int. J. Appl. Sci. Eng. Res 4, 2015, 564-571.

[0081] Reactor

[0082] The depolymerization process according to the present disclosure can be carried out in a reactor comprising: (a) a feeding device for introducing polymer waste materials and a catalyst into the reactor; (b) a pyrolysis device equipped with a heating unit, a gas discharge unit and a solid discharge unit; and (c) a condensing device.

[0083] Preferably, the gas discharge unit is distributed throughout the pyrolysis device and is provided with an outlet for discharging the depolymerized gaseous fraction and an inlet for introducing clean gas into the pyrolysis device.

[0084] In a preferred embodiment, the reactor may comprise more than one pyrolysis unit.

[0085] The polymer waste feedstock and catalyst are introduced into the pyrolysis unit through at least one feeding device and then heated to achieve depolymerization. The gaseous fraction produced during the depolymerization process is discharged through the outlet of the gas discharge unit and transported to the condensation unit for further treatment. Any solid residues of the depolymerization are discharged via the solid discharge unit. Clean gas for cleaning the gas discharge unit and the pyrolysis unit can be introduced through the inlet of the gas discharge unit.

[0086] In a preferred embodiment, the gas discharge unit is equipped with a filter membrane to avoid the presence of solids in the gaseous fraction after discharge from the pyrolysis device.The gas discharge unit is preferably made of metallic or ceramic granular or fibrous material.

[0087] The pyrolysis device is preferably also equipped with a screw for uniform mixing of the polymer waste material in the pyrolysis device throughout the depolymerization process. The residence time of the solids in the pyrolysis device can be well defined by adjusting the rotation speed of the screw. The pyrolysis device is preferably operated at a temperature of 350 to 550°C.

[0088] The depolymerized gaseous fraction is transported to a condensation device to obtain liquid and gaseous depolymerization products. In a preferred embodiment, the condensation device comprises several condensers preferably operated at different temperatures. The temperature of the condenser can be set according to the boiling point of the condensate.

[0089] Depolymerization products

[0090] The process of the present disclosure produces depolymerization products with surprising selectivity.The gaseous fraction produced during pyrolysis is separated into liquid and gaseous depolymerization products, for example by condensation.

[0091] Liquid depolymerization product

[0092] The obtained liquid depolymerization product shows surprisingly low content of aromatic compounds, in particular surprisingly low content of polycyclic aromatic compounds and asphaltenes. Thus, the liquid depolymerization product obtained by the process of the present disclosure is characterized by low content of aromatic and olefinic components and high purity.

[0093] Preferably, the liquid depolymerization product obtained has an aromatic content of less than 10 mol%, preferably less than 5 mol%, in particular not more than 3 mol%, the content of aromatic components being measured as the content of aromatic protons in mol% determined by 1H-NMR spectroscopy.

[0094] In addition, the liquid depolymerization product obtained by the depolymerization process of the present disclosure is characterized by a low content of olefinic compounds. The content of olefinic compounds in the liquid depolymerization product is preferably less than 7 mol%, more preferably less than 5 mol%, and even more preferably less than 3 mol%, based on the total number of hydrocarbon protons; the content of olefinic compounds is determined based on the content of olefinic protons determined by 1H-NMR spectroscopy.

[0095] Another measure of the double bond content in a given sample is the bromine number (Br No.), which indicates the degree of unsaturation. In a preferred embodiment, the liquid depolymerized product obtained by the process of the present disclosure has a bromine number of less than 150, preferably 10 to 100, more preferably 15 to 80, even more preferably 20 to 70, especially 25 to 100, measured according to ASTM D1159-01, expressed as grams of bromine / 100 grams of sample.

[0096] The liquid depolymerization product obtained in the process of the present disclosure preferably has a boiling range of 30 to 650° C., more preferably 50 to 250° C. By separation techniques such as distillation, the depolymerization product can be separated into hydrocarbon fractions with different boiling ranges, for example, a light naphtha fraction mainly containing C5 and C6 hydrocarbons with a boiling range of 30° C. to 130° C., a fraction mainly containing C6 and C6 hydrocarbons with a boiling range of 130° C. to 220° C., and a fraction mainly containing C7 and C8 hydrocarbons with a boiling range of 150° C. to 220° C. 12 The heavy naphtha fraction of hydrocarbons mainly contains C9 and C 17 The kerosene fraction of hydrocarbons may be separated into other high boiling fractions such as diesel fuel, heating oil or wax oil.

[0097] It has also surprisingly been found that the liquid depolymerization product contains virtually no solid residues. In a preferred embodiment, the residue content of the liquid depolymerization product upon evaporation, determined according to ASTM D381, does not exceed 5 ppm (w).

[0098] Gaseous depolymerization products

[0099] The obtained gaseous depolymerization product shows a surprisingly low content of low molecular weight hydrocarbons, such as methane or ethane. On the contrary, it is surprisingly found that the gaseous depolymerization product contains an unusually high content of higher olefins, such as ethylene, propylene and butene, which are usually required for polyolefin production. Therefore, the gaseous depolymerization product obtained by the process of the present disclosure is characterized by a high content of any one of ethylene, propylene and butene and / or a low content of saturated low molecular weight hydrocarbons, especially those of the general formula Cn H 2n+2 wherein n is a real number from 1 to 4.

[0100] Therefore, in a preferred embodiment, the gaseous depolymerization product of the process of the present disclosure is characterized in that the methane content is at most 6 wt%, preferably at most 4 wt%, more preferably at most 3 wt%, most preferably at most 2 wt%, in particular at most 0.5-1.5 wt%, based on the total weight of the gaseous depolymerization product after step (e) of the process of the present disclosure.

[0101] Surprisingly, it has been found that the gaseous depolymerization product obtained by the process of the present disclosure contains a large amount of low molecular weight olefinic compounds, especially C n H 2n species, wherein n=2-4. The gaseous fraction can thus be used directly as a feedstock for further processing in a cracker downstream (e.g., a feed gas compressor) to obtain a purified monomer stream and thereafter for subsequent polymer production, thereby allowing bypassing the energy-intensive stream cracking furnaces that are usually required while reducing the output of CO2. Therefore, in a preferred embodiment, the gaseous depolymerization product of the process of the present disclosure is characterized in that, based on the total weight of the gaseous depolymerization product after step (e) of the process of the present disclosure, the general formula C n H 2n The content of compounds of (olefins) (wherein n=2-4) is at least 50 wt%, preferably at least 60 wt%, more preferably at least 65 wt%, most preferably at least 70 wt%, especially at least 75 wt%.

[0102] The gaseous depolymerization products may contain small amounts of HCl, HCN, H2S, H2O, NH3, COS, etc., which may optionally be separated in a refining step before introduction into the downstream section of the steam cracker.

[0103] The present disclosure will be explained in more detail with reference to the drawings and examples provided below.

[0104] Attached photos

[0105] Figure 1A flow chart of a process according to an embodiment of the present disclosure is presented. In process 500, a waste stream 502 is sorted to separate any polymer waste material from undesirable materials, and optionally, mechanically and / or chemically pretreated 504 to produce a polymer waste material feedstock 506. The polymer waste material feedstock 506 is then mixed with a catalyst 508 and subjected to catalytic pyrolysis to depolymerize 510 the polymer material. Depolymerization of the polymer material produces a gaseous product 520, a liquid product 530, and a solid product 540. The products are separated from one another, and optionally, the gaseous and liquid products 520, 530 are further processed. The solid product 540 may also be further processed to separate the char produced by the depolymerization from the catalyst 508. The recovered catalyst may then be used in a subsequent repetition of the process.

[0106] Figure 2 A flow chart of a process according to an embodiment of the present disclosure is presented. In process 600, polymer waste material 605 is mixed with a catalyst 610 to form a mixture and sent to a first pyrolysis reactor 615. In the first pyrolysis reactor 615, the mixture is heated to depolymerize at least a portion of the polymer waste material. After removing the undesirable solids and char 625 produced in the first pyrolysis reactor, the remaining mixture is transferred to a second pyrolysis reactor 620. In the second pyrolysis reactor 620, the remaining mixture is heated again to depolymerize the remaining polymer waste material. The gas 645 produced during the depolymerization can be sent to a steam cracker (not shown), while the liquid and wax 640 are directed to further processing.

[0107] Example

[0108] The following analytical methods were used:

[0109] 1) GC MS is used for liquid and gas phase analysis.

[0110] 2) After decoking the reactor residue at 800° C., the carbon residue was determined based on a mass balance.

[0111] 3) Liquid content was characterized using simulated distillation (SimDist) analysis according to ASTM D 7213: 2012. Final boiling point (FBP), boiling temperature at 50%, and initial boiling point (IBP) were taken from SimDist.

[0112] 4) The total content of unsaturated components in the liquid condensate was characterized by bromine number determination using an 848 Titrino Plus (Metrohm AG, Herisau, Switzerland) equipped with a double PT wire electrode with an integrated PT1000 temperature sensor and a 10 ml burette according to ASTM D1159-01 as described in Metrohm Application Bulletin 177 / 5e, December 2018. The bromine number (Br No.) indicates the amount of bromine absorbed by 100 grams of sample in grams.

[0113] 5) 1H-NMR analysis was performed by dissolving a sample of the liquid condensate in CDCl3 and characterizing the sample using proton NMR spectroscopy. Aromatic, olefinic and aliphatic protons were assigned according to the chemical shifts summarized in Table 1:

[0114] Table 1-1 Integration area in H-NMR spectrum

[0115] Peak attribution 1H chemical shift (ppm) <![CDATA[I1 (Aromatic protons)]]> 8.25-7.27 <![CDATA[CDCl3 - solvent]]> 7.26 <![CDATA[I2 (aromatic protons)]]> 7.25-6.60 <![CDATA[I3 (vinylic proton - type 2)]]> 6.60-5.95 <![CDATA[I4 (olefinic proton - type 1)]]> 5.95-5.67 <![CDATA[I5 (olefinic proton - type 2)]]> 5.67-5.35 <![CDATA[I6 (olefinic proton - type 3)]]> 5.35-5.15 <![CDATA[I7 (olefinic proton - type 1)]]> 5.15-4.85 <![CDATA[I8 (olefinic proton - type 4)]]> 4.85-4.40 <![CDATA[I9… (protons of alkane)]]> 4.40-0.25

[0116] The listed types of olefinic protons are assumed to correspond to the following structures:

[0117]

[0118] The amount of aromatic, olefinic, and aliphatic protons can be determined based on the specified peak integrations according to the following equations:

[0119] Aromatic proton mol% = [(I1+I2) / (I1+I2+I3+I4+I5+I6+I7+I8+I9)]%

[0120] Olefinic proton type 1 mol% = [(I4+I7) / (I1+I2+I3+I4+I5+I6+I7+I8+I9)]%

[0121] Olefinic proton type 2 mol% = [(I3+I5) / (I1+I2+I3+I4+I5+I6+I7+I8+I9)]%

[0122] Olefinic proton type 3 mol% = [(I6) / (I1+I2+I3+I4+I5+I6+I7+I8+I9)]%

[0123] Olefinic proton type 4 mol% = [(I8) / (I1+I2+I3+I4+I5+I6+I7+I8+I9)]%

[0124] Alkane proton mol% = [(I9) / (I1+I2+I3+I4+I5+I6+I7+I8+I9)]%

[0125] 6) The water content of the catalyst was determined at 180° C. on 0.5-1 g samples using a Sartorius MA45 (Sartorius AG, Goettingen, Germany).

[0126] 7) To determine the pH value of the hydrodepolymerization product, a liquid sample of the hydrodepolymerization product was extracted with water at a water:sample volume ratio of 1:5, and the pH value of the aqueous solution was measured.

[0127] 8) The particle size distribution of the particulate non-porous support and catalyst was determined by Coulter Counter analysis according to ASTM D4438.

[0128] 9) The properties of the organic waste materials used are determined as follows:

[0129] Since the composition of organic waste materials can vary, grind and analyze 20 to 100 g samples of polymer waste. Alternatively, analyze a pelletized sample of polymer waste. Use the following method:

[0130] i) Total volatiles (TV) were measured as the weight loss of a 10 g sample after 2 hours at 100° C. and 200 mbar.

[0131] ii) The water content was determined by Karl-Fischer titration according to Metrohm Application Bulletin 77 / 3e in accordance with ASTM E203 using an apparatus from Metrohm 915KF Ti-Touch equipped with a PT100 indicator electrode for volumetric KF titration.

[0132] iii) IR-spectroscopy is used for qualitative identification of various polymers (PP, PE, PS, PA, PET, PU, ​​polyester) and additives like CaCO3.

[0133] iv) Standard elemental analysis was used to determine the wt% of H, C, N (DIN 51732:2014-07) and S (tube furnace, ELTRA GmbH, Haan, Germany, DIN 51724-3:2012-07).

[0134] v) 1H-NMR is used to determine the composition of polymers soluble in solvents sufficient for recording 1H-NMR spectra: PE / PP equilibrium (also copolymers), PET, PS.

[0135] vi) Ash content analysis of plastics is determined at 800 °C in accordance with DIN EN ISO 3451-1 (2019-05).

[0136] vii) Determination of bulk density of polymer waste in accordance with DIN 53466.

[0137] viii) Corrosivity was determined as the pH value of the aqueous solution after a contact time of 3 hours (5 g sample in 50 ml distilled water)

[0138] ix) Inductively coupled plasma atomic emission spectrometry (ICP-AES) for quantitative elemental determination (total chlorine content, Si or metal content)

[0139] x) The ash content of liquid feedstock such as pyrolysis oil is measured according to ASTM D482-19.

[0140] Various catalysts were prepared and tested in the depolymerization of different polymer waste materials. The granular non-porous support used in the catalysts was sand with a particle size distribution as summarized in Table 2, where 99% of the particles were smaller than 3 mm. Before being used to form the catalysts, the sand was predried in a drying oven with circulating air at 80°C for 24 h.

[0141] Table 2: Particle size distribution

[0142] Sand, wt% >1400μm 40.55% >1400μm->1000μm 55.30% <1000μm 48.01%5%

[0143] Comparative Example:

[0144] Comparative catalysts were formed by mixing an acidic compound with 25 kg of the above sand to obtain comparative catalysts shown in Table 4 (Comparative-1, Comparative-2, and Comparative-3).

[0145] Embodiments of the present disclosure:

[0146] The catalyst of the present disclosure using a mineral oil coating agent was prepared as follows:

[0147] 25.0kg sand is put into the 60L steel drum with nut and equipped with Teflon inlay.Add 350ml mineral oil (corresponding to 1.4wt% with respect to sand).Tumbler is placed on tumbler hoop mixer and rotated 1 hour (about 100rpm).The mixture that 24.5kg obtains is placed in another tumbler, and 500g corresponding acidic components (corresponding to the load of 2wt%) are added.Tumbler is placed on tumbler hoop mixer and rotated 1 hour (about 100rpm).When mixing process finishes, obtain free-flowing catalyst, wherein the particles of acidic components are evenly distributed on the surface of sand particles.

[0148] The mineral oil used was Ondina X 432, commercially available from Shell, having the following properties:

[0149] Table 3:

[0150] nature method Shell Ondina X 432 <![CDATA[Kinematic viscosity at 20 °C, in mm 2 / s]]> ISO 3104 165 <![CDATA[Kinematic viscosity at 40 °C, unit: mm 2 / s]]> ISO 3104 59 <![CDATA[Kinematic viscosity at 100 °C, unit: mm 2 / s]]> ISO 3104 9.0

[0151] The catalyst of the present disclosure using a silica hydrogel coating agent was prepared as follows:

[0152] 25.0kg of sand is placed in a 60L steel drum with a nut and equipped with a Teflon inlay. 500ml of water (corresponding to 2.0wt% relative to sand) is added, and the drum is placed on a drum hoop mixer and rotated for 1 hour (about 100rpm). 24.5kg of the resulting mixture is placed in another drum, and 1000g of a 1:1 ground free-flowing mixture of silica hydrogel and acidic compounds (equivalent to a loading of 2wt%) is added. The drum is placed on a drum hoop mixer and rotated for 1 hour (about 100rpm). At the end of the mixing process, a free-flowing catalyst is obtained, in which the particles of the acidic compound are evenly distributed on the surface of the sand particles. The obtained mixture is dried in vacuo at 120°C for 6h.

[0153] The silica hydrogel was prepared according to the procedure described in Example 1 of EP 1290042. The solid content of the hydrogel sample was 20 wt%. The D50 of the ground mixture of silica hydrogel and acidic component was 80-100 μm according to ASTM D4438.

[0154] Table 4 summarizes the catalysts used, where the amount of acidic compound is given in wt% relative to the sand.

[0155] Table 4

[0156] catalyst# Coating agent Acidic compounds Amount of acidic compound (wt%) 1 Oil Siral 40HPV 1 2 Oil Siral 40HPV 2 3 Oil Zeolite CFG-1 1 4 Silicone hydrogel Siral 40HPV 1 5 Silicone hydrogel Siral 40HPV 2 6 Silicone hydrogel Zeolyst β 2 7 Silicone hydrogel Zeolyst ZSM-5 2 8 Oil Zeolyst β 2 9 Oil Zeolyst ZSM5 2 Contrast-1 none Zeolite CFG-1 2 Contrast-2 none Siral 40HPV 2 Contrast-3 none Zeolyst β 2 Contrast -4 none Zeolyst ZSM5 2

[0157] Acidic compounds:

[0158] Zeolite CFG-1, Zeolyst ZSM-5 and Zeolyst Beta (CP811E-75), commercially available from PQ Corporation, Malvern, PA, USA

[0159] Siral 40HPV: Si / Al mixed oxide with Al2O3 / SiO2 60 / 40 [%], commercially available from SasolGermany GmbH, Hamburg, Germany.

[0160] raw material:

[0161] Some of the following organic waste materials are used as raw materials:

[0162] A: Granular agricultural and industrial packaging films.

[0163] B: shredded flakes and small pieces of membrane.

[0164] C: Flakes, villi and small pieces of membrane, compacted.

[0165] D: Shredded membrane.

[0166] E: shredded and granulated multilayer films.

[0167] G) 50 / 50 PE / PP blend raw polymer in pellet form.

[0168] H) Shredded plastic waste fraction of ELVs with metallic impurities.

[0169] The raw material properties averaged over the analysis of three samples are summarized in Table 5.

[0170] Table 5:

[0171]

[0172] *) Other contents include inorganic, polymeric or organic pollutants and volatile components Ash: Ash content

[0173] TV: Total Volatile Matter

[0174] BD: Bulk density

[0175] Cl: total chlorine content

[0176] PE: Polyethylene content

[0177] PP: Polypropylene content

[0178] PET: polyethylene terephthalate content

[0179] PS: polystyrene content

[0180] PA: polyamide content

[0181] Other contents: Content of other pollutants

[0182] The feedstock and catalyst were introduced into a reactor unit equipped with a heating unit, a gas discharge unit, a solid discharge unit; a condensation unit and a screw for uniform mixing of the reactor contents during depolymerization. The conditions of the depolymerization performed are summarized in Table 6. The obtained gaseous fraction was further separated into liquid and gaseous depolymerization products by condensation. The amounts of the obtained fractions are also given in Table 6.

[0183] Table 6: Process parameters and mass balance (a)

[0184] run# temperature time catalyst# raw material <![CDATA[Wax % **) > liquid% gas% 1 500℃ 30min none G 44.7 0 51.7 2 500℃ 30min Contrast-1 G 0* 37.4* 58.7 3 500℃ 30min Contrast-2 G 0* 43.4* 54.5 4 500℃ 30min Contrast-3 G 0* 58.3* 36.5 5 450℃ 30min Contrast-1 G 54.4* 0* 32.1 6 500℃ 30min 1 G 0 61.8 37.1 7 450℃ 30min 1 G 0 64.7 26.6 8 450℃ 30min 2 G 0 58.8 31.8 9 450℃ 30min 3 G 0 63.8 24.0 10 450℃ 30min Contrast-2 G 56.4 - 32.1

[0185] (a) The amount missing to 100% is due to loss

[0186] *) Large amounts of wax floating in an inhomogeneous liquid

[0187] **) Wax %: solid product at room temperature

[0188] Referring to the results in Table 6, it can be observed that Comparative Runs #2-5 showed unstable depolymerization, where the peak of gas generation corresponded to a black / brown liquid with a large amount of wax floating. This indicates that thermal and catalytic depolymerization occurred simultaneously. Although Run #5 was conducted at 50°C lower than Run #2, it delivered a much higher amount of wax.

[0189] Catalysts 1, 2, and 3 provided with a coating agent enabled smooth runs (Runs #6-9), producing constant gas at lower temperatures and a uniform clear tan liquid.

[0190] The obtained liquid and gaseous depolymerization products were further analyzed. The analysis results of the liquid depolymerization products are summarized in Table 7.

[0191] Table 7: Composition of liquid depolymerization product

[0192]

[0193] 1-H NMR was used to obtain the Mol % of aromatic, olefinic and aliphatic protons in the sample.

[0194] *) Final boiling point (FBP), boiling temperature at 50% and initial boiling point (IBP) are taken from SimDist.

[0195] It is clear from the data presented that depolymerization of polymer waste materials using the catalysts of the present disclosure produces large amounts of liquefiable products containing only small amounts of aromatic and olefinic content.

[0196] In another set of tests, different feedstocks were depolymerized to show that for a given feedstock, the catalyst of the present disclosure is able to produce an increased portion of the gaseous fraction in the depolymerization reaction relative to pure thermal depolymerization (Run 11) and the comparative catalyst. The process parameters and mass balance of the resulting depolymerization products are summarized in Table 8.

[0197] Table 8: Process parameters and mass balance (a)

[0198]

[0199] (a) The amount missing to 100% is due to losses; (b) large amounts of wax floating in an inhomogeneous liquid +) The liquid is a combination of all fractions and may contain some waxy solid particles and agglomerates which disappear on heating to >50°C.

[0200] *)The catalyst used in three consecutive runs maintained good selectivity and was then regenerated by heating to 800°C in air and sieving out smaller particles (ash) <500 μm.

[0201] The above data show that the catalyst of the present disclosure produces a large amount of gaseous depolymerization products and can maintain good performance even when the feedstock is added with heterogeneous materials. In addition, they also show that the catalyst of the present disclosure can be effectively regenerated, thereby allowing the possibility of increasing the sustainability of the process.

[0202] The analysis results of the gaseous depolymerization products are summarized in Table 9.

[0203] Table 9: Mass balance of gaseous depolymerization products

[0204] run# 11 12 13 14 15 17 18 19 raw material A A A+1%PA A+5% paper A+10%PA A A A catalyst# none 8 8 8 8 7 6 7*) Components Wt.% Wt.% Wt.% Wt.% Wt.% Wt.% Wt.% Wt.% <![CDATA[H2]]> 0.1 0 0 0 0 0.1 0.1 0.2 CO 1.1 1.8 2 3.2 2.7 0 0 0 <![CDATA[CO2]]> 4 11.2 11.5 13.9 11.8 0.4 2.4 0.6 <![CDATA[CH4]]> 6.1 0.5 0.9 0.7 5.6 0 0 0.2 <![CDATA[C2H6]]> 13.5 0.4 1 0.6 10.8 0.8 0.3 1.1 <![CDATA[C2H4]]> 11.1 0.9 1.3 1 10.2 5.4 0.8 5.8 <![CDATA[C3H8]]> 14.8 2.1 2.1 1.9 11.5 13.3 1.3 16.6 <![CDATA[C3H6]]> 20.3 27.9 27.7 25.9 18.9 29.2 33.3 25.5 Butane 11.9 23.3 20 19.6 9.7 24.7 21.5 23 Butene 16.3 32 33.5 33.2 18.7 26 40.4 26.9 Remaining 0.7 0 0 0 0 0 0 0 Olefins 47.7 60.8 62.5 60.1 47.8 60.6 74.5 58.2 Total HC 94 87.1 86.5 82.9 85.4 99.4 97.6 99.1 Olefins / HC 50.7 69.8 72.3 72.5 56.0 61.0 76.3 58.7

[0205] *) The catalyst used in three consecutive runs maintained good selectivity and was then regenerated by heating to 800°C in air and sieving out smaller particles (ash) <500 μm.

[0206] HC: Hydrocarbon

[0207] Olefins: Sum of ethylene, propylene and butene

[0208] Olefins / HC: The percentage of all olefins relative to total hydrocarbons

[0209] As can be seen from Table 9, the process and catalyst of the present disclosure produces a gaseous depolymerization product with a large amount of monomers which, after purification, can be used as a polymerization feed. Any saturated gaseous hydrocarbons can be processed back to the steam cracker in the usual manner. In contrast, thermal cracking, as reflected in Run #11, does not show any selectivity for olefins and produces a large amount of methane.

Claims

1. A catalyst for depolymerizing polymer waste materials, comprising as active component an acidic compound deposited on a particulate non-porous support with the aid of a coating agent.

2. The catalyst according to claim 1, It is characterized in that The particle carrier is selected from the group consisting of sand, glass beads and metal particles.

3. The catalyst according to claim 2, wherein the support has an average particle size D50 determined by sieve analysis according to ISO 3310-1 / ASTM E11 of 0.2 to 20 mm, preferably 0.5 to 10 mm.

4. The catalyst according to claim 3, wherein the support is sand.

5. The catalyst according to any one of the preceding claims, It is characterized in that The acidic compound is selected from the group consisting of: Al / Si mixed oxide, Al 2 O 3 , aluminosilicates, silica and zeolites.

6. The catalyst according to any one of the preceding claims, It is characterized in that The active compound is contained in the catalyst in an amount of 0.5 to 6 wt%, preferably 2 to 4 wt%, based on the total weight of the catalyst.

7. The catalyst according to any one of the preceding claims, It is characterized in that The coating agent is selected from the group consisting of oil, inorganic hydrogel or a combination thereof.

8. The catalyst according to any one of the preceding claims, It is characterized in that The coating agent is 1 to 300 wt %, preferably 2 to 150 wt %, more preferably 5 to 100 wt % of the agent based on the amount of the acidic compound.

9. A method for depolymerizing polymer waste materials, the method The following steps are involved: (a) providing feedstock of polymer waste materials; (b) mixing the feedstock with a catalyst according to any one of claims 1 to 8; (c) pyrolyzing the mixture; (d) collecting gaseous fractions produced during the pyrolysis process, and (e) separating the collected gaseous fraction to obtain gaseous and liquid depolymerization products.

10. The method according to claim 9, It is characterized in that The method further comprises distilling the liquid depolymerization product.

11. The method according to claim 9 or 10, It is characterized in that The polymer waste material consists of or comprises a plastic material selected from the group consisting of polyethylene (PE), polypropylene (PP), polystyrene (PS), polyethylene terephthalate (PET), polyvinyl chloride (PVC), polyamide (PA), polyurethane (PU), polyacrylonitrile (PAN) and polybutylene (PB) and mixtures thereof or consists thereof.

12. The method according to any one of claims 9 to 11, It is characterized in that The gas content of the depolymerization product after step (e) is preferably greater than 30 wt%, more preferably greater than 50 wt%, especially greater than 70 wt%, based on the combined weight of gaseous and liquid depolymerization products.

13. The method according to any one of claims 9 to 12, It is characterized in that Based on the total weight of the gaseous depolymerization product after step (e) of the method of the present disclosure, the gaseous depolymerization product contains n H 2n The content of the compound is at least 50 wt%, preferably at least 60 wt%, in particular at least 65 wt%, wherein n=2-4.

14. The method according to any one of claims 9 to 13, It is characterized in that The depolymerization catalyst is separated from any solid content remaining after the depolymerization process and reintroduced into the process.

15. A method according to claim 14, wherein the catalyst is reactivated by heating before being reintroduced into the process.