Ethylene-vinyl alcohol copolymer composition and method for producing same, melting molding material using same, particles, and multilayer structure and method

By adding specific metal compounds and resin compositions to EVOH resin, the problem of thermal degradation of EVOH resin during melt molding is solved, thermal stability and productivity are improved, and it is suitable for highly functional packaging materials.

CN118786175APending Publication Date: 2024-10-15MITSUBISHI CHEM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380024609.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-30
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

EVOH resin is easily degraded by heat during melt molding, resulting in reduced product productivity. Especially in highly functional molding equipment, the problem of thermal degradation is more prominent.

Method used

Add metal compounds from the d area of ​​the 4th period of the long-period periodic table of elements, polyolefin resins, olefin polymers, polyamide resins, styrene derivatives with substituents at the α position, and specific trace amounts to the EVOH resin. Titanium compounds that form alloy compounds to inhibit thermal degradation.

Benefits of technology

It effectively suppresses the thermal deterioration of EVOH resin, improves the thermal stability during melt molding, extends the long-term operability of the product, is suitable for the manufacture of multi-layer structures, and improves the mechanical strength and appearance quality of molded products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005019442560000681
    Figure BDA0005019442560000681
  • Figure BDA0005019442560000711
    Figure BDA0005019442560000711
  • Figure BDA0005019442560000731
    Figure BDA0005019442560000731
Patent Text Reader

Abstract

The present invention provides a composition as an ethylene-vinyl alcohol copolymer composition in which thermal deterioration during melt molding is suppressed. An ethylene-vinyl alcohol copolymer composition containing: an ethylene-vinyl alcohol copolymer (A); at least one compound (B) selected from the group consisting of (B1) metal compounds (excluding titanium compounds) belonging to the d region of the fourth period of the long-period periodic table, (B2) specific polyolefin resins, (B3) olefin polymers, (B4) polyamide resins, and (B5) styrene derivatives having a substituent at the alpha position; and a titanium compound (C). The content of the titanium compound (C) in terms of metal is 0.00005 ppm or more and less than 5 ppm relative to the mass of the ethylene-vinyl alcohol copolymer composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an ethylene-vinyl alcohol copolymer (hereinafter sometimes referred to as "EVOH resin") composition and a method for producing the same, a melt-molding material and pellets using the same, and a multilayer structure and a method for producing the same. Background Art

[0002] EVOH resin has excellent transparency, oxygen and other gas barrier properties, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and is molded into films, sheets, bottles, etc., and is widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and pesticide packaging materials.

[0003] However, EVOH resin has relatively active hydroxyl groups in its molecules and therefore tends to be easily degraded by heat, and is prone to coloring during melt molding.

[0004] In order to solve the above problems, for example, Patent Document 1 discloses a resin composition, characterized in that it contains EVOH resin (A), acetic acid (B), magnesium acetate and / or calcium acetate (C), wherein the content of (B) is 0.05 parts by mass or less relative to 100 parts by mass of (A), and the content of (C) is 0.001 to 0.02 parts by mass relative to 100 parts by mass of (A) in terms of metal conversion. It is disclosed that by using the resin composition, a molded product having excellent long-term running performance during melt molding, less fish eyes, streaks, and coloring, and excellent appearance can be obtained, and further, when the molded product is made into a laminate, the odor is reduced, and the laminate has excellent interlayer adhesion after secondary processing such as stretching and deep drawing.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 11-106592 Summary of the invention

[0008] The technology disclosed in the above-mentioned Patent Document 1 can obtain a molded product with excellent long-term operation performance during melt molding, less fish eyes, streaks, and coloring, and excellent appearance. However, in recent years, with the diversification of feed blocks and mold shapes in molding devices, the thinning of multilayer structures in final products, and the increase in the number of layers, there is a trend of high-functionality in molding devices. Therefore, in molding devices that have become complicated due to high functionality, there is a trend that the resin thermally deteriorates and the productivity (long-term operation performance) of the product decreases, and further improvement is sought.

[0009] The present invention provides an EVOH resin composition in which thermal degradation of the EVOH resin during heating such as melt molding is suppressed.

[0010] Therefore, in view of the above situation, the inventors have discovered that by adding at least one compound (B) selected from metal compounds (excluding titanium compounds) (B1) belonging to the 4th period d zone of the long-period periodic table, polyolefin resins (B2), olefin polymers (B3), polyamide resins (B4) and styrene derivatives having a substituent at the α position (B5), as well as a specific trace amount of titanium compound to the EVOH resin, an EVOH resin composition can be obtained in which thermal degradation of the EVOH resin during heating such as melt molding is suppressed.

[0011] That is, the present invention has the following aspects.

[0012] [1] An ethylene-vinyl alcohol copolymer composition comprising:

[0013] Ethylene-vinyl alcohol copolymer (A),

[0014] At least one compound (B) selected from the group consisting of metal compounds (excluding titanium compounds) (B1) belonging to the 4th period d-block of the long period periodic table, polyolefin resins (B2), olefin polymers (B3), polyamide resins (B4) and styrene derivatives having a substituent at the α-position (B5), and

[0015] Titanium compound (C);

[0016] The olefin polymer (B2) is at least one selected from the group consisting of olefin thermoplastic elastomers, aliphatic rubbers and ionomers.

[0017] The metal equivalent content of the titanium compound (C) is 0.00005 ppm or more and less than 5 ppm based on the mass of the ethylene-vinyl alcohol copolymer composition.

[0018] [2] The ethylene-vinyl alcohol copolymer composition according to [1], wherein the mass content ratio (A) / (B) of the ethylene-vinyl alcohol copolymer (A) to the component (B) is 1 / 99 to 99 / 1.

[0019] [3] The ethylene-vinyl alcohol copolymer composition according to [1] or [2], wherein the metal conversion content of the titanium compound (C) is 0.001 to 3 ppm relative to the total mass of the ethylene-vinyl alcohol copolymer (A) and the titanium compound (C).

[0020] [4] An ethylene-vinyl alcohol copolymer composition according to any one of [1] to [3], wherein the metal conversion content of the metal compound (B1) belonging to the 4th period d-block of the long-period periodic table is 0.1 to 500 ppm relative to the mass of the ethylene-vinyl alcohol copolymer composition.

[0021] [5] The ethylene-vinyl alcohol copolymer composition according to any one of [1] to [4], wherein the metal compound (B1) belonging to the d-block of period 4 of the long-form periodic table is a zinc compound.

[0022] [6] The ethylene-vinyl alcohol copolymer composition according to any one of [1] to [5], wherein the metal compound (B1) belonging to the d-block of period 4 of the long-form periodic table is a carboxylate.

[0023] [7] The ethylene-vinyl alcohol copolymer composition according to any one of [1] to [3], wherein the polyolefin resin (B2) has a density of 0.89 g / cm 3 The above polyolefin resins.

[0024] [8] The ethylene-vinyl alcohol copolymer composition according to any one of [1] to [3] and [7], wherein the polyolefin resin (B2) is polypropylene.

[0025] [9] The ethylene-vinyl alcohol copolymer composition according to any one of [1] to [3], wherein the content of the styrene derivative (B5) having a substituent at the α-position is 1 to 10,000 ppm relative to the mass of the ethylene-vinyl alcohol copolymer composition.

[0026]

[10] The ethylene-vinyl alcohol copolymer composition according to any one of [1] to [3] and [9], wherein the styrene derivative (B5) having a substituent at the α-position is an α-methylstyrene derivative.

[0027]

[11] A method for producing an ethylene-vinyl alcohol copolymer composition, which is a method for producing the ethylene-vinyl alcohol copolymer composition described in any one of [1] to

[10] , comprising the step of melt-mixing composition raw materials containing the above-mentioned (A), the above-mentioned (B) and the above-mentioned (C).

[0028]

[12] A melt molding material comprising the ethylene-vinyl alcohol copolymer composition according to any one of [1] to

[10] .

[0029]

[13] A pellet comprising the ethylene-vinyl alcohol copolymer composition according to any one of [1] to

[10] .

[0030]

[14] A multilayer structure comprising at least one layer comprising the ethylene-vinyl alcohol copolymer composition according to any one of [1] to

[10] .

[0031]

[15] A method for manufacturing a multilayer structure, which is the method for manufacturing the multilayer structure described in

[14] , includes a step of melt-molding a layer made of the ethylene-vinyl alcohol copolymer composition.

[0032] The EVOH resin composition of the present invention has excellent thermal stability. Therefore, thermal degradation of the EVOH resin during melt molding can be suppressed. Detailed Embodiments

[0033] Hereinafter, the present invention will be described in more detail based on embodiments of the present invention, but the present invention is not limited to these embodiments.

[0034] It should be noted that in the present invention, when expressed as "X to Y" (X and Y are arbitrary numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", and also includes the meaning of "preferably greater than X" or "preferably less than Y".

[0035] In addition, when expressed as "X or more" (X is an arbitrary number) or "Y or less" (Y is an arbitrary number), it also includes the meaning of "preferably greater than X" or "preferably less than Y".

[0036] It should be noted that in the present invention, "x and / or y (x and y are arbitrary components or ingredients)" means only x, only y, and the three combinations of x and y.

[0037] The EVOH resin composition of the present invention has the "first mode" in which the component (B) is a metal compound (excluding titanium compounds) (B1) belonging to the d-block of the fourth period of the long-period type periodic table, the "second mode" in which the component (B) is a polyolefin resin (B2), the "third mode" in which the component (B) is an olefin polymer (B3), the "fourth mode" in which the component (B) is a polyamide resin (B4), and the "fifth mode" in which the component (B) is a styrene derivative having a substituent at the α-position (B5). Each mode will be described below.

[0038] <<First Mode>>

[0039] <EVOH Resin Composition>

[0040] An EVOH resin composition according to an embodiment of the present invention (hereinafter referred to as "this EVOH resin composition") has an EVOH resin (A) as a main component, and contains a metal compound (B1) belonging to the d-block of the fourth period of the long-period type periodic table and a specific trace amount of a titanium compound (C).

[0041] That is, the present invention has the following mode.

[0042] [1-1] An EVOH resin composition, comprising:

[0043] EVOH resin (A), a metal compound (excluding titanium compounds) (B1) belonging to the 4th period d-zone of the long period periodic table, and a titanium compound (C);

[0044] The metal-equivalent content of the titanium compound (C) is 0.001 ppm or more and less than 5 ppm based on the mass of the EVOH resin composition.

[0045] [1-2] The EVOH resin composition according to [1-1], wherein the metal conversion content of the metal compound (B1) belonging to the 4th period d-block of the long period periodic table is 0.1 to 500 ppm based on the mass of the EVOH resin composition.

[0046] [1-3] The EVOH resin composition according to [1-1] or [1-2], wherein the mass ratio of the metal conversion content of the metal compound (B1) belonging to the 4th period d-block of the long period periodic table to the metal conversion content of the titanium compound (C) is 0.03 to 50000.

[0047] [1-4] The EVOH resin composition according to any one of [1-1] to [1-3], wherein the metal compound (B1) belonging to the d-block of the fourth period of the long-form periodic table is a zinc compound.

[0048] [1-5] The EVOH resin composition according to any one of [1-1] to [1-4], wherein the metal compound (B1) belonging to the d-block of the fourth period of the long-form periodic table is a carboxylate.

[0049] [1-6] A melt-molding EVOH resin composition comprising the EVOH resin composition described in any one of [1-1] to [1-5].

[0050] [1-7] A pellet comprising the EVOH resin composition according to any one of [1-1] to [1-5].

[0051] [1-8] A multilayer structure comprising at least one layer comprising the EVOH resin composition according to any one of [1-1] to [1-5].

[0052] [1-9] A method for producing an EVOH resin composition, which is the method for producing the EVOH resin composition according to any one of [1-1] to [1-5], comprising the step of melt-mixing a composition raw material containing the EVOH resin and a titanium compound.

[0053] [1-10] A method for producing a multilayer structure, which is a method for producing the multilayer structure described in [1-8], comprising the step of melt-molding a layer composed of the EVOH resin composition.

[0054] In the present EVOH resin composition, the base resin is EVOH resin (A), and the content of EVOH resin (A) in the present EVOH resin composition is usually 70% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 95% by mass or more.

[0055] Hereinafter, each component will be described.

[0056] [EVOH resin (A)]

[0057] The EVOH resin (A) used in the present invention is generally a resin obtained by saponifying an ethylene-vinyl ester copolymer which is a copolymer of ethylene and a vinyl ester monomer, and is a water-insoluble thermoplastic resin.

[0058] As the vinyl ester monomer, vinyl acetate can be used representatively from the aspects of market availability and good impurity treatment efficiency during production. As other vinyl ester monomers other than vinyl acetate, for example, aliphatic vinyl esters such as vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, and vinyl versatate, and aromatic vinyl esters such as vinyl benzoate can be mentioned. Usually, aliphatic vinyl esters having 3 to 20 carbon atoms, preferably 4 to 10 carbon atoms, and particularly preferably 4 to 7 carbon atoms can be used. These are usually used alone, and multiple types can be used simultaneously as needed.

[0059] As the polymerization method for copolymerizing the above-mentioned ethylene and vinyl ester monomers, any known polymerization method can be used, such as solution polymerization, suspension polymerization, emulsion polymerization, etc. Generally speaking, solution polymerization using methanol as a solvent is used. In addition, the saponification of the obtained ethylene-vinyl ester copolymer can also be carried out by a known method.

[0060] The EVOH resin (A) produced in this manner mainly comprises structural units derived from ethylene and vinyl alcohol structural units, and also contains a certain amount of vinyl ester structural units which remain without being saponified.

[0061] The content of the ethylene structural unit in the EVOH resin (A) is usually 20 to 60 mol%, preferably 25 to 50 mol%, and particularly preferably 25 to 35 mol%. The content of the ethylene structural unit can be controlled by the pressure of ethylene when copolymerizing the vinyl ester monomer with ethylene. When the content is too low, the gas barrier properties and melt moldability under high humidity tend to decrease, and when it is too high, the gas barrier properties tend to decrease.

[0062] In addition, the content of the ethylene structural unit can be measured based on ISO14663.

[0063] The saponification degree of the EVOH resin (A) is usually 90 to 100 mol%, preferably 95 to 100 mol%, and particularly preferably 99 to 100 mol%. The saponification degree can be controlled by the amount of a saponification catalyst (usually a basic catalyst such as sodium hydroxide is used) when saponifying the ethylene-vinyl ester copolymer, temperature, time, etc. When the saponification degree is too low, the gas barrier properties, thermal stability, moisture resistance, etc. tend to be reduced.

[0064] The saponification degree of the EVOH resin can be measured in accordance with JIS K6726 (wherein the EVOH resin is used in the form of a solution uniformly dissolved in a water / methanol solvent).

[0065] The melt flow rate (MFR) (210°C, load 2160g) of the EVOH resin (A) is usually 0.5 to 100 g / 10 minutes, preferably 1 to 50 g / 10 minutes, and particularly preferably 3 to 35 g / 10 minutes. If the MFR is too large, the stability during film formation tends to be impaired, while if it is too small, the viscosity becomes too high, and melt extrusion tends to become difficult.

[0066] The MFR is an index of the degree of polymerization of the EVOH resin (A), and can be adjusted by the amount of the polymerization initiator and the amount of the solvent when ethylene and the vinyl ester monomer are copolymerized.

[0067] The EVOH resin (A) may further contain a structural unit derived from a comonomer shown below (for example, 10 mol% or less of the EVOH resin (A)) within a range not inhibiting the effects of the present invention.

[0068] Examples of the comonomer include olefins such as propylene, 1-butene, and isobutylene; hydroxyl-containing α-olefins such as 3-butene-1-ol, 3-butene-1,2-diol, 4-pentene-1-ol, and 5-hexene-1,2-diol, and derivatives thereof such as esters and acylates; hydroxyalkyl vinylides such as 2-methylenepropane-1,3-diol and 3-methylenepentane-1,5-diol; 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2- Hydroxyalkyl vinylene diacetates such as methylenepropane and 1,3-dibutyryloxy-2-methylenepropane; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, phthalic acid (anhydride), maleic acid (anhydride), itaconic acid (anhydride) or their salts or mono- or di-alkyl esters having 1 to 18 carbon atoms in the alkyl group; acrylamide, N-alkyl acrylamide having 1 to 18 carbon atoms in the alkyl group, N,N-dimethylacrylamide, 2-acrylamidopropanesulfonic acid or its salts, acrylamidopropyl dimethylamine or its salts acrylamides such as methacrylamide, N-alkylmethacrylamide with an alkyl group having 1 to 18 carbon atoms, N,N-dimethylmethacrylamide, 2-methacrylamidepropanesulfonic acid or its salt, methacrylamidepropyldimethylamine or its acid salt or its quaternary ammonium salt; N-vinyl amides such as N-vinylpyrrolidone, N-vinylformamide, N-vinylacetamide; vinyl cyanides such as acrylonitrile and methacrylonitrile; 18 alkyl vinyl ethers, hydroxyalkyl vinyl ethers, alkoxyalkyl vinyl ethers and other vinyl ethers; vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, vinyl bromide and other vinyl halides; vinyl silanes such as trimethoxyvinylsilane; allyl acetate, allyl chloride and other halogenated allyl compounds; allyl alcohols such as allyl alcohol and dimethoxyallyl alcohol; trimethyl-(3-acrylamide-3-dimethylpropyl)-ammonium chloride, acrylamide-2-methylpropanesulfonic acid and other copolymer monomers. These can be used alone or in combination of two or more.

[0069] Among them, α-olefins containing hydroxyl groups are preferred, and 3-butene-1,2-diol and 5-hexene-1,2-diol are particularly preferred. When the above α-olefins containing hydroxyl groups are copolymerized, the obtained EVOH resin has a primary hydroxyl group in the side chain. Such EVOH resins having primary hydroxyl groups in the side chain, especially EVOH resins having a 1,2-diol structure in the side chain, are preferred in terms of maintaining gas barrier properties and improving secondary moldability.

[0070] When the EVOH resin (A) used in the present invention has a primary hydroxyl group in the side chain, the content of the structural unit derived from the monomer having the primary hydroxyl group is usually 0.1 to 20 mol %, preferably 0.5 to 15 mol %, particularly preferably 1 to 10 mol % of the EVOH resin (A).

[0071] As the EVOH resin (A), an EVOH resin “post-modified” by esterification, ureation, acetalization, cyanoethylation, oxyalkylene or the like may be used.

[0072] When the post-modified EVOH resin is used, the modification rate is usually 10 mol% or less, preferably 4 mol% or less. When the modification rate of the EVOH resin used is too high, it is easily thermally degraded, and the long-term operating performance tends to decrease.

[0073] Furthermore, the EVOH resin (A) may be a mixture of EVOH resins having different contents of ethylene structural units, saponification degrees, polymerization degrees, copolymer components, and the like.

[0074] [Metal compounds belonging to the d-block of the 4th period of the long-period periodic table (B1) (excluding titanium compounds)]

[0075] As the metal compound (B1) (excluding titanium compounds, the same below) belonging to the 4th period d-block of the long period periodic table (hereinafter sometimes referred to as "specific period d-block") used in the present invention, for example, there can be mentioned scandium compounds, vanadium compounds, chromium compounds, manganese compounds, cobalt compounds, nickel compounds, copper compounds, zinc compounds, etc. In particular, zinc compounds are preferred from the aspect of easily obtaining the effects of the present invention.

[0076] In addition, as the metal compound (B1) belonging to the d region, salts, oxides, hydroxides, etc. of the metal belonging to the specific period d region can be cited. Among them, metal oxides and metal salts belonging to the specific period d region are preferred from the aspects of economy and dispersibility. In particular, metal salts of the specific period d region are preferred from the aspect of easy to obtain the effect of the invention.

[0077] Examples of the metal salt belonging to the specific period d-block include inorganic salts such as carbonates, hydrogen carbonates, phosphates, borates, sulfates, and chlorides, and organic salts such as carboxylates.

[0078] Among them, carboxylate salts are particularly preferred because the effects of the invention can be easily obtained.

[0079] As the above-mentioned carboxylate, from the aspect of market availability, saturated carboxylates are usually used, but unsaturated carboxylates can also be used. As the above-mentioned saturated carboxylates, for example, monocarboxylates such as acetate, butyrate, propionate, enanthate, caprylate, caprate, laurate, palmitate, stearate, 12-hydroxystearate, behenic acid, montanate, oxalate, malonate, succinate, adipate, suberate, sebacate, etc. can be enumerated. They can be used alone or in combination of more than two kinds. Among them, from the aspect of market availability, it is preferably a straight-chain carboxylate, more preferably a monocarboxylate, particularly preferably butyrate, caproate, caprylate, caprate, laurate, stearate, especially preferably caproate, caprylate, caprate, laurate.

[0080] The carboxylate salt has an anion having generally 2 to 25 carbon atoms, preferably 2 to 22 carbon atoms, particularly preferably 4 to 20 carbon atoms, and particularly preferably 6 to 18 carbon atoms from the viewpoint of productivity.

[0081] From these aspects, the metal compound (B1) belonging to the specific period d region is preferably a zinc compound, preferably a zinc carboxylate, more preferably a zinc carboxylate having an anion with 2 to 25 carbon atoms, particularly preferably a zinc carboxylate having an anion with 2 to 22 carbon atoms, particularly preferably a zinc carboxylate having an anion with 4 to 20 carbon atoms, and even more preferably a zinc carboxylate having 6 to 18 carbon atoms.

[0082] The molecular weight of the metal compound (B1) belonging to the specific period d-block is usually 100 to 10,000, preferably 150 to 1,000, and particularly preferably 200 to 800, from the viewpoint of dispersibility and productivity of the EVOH resin composition.

[0083] In addition, from the viewpoint of economic efficiency and dispersibility, the metal compound (B1) belonging to the specific period d-block used in the present invention preferably does not include a layered inorganic compound such as montmorillonite or a complex salt such as hydrotalcite.

[0084] As the form of the metal compound (B1) belonging to the specific period d region, for example, any form of solid (powder, fine powder, flake, etc.), semi-solid, liquid, paste, solution, emulsion (aqueous dispersion), etc. can be used. Among them, powder is preferred from the aspect of easy handling.

[0085] In addition, the above-mentioned metal compound (B1) belonging to the specific period d zone can be used alone or in combination of two or more kinds. When using multiple metal compounds belonging to the specific period d zone, the content is obtained by adding up the contents of the multiple metal compounds belonging to the specific period d zone calculated on the basis of metal mass.

[0086] The content of the metal compound (B1) belonging to the specific period d zone, calculated as metal mass, relative to the mass of the EVOH resin composition is usually 0.1 to 500 ppm, preferably 1 to 300 ppm, more preferably 3 to 200 ppm, particularly preferably 8 to 150 ppm, further preferably 10 to 100 ppm, and particularly preferably 15 to 80 ppm.

[0087] If the content of the metal compound (B1) belonging to the specific period d-block is too high, thermal stability may be impaired, whereas if it is too low, the effect of the invention may become insufficient.

[0088] It should be noted that the EVOH resin composition that serves as the basis for the content ratio of the metal compound (B1) belonging to the specific period d region is an EVOH resin composition as a final product containing EVOH resin (A), the metal compound (B1) belonging to the specific period d region, the titanium compound (C), and various additives formulated as needed.

[0089] Moreover, the content of the above-mentioned metal compound (B1) belonging to the specific period d zone in the present EVOH resin composition in terms of metal conversion can be calculated, for example, by the following operation: the above-mentioned EVOH resin composition is heated and incinerated and acid-treated with hydrochloric acid or the like, pure water is added to the obtained solution to make up the volume, and the obtained liquid is used as a test solution and measured with an atomic absorption photometer.

[0090] [Titanium compound (C)]

[0091] Examples of the titanium compound (C) used in the present invention include inorganic titanium compounds and organic titanium compounds. The titanium compound may be used alone or in combination of two or more. Among them, inorganic titanium compounds are preferred.

[0092] Examples of the inorganic titanium compound include titanium oxide, titanium hydroxide, titanium chloride, and inorganic titanium salts.

[0093] Examples of the titanium oxide include titanium (II) oxide, titanium (III) oxide, titanium (IV) oxide, and titanium oxyoxide.

[0094] Examples of the titanium hydroxide include titanium hydroxide and titanium hydroxide.

[0095] Examples of the titanium chloride include titanous chloride and titanium chloride.

[0096] Examples of the inorganic salt of titanium include titanium phosphate and titanium sulfate.

[0097] Among them, titanium oxide is preferred, titanium (IV) oxide is more preferred, and rutile titanium (IV) oxide is particularly preferred.

[0098] Examples of the organic titanium compound include titanium acetate, titanium butyrate, titanium stearate and other titanium carboxylates.

[0099] The titanium compound (C) may be present in the EVOH resin composition as a titanium compound or in an ionized state or in a complex state interacting with the EVOH resin or other ligands.

[0100] The average particle size of the titanium compound (C) is usually 0.001 to 100 μm, preferably 0.01 to 50 μm, and more preferably 0.015 to 20 μm. When the average particle size of the titanium compound is within the above range, thermal stability tends to be further improved.

[0101] The metal conversion content of the above-mentioned titanium compound (C) is greater than 0.001ppm and less than 5ppm relative to the mass of the EVOH resin composition. It is preferably 0.01 to 3ppm, more preferably 0.03 to 1ppm, and particularly preferably 0.05 to 0.5ppm. By making the content of the titanium compound (C) within the above range, thermal degradation during melt molding can be suppressed, and long-term operation performance is excellent. In addition, if the content of the titanium compound (C) is too little, the effect of suppressing thermal degradation is reduced. If the content is too much, thermal decomposition of the EVOH resin is likely to occur, and it is easy to color.

[0102] The metal conversion content of the above-mentioned titanium compound (C) can be quantified by the following operation: weigh the EVOH resin composition into a platinum crucible, incinerate it using a burner and an electric furnace in sequence, heat and decompose the ash with nitric acid and hydrofluoric acid, treat it with a mixed acid of dilute nitric acid and dilute hydrofluoric acid and make it constant, and use an ICP mass spectrometer (manufactured by Agilent Technologies, Agilent 8800) to determine the titanium in the obtained constant solution by ICP mass spectrometry.

[0103] The mass ratio of the content of the metal compound (B1) belonging to the specific period d-block to the metal equivalent content of the titanium compound (C) is usually 0.4 to 700,000, preferably 10 to 150,000, particularly preferably 50 to 55,000.

[0104] The mass ratio of the metal conversion content of the metal compound (B1) belonging to the specific period d zone to the metal conversion content of the titanium compound (C) is preferably 0.03 to 50,000, more preferably 1 to 10,000, particularly preferably 6 to 4,000, further preferably 10 to 1,000, and particularly preferably 15 to 500.

[0105] If the mass ratio is within the above range, there is a tendency to further suppress the color change due to thermal degradation. In addition, if the mass ratio is too large, there is a tendency to hinder thermal stability, and if it is too small, the molded product tends to be colored.

[0106] Here, it is generally known that EVOH resin deteriorates due to heat. It is believed that this is because the EVOH resin deteriorates due to heat and generates free radicals, and the hydroxyl groups possessed by the EVOH resin undergo a dehydration reaction due to the free radicals, thereby generating a double bond structure in the main chain of the EVOH resin. In addition, this site becomes a reaction starting point, and further dehydration reactions occur, forming a polyene structure in the main chain of the EVOH resin.

[0107] Furthermore, generally, when a titanium compound is contained in an EVOH resin composition, it is considered that the EVOH resin composition is colored by titanium ions. Therefore, it is common technical knowledge for those skilled in the art to avoid using titanium compounds.

[0108] However, the present invention goes against such common technical knowledge and finds that when a metal compound (B1) belonging to a specific period d-block is used in combination with a specific trace amount of a titanium compound (C), an EVOH resin composition with significantly suppressed thermal degradation can be obtained.

[0109] That is, it is speculated that titanium is stable as a tetravalent ion, and even a trace amount thereof will coordinate to the double bonds of the main chain of the EVOH resin as described above, forming a chelate or the like to stabilize, thereby further suppressing the formation of a polyene structure. In addition, it is speculated that the coexistence of the metal compound (B1) belonging to the specific period d region and the titanium compound (C) can more effectively exert the stabilizing effect based on the titanium compound (C).

[0110] On the other hand, if the content of the titanium compound (C) is too large, it is considered that thermal decomposition of the EVOH resin occurs due to the titanium compound (C). Therefore, in the present invention, the content of the titanium compound (C) is limited to a specific trace amount.

[0111] [Other thermoplastic resins]

[0112] The present EVOH resin composition may contain a thermoplastic resin other than the EVOH resin (A) within a range that does not inhibit the effects of the present invention (e.g., usually 30% by mass or less, preferably 20% by mass or less, particularly preferably 10% by mass or less of the present EVOH resin composition).

[0113] As other thermoplastic resins, known thermoplastic resins can be used, for example, polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, ionomers, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more.

[0114] [Other compounding ingredients]

[0115] In addition, the EVOH resin composition may contain a compounding agent generally used in EVOH resin within a range that does not hinder the effect of the present invention. As the above-mentioned compounding agent, for example, inorganic complex salts (such as hydrotalcite), plasticizers (such as aliphatic polyols such as ethylene glycol, glycerol, hexylene glycol, etc.), oxygen absorbers [such as inorganic oxygen absorbers such as aluminum powder and potassium sulfite; ascorbic acid, and its fatty acid esters, metal salts, etc., gallic acid, polyphenols such as phenolic resin containing hydroxyl groups, terpene compounds, blends of resins containing tertiary hydrogen and transition metals (such as a combination of polypropylene and cobalt), blends of resins containing carbon-carbon unsaturated bonds and transition metals (such as polypropylene and cobalt), etc.] can be added. Combination of butadiene and cobalt), photo-oxidative degradable resins (e.g., polyketone), anthraquinone polymers (e.g., polyvinyl anthraquinone), etc., and polymeric oxygen absorbers obtained by adding photoinitiators (e.g., benzophenone), antioxidants other than the above, deodorants (e.g., activated carbon), etc. to these complexes], heat stabilizers, light stabilizers, ultraviolet absorbers, colorants, antistatic agents, surfactants (excluding those used as lubricants), antibacterial agents, anti-blocking agents, fillers (e.g., inorganic fillers), etc. These compounds can be used alone or in combination of two or more.

[0116] [Method for producing EVOH resin composition]

[0117] The present EVOH resin composition can be produced, for example, by mixing the above-mentioned EVOH resin (A), the metal compound (B1) belonging to the specific period d region and the titanium compound (C) by a known method such as dry blending, melt mixing, solution mixing, impregnation, etc. Among these, it is preferably produced by a process of melt mixing the composition raw materials containing the above-mentioned EVOH resin and the titanium compound. In addition, these production methods can also be arbitrarily combined.

[0118] Examples of the dry blending method include (i) a method of dry blending a pelletized EVOH resin (A), a metal compound (B1) belonging to a specific period d region, and a titanium compound (C) using a tumbler or the like.

[0119] As the above-mentioned melt mixing method, for example, there can be cited the following methods: (ii) dry blending a granular EVOH resin (A) and a metal compound (B1) and / or a titanium compound (C) belonging to a specific period d region, and melt-kneading the obtained dry blend to obtain granules and molded products; (iii) adding a metal compound (B1) and / or a titanium compound (C) belonging to a specific period d region to a molten EVOH resin (A) and melt-kneading the mixture to obtain granules and molded products, etc.

[0120] As the above-mentioned solution mixing method, for example, there can be cited the following method: (iv) a solution is prepared using a granular EVOH resin (A), a metal compound (B1) and / or a titanium compound (C) belonging to a specific period d zone is added thereto, the solution is solidified and granulated, and then the solid-liquid separation and drying are carried out by a known method; (v) in the manufacturing process of the EVOH resin (A), a uniform solution of the EVOH resin before saponification (water / alcohol solution, etc.) is made to contain a metal compound (B1) and / or a titanium compound (C) belonging to a specific period d zone, the solution is solidified and granulated, and then the solid-liquid separation and drying are carried out by a known method, etc.

[0121] As the above-mentioned impregnation method, for example, there can be cited a method of (vi) contacting a granular EVOH resin (A) with an aqueous solution containing a metal compound (B1) and / or a titanium compound (C) belonging to a specific period d region, so that the EVOH resin (A) contains the above-mentioned metal compound (B1) and / or titanium compound (C) belonging to the specific period d region, and then drying the mixture.

[0122] As the aqueous solution containing the titanium compound (C), an aqueous solution of the titanium compound (C) or an aqueous solution obtained by immersing the titanium compound (C) in water containing various chemicals to dissolve titanium ions can be used. The same applies to the aqueous solution containing the metal compound (B1) belonging to the period d block.

[0123] It should be noted that in the above-mentioned impregnation method, the content (metal conversion) of the metal compound (B1) and the titanium compound (C) belonging to the specific period d zone can be controlled by the concentration of the metal compound (B1) and the titanium compound (C) belonging to the specific period d zone in the aqueous solution in which the EVOH resin (A) is impregnated, the impregnation temperature, the impregnation time, etc.

[0124] Regarding the immersion temperature and immersion time, the immersion time is usually 0.5 to 48 hours, preferably 1 to 36 hours, and the immersion temperature is usually 10 to 40°C, preferably 20 to 35°C.

[0125] In addition, various drying methods can be used as the drying method in each of the above-mentioned production methods, and any of static drying and fluidized drying can be used. In addition, these methods can also be combined.

[0126] In order to obtain the present EVOH resin composition, as described above, these various methods can be combined. Among them, from the perspective of productivity and obtaining a resin composition with a more significant effect of the present invention, the melt mixing method is preferred, and the method (ii) is particularly preferred. In addition, when using the above-mentioned other thermoplastic resins and other compounding agents, they can be compounded by conventional methods according to the above-mentioned manufacturing method.

[0127] The EVOH resin composition obtained in this manner may be in any shape, but is preferably in the form of pellets.

[0128] As the above-mentioned particles, for example, there are spherical, elliptical, cylindrical, cubic, rectangular parallelepiped, etc., but they are usually elliptical or cylindrical. Regarding their size, from the perspective of convenience when used as a molding material later, in the case of an elliptical shape, the short diameter is usually 1 to 10 mm, preferably 2 to 6 mm, and more preferably 2.5 to 5.5 mm, and the long diameter is usually 1.5 to 30 mm, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm. In addition, in the case of a cylindrical shape, the diameter of the bottom surface is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm.

[0129] In addition, it is preferable that the shape and size of the pelletized EVOH resin (A) used in each of the above-mentioned production methods are also the same.

[0130] It should be noted that when the EVOH resin composition is in the form of pellets, it is preferred to attach a known lubricant to the surface of the pellets from the perspective of stabilizing the feeding property during melt molding. Examples of the lubricant include higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters, etc. of higher fatty acids), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, behenic acid amide; unsaturated higher fatty acid amides such as oleic acid amide, erucic acid amide, bis-higher fatty acid amides such as ethylene bisstearic acid amide, ethylene bisoleic acid amide, ethylene biserucic acid amide, ethylene bislauric acid amide, etc.), low molecular weight polyolefins (e.g., low molecular weight polyethylene or low molecular weight polypropylene having a molecular weight of about 500 to 10,000, or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, fluorinated vinyl resins, etc. These compounds can be used alone or in combination of two or more. In addition, the content of the lubricant is usually 5% by mass or less, preferably 1% by mass or less of the EVOH resin composition. It should be noted that the lower limit is usually 0% by mass.

[0131] The EVOH resin composition is suppressed from thermal degradation during melt molding, and the weight loss rate of the EVOH resin composition is usually less than 1.2%, preferably less than 1.1%, and particularly preferably less than 1.0%. The lower limit of the weight loss rate is preferably as low as possible.

[0132] In addition, since the difference of 0.1% in the weight reduction rate shows a significant difference in yield in actual production, the difference is very large.

[0133] The above-mentioned weight reduction rate is obtained by measuring the weight of 5 mg of pellets of the present EVOH resin composition using a thermogravimetric measuring apparatus (Pyris 1TGA manufactured by PerkinElmer) under nitrogen atmosphere at an air flow rate of 20 mL / min, a temperature of 230° C., and a time of 1 hour, and using the following formula.

[0134] <Formula>

[0135] Weight reduction rate (%) = [(weight before heating - weight after heating) / weight before heating] × 100

[0136] The water content of the present EVOH resin composition is usually 0.01 to 0.5% by mass, preferably 0.05 to 0.35% by mass, and particularly preferably 0.1 to 0.3% by mass.

[0137] The water content of the present EVOH resin composition is measured and calculated by the following method.

[0138] The mass (W1) of the EVOH resin composition before drying was measured using an electronic balance, dried in a hot air dryer at 150°C for 5 hours, cooled in the dryer for 30 minutes, and then the mass (W2) was measured and calculated using the following formula.

[0139] <Formula>

[0140] Water content (mass %) = [(W1-W2) / W1] × 100

[0141] The EVOH resin composition can be prepared into various forms such as powder and liquid in addition to pellets, and provided as a molding material for various molded objects. In particular, in the present invention, it is preferably provided as a material for melt molding, which tends to more effectively obtain the effects of the present invention.

[0142] In addition, the present EVOH resin composition also includes a resin composition obtained by mixing a resin other than the EVOH resin (A) used in the present EVOH resin composition.

[0143] Examples of the molded product include a single-layer film molded from the present EVOH resin composition, and a multilayer structure having a layer composed of the present EVOH resin composition.

[0144] [Multilayer structure]

[0145] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the present multilayer structure") comprises a layer composed of the present EVOH resin composition. The layer composed of the present EVOH resin composition (hereinafter referred to as "the present EVOH resin composition layer") can be further provided with strength, or the present EVOH resin composition layer can be protected from the influence of moisture, etc., or other functions can be provided by laminating it with another substrate having a thermoplastic resin other than the present EVOH resin composition as a main component (hereinafter, the resin used in the substrate is sometimes referred to as "substrate resin").

[0146] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers, ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polybutene, polypentene, (unmodified) polyolefin resins including polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and these polyolefin resins. The polyolefin resins in a broad sense of modified olefin resins such as unsaturated carboxylic acid-modified polyolefin resins obtained by adhesively grafting hydrocarbons with unsaturated carboxylic acids or their esters, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, chlorinated polyethylene, chlorinated polypropylene and other halogenated polyolefins, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.

[0147] Among these, polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred as the hydrophobic resin, and polyethylene resins, polypropylene resins, polycyclic olefin resins, and polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins thereof are more preferred. It is particularly preferred to use polycyclic olefin resins as the hydrophobic resin.

[0148] When the EVOH resin composition layer is a (a1, a2, ...) and the substrate resin layer is b (b1, b2, ...), the layer structure of the multilayer structure may be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc. In addition, when the recycled layer including a mixture of the EVOH resin composition and a thermoplastic resin other than the EVOH resin composition obtained by remelting and molding the end portions, defective products, etc. generated in the process of manufacturing the multilayer structure is R, it may be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The number of layers of the multilayer structure is usually 2 to 15 in total, preferably 3 to 10. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be interposed between the layers as necessary.

[0149] As the above-mentioned adhesive resin, a known resin can be used, as long as it is appropriately selected according to the type of thermoplastic resin used in the substrate resin layer "b". Representative examples include modified polyolefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to polyolefin resins using addition reactions, grafting reactions, etc. As the above-mentioned modified polyolefin polymers containing carboxyl groups, for example, maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block and random) copolymers, maleic anhydride grafted modified ethylene-ethyl acrylate copolymers, maleic anhydride grafted modified ethylene-vinyl acetate copolymers, maleic anhydride modified polycyclic olefin resins, maleic anhydride grafted modified polyolefin resins, etc. can be cited. They can be used alone or in combination of two or more.

[0150] In the present multilayer structure, when an adhesive resin layer is used between the present EVOH resin composition layer and the base resin layer, since the adhesive resin layer is located on both sides of the present EVOH resin composition layer, an adhesive resin having excellent hydrophobicity is preferably used.

[0151] The above-mentioned base resin and adhesive resin may also contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, nucleating agents, antiblocking agents, waxes, etc. within a range that does not hinder the purpose of the present invention (for example, 30% by mass or less, preferably 10% by mass or less relative to the entire resin). These may be used alone or in combination of two or more.

[0152] The lamination of the above-mentioned EVOH resin composition layer and the above-mentioned substrate resin layer (including the case where an adhesive resin layer is interposed) can be carried out by a known method. For example, there can be cited a method of melt-extrusion lamination of the substrate resin on a film, sheet, etc. of the present EVOH resin composition; a method of melt-extrusion lamination of the present EVOH resin composition on a substrate resin layer; a method of co-extruding the present EVOH resin composition and the substrate resin; a method of dry lamination of the present EVOH resin composition (layer) and the substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc.; a method of removing the solvent after applying a solution of the present EVOH resin composition on the substrate resin, etc. Among these, from the viewpoint of cost and environment, it is preferred to manufacture by a process of melt-molding the present EVOH resin composition layer, and specifically, a co-extrusion method is preferred.

[0153] The present multilayer structure may also be subjected to (heating) stretching treatment as required. The stretching treatment may be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, it may be simultaneous stretching or sequential stretching. In addition, as a stretching method, a stretching method with a high stretching ratio such as a roller stretching method, a tentering stretching method, a tubular stretching method, a stretch blow molding method, and a vacuum pressure molding method may be adopted. The stretching temperature is a temperature near the melting point of the multilayer structure, usually selected from the range of 40 to 170°C, preferably about 60 to 160°C. When the stretching temperature is too low, the stretchability becomes poor, and when it is too high, it is difficult to maintain a stable stretched state.

[0154] In addition, for the purpose of imparting dimensional stability, the stretched multilayer structure may be heat-fixed. Heat-fixing may be performed by a known method, for example, by heat-treating the stretched multilayer structure at a temperature of usually 80 to 180° C., preferably 100 to 165° C., for usually 2 to 600 seconds while maintaining the stretched multilayer structure in a tensioned state.

[0155] When the stretched multilayer structure is used as a shrink film, in order to impart heat shrinkage, the stretched multilayer structure may be cooled and fixed by blowing cold air instead of the heat setting.

[0156] The thickness of the present multilayer structure (including the stretched multilayer structure), and the thickness of the present EVOH resin composition layer, the base resin layer and the adhesive resin layer constituting the multilayer structure vary depending on the layer constitution, the type of base resin, the type of adhesive resin, the application, the packaging form, the required physical properties, etc., and cannot be generalized. The thickness of the present multilayer structure (including the stretched multilayer structure) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0157] Furthermore, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the substrate resin layer in the present multilayer structure (present EVOH resin composition layer / substrate resin layer) is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60, as a ratio of the thickest layers. In addition, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the adhesive resin layer in the present multilayer structure (present EVOH resin composition layer / adhesive resin layer) is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10, as a ratio of the thickest layers.

[0158] In addition, the present multilayer structure can also be used to obtain a cup or tray-shaped multilayer container. In this case, a deep drawing method is usually used, and specifically, vacuum forming, pressure forming, vacuum pressure forming, plunger-assisted vacuum pressure forming, etc. can be cited. Furthermore, when a tubular or bottle-shaped multilayer container (laminated structure) is obtained from a multilayer parison (a hollow tubular preform before blow molding), a blow molding method can be used. Specifically, extrusion blow molding (double-head type, mold moving type, parison moving type, rotary type, accumulation type, horizontal parison type, etc.), cold parison blow molding, injection blow molding, biaxial stretch blow molding (extrusion cold parison biaxial stretch blow molding, injection cold parison biaxial stretch blow molding, injection molding embedded biaxial stretch blow molding, etc.) can be cited. The obtained laminate can be subjected to heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making processing, deep drawing processing, box processing, tube processing, slitting processing, etc. as needed.

[0159] The single-layer film formed from the present EVOH resin composition, the bag composed of the present multilayer structure, and the container and cover materials composed of cups, trays, tubes, bottles, etc. are useful as various packaging materials for not only general foods but also seasonings such as mayonnaise and sauces, fermented foods such as miso, oily foods such as salad oils, beverages, cosmetics, and pharmaceuticals.

[0160] <<Method 2>>

[0161] EVOH resin has excellent transparency, oxygen and other gas barrier properties, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and is formed into films, sheets, bottles, etc., and is widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial drug packaging materials, and pesticide packaging materials. Moreover, such sheet-shaped and film-shaped packaging materials can be made from the above-mentioned EVOH resin alone, but in order to impart water resistance, strength, and other functions, they are usually used in the form of a multilayer structure of a polyolefin resin or the like laminated via an adhesive layer.

[0162] In addition, scraps, unwanted parts such as ends, defective products, or waste such as garbage after the molded products are used for various purposes, which are produced after the above-mentioned multilayer structure is manufactured into molded products such as containers, are sometimes recovered and melt-molded, and the recovered products are reused in the form of a recycled layer (hereinafter sometimes referred to as a "regrinding layer") for at least one layer of the multilayer structure. When such recycled products are used, it is sought to prevent discoloration of the molded products and suppress the occurrence of accumulation of decomposition products from EVOH resin and to have an excellent appearance of the molded products.

[0163] In order to improve the above-mentioned appearance defects, a resin composition obtained by blending a higher fatty acid metal salt and hydrotalcite with a composition of a saponified ethylene-vinyl acetate copolymer and a thermoplastic resin such as a polyolefin resin has been proposed (see Patent Document 1).

[0164] Patent Document 1: Japanese Patent Application Laid-Open No. 8-311254

[0165] Although the resin composition disclosed in the above-mentioned patent document 1 improves the appearance defect to some extent, it has a tendency to be easily thermally deteriorated when heated during melt kneading, melt molding, etc., so improvement of long-term operation performance is sought. In addition, it is also sought to further improve the quality of the molded product when the molded product is recycled and reused.

[0166] An object of the present invention is to provide an EVOH resin composition in which thermal degradation of the EVOH resin during heating such as melt molding is suppressed, long-term operating properties are excellent, and the composition is suitable for recycling.

[0167] In view of the above circumstances, the present inventors have found that by adding a polyolefin resin and a specific trace amount of a titanium compound to an EVOH resin, an EVOH resin composition can be obtained in which thermal degradation of the EVOH resin is suppressed during heating such as melt molding.

[0168] That is, the present invention has the following aspects.

[0169] [2-1] An EVOH resin composition comprising an EVOH resin (A), a polyolefin resin (B2) and a titanium compound (C),

[0170] The metal-equivalent content of the titanium compound (C) is 0.00005 ppm or more and less than 0.5 ppm based on the mass of the EVOH resin composition.

[0171] [2-2] The EVOH resin composition according to [2-1], wherein the mass content ratio (A) / (B2) of the EVOH resin (A) to the polyolefin resin (B2) is 1 / 99 to 99 / 1.

[0172] [2-3] The EVOH resin composition according to [2-1] or [2-2], wherein the metal-equivalent content of the titanium compound (C) is 0.001 to 3 ppm relative to the total mass of the EVOH resin (A) and the titanium compound (C).

[0173] [2-4] The EVOH resin composition according to any one of [2-1] to [2-3], wherein the polyolefin resin (B2) has a density of 0.89 g / cm 3 The above polyolefin resins.

[0174] [2-5] The EVOH resin composition according to [2-4], wherein the polyolefin-based resin (B2) is polypropylene.

[0175] [2-6] A multilayer structure comprising at least one layer comprising the EVOH resin composition according to any one of [2-1] to [2-5].

[0176] [2-7] A method for producing an EVOH resin composition, which is the method for producing the EVOH resin composition according to any one of [2-1] to [2-5], comprising the step of melt-mixing a composition raw material containing the EVOH resin and a titanium compound.

[0177] [2-8] A method for producing a multilayer structure, which is the method for producing the multilayer structure of [2-6], comprising the step of melt-molding a layer composed of the above-mentioned EVOH resin composition.

[0178] The EVOH resin composition of the present invention has excellent thermal stability, and thus can suppress the thermal deterioration of the EVOH resin during heating such as during melt-kneading and melt-molding. In particular, an EVOH resin composition containing a polyolefin resin (B2) having a relatively high density and excellent mechanical strength can obtain a molded article of particularly high quality, and is thus preferred.

[0179] In addition, the thermal deterioration of the EVOH resin during heating such as during melt-kneading and melt-molding of a multilayer structure having a layer composed of the resin composition of the present invention is suppressed, and thus it can be suitably used as various molded articles, for example, packaging materials for foods, pharmaceuticals, agricultural chemicals, etc. Moreover, in the case of obtaining a molded article on the premise of reuse or in the case of obtaining a molded article that requires relatively high mechanical strength, a higher-quality molded article can be provided, and is thus preferred.

[0180] Hereinafter, the present invention will be described in more detail based on examples of embodiments of the present invention, but the present invention is not limited to these embodiments.

[0181] <EVOH resin composition>

[0182] An EVOH resin composition (hereinafter referred to as "this EVOH resin composition") according to an embodiment of the present invention contains an EVOH resin (A), a specific polyolefin resin (B2), and a specific trace amount of a titanium compound (C).

[0183] Hereinafter, each component will be described.

[0184] [EVOH resin (A)]

[0185] The EVOH resin (A) used in the present invention is usually a resin obtained by saponifying an ethylene-vinyl ester copolymer which is a copolymer of ethylene and a vinyl ester monomer, and the same resin as the (A) component described in the above first mode can be used.

[0186] [Polyolefin resin (B2)]

[0187] The polyolefin resin (B2) used in the present invention is not particularly limited, and examples thereof include linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), ultra-low-density polyethylene (VLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), ionomers, ethylene-propylene (block or random) copolymers, ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, polypropylene (PP), propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, homopolymers or copolymers of olefins such as polybutene, polypentene, and polymethylpentene, or polyolefin resins obtained by grafting these homopolymers or copolymers of olefins with unsaturated carboxylic acids or esters thereof. These resins may be used alone or in combination of two or more, and polypropylene (PP), polyethylene (MDPE, HDPE), and blends thereof are preferred from the viewpoint of obtaining a molded product having excellent mechanical strength. In particular, polypropylene is most preferred from the viewpoint of effect.

[0188] The density of the polyolefin resin (B2) used in the present invention is usually 0.89 g / cm 3 Above, preferably 0.90 g / cm 3 Above and less than 0.98g / cm 3 For example, when a molded article obtained using the present EVOH resin composition is recycled, it is sometimes used to enhance the mechanical strength of the EVOH resin composition. When such an application is sought, in order to produce a resin composition with excellent mechanical strength at a higher density, it is preferred to use a polyolefin-based resin (B2) with a higher density.

[0189] In the present EVOH resin composition, the mass content ratio (A) / (B2) of the EVOH resin (A) relative to the polyolefin resin (B2) is preferably 1 / 99 to 99 / 1, more preferably 2 / 98 to 75 / 25, further preferably 3 / 97 to 50 / 50, particularly preferably 4 / 96 to 25 / 75, and particularly preferably 5 / 95 to 10 / 90. If the mass content ratio of the EVOH resin (A) to the olefin polymer (B2) is within the above range, the thermal degradation inhibition effect is more excellent.

[0190] In addition, in the present EVOH resin composition, the total content of the EVOH resin (A) and the polyolefin resin (B2) is usually 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more. It should be noted that the upper limit of the total content of the EVOH resin (A) and the polyolefin resin (B2) is the total mass obtained by removing the titanium compound (C) from the resin composition.

[0191] [Titanium compound (C)]

[0192] Examples of the titanium compound (C) used in the present invention include inorganic titanium compounds and organic titanium compounds. As the titanium compound, the same titanium compound as the component (C) described in the first embodiment can be used.

[0193] The metal conversion content of the above-mentioned titanium compound (C) is greater than 0.00005ppm and less than 0.5ppm relative to the mass of the EVOH resin composition. It is preferably 0.0005-0.3ppm, more preferably 0.0015-0.2ppm, and particularly preferably 0.005-0.1ppm. By making the content of the titanium compound (C) within the above range, thermal degradation during melt molding can be suppressed, and long-term operation performance is excellent. In addition, if the content of the titanium compound (C) is too little, the effect of suppressing thermal degradation is reduced. If the content is too much, thermal decomposition of the EVOH resin (A) is likely to occur, and it is easy to color.

[0194] The metal conversion content of the above-mentioned titanium compound (C) can be quantified by the following operation: weigh the EVOH resin composition into a platinum crucible, incinerate it using a burner and an electric furnace in sequence, heat and decompose the ash with nitric acid and hydrofluoric acid, treat it with a mixed acid of dilute nitric acid and dilute hydrofluoric acid and fix the volume, and use an ICP mass spectrometer (manufactured by Agilent Technologies, Agilent 8800) to determine the titanium in the obtained fixed volume solution by ICP mass spectrometry.

[0195] The metal equivalent content of the titanium compound (C) is preferably 0.001 to 3 ppm, more preferably 0.03 to 1 ppm, and particularly preferably 0.05 to 0.5 ppm, based on the total mass of the EVOH resin (A) and the titanium compound (C).

[0196] If the content of the titanium compound (C) is too small, the effect of suppressing thermal degradation decreases, while if the content is too large, thermal decomposition of the EVOH resin (A) tends to occur, and coloration tends to occur.

[0197] It is generally known that EVOH resin deteriorates due to heat. The mechanism is not clear, but it is believed that thermal degradation proceeds because a double bond structure is generated in the main chain of the EVOH resin during the above reaction, and this site becomes the starting point of the reaction, and further dehydration reaction occurs to form a polyene structure in the main chain of the EVOH resin.

[0198] On the other hand, when a titanium compound is contained in an EVOH resin composition, it is considered that the EVOH resin composition is colored by titanium ions, and therefore it is common technical knowledge for those skilled in the art to avoid using the titanium compound.

[0199] However, the present invention goes against such common technical knowledge and finds that when a polyolefin-based resin (B2) is used in combination with a specific trace amount of a titanium compound (C), an EVOH resin composition in which thermal degradation is significantly suppressed can be obtained.

[0200] That is, it is speculated that titanium is stable as a tetravalent ion, and even a trace amount thereof will coordinate to the double bonds of the main chain of the EVOH resin as described above, forming a chelate or the like to stabilize, thereby further suppressing the formation of a polyene structure. In addition, it is speculated that due to the coexistence of the polyolefin resin and the titanium compound, since a plurality of double bond sites are distributed in the resin composition, the formation of double bonds is further suppressed, and the thermal stability is further improved.

[0201] On the other hand, if the content of the titanium compound (C) is too large, it is considered that thermal decomposition of the EVOH resin occurs due to the titanium compound (C). Therefore, in the present invention, the content of the titanium compound (C) is limited to a specific trace amount.

[0202] [Other thermoplastic resins]

[0203] The present EVOH resin composition may contain, in addition to the EVOH resin (A) and the polyolefin resin (B2), other thermoplastic resins as resin components within a range that does not hinder the effects of the present invention (e.g., usually 30% by mass or less, preferably 20% by mass or less, and particularly preferably 10% by mass or less of the present EVOH resin composition).

[0204] As other thermoplastic resins, known thermoplastic resins can be used, for example, polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more.

[0205] [Other compounding ingredients]

[0206] The EVOH resin composition may contain a compounding agent generally compounded with EVOH resin within a range that does not inhibit the effects of the present invention. As the compounding agent, the same compounding agent as described in the first embodiment can be used.

[0207] [Method for producing EVOH resin composition]

[0208] The present EVOH resin composition can be manufactured using the above-mentioned essential components, i.e., EVOH resin (A), polyolefin resin (B2) and titanium compound (C), and the above-mentioned optional components as required. As a manufacturing method, for example, known methods such as dry blending method, melt mixing method, solution mixing method, impregnation method, etc. can be cited. Among these, it is preferably manufactured by a process of melt mixing the composition raw materials containing the above-mentioned EVOH resin and titanium compound. In addition, these manufacturing methods can also be arbitrarily combined.

[0209] Examples of the dry blending method include (I) a method of dry blending EVOH resin (A) pellets, a polyolefin resin (B2) and a titanium compound (C) using a tumbler or the like.

[0210] As the above-mentioned melt mixing method, for example, there can be cited (II) a method in which EVOH resin (A) particles are melt-kneaded with a dry blend of a polyolefin-based resin (B2) and a titanium compound (C) to obtain particles or other molded products; (III) a method in which a polyolefin-based resin (B2) and a titanium compound (C) are added to a molten EVOH resin (A) and the mixture is melt-kneaded to obtain particles or other molded products.

[0211] As the above-mentioned solution mixing method, for example, there can be cited the method of (IV) using EVOH resin (A) particles to prepare a solution, adding a polyolefin-based resin (B2) and / or a titanium compound (C) thereto, coagulating and forming a solution, granulating the solution, and performing solid-liquid separation and drying; (V) in the manufacturing process of EVOH resin (A), a method in which an ethylene-vinyl ester copolymer solution before saponification or a uniform solution (water / alcohol solution, etc.) of EVOH resin (A) after saponification is made to contain a polyolefin-based resin (B2) and / or a titanium compound (C), coagulating and forming the solution, granulating the solution, and performing solid-liquid separation and drying; etc.

[0212] As the above-mentioned impregnation method, for example, there can be cited a method (VI) of contacting EVOH resin (A) particles with an aqueous solution containing a polyolefin-based resin (B2) and / or a titanium compound (C), impregnating the polyolefin-based resin (B2) and / or the titanium compound (C) into the above-mentioned EVOH resin (A) particles and then drying the particles.

[0213] In addition, in each of the above methods, EVOH resin (A) and / or polyolefin resin (B2) and titanium compound (C) may be pre-blended in a specified ratio to prepare a composition (masterbatch) having a high concentration of titanium compound (C), and the composition (masterbatch) may be blended with EVOH resin (A) or polyolefin resin (B2) to obtain a resin composition of the desired concentration.

[0214] Furthermore, in the present invention, the above-mentioned different methods may be combined. Among them, from the viewpoint of productivity and obtaining a resin composition having a more remarkable effect of the present invention, the melt mixing method is preferred, and the method (II) is particularly preferred.

[0215] It should be noted that the shape of the pellets of the resin composition obtained by the above methods and the pellets containing the EVOH resin (A) and / or the polyamide resin (B2) used in the above methods is arbitrary, and any shape such as spherical, elliptical, cylindrical, cubic, and rectangular can be adopted. The shape of the pellets is usually elliptical or cylindrical. Regarding the size, in the case of a cylindrical shape, the diameter of the bottom surface is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm, from the viewpoint of convenience when used as a molding material later. In the case of an elliptical shape, the major diameter is usually 1.5 to 30 mm, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm, and the minor diameter is usually 1 to 10 mm, preferably 2 to 6 mm, and particularly preferably 2.5 to 5.5 mm. The method for measuring the major axis and the minor axis is, for example, as follows: observe the particle in hand, measure the major axis using a measuring instrument such as a vernier caliper, determine the position of the cross section with the largest area in the cross section perpendicular to the major axis by visual inspection and touch, and similarly measure the minor axis when assuming the cross section.

[0216] It should be noted that when the EVOH resin composition is in the form of pellets, it is preferred to attach a known lubricant to the surface of the pellets from the perspective of stabilizing the feeding property during melt molding. Examples of the lubricant include higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters of higher fatty acids, etc.), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, behenic acid amide; unsaturated higher fatty acid amides such as oleic acid amide, erucic acid amide, bis-higher fatty acid amides such as ethylene bisstearic acid amide, ethylene bisoleic acid amide, ethylene biserucic acid amide, ethylene bislauric acid amide, etc.), low molecular weight polyolefins (e.g., low molecular weight polyethylene or low molecular weight polypropylene having a molecular weight of about 500 to 10,000, or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, fluorinated vinyl resins, etc. These compounds can be used alone or in combination of two or more. In addition, the content of the lubricant is usually 5% by mass or less, preferably 1% by mass or less of the EVOH resin composition. It should be noted that the lower limit is usually 0% by mass.

[0217] The EVOH resin composition thus obtained can suppress thermal degradation during heating, and the weight loss rate of the EVOH resin composition is usually 1.8% or less, preferably 1.6% or less, and particularly preferably 1.5% or less. The lower limit of the weight loss rate is preferably as low as possible.

[0218] In addition, since the difference of 0.1% in the weight reduction rate shows a significant difference in yield in actual production, the difference is very large.

[0219] The above-mentioned weight reduction rate is obtained by measuring the weight of 5 mg of pellets of the present EVOH resin composition using a thermogravimetric measuring apparatus (Pyris 1TGA manufactured by PerkinElmer) under nitrogen atmosphere at an air flow rate of 20 mL / min, a temperature of 230° C., and a time of 1 hour, and using the following formula.

[0220] <Formula>

[0221] Weight reduction rate (%) = [(weight before heating - weight after heating) / weight before heating] × 100

[0222] The water content of the present EVOH resin composition is usually 0.01 to 0.5% by mass, preferably 0.05 to 0.35% by mass, and particularly preferably 0.1 to 0.3% by mass.

[0223] The water content of the present EVOH resin composition is measured and calculated by the following method.

[0224] The mass (W1) of the EVOH resin composition before drying was measured using an electronic balance, dried in a hot air dryer at 150°C for 5 hours, cooled in the dryer for 30 minutes, and then the mass (W2) was measured and calculated using the following formula.

[0225] <Formula>

[0226] Water content (mass %) = [(W1-W2) / W1] × 100

[0227] The EVOH resin composition can be prepared into various forms such as powder and liquid in addition to pellets, and provided as a molding material for various molded objects. In particular, in the present invention, when provided as a material for melt molding, there is a tendency to more effectively obtain the effect of the present invention, so it is preferred.

[0228] The present EVOH resin composition also includes a resin composition obtained by mixing the EVOH resin (A) used in the present EVOH resin composition with a resin other than the polyamide-based resin (B2).

[0229] Examples of the molded product include a single-layer film molded from the present EVOH resin composition, and a multilayer structure having a layer composed of the present EVOH resin composition.

[0230] [Multilayer structure]

[0231] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the present multilayer structure") comprises a layer composed of the present EVOH resin composition. The layer composed of the present EVOH resin composition (hereinafter referred to as "the present EVOH resin composition layer") can be further provided with strength, or the present EVOH resin composition layer can be protected from the influence of moisture, etc., or other functions can be provided by laminating it with another substrate having a thermoplastic resin other than the present EVOH resin composition as a main component (hereinafter, the resin used in the substrate is sometimes referred to as "substrate resin").

[0232] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers, ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polybutene, polypentene, (unmodified) polyolefin resins including polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and these polyolefin resins. The polyolefin resins in a broad sense of modified olefin resins such as unsaturated carboxylic acid-modified polyolefin resins obtained by adhesively grafting hydrocarbons with unsaturated carboxylic acids or their esters, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, chlorinated polyethylene, chlorinated polypropylene and other halogenated polyolefins, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.

[0233] Among these, polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred as the hydrophobic resin, and polyethylene resins, polypropylene resins, polycyclic olefin resins, and polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins thereof are more preferred. It is particularly preferred to use polycyclic olefin resins as the hydrophobic resin.

[0234] When the EVOH resin composition layer is a (a1, a2, ...) and the substrate resin layer is b (b1, b2, ...), the layer structure of the multilayer structure may be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc. In addition, when the recycled layer including a mixture of the EVOH resin composition and a thermoplastic resin other than the EVOH resin composition obtained by remelting and molding the end portions, defective products, etc. generated in the process of manufacturing the multilayer structure is R, it may be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The number of layers of the multilayer structure is usually 2 to 15 in total, preferably 3 to 10. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be interposed between the layers as necessary.

[0235] As the above-mentioned adhesive resin, a known resin can be used, as long as it is appropriately selected according to the type of thermoplastic resin used in the substrate resin layer "b". Representative examples include modified polyolefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to polyolefin resins using addition reactions, grafting reactions, etc. As the above-mentioned modified polyolefin polymers containing carboxyl groups, for example, maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block and random) copolymers, maleic anhydride grafted modified ethylene-ethyl acrylate copolymers, maleic anhydride grafted modified ethylene-vinyl acetate copolymers, maleic anhydride modified polycyclic olefin resins, maleic anhydride grafted modified polyolefin resins, etc. can be cited. They can be used alone or in combination of two or more.

[0236] In the present multilayer structure, when an adhesive resin layer is used between the present EVOH resin composition layer and the base resin layer, since the adhesive resin layer is located on both sides of the present EVOH resin composition layer, an adhesive resin having excellent hydrophobicity is preferably used.

[0237] The above-mentioned base resin and adhesive resin may also contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, nucleating agents, antiblocking agents, waxes, etc. within a range that does not hinder the purpose of the present invention (for example, 30% by mass or less, preferably 10% by mass or less relative to the entire resin). These may be used alone or in combination of two or more.

[0238] The lamination of the above-mentioned EVOH resin composition layer and the above-mentioned substrate resin layer (including the case where an adhesive resin layer is interposed) can be carried out by a known method. For example, there can be cited a method of melt-extrusion lamination of the substrate resin on a film, sheet, etc. of the present EVOH resin composition; a method of melt-extrusion lamination of the present EVOH resin composition on a substrate resin layer; a method of co-extruding the present EVOH resin composition and the substrate resin; a method of dry laminating the present EVOH resin composition (layer) and the substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc.; a method of removing the solvent after applying a solution of the present EVOH resin composition on the substrate resin, etc. Among these, from the viewpoint of cost and environment, it can be manufactured by a process of melt-molding the present EVOH resin composition layer, and specifically, the co-extrusion method is preferred.

[0239] The present multilayer structure may also be subjected to (heating) stretching treatment as required. The stretching treatment may be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, it may be simultaneous stretching or sequential stretching. In addition, as a stretching method, a stretching method with a high stretching ratio such as a roller stretching method, a tentering stretching method, a tubular stretching method, a stretch blow molding method, and a vacuum pressure molding method may be adopted. The stretching temperature is a temperature near the melting point of the multilayer structure, usually selected from the range of 40 to 170°C, preferably about 60 to 160°C. When the stretching temperature is too low, the stretchability becomes poor, and when it is too high, it is difficult to maintain a stable stretched state.

[0240] In addition, for the purpose of imparting dimensional stability, the stretched multilayer structure may be heat-fixed. Heat-fixing may be performed by a known method, for example, by heat-treating the stretched multilayer structure at a temperature of usually 80 to 180° C., preferably 100 to 165° C., for usually 2 to 600 seconds while maintaining the stretched multilayer structure in a tensioned state.

[0241] When the stretched multilayer structure is used as a shrink film, in order to impart heat shrinkage, the stretched multilayer structure may be cooled and fixed by blowing cold air instead of the heat setting.

[0242] The thickness of the present multilayer structure (including the stretched multilayer structure), and the thickness of the present EVOH resin composition layer, the base resin layer and the adhesive resin layer constituting the multilayer structure vary depending on the layer constitution, the type of base resin, the type of adhesive resin, the application, the packaging form, the required physical properties, etc., and cannot be generalized. The thickness of the present multilayer structure (including the stretched multilayer structure) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0243] Furthermore, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the substrate resin layer in the present multilayer structure (present EVOH resin composition layer / substrate resin layer) is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60, as a ratio of the thickest layers. In addition, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the adhesive resin layer in the present multilayer structure (present EVOH resin composition layer / adhesive resin layer) is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10, as a ratio of the thickest layers.

[0244] In addition, the present multilayer structure can also be used to obtain a cup or tray-shaped multilayer container. In this case, a deep drawing method is usually used, and specifically, vacuum forming, pressure forming, vacuum pressure forming, plunger-assisted vacuum pressure forming, etc. can be cited. Furthermore, when a tubular or bottle-shaped multilayer container (laminated structure) is obtained from a multilayer parison (a hollow tubular preform before blow molding), a blow molding method can be used. Specifically, extrusion blow molding (double-head type, mold moving type, parison moving type, rotary type, accumulation type, horizontal parison type, etc.), cold parison blow molding, injection blow molding, biaxial stretch blow molding (extrusion cold parison biaxial stretch blow molding, injection cold parison biaxial stretch blow molding, injection molding embedded biaxial stretch blow molding, etc.) can be cited. The obtained laminate can be subjected to heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making processing, deep drawing processing, box processing, tube processing, slitting processing, etc. as needed.

[0245] And, in addition, the bag consisting of the film, sheet, and stretch film obtained by using this multilayer structure and the container and cover material consisting of cup, tray, tube, bottle, etc. are useful as various packaging materials for general food, seasonings such as mayonnaise and sauce, fermented food such as miso, grease food such as salad oil, beverage, cosmetics, pharmaceuticals, etc. Particularly as this EVOH resin composition, the composition of the polyolefin resin (B2) having excellent mechanical strength is excellent in mechanical strength and the coloring due to thermal degradation is suppressed, therefore, it is particularly useful as a packaging material requiring high mechanical strength and beautiful appearance. In addition, even if it is repeatedly subjected to thermal history, thermal stability is also excellent, therefore, it is also useful as a packaging material with reuse as a prerequisite, etc.

[0246] <<Third Method>>

[0247] EVOH resin has excellent transparency, oxygen and other gas barrier properties, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and is molded into films, sheets, bottles, etc., and is widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and pesticide packaging materials. However, although EVOH has excellent gas barrier properties, it has a tendency to be brittle due to the high hydroxyl content in the molecular chain and high crystallinity, and has the disadvantage of insufficient flexibility.

[0248] Therefore, in applications requiring flexibility, such as packaging of liquids, EVOH is generally used by blending with a soft resin in order to impart flexibility to EVOH molded products.

[0249] For example, Patent Document 1 proposes a resin composition as a resin composition having flexibility and excellent molding stability such that pinholes are not generated even when subjected to repeated bending or exposure to deformation for a long period of time, such as a bag in a box, and the like. The resin composition is prepared by blending an olefin polymer (B3), a carboxylic acid-modified olefin polymer (C), and a hydrocarbon resin (D) having a number average molecular weight of 100 to 3000 and a softening point of 60° C. or higher and less than 170° C. into a saponified ethylene-vinyl ester copolymer (A) having an ethylene content of 20 to 60 mol%.

[0250] In addition, in Patent Document 2, for the purpose of providing a resin composition with excellent extrusion processing stability, it is proposed to use a resin composition containing an ethylene-vinyl alcohol copolymer (A), an unmodified ethylene-α-olefin copolymer (B3), an acid-modified ethylene-α-olefin copolymer (C) and an alkali metal salt (D) in a specific formulating ratio.

[0251] Patent Document 1: Japanese Patent Application Publication No. 2011-202147

[0252] Patent Document 2: International Publication No. 2015 / 141610

[0253] The resin compositions comprising EVOH and an olefin polymer disclosed in Patent Documents 1 and 2 are excellent in flexibility, but tend to be thermally degraded when heated during melt kneading, melt molding, etc., and improvement in long-term operability is sought.

[0254] An object of the present invention is to provide an EVOH resin composition which has flexibility and in which thermal degradation of the EVOH resin during heating such as melt molding is suppressed.

[0255] In view of the above circumstances, the present inventors have found that by adding a specific olefin polymer and a specific trace amount of a titanium compound to an EVOH resin, an EVOH resin composition can be obtained in which thermal degradation of the EVOH resin is suppressed during heating such as melt molding.

[0256] That is, the present invention has the following aspects.

[0257] [3-1] An EVOH resin composition comprising an EVOH resin (A), an olefin polymer (B3) and a titanium compound (C),

[0258] The olefin polymer (B3) is at least one selected from olefin thermoplastic elastomers, aliphatic rubbers and ionomers, and the metal conversion content of the titanium compound (C) is 0.0004 ppm or more and less than 4 ppm based on the mass of the EVOH resin composition.

[0259] [3-2] The EVOH resin composition according to [3-1], wherein the mass content ratio (A) / (B3) of the EVOH resin (A) to the olefin polymer (B3) is 1 / 99 to 99 / 1.

[0260] [3-3] The EVOH resin composition according to [3-1] or [3-2], wherein the metal-equivalent content of the titanium compound (C) is 0.01 to 3 ppm relative to the total mass of the EVOH resin (A) and the titanium compound (C).

[0261] [3-4] A melt molding material comprising the EVOH resin composition according to any one of [3-1] to [3-3].

[0262] [3-5] A multilayer structure comprising at least one layer comprising the EVOH resin composition according to any one of [3-1] to [3-3].

[0263] [3-6] A liquid packaging material, comprising the multilayer structure of [3-5].

[0264] [3-7]A method for producing an EVOH resin composition, which is a method for producing the EVOH resin composition described in any one of [3-1] to [3-3], includes a step of melt-mixing a composition raw material containing the above EVOH resin and a titanium compound.

[0265] [3-8]A method for producing a multilayer structure, which is a method for producing the multilayer structure of [3-5], includes a step of melt-molding a layer composed of the above EVOH resin composition.

[0266] The EVOH resin composition of the present invention has excellent thermal stability. Therefore, thermal degradation of the EVOH resin during heating such as during melt-kneading and melt-molding can be suppressed.

[0267] In addition, thermal degradation of the EVOH resin during heating such as during melt-kneading and melt-molding of the melt-kneading material composed of the resin composition of the present invention is suppressed. Therefore, it can be suitably used as a molding material for various molded articles obtained by melt-molding, such as packaging materials for foods, pharmaceuticals, pesticides, etc., especially liquid packaging materials.

[0268] Furthermore, thermal degradation of the EVOH resin during heating such as during melt-kneading and melt-molding of a multilayer structure having a layer composed of the resin composition of the present invention is suppressed. Therefore, it can be suitably used as various molded articles, such as packaging materials for foods, pharmaceuticals, pesticides, etc., especially liquid packaging materials.

[0269] Hereinafter, the present invention will be described in more detail based on embodiments of the present invention, but the present invention is not limited to these embodiments.

[0270] <EVOH resin composition>

[0271] The EVOH resin composition (hereinafter referred to as "this EVOH resin composition") according to an embodiment of the present invention contains an EVOH resin (A), a specific olefin-based polymer (B3), and a specific trace amount of a titanium compound (C).

[0272] Each component will be described below.

[0273] [EVOH resin (A)]

[0274] The EVOH resin (A) used in the present invention is usually a resin obtained by saponifying an ethylene-vinyl ester copolymer, which is a copolymer of ethylene and a vinyl ester-based monomer, and the same resin as the (A) component described in the above first mode can be used.

[0275] [Olefin-based polymer (B3)]

[0276] The olefin polymer (B3) used in the present invention refers to a polymer having an aliphatic hydrocarbon monomer olefin containing a carbon-carbon double bond as the main monomer, usually having a number average molecular weight of 10,000 or more, and a lipophilic polymer whose main chain is composed only of carbon bonds. Specifically, it is at least one selected from olefin thermoplastic elastomers, aliphatic rubbers, and ionomers.

[0277] The olefin polymer (B3) used in the present invention will be described in detail below.

[0278] The above-mentioned olefin-based thermoplastic elastomer is an elastomer resin showing thermoplasticity using polyolefin (polyethylene or polypropylene, etc.) as a hard segment and the above-mentioned aliphatic rubber (EPDM or EPM, etc.) as a soft segment, and examples thereof include resins synthesized by a method of compounding polyolefin and aliphatic rubber (compound type) or a method of introducing aliphatic rubber during olefin polymerization (reactor type). As the composite type, there are two types: a simple blend product (non-crosslinked type) and a dynamically crosslinked product (two types of fully crosslinked type or partially crosslinked type).

[0279] In addition, in the present invention, polyolefins with low density or low crystallinity that have certain flexibility even without rubber components are also included in the above-mentioned olefin-based thermoplastic resin elastomer. Such polyolefins include, for example, homopolymers of olefin monomers such as ethylene, propylene, and butene, random copolymers of two or more olefin monomers, and block copolymers. Among them, as olefin homopolymers, for example, polyethylene such as ultra-low density polyethylene, (straight-chain) low-density polyethylene, polypropylene, polybutene, polymethylpentene, etc. can be cited. As olefin block copolymers, ethylene-α-olefin copolymers such as ethylene-propylene copolymers, ethylene-butene copolymers, ethylene-hexene copolymers, and ethylene-octene copolymers; propylene-α-olefin copolymers such as propylene-ethylene copolymers and propylene-butene copolymers; butene-α-olefin copolymers such as butene-ethylene copolymers and butene-propylene copolymers, etc. can be cited. Olefin random copolymers are copolymers obtained by random copolymerization of two or more olefin monomers described above and have low crystallinity, and examples thereof include TAFMER series (trade names) such as ethylene-based TAFMER, propylene-based TAFMER, and butene-based TAFMER manufactured by Mitsui Chemicals, Inc.

[0280] The aliphatic rubber is a copolymer of an olefin monomer and a diene monomer or a hydrogenated product thereof, and is a polymer having rubber-like elasticity. Specifically, synthetic rubbers such as ethylene-propylene rubber (EPM), ethylene-propylene-diene rubber (EPDM), isoprene rubber (IR), butadiene rubber (BR), and butyl rubber (IIR) can be cited.

[0281] The above-mentioned ionomer is a metal salt of an ethylene-unsaturated carboxylic acid copolymer, and the carboxyl groups in the ionomer are neutralized by metal.

[0282] In order to obtain a more excellent accumulated fatigue absorption effect, the density of the olefin polymer (B3) is usually less than 0.890 g / cm 3 , wherein 0.820 g / cm 3 Above and less than 0.890g / cm 3 Examples of the olefin polymer (B3) satisfying such conditions include low-crystalline ethylene-α-olefin random copolymers, EPM, and EPDM.

[0283] Furthermore, the glass transition temperature of the above-mentioned olefin polymer (B3) is usually -110 to 0°C, preferably -80 to -20°C, and more preferably -70 to -40°C. The glass transition temperature of the olefin polymer (B3) is in a temperature range far below room temperature, and it has low crystallinity, so the resulting resin composition has excellent flexibility in a wide temperature range from low temperature to room temperature. In addition, by adding the olefin polymer (B3) to the EVOH resin (A), a high accumulated fatigue absorption effect can be imparted. Here, the glass transition temperature refers to the temperature at which the amorphous part of the olefin polymer (B3) changes from a glass state to a rubber state, and can usually be measured using a differential scanning calorimeter by a method based on JIS K 7121.

[0284] The melt flow rate (MFR) of the olefin polymer (B3) is generally 0.01 to 150 g / 10 min, preferably 0.1 to 50 g / 10 min, more preferably 1 to 25 g / 10 min, and further preferably 2 to 10 g / 10 min, at 210°C and a load of 2160 g.

[0285] The closer the melt viscosity of the EVOH resin (A) is to the melt viscosity of the olefin polymer (B3), the easier it is to melt-knead, and it is easy to obtain a resin composition in which the olefin polymer (B3) is uniformly dispersed in the EVOH resin (A), and it is easy to obtain a resin composition with excellent bending resistance and transparency. Specifically, the ratio of the MFR values ​​measured at 210°C and a load of 2160g (EVOH resin (A) / olefin polymer (B3)) is usually 0.1 to 10, preferably 0.3 to 4, and more preferably 0.5 to 3.

[0286] The olefin polymer (B3) can be blended with the high-crystalline EVOH resin (A) to obtain a resin composition imparted with flexibility due to its low crystallinity and rubber properties, and can also obtain a composition having excellent flex resistance.

[0287] In the present EVOH resin composition, the mass content ratio of EVOH resin (A) to olefin polymer (B3) is preferably 1 / 99 to 99 / 1, more preferably 25 / 75 to 98 / 2, further preferably 50 / 50 to 97 / 3, particularly preferably 65 / 35 to 96 / 4, and particularly preferably 75 / 25 to 95 / 5. If the mass content ratio of EVOH resin (A) to olefin polymer (B3) is within the above range, the coloring suppression effect is more excellent.

[0288] In addition, the total content of the EVOH resin (A) and the olefin polymer (B3) in the present EVOH resin composition is usually 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more. It should be noted that the upper limit of the total content of the EVOH resin (A) and the olefin polymer (B3) is the total mass obtained by removing the titanium compound (C) from the resin composition.

[0289] The olefin polymer (B3) used in the present invention may be an unmodified olefin polymer (B3-1) not containing a polar group in its structure, or may be a carboxylic acid-modified olefin polymer (B3-2) containing a carbonyl group in its structure. In addition, an unmodified olefin polymer (B3-1) and a carboxylic acid-modified olefin polymer (B3-2) may be used in combination. When an unmodified olefin polymer (B3-1) and a carboxylic acid-modified olefin polymer (B3-2) are used in combination, the sum of the two is regarded as the olefin polymer (B3).

[0290] The unmodified olefin polymer (B3-1) is an olefin polymer having the above-mentioned structure and having no modified group. The unmodified olefin polymer (B3-1) can be used alone or in combination of two or more. Among them, ethylene-butene random copolymer is preferably used.

[0291] The density and MFR of the unmodified olefin polymer (B3-1) are the same as those of the above-mentioned olefin polymer (B3).

[0292] As such an unmodified olefin-based polymer (B3-1), a commercially available product can be used.

[0293] Examples of commercially available products include ethylene polymers (TAFMER DF & H manufactured by Mitsui Chemicals, Inc.), propylene polymers (TAFMER H and TAFMER XM manufactured by Mitsui Chemicals, Inc.), and butene polymers (TAFMER BL manufactured by Mitsui Chemicals, Inc.).

[0294] Next, the carboxylic acid-modified olefin polymer (B3-2) will be described in detail.

[0295] The above-mentioned carboxylic acid-modified olefin polymer (B3-2) is obtained by modifying the above-mentioned olefin polymer, i.e., polyolefin, olefin thermoplastic elastomer, aliphatic rubber, ionomer, etc., which are generally high molecular weights of 10,000 or more and whose main chains are composed only of carbon bonds, with carboxylic acid.

[0296] Since the carboxylic acid-modified olefin polymer (B3-2) has a carboxyl group, it has affinity with the EVOH resin (A) having a hydroxyl group as a polar group, and further, the olefin polymer part of the carboxylic acid-modified olefin polymer (B3-2) has affinity with the above-mentioned unmodified olefin polymer (B3-1). Therefore, when the carboxylic acid-modified olefin polymer (B3-2) is used as the olefin polymer (B3), the mixing efficiency and reaction efficiency with the EVOH resin (A) tend to be improved. In addition, when the above-mentioned unmodified olefin polymer (B3-1) is used in combination with the carboxylic acid-modified olefin polymer (B3-2), the carboxylic acid-modified olefin polymer (B3-2) can play a role as a compatibilizer with the EVOH resin (A) and the unmodified olefin polymer (B3-1).

[0297] Here, the carboxylic acid modification is performed by replacing part of the monomers constituting the olefin polymer with an α,β-unsaturated carboxylic acid or an anhydride monomer thereof and copolymerizing the monomers, or by introducing an α,β-unsaturated carboxylic acid or an anhydride monomer thereof into part of the side chain by a graft reaction or the like.

[0298] Examples of the α,β-unsaturated carboxylic acid or anhydride thereof used in the above-mentioned carboxylic acid modification include maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, itaconic anhydride, etc. Among them, maleic anhydride is preferred.

[0299] The modification amount (modification carboxylic acid amount) of the carboxylic acid-modified olefin polymer (B3-2) is usually 0.01 to 10% by mass of the base olefin polymer, preferably 0.01 to 5% by mass, particularly preferably 0.1 to 2% by mass, and particularly preferably 0.2 to 1% by mass. If the modification amount is too small, the compatibility of the resulting resin composition is reduced and the effect of the present invention is not easily obtained. On the contrary, if it is too large, the reaction points with the hydroxyl group in the EVOH resin (A) increase, a high degree of polymerization is generated during melt kneading, and there is a tendency for the moldability and thermal stability during film molding to decrease.

[0300] The density of the carboxylic acid-modified olefin polymer (B3-2) is usually 0.85 to 0.96 g / cm 3 , preferably 0.85 to 0.92 g / cm 3 , more preferably 0.85 to 0.90 g / cm 3 .

[0301] In addition, the melt flow rate (MFR) of the carboxylic acid-modified olefin polymer (B3-2) is generally 0.01 to 150 g / 10 min, preferably 0.1 to 50 g / 10 min, more preferably 1 to 25 g / 10 min, and further preferably 1.5 to 10 g / 10 min at 210°C and a load of 2160 g.

[0302] The closer the melt viscosity of EVOH resin (A) is to the melt viscosity of carboxylic acid-modified olefin polymer (B3-2), the easier it is to melt-knead, and it is easy to obtain a resin composition with excellent bending resistance and transparency. Specifically, the ratio of MFR values ​​measured at 210°C and a load of 2160g (EVOH resin (A) / carboxylic acid-modified olefin polymer (B3-2)) is usually 0.1 to 10, preferably 0.5 to 7.5.

[0303] As such a carboxylic acid-modified olefin polymer (B3-2), a commercially available product may also be used. Commercially available products of the carboxylic acid-modified olefin polymer (B3-2) include, for example, "Admer", "TAFMER" M series (manufactured by Mitsui Chemicals, Inc.), "Bynel", "Fusabond" (manufactured by DuPont), "Orevac" (manufactured by Arkema), "Plexar" (manufactured by LyondellBasell), "Modic AP" (manufactured by Mitsubishi Chemical Corporation), etc.

[0304] In addition, the carboxylic acid-modified olefin polymer (B3-2) component used in the present invention may be a modified polymer obtained by post-modifying part of the carboxylic acid component contained in the carboxylic acid-modified olefin polymer (B3-2) component using other compounds (for example, polyamide resins such as polyamide 6 and polyamide 6 / 12), within the range not impairing the effects of the present invention.

[0305] As an olefin polymer (B3), the mass content ratio [carboxylic acid-modified olefin polymer (B3-2) / unmodified olefin polymer (B3-1)] when an unmodified olefin polymer (B3-1) and a carboxylic acid-modified olefin polymer (B3-2) are used together also depends on the modification rate of the carboxylic acid-modified olefin polymer (B3-2), but is generally 0.01 to 100, preferably 0.1 to 10, more preferably 0.3 to 5, and particularly preferably 0.5 to 2.

[0306] [Titanium compound (C)]

[0307] Examples of the titanium compound (C) used in the present invention include inorganic titanium compounds and organic titanium compounds. The titanium compound may be the same as the component (C) described in the first embodiment.

[0308] The metal conversion content of the titanium compound (C) is 0.0004 ppm or more and less than 4 ppm relative to the mass of the EVOH resin composition, preferably 0.004 to 3 ppm, more preferably 0.0015 to 1 ppm, and particularly preferably 0.025 to 0.5 ppm. By making the content of the titanium compound (C) within the above range, thermal degradation during melt molding can be suppressed, and long-term operation performance is excellent. In addition, if the content of the titanium compound (C) is too little, the effect of suppressing thermal degradation is reduced, and if the content is too much, thermal decomposition of the EVOH resin (A) is likely to occur, and it is easy to color.

[0309] The metal conversion content of the above-mentioned titanium compound (C) can be quantified by the following operation: weigh the EVOH resin composition into a platinum crucible, incinerate it using a burner and an electric furnace in sequence, heat and decompose the ash with nitric acid and hydrofluoric acid, treat it with a mixed acid of dilute nitric acid and dilute hydrofluoric acid and fix the volume, and use an ICP mass spectrometer (manufactured by Agilent Technologies, Agilent 8800) to determine the titanium in the obtained fixed volume solution by ICP mass spectrometry.

[0310] The metal equivalent content of the titanium compound (C) is preferably 0.001 to 3 ppm, more preferably 0.03 to 1 ppm, and particularly preferably 0.05 to 0.5 ppm, based on the total mass of the EVOH resin (A) and the titanium compound (C).

[0311] If the content of the titanium compound (C) is too small, the effect of suppressing thermal degradation decreases, while if the content is too large, thermal decomposition of the EVOH resin (A) tends to occur, and coloration tends to occur.

[0312] It is generally known that EVOH resin deteriorates due to heat. The mechanism is not clear, but it is believed that thermal degradation proceeds because a double bond structure is generated in the main chain of the EVOH resin during the above reaction, and this site becomes the starting point of the reaction, and further dehydration reaction occurs to form a polyene structure in the main chain of the EVOH resin.

[0313] On the other hand, when a titanium compound is contained in an EVOH resin composition, it is considered that the EVOH resin composition is colored by titanium ions, and therefore it is common technical knowledge for those skilled in the art to avoid using the titanium compound.

[0314] However, the present invention goes against such common technical knowledge and finds that when a specific olefin resin (B3) and a specific trace amount of a titanium compound (C) are used in combination, an EVOH resin composition in which thermal degradation is significantly suppressed can be obtained.

[0315] That is, it is speculated that titanium is stable as a tetravalent ion, and even a trace amount thereof will coordinate to the double bonds of the main chain of the EVOH resin as described above, forming a chelate or the like to stabilize, thereby further suppressing the formation of a polyene structure. In addition, it is speculated that due to the coexistence of the polyolefin resin and the titanium compound, since a plurality of double bond sites are distributed in the resin composition, the formation of double bonds is further suppressed, and the thermal stability is further improved.

[0316] On the other hand, if the content of the titanium compound (C) is too large, it is considered that thermal decomposition of the EVOH resin occurs due to the titanium compound (C). Therefore, in the present invention, the content of the titanium compound (C) is limited to a specific trace amount.

[0317] [Other thermoplastic resins]

[0318] The present EVOH resin composition may contain, in addition to the EVOH resin (A) and the specific olefin resin (B3), other thermoplastic resins as resin components within a range that does not hinder the effects of the present invention (e.g., usually 30% by mass or less, preferably 20% by mass or less, and particularly preferably 10% by mass or less of the present EVOH resin composition).

[0319] As other thermoplastic resins, known thermoplastic resins can be used, for example, polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more.

[0320] [Other compounding ingredients]

[0321] The EVOH resin composition may contain a compounding agent generally compounded with EVOH resin within a range that does not inhibit the effects of the present invention. As the compounding agent, the same compounding agent as described in the first embodiment can be used.

[0322] [Method for producing EVOH resin composition]

[0323] The present EVOH resin composition can be produced by using the above-mentioned essential components, i.e., EVOH resin (A), olefin resin (B3) and titanium compound (C), and the above-mentioned optional components as required. As a production method, for example, known methods such as dry blending method, melt mixing method, solution mixing method, impregnation method, etc. can be cited. Among these, it is preferably produced by a process of melt mixing the composition raw materials containing the above-mentioned EVOH resin and titanium compound. In addition, these production methods can also be arbitrarily combined.

[0324] Examples of the dry blending method include (I) a method in which pellets containing the EVOH resin (A) and / or the olefin resin (B3) and the titanium compound (C) are dry blended using a tumbler or the like.

[0325] As the above-mentioned melt mixing method, for example, there can be cited (II) a method of melt-kneading a dry blend of particles containing EVOH resin (A) and / or olefin-based resin (B3) and a titanium compound (C) to obtain particles or other molded products; (III) a method of adding a titanium compound (C) to a melt of EVOH resin (A) and / or olefin-based resin (B3) in a molten state and melt-kneading to obtain particles or other molded products, etc.

[0326] As the above-mentioned solution mixing method, for example, there can be cited the method of (IV) using particles containing EVOH resin (A) and / or olefin-based resin (B3) to prepare a solution, adding a titanium compound (C) thereto, coagulating and forming it into particles, performing solid-liquid separation and drying; (V) in the manufacturing process of EVOH resin (A), making a uniform solution (water / alcohol solution, etc.) of saponified EVOH resin contain a solution of olefin-based resin (B3) and / or titanium compound (C), coagulating and forming it into particles, performing solid-liquid separation and drying, etc.

[0327] Examples of the impregnation method include (VI) a method in which particles containing the EVOH resin (A) and / or the olefin resin (B3) are brought into contact with an aqueous solution containing the titanium compound (C), the particles are impregnated with the titanium compound (C), and then dried.

[0328] In addition, in each of the above methods, EVOH resin (A) and / or olefin-based resin (B3) and titanium compound (C) may be pre-blended in a specified ratio to prepare a composition (masterbatch) having a high concentration of titanium compound (C), and the composition (masterbatch) may be blended with EVOH resin (A) or olefin-based resin (B3) to obtain a resin composition of the desired concentration.

[0329] Furthermore, in the present invention, the above-mentioned different methods may be combined. Among them, from the viewpoint of productivity and obtaining a resin composition having a more remarkable effect of the present invention, the melt mixing method is preferred, and the method (II) is particularly preferred.

[0330] It should be noted that the shape of the pellets of the resin composition obtained by the above methods and the pellets containing the EVOH resin (A) and / or the polyamide resin (B3) used in the above methods is arbitrary, and any shape such as spherical, elliptical, cylindrical, cubic, and rectangular can be adopted. The shape of the pellets is usually elliptical or cylindrical. Regarding the size, in the case of a cylindrical shape, the diameter of the bottom surface is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm, from the viewpoint of convenience when used as a molding material later. In the case of an elliptical shape, the major diameter is usually 1.5 to 30 mm, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm, and the minor diameter is usually 1 to 10 mm, preferably 2 to 6 mm, and particularly preferably 2.5 to 5.5 mm. The method for measuring the major axis and the minor axis is, for example, as follows: observe the particle in hand, measure the major axis using a measuring instrument such as a vernier caliper, determine the position of the cross section with the largest area in the cross section perpendicular to the major axis by visual inspection and touch, and similarly measure the minor axis when assuming the cross section.

[0331] It should be noted that when the EVOH resin composition is in the form of pellets, it is preferred to attach a known lubricant to the surface of the pellets from the perspective of stabilizing the feeding property during melt molding. Examples of the lubricant include higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters of higher fatty acids, etc.), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, behenic acid amide; unsaturated higher fatty acid amides such as oleic acid amide, erucic acid amide, bis-higher fatty acid amides such as ethylene bisstearic acid amide, ethylene bisoleic acid amide, ethylene biserucic acid amide, ethylene bislauric acid amide, etc.), low molecular weight polyolefins (e.g., low molecular weight polyethylene or low molecular weight polypropylene having a molecular weight of about 500 to 10,000, or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, fluorinated vinyl resins, etc. These compounds can be used alone or in combination of two or more. In addition, the content of the lubricant is usually 5% by mass or less, preferably 1% by mass or less of the EVOH resin composition. It should be noted that the lower limit is usually 0% by mass.

[0332] The present EVOH resin composition obtained in this manner can suppress thermal degradation during heating, and the 5% weight loss temperature of the present EVOH resin composition is usually 355° C. or higher, preferably 357° C. or higher, and more preferably 358° C. or higher.

[0333] The upper limit of the 5% weight reduction temperature is preferably as high as possible, and is usually 450°C.

[0334] A difference of 1° C. in the above-mentioned weight loss temperature represents a significant difference in yield in actual production, and therefore, the difference is very large.

[0335] The above-mentioned "5% weight loss temperature" refers to the temperature at which the weight of 5 mg of the present EVOH resin composition is reduced to 95% of the weight before measurement using a thermogravimetric measuring apparatus (manufactured by Perkin Elmer, Pyris 1TGA) under a nitrogen atmosphere at an air flow rate of 20 mL / min, a heating rate of 10°C / min, and a temperature range of 30 to 550°C.

[0336] The water content of the present EVOH resin composition is usually 0.01 to 0.5% by mass, preferably 0.05 to 0.35% by mass, and particularly preferably 0.1 to 0.3% by mass.

[0337] The water content of the present EVOH resin composition is measured and calculated by the following method.

[0338] The mass (W1) of the EVOH resin composition before drying was measured using an electronic balance, dried in a hot air dryer at 150°C for 5 hours, cooled in the dryer for 30 minutes, and then the mass (W2) was measured and calculated using the following formula.

[0339] <Formula>

[0340] Water content (mass %) = [(W1-W2) / W1] × 100

[0341] The EVOH resin composition can be prepared into various forms such as powder and liquid in addition to pellets, and provided as a molding material for various molded objects. In particular, in the present invention, when provided as a material for melt molding, there is a tendency to more effectively obtain the effects of the present invention, and thus it is preferred.

[0342] The present EVOH resin composition also includes a resin composition obtained by mixing the EVOH resin (A) used in the present EVOH resin composition with a resin other than the polyamide-based resin (B3).

[0343] Examples of the molded product include a single-layer film molded from the present EVOH resin composition, and a multilayer structure having a layer composed of the present EVOH resin composition.

[0344] [Multilayer structure]

[0345] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the present multilayer structure") comprises a layer composed of the present EVOH resin composition. The layer composed of the present EVOH resin composition (hereinafter referred to as "the present EVOH resin composition layer") can be further provided with strength, or the present EVOH resin composition layer can be protected from the influence of moisture, etc., or other functions can be provided by laminating it with another substrate having a thermoplastic resin as a main component other than the present EVOH resin composition (hereinafter, the resin used in the substrate is sometimes referred to as "substrate resin").

[0346] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers, ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polybutene, polypentene, (unmodified) polyolefin resins including polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and these polyolefin resins. The polyolefin resins in a broad sense of modified olefin resins such as unsaturated carboxylic acid-modified polyolefin resins obtained by adhesively grafting hydrocarbons with unsaturated carboxylic acids or their esters, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, chlorinated polyethylene, chlorinated polypropylene and other halogenated polyolefins, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.

[0347] Among these, polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred as the hydrophobic resin, and polyethylene resins, polypropylene resins, polycyclic olefin resins, and polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins thereof are more preferred. It is particularly preferred to use polycyclic olefin resins as the hydrophobic resin.

[0348] When the EVOH resin composition layer is a (a1, a2, ...) and the substrate resin layer is b (b1, b2, ...), the layer structure of the multilayer structure may be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc. In addition, when the recycled layer including a mixture of the EVOH resin composition and a thermoplastic resin other than the EVOH resin composition obtained by remelting and molding the end portions, defective products, etc. generated in the process of manufacturing the multilayer structure is R, it may be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The number of layers of the multilayer structure is usually 2 to 15 in total, preferably 3 to 10. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be interposed between the layers as necessary.

[0349] As the above-mentioned adhesive resin, a known resin can be used, as long as it is appropriately selected according to the type of thermoplastic resin used in the substrate resin layer "b". Representative examples include modified polyolefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to polyolefin resins using addition reactions, grafting reactions, etc. As the above-mentioned modified polyolefin polymers containing carboxyl groups, for example, maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block and random) copolymers, maleic anhydride grafted modified ethylene-ethyl acrylate copolymers, maleic anhydride grafted modified ethylene-vinyl acetate copolymers, maleic anhydride modified polycyclic olefin resins, maleic anhydride grafted modified polyolefin resins, etc. can be cited. They can be used alone or in combination of two or more.

[0350] In the present multilayer structure, when an adhesive resin layer is used between the present EVOH resin composition layer and the base resin layer, since the adhesive resin layer is located on both sides of the present EVOH resin composition layer, an adhesive resin having excellent hydrophobicity is preferably used.

[0351] The above-mentioned base resin and adhesive resin may also contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, nucleating agents, antiblocking agents, waxes, etc. within a range that does not hinder the purpose of the present invention (for example, 30% by mass or less, preferably 10% by mass or less relative to the entire resin). These may be used alone or in combination of two or more.

[0352] The lamination of the above-mentioned EVOH resin composition layer and the above-mentioned substrate resin layer (including the case where an adhesive resin layer is interposed) can be carried out by a known method. For example, there can be cited a method of melt-extrusion lamination of the substrate resin on a film, sheet, etc. of the present EVOH resin composition; a method of melt-extrusion lamination of the present EVOH resin composition on a substrate resin layer; a method of co-extruding the present EVOH resin composition and the substrate resin; a method of dry laminating the present EVOH resin composition (layer) and the substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc.; a method of removing the solvent after applying a solution of the present EVOH resin composition on the substrate resin, etc. Among these, from the viewpoint of cost and environment, it can be manufactured by a process of melt-molding the present EVOH resin composition layer, and specifically, the co-extrusion method is preferred.

[0353] The present multilayer structure may also be subjected to (heating) stretching treatment as required. The stretching treatment may be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, it may be simultaneous stretching or sequential stretching. In addition, as a stretching method, a stretching method with a high stretching ratio such as a roller stretching method, a tentering stretching method, a tubular stretching method, a stretch blow molding method, and a vacuum pressure molding method may be adopted. The stretching temperature is a temperature near the melting point of the multilayer structure, usually selected from the range of 40 to 170°C, preferably about 60 to 160°C. When the stretching temperature is too low, the stretchability becomes poor, and when it is too high, it is difficult to maintain a stable stretched state.

[0354] In addition, for the purpose of imparting dimensional stability, the stretched multilayer structure may be heat-fixed. Heat-fixing may be performed by a known method, for example, by heat-treating the stretched multilayer structure at a temperature of usually 80 to 180° C., preferably 100 to 165° C., for usually 2 to 600 seconds while maintaining the stretched multilayer structure in a tensioned state.

[0355] When the stretched multilayer structure is used as a shrink film, in order to impart heat shrinkage, the stretched multilayer structure may be cooled and fixed by blowing cold air instead of the heat setting.

[0356] The thickness of the present multilayer structure (including the stretched multilayer structure), and the thickness of the present EVOH resin composition layer, the base resin layer and the adhesive resin layer constituting the multilayer structure vary depending on the layer constitution, the type of base resin, the type of adhesive resin, the application, the packaging form, the required physical properties, etc., and cannot be generalized. The thickness of the present multilayer structure (including the stretched multilayer structure) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0357] Furthermore, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the substrate resin layer in the present multilayer structure (present EVOH resin composition layer / substrate resin layer) is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60, as a ratio of the thickest layers. In addition, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the adhesive resin layer in the present multilayer structure (present EVOH resin composition layer / adhesive resin layer) is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10, as a ratio of the thickest layers.

[0358] In addition, the present multilayer structure can also be used to obtain a cup or tray-shaped multilayer container. In this case, a deep drawing method is usually used, and specifically, vacuum forming, pressure forming, vacuum pressure forming, plunger-assisted vacuum pressure forming, etc. can be cited. Furthermore, when a tubular or bottle-shaped multilayer container (laminated structure) is obtained from a multilayer parison (a hollow tubular preform before blow molding), a blow molding method can be used. Specifically, extrusion blow molding (double-head type, mold moving type, parison moving type, rotary type, accumulation type, horizontal parison type, etc.), cold parison blow molding, injection blow molding, biaxial stretch blow molding (extrusion cold parison biaxial stretch blow molding, injection cold parison biaxial stretch blow molding, injection molding embedded biaxial stretch blow molding, etc.) can be cited. The obtained laminate can be subjected to heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making processing, deep drawing processing, box processing, tube processing, slitting processing, etc. as needed.

[0359] Furthermore, bags made of films, sheets, and stretched films obtained using the present multilayer structure, and containers and covers made of cups, trays, tubes, bottles, etc., are useful as various packaging material containers for general foods, seasonings such as mayonnaise and sauces, fermented foods such as miso, oily foods such as salad oils, beverages, cosmetics, pharmaceuticals, etc. In particular, since the layer made of the present EVOH resin composition has flexibility and coloring is suppressed, the present EVOH resin composition and the present multilayer structure are particularly useful as liquid packaging materials for water, food, pharmaceuticals, pesticides, etc. (e.g., bags for bag-in-box, liner bags for pouch-in dispensers, etc.).

[0360] <<Method 4>>

[0361] EVOH resin has excellent transparency, oxygen and other gas barrier properties, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and is molded into films, sheets, bottles, etc. and is widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and pesticide packaging materials.

[0362] However, if a packaging material including an EVOH resin layer composed of EVOH resin is subjected to hot water sterilization treatment such as retorting or boiling, the EVOH resin layer tends to dissolve or the gas barrier properties of the EVOH resin layer decrease. In this regard, there is a known technology for using a polyamide resin in combination (see, for example, Patent Documents 1 and 2).

[0363] Patent Document 1: Japanese Patent Application Publication No. 2005-178324

[0364] Patent Document 2: Japanese Patent Application Publication No. 2009-242591

[0365] The resin compositions comprising EVOH resin and polyamide resin disclosed in Patent Documents 1 and 2 are excellent in hot water treatment resistance, but tend to be thermally deteriorated by heating during melt kneading, melt molding, etc., and improvement of this has been sought.

[0366] An object of the present invention is to provide an EVOH resin composition which has resistance to hot water treatment and in which thermal degradation of the EVOH resin during heating such as melt molding is suppressed.

[0367] The present inventors have found that, in view of the situation of cedar trees, by adding a polyamide resin and a specific trace amount of a titanium compound to an EVOH resin, an EVOH resin composition can be obtained in which thermal degradation of the EVOH resin during heating such as melt molding is suppressed.

[0368] That is, the present invention has the following aspects.

[0369] [4-1] An EVOH resin composition comprising an EVOH resin (A), a polyamide resin (B4) and a titanium compound (C),

[0370] The metal-equivalent content of the titanium compound (C) is 0.001 ppm or more and less than 5 ppm based on the mass of the EVOH resin composition.

[0371] [4-2] The EVOH resin composition according to [4-1], wherein the mass content ratio (A) / (B4) of the EVOH resin (A) to the polyamide resin (B4) is 1 / 99 to 99 / 1.

[0372] [4-3] The EVOH resin composition according to [4-1] or [4-2], wherein the metal-equivalent content of the titanium compound (C) is 0.01 to 3 ppm relative to the total mass of the EVOH resin (A) and the titanium compound (C).

[0373] [4-4] A melt molding material comprising the EVOH resin composition according to any one of [4-1] to [4-3].

[0374] [4-5] A multilayer structure comprising at least one layer comprising the EVOH resin composition according to any one of [4-1] to [4-3].

[0375] [4-6] A packaging material for hot water sterilization, comprising the multilayer structure described in [4-5].

[0376] [4-7] A method for producing an EVOH resin composition, which is the method for producing the EVOH resin composition according to any one of [4-1] to [4-3], comprising the step of melt-mixing a composition raw material containing the EVOH resin and a titanium compound.

[0377] [4-8] A method for producing a multilayer structure, which is a method for producing the multilayer structure described in [4-5], comprising the step of melt-molding a layer composed of the EVOH resin composition.

[0378] The EVOH resin composition of the present invention has excellent thermal stability, and therefore can suppress thermal degradation of the EVOH resin during heating such as during melt kneading and melt molding.

[0379] In addition, the melt molding material composed of the resin composition of the present invention has resistance to hot water treatment and the thermal degradation of the EVOH resin during heating during melt kneading, melt molding, etc. is suppressed. Therefore, it can be used as a packaging material for food, medicine, pesticides, etc., especially a molding material for various molded products obtained by melt molding, such as packaging materials for hot water sterilization.

[0380] Furthermore, since the thermal degradation of the EVOH resin during heating such as during melt-kneading and melt-molding is suppressed in the multilayer structure having a layer composed of the resin composition of the present invention, it can be applied as various molded articles, for example, packaging materials for foods, pharmaceuticals, agricultural chemicals, etc., particularly packaging materials for hot water sterilization.

[0381] Hereinafter, the present invention will be described in more detail based on examples of embodiments of the present invention, but the present invention is not limited to these embodiments.

[0382] <EVOH resin composition>

[0383] The EVOH resin composition (hereinafter referred to as "the present EVOH resin composition") according to an embodiment of the present invention contains an EVOH resin (A), a polyamide resin (B4), and a specific trace amount of a titanium compound (C).

[0384] Hereinafter, each component will be described.

[0385] [EVOH resin (A)]

[0386] The EVOH resin (A) used in the present invention is usually a resin obtained by saponifying an ethylene-vinyl ester copolymer which is a copolymer of ethylene and a vinyl ester monomer, and the same resin as the (A) component described in the above first mode can be used.

[0387] The content of the above EVOH resin (A) in the present EVOH resin composition is usually 1% by mass or more, preferably 10% by mass or more, more preferably 50% by mass or more, more preferably 60% by mass or more, further preferably 70% by mass or more, and particularly preferably 85% by mass or more. In addition, the upper limit of the content of the EVOH resin (A) is usually 99% by mass. When the value is in the above range, there is a tendency to more effectively obtain the effects of the present invention.

[0388] [Polyamide resin (B4)]

[0389] The polyamide resin (B4) used in the present invention is a water-insoluble thermoplastic resin, and a publicly known general polyamide resin can be used.

[0390] Examples of the polyamide resin (B4) include homopolymers such as polycaprolactam (nylon 6), poly-ω-aminoheptanoic acid (nylon 7), poly-ω-aminononanoic acid (nylon 9), polyundecamide (nylon 11), and polylaurolactam (nylon 12). Examples of the copolymer polyamide resin include polyethylene adipamide (nylon 26), polybutylene adipamide (nylon 46), polyhexamethylene adipamide (nylon 66), polyhexamethylene sebacamide (nylon 610), polyhexamethylene dodecanoic acid (nylon 612), polyoctylene adipamide (nylon 86), polydecamethylene adipamide (nylon 108), caprolactam / laurolactam copolymer (nylon 6 / 12), caprolactam / ω-aminononanoic acid copolymer (nylon 6 / 9), caprolactam / hexamethylene adipamide copolymer (nylon 6 / 66), laurolactam / hexamethylene adipamide copolymer (nylon 12 / 66), ethylene adipamide / hexamethylene adipamide copolymer (nylon 26 / 66), caprolactam / ω-aminononanoic acid copolymer (nylon 6 / 9), caprolactam / hexamethylene adipamide copolymer (nylon 6 / 66), laurolactam / hexamethylene adipamide copolymer (nylon 12 / 66), Aliphatic polyamides such as lactam / hexamethylene diammonium adipate / hexamethylene diammonium sebacic acid copolymer (nylon 66 / 610), ethylene diammonium adipate / hexamethylene diammonium adipate / hexamethylene diammonium sebacic acid copolymer (nylon 6 / 66 / 610), polyhexamethylene isophthalamide, polyhexamethylene terephthalamide, polym-xylylene adipamide, hexamethylene isophthalamide / terephthalamide copolymer, poly-p-phenylene terephthalamide, poly-p-phenylene-3,4' diphenyl ether terephthalamide, amorphous polyamide, these polyamide resins modified with aromatic amines such as methylene benzylamine and m-xylylenediamine, m-xylylene diammonium adipate, or their terminal modified polyamide resins. Among them, terminal modified polyamide resins are preferred. These polyamide-based resins (B4) can be used alone or in combination of two or more.

[0391] The polyamide resin (B4) tends to have a higher bonding strength with a resin containing a polar group such as the EVOH resin (A). Therefore, a resin composition containing the EVOH resin (A) and the polyamide resin (B4) can be preferably used to improve the moisture resistance of a multilayer structure in which a layer composed of the resin composition and a layer composed of other thermoplastic resins are laminated.

[0392] The ratio of the amide bond in the amide monomer unit constituting the polyamide resin (B4) is preferably 20 to 60%, more preferably 30 to 50%, and particularly preferably 35 to 45%, when the amide monomer unit (for example, the amide bond (-CONH-) in [-C6H5-CONH-] in the case of nylon 6) is calculated as the ratio of the molecular weight. When the ratio of the amide bond is too low, the bonding strength at the interface with the polar resin such as the EVOH resin (A) tends to be easily reduced. On the contrary, when it is too high, the reactivity with the polar resin such as the EVOH resin (A) is too strong during melt molding, and there is a tendency to cause poor appearance due to rough bonding interface during coextrusion.

[0393] In addition, the melting point of the polyamide resin (B4) is preferably 160 to 270°C, more preferably 175 to 250°C, and particularly preferably 190 to 230°C. When the melting point of the polyamide resin (B4) is too low, there is a tendency for heat resistance to decrease when a multilayer structure is made. On the other hand, if the melting point of the polyamide resin (B4) is too high, in the case of a multilayer structure comprising other resin layers, the melting point difference with the resin used in the other layers becomes larger. This will cause layer confusion when co-extrusion molding with other resins, resulting in a tendency to reduce the appearance when the multilayer structure is made. Furthermore, when co-extrusion molding with EVOH resin (A), the mold temperature is too high, and there is a concern that the coloring of EVOH resin (A) due to thermal degradation is promoted.

[0394] From the above viewpoints, the preferred polyamide resin (B4) has a melting point of 160 to 270° C., preferably 175 to 250° C., particularly preferably 190 to 230° C., and an amide bond ratio of 20 to 60%, preferably 30 to 50%, particularly preferably 35 to 45%. Specifically, for example, nylon 6 (melting point: about 225° C., amide bond ratio: 38%) and nylon 6 / 66 (melting point: about 195° C., amide bond ratio: 38%) are preferred.

[0395] The degree of polymerization of the polyamide resin (B4) can generally be expressed by relative viscosity, which is usually preferably 1.5 to 6, more preferably 2.0 to 6, and further preferably 2.5 to 5. This is because when the relative viscosity is too low, the extruder becomes in a high torque state during molding, and a tendency is observed that the extrusion process becomes difficult, and when it is too high, a tendency is observed that the thickness accuracy of the obtained film or sheet decreases. It should be noted that the above relative viscosity can be measured according to JIS K6933 by completely dissolving 1 g of the polyamide resin in 100 mL of 96% concentrated sulfuric acid and using a capillary viscometer at 25°C.

[0396] The EVOH resin composition preferably has a mass content ratio (A) / (B4) of EVOH resin (A) relative to polyamide resin (B4) of 1 / 99 to 99 / 1, more preferably 10 / 90 to 99 / 1, further preferably 50 / 50 to 98 / 2, particularly preferably 60 / 40 to 95 / 5, particularly preferably 70 / 30 to 95 / 5, and particularly preferably 75 / 25 to 95 / 5. If the mass content ratio of the polyamide resin (B4) is too small, the compounding effect (e.g., hot water sterilization resistance) of the polyamide resin (B4) in the obtained molded article tends to be reduced, and conversely, if it is too large, the gas barrier properties tend to be reduced.

[0397] In addition, the total content of the EVOH resin (A) and the polyamide resin (B4) in the present EVOH resin composition is usually 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more. It should be noted that the upper limit of the total content of the EVOH resin (A) and the polyamide resin (B4) is the total mass obtained by removing the content of the titanium compound (C) from the resin composition.

[0398] [Titanium compound (C)]

[0399] Examples of the titanium compound (C) used in the present invention include inorganic titanium compounds and organic titanium compounds. As the titanium compound, the same titanium compound as the component (C) described in the first embodiment can be used.

[0400] The metal conversion content of the above-mentioned titanium compound (C) is greater than 0.001ppm and less than 5ppm relative to the mass of the EVOH resin composition. It is preferably 0.01 to 3ppm, more preferably 0.03 to 1ppm, and particularly preferably 0.05 to 0.5ppm. By making the content of the titanium compound (C) within the above range, thermal degradation during melt molding can be suppressed, and long-term operation performance is excellent. In addition, if the content of the titanium compound (C) is too little, the effect of suppressing thermal degradation is reduced. If the content is too much, thermal decomposition of the EVOH resin (A) is likely to occur, and it is easy to color.

[0401] The metal conversion content of the above-mentioned titanium compound (C) can be quantified by the following operation: weigh the EVOH resin composition into a platinum crucible, incinerate it using a burner and an electric furnace in sequence, heat and decompose the ash with nitric acid and hydrofluoric acid, treat it with a mixed acid of dilute nitric acid and dilute hydrofluoric acid and make it constant, and use an ICP mass spectrometer (manufactured by Agilent Technologies, Agilent 8800) to determine the titanium in the obtained constant solution by ICP mass spectrometry.

[0402] The metal equivalent content of the titanium compound (C) is preferably 0.01 to 3 ppm, more preferably 0.03 to 1 ppm, and particularly preferably 0.05 to 0.5 ppm, based on the total mass of the EVOH resin (A) and the titanium compound (C).

[0403] If the content of the titanium compound (C) is too small, the effect of suppressing thermal degradation decreases, while if the content is too large, thermal decomposition of the EVOH resin (A) is likely to occur, and coloration is likely to occur.

[0404] Here, it is generally known that EVOH resin deteriorates due to heat. In addition, it is known that if a polyamide resin is mixed with EVOH resin, it is more susceptible to thermal degradation and shows a tendency to thicken when heated. The mechanism is not clear, but it is speculated that the thickening is due to the reaction of the mixed polyamide resin with the EVOH resin composition. In addition, it is believed that thermal degradation proceeds because a double bond structure is generated in the main chain of the EVOH resin during the above reaction, and this site becomes the starting point of the reaction, and further a dehydration reaction occurs, forming a polyene structure in the main chain of the EVOH resin.

[0405] On the other hand, when a titanium compound is contained in an EVOH resin composition, it is considered that the EVOH resin composition is colored by titanium ions, and therefore it is common technical knowledge for those skilled in the art to avoid using titanium compounds.

[0406] However, the present invention goes against such common technical knowledge and finds that when a polyamide-based resin (B4) is used in combination with a specific trace amount of a titanium compound (C), an EVOH resin composition in which thermal degradation is significantly suppressed can be obtained.

[0407] That is, it is speculated that titanium is stable as a tetravalent ion, and even a trace amount thereof will coordinate to the double bonds of the main chain of the EVOH resin as described above, forming a chelate or the like to stabilize, thereby further suppressing the formation of a polyene structure. In addition, it is speculated that the reaction between the polyamide resin and the titanium compound is also suppressed, the thickening tendency is suppressed, and the thermal stability is improved.

[0408] On the other hand, if the content of the titanium compound (C) is too large, it is considered that thermal decomposition of the EVOH resin occurs due to the titanium compound (C). Therefore, in the present invention, the content of the titanium compound (C) is limited to a specific trace amount.

[0409] [Other thermoplastic resins]

[0410] The present EVOH resin composition may contain, in addition to the EVOH resin (A) and the polyamide resin (B4), other thermoplastic resins as resin components within a range that does not hinder the effects of the present invention (e.g., usually 30% by mass or less, preferably 20% by mass or less, and particularly preferably 10% by mass or less of the present EVOH resin composition).

[0411] As the other thermoplastic resins, known thermoplastic resins can be used, for example, polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, ionomers, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more.

[0412] [Other compounding ingredients]

[0413] The EVOH resin composition may contain a compounding agent generally compounded with EVOH resin within a range that does not inhibit the effects of the present invention. As the compounding agent, the same compounding agent as described in the first embodiment can be used.

[0414] [Method for producing EVOH resin composition]

[0415] The EVOH resin composition can be produced by using the above-mentioned essential components, i.e., EVOH resin (A), polyamide resin (B4) and titanium compound (C), and the above-mentioned optional components as required. As its production method, for example, known methods such as dry blending method, melt mixing method, solution mixing method, impregnation method, etc. can be cited. Among these, it is preferably produced by a process of melt mixing the composition raw materials containing the above-mentioned EVOH resin and titanium compound. In addition, these production methods can also be arbitrarily combined.

[0416] Examples of the dry blending method include (I) a method of dry blending pellets containing the EVOH resin (A) and / or the polyamide resin (B4) and the titanium compound (C) using a tumbler or the like.

[0417] Examples of the melt mixing method include (II) a method of melt-kneading a dry blend of particles containing EVOH resin (A) and / or polyamide resin (B4) and a titanium compound (C) to obtain particles or other molded products; (III) a method of adding a titanium compound (C) to a molten EVOH resin (A) and / or polyamide resin (B4) and melt-kneading the mixture to obtain particles or other molded products; and a method of making the titanium compound (C) contained in EVOH resin (A) and / or polyamide resin (B4), using the EVOH resin (A) and / or polyamide resin (B4) to produce particles of a core-sheath structure in which the EVOH resin (A) is a core and the polyamide resin (B4) is a sheath, or using the EVOH resin (A) and / or polyamide resin (B4) to produce particles of a core-sheath structure in which the EVOH resin (A) is a sheath and the polyamide resin (B4) is a core, and then melt-molding the particles.

[0418] As the above-mentioned solution mixing method, for example, there can be cited the method of (IV) using commercially available particles containing EVOH resin (A) and / or polyamide resin (B4) to prepare a solution, adding a titanium compound (C) thereto, coagulating and forming it into particles, performing solid-liquid separation and drying; (V) in the manufacturing process of EVOH resin (A), making a uniform solution of saponified EVOH resin (water / alcohol solution, etc.) contain a solution of polyamide resin (B4) and / or titanium compound (C), coagulating and forming it into particles, performing solid-liquid separation and drying, etc.

[0419] Examples of the impregnation method include (VI) a method in which particles containing an EVOH resin (A) and / or a polyamide resin (B4) are brought into contact with an aqueous solution containing a titanium compound (C), the particles are impregnated with the titanium compound (C), and then dried.

[0420] In addition, in each of the above methods, EVOH resin (A) and / or polyamide resin (B4) and titanium compound (C) may be pre-blended in a specified ratio to prepare a composition (masterbatch) having a high concentration of titanium compound (C), and the composition (masterbatch) may be blended with EVOH resin (A) or polyamide resin (B4) to obtain a resin composition of the desired concentration.

[0421] Furthermore, the present invention may also combine the above-mentioned different methods. Among them, the melt mixing method is preferred, and the method (II) is particularly preferred, from the viewpoint of productivity and obtaining a resin composition having a more remarkable effect of the present invention.

[0422] Furthermore, when the above-mentioned optional components are blended into the resin composition, they may be blended into the resin composition by a method according to the above-mentioned production methods.

[0423] It should be noted that the shape of the pellets of the resin composition obtained by the above methods and the pellets containing the EVOH resin (A) and / or the polyamide resin (B4) used in the above methods is arbitrary, and any shape such as spherical, elliptical, cylindrical, cubic, and rectangular can be adopted. The shape of the pellets is usually elliptical or cylindrical. Regarding the size, in the case of a cylindrical shape, the diameter of the bottom surface is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm, from the perspective of convenience when used as a molding material later. In the case of an elliptical shape, the major diameter is usually 1.5 to 30 mm, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm, and the minor diameter is usually 1 to 10 mm, preferably 2 to 6 mm, and particularly preferably 2.5 to 5.5 mm. The method of measuring the major diameter and the minor diameter is, for example, to take a particle and observe it in the hand, measure the major diameter with a measuring instrument such as a vernier caliper, and then determine the position of the cross-section with the largest area in the cross-section perpendicular to the major diameter by visual inspection and touch, and similarly measure the minor diameter when assuming the cross-section.

[0424] It should be noted that when the EVOH resin composition is in the form of pellets, it is preferred to attach a known lubricant to the surface of the pellets from the perspective of stabilizing the feeding property during melt molding. Examples of the lubricant include higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters of higher fatty acids, etc.), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, behenic acid amide; unsaturated higher fatty acid amides such as oleic acid amide, erucic acid amide, bis-higher fatty acid amides such as ethylene bisstearic acid amide, ethylene bisoleic acid amide, ethylene biserucic acid amide, ethylene bislauric acid amide, etc.), low molecular weight polyolefins (e.g., low molecular weight polyethylene or low molecular weight polypropylene having a molecular weight of about 500 to 10,000, or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, fluorinated vinyl resins, etc. These compounds can be used alone or in combination of two or more. In addition, the content of the lubricant is usually 5% by mass or less, preferably 1% by mass or less of the EVOH resin composition. It should be noted that the lower limit is usually 0% by mass.

[0425] The EVOH resin composition obtained in this manner can suppress thermal degradation during heating, and the 5% weight loss temperature of the EVOH resin composition is usually 340°C or higher, preferably 341°C or higher, and particularly preferably 342°C or higher. In addition, the 10% weight loss temperature of the EVOH resin composition is usually 360°C or higher, preferably 361°C or higher, and particularly preferably 362°C or higher.

[0426] The upper limits of the 5% weight loss temperature and the 10% weight loss temperature are preferably as high as possible and are usually 450°C.

[0427] A difference of 1° C. in the above-mentioned weight loss temperature represents a significant difference in yield in actual production, and therefore, the difference is very large.

[0428] The above-mentioned "5% weight loss temperature" and "10% weight loss temperature" refer to the temperature (5% weight loss temperature) at which the weight of 5 mg of the present EVOH resin composition is reduced to 95% of the weight before measurement and the temperature (10% weight loss temperature) at which the weight is reduced to 90% of the weight before measurement, measured using a thermogravimetric measuring apparatus (manufactured by Perkin Elmer, Pyris 1TGA) in a nitrogen atmosphere at an air flow rate of 20 mL / min, a heating rate of 10°C / min, and a temperature range of 30 to 550°C.

[0429] The water content of the present EVOH resin composition is usually 0.01 to 0.5% by mass, preferably 0.05 to 0.35% by mass, and particularly preferably 0.1 to 0.3% by mass.

[0430] The water content of the present EVOH resin composition is measured and calculated by the following method.

[0431] The mass (W1) of the EVOH resin composition before drying was measured using an electronic balance, dried in a hot air dryer at 150°C for 5 hours, cooled in the dryer for 30 minutes, and then the mass (W2) was measured and calculated using the following formula.

[0432] <Formula>

[0433] Water content (mass %) = [(W1-W2) / W1] × 100

[0434] The EVOH resin composition can be prepared into various forms such as powder and liquid in addition to pellets, and provided as a molding material for various molded objects. In particular, in the present invention, when provided as a material for melt molding, there is a tendency to more effectively obtain the effect of the present invention, so it is preferred.

[0435] The present EVOH resin composition also includes a resin composition obtained by mixing the EVOH resin (A) used in the present EVOH resin composition with a resin other than the polyamide-based resin (B4).

[0436] Examples of the molded product include a single-layer film molded from the present EVOH resin composition, and a multilayer structure having a layer composed of the present EVOH resin composition.

[0437] [Multilayer structure]

[0438] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the present multilayer structure") comprises a layer composed of the present EVOH resin composition. The layer composed of the present EVOH resin composition (hereinafter referred to as "the present EVOH resin composition layer") can be further provided with strength, or the present EVOH resin composition layer can be protected from the influence of moisture, etc., or other functions can be provided by laminating it with another substrate having a thermoplastic resin other than the EVOH resin composition as a main component (hereinafter, the resin used in the substrate is sometimes referred to as "substrate resin").

[0439] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers, ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polybutene, polypentene, (unmodified) polyolefin resins including polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and these polyolefin resins. The polyolefin resins in a broad sense of modified olefin resins such as unsaturated carboxylic acid-modified polyolefin resins obtained by adhesively grafting hydrocarbons with unsaturated carboxylic acids or their esters, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, chlorinated polyethylene, chlorinated polypropylene and other halogenated polyolefins, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.

[0440] Among these, polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred as the hydrophobic resin, and polyethylene resins, polypropylene resins, polycyclic olefin resins, and polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins thereof are more preferred. It is particularly preferred to use polycyclic olefin resins as the hydrophobic resin.

[0441] When the EVOH resin composition layer is a (a1, a2, ...) and the substrate resin layer is b (b1, b2, ...), the layer structure of the multilayer structure may be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc. In addition, when the recycled layer including a mixture of the EVOH resin composition and a thermoplastic resin other than the EVOH resin composition obtained by remelting and molding the end portions, defective products, etc. generated in the process of manufacturing the multilayer structure is R, it may be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The number of layers of the multilayer structure is usually 2 to 15 in total, preferably 3 to 10. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be interposed between the layers as necessary.

[0442] As the above-mentioned adhesive resin, a known resin can be used, as long as it is appropriately selected according to the type of thermoplastic resin used in the substrate resin layer "b". Representative examples include modified polyolefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to polyolefin resins using addition reactions, grafting reactions, etc. As the above-mentioned modified polyolefin polymers containing carboxyl groups, for example, maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block and random) copolymers, maleic anhydride grafted modified ethylene-ethyl acrylate copolymers, maleic anhydride grafted modified ethylene-vinyl acetate copolymers, maleic anhydride modified polycyclic olefin resins, maleic anhydride grafted modified polyolefin resins, etc. can be cited. They can be used alone or in combination of two or more.

[0443] In the present multilayer structure, when an adhesive resin layer is used between the present EVOH resin composition layer and the base resin layer, since the adhesive resin layer is located on both sides of the present EVOH resin composition layer, an adhesive resin having excellent hydrophobicity is preferably used.

[0444] The above-mentioned base resin and adhesive resin may also contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, nucleating agents, antiblocking agents, waxes, etc. within a range that does not hinder the purpose of the present invention (for example, 30% by mass or less, preferably 10% by mass or less relative to the entire resin). These may be used alone or in combination of two or more.

[0445] The lamination of the above-mentioned EVOH resin composition layer and the above-mentioned substrate resin layer (including the case where an adhesive resin layer is interposed) can be carried out by a known method. For example, there can be cited a method of melt-extrusion lamination of the substrate resin on a film, sheet, etc. of the present EVOH resin composition; a method of melt-extrusion lamination of the present EVOH resin composition on a substrate resin layer; a method of co-extruding the present EVOH resin composition and the substrate resin; a method of dry lamination of the present EVOH resin composition (layer) and the substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc.; a method of removing the solvent after applying a solution of the present EVOH resin composition on the substrate resin, etc. Among these, from the viewpoint of cost and environment, it is preferred to manufacture by a process of melt-molding the present EVOH resin composition layer, and specifically, a co-extrusion method is preferred.

[0446] The present multilayer structure may also be subjected to (heating) stretching treatment as required. The stretching treatment may be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, it may be simultaneous stretching or sequential stretching. In addition, as a stretching method, a stretching method with a high stretching ratio such as a roller stretching method, a tentering stretching method, a tubular stretching method, a stretch blow molding method, and a vacuum pressure molding method may be adopted. The stretching temperature is a temperature near the melting point of the multilayer structure, usually selected from the range of 40 to 170°C, preferably about 60 to 160°C. When the stretching temperature is too low, the stretchability becomes poor, and when it is too high, it is difficult to maintain a stable stretched state.

[0447] In addition, for the purpose of imparting dimensional stability, the stretched multilayer structure may be heat-fixed. Heat-fixing may be performed by a known method, for example, by heat-treating the stretched multilayer structure at a temperature of usually 80 to 180° C., preferably 100 to 165° C., for usually 2 to 600 seconds while maintaining the stretched multilayer structure in a tensioned state.

[0448] When the stretched multilayer structure is used as a shrink film, in order to impart heat shrinkage, the stretched multilayer structure may be cooled and fixed by blowing cold air instead of the heat setting.

[0449] The thickness of the present multilayer structure (including the stretched multilayer structure), and the thickness of the present EVOH resin composition layer, the base resin layer and the adhesive resin layer constituting the multilayer structure vary depending on the layer constitution, the type of base resin, the type of adhesive resin, the application, the packaging form, the required physical properties, etc., and cannot be generalized. The thickness of the present multilayer structure (including the stretched multilayer structure) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0450] Furthermore, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the substrate resin layer in the present multilayer structure (present EVOH resin composition layer / substrate resin layer) is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60, as a ratio of the thickest layers. In addition, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the adhesive resin layer in the present multilayer structure (present EVOH resin composition layer / adhesive resin layer) is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10, as a ratio of the thickest layers.

[0451] In addition, the present multilayer structure can also be used to obtain a cup or tray-shaped multilayer container. In this case, a deep drawing method is usually used, and specifically, vacuum forming, pressure forming, vacuum pressure forming, plunger-assisted vacuum pressure forming, etc. can be cited. Furthermore, when a tubular or bottle-shaped multilayer container (laminated structure) is obtained from a multilayer parison (a hollow tubular preform before blow molding), a blow molding method can be used. Specifically, extrusion blow molding (double-head type, mold moving type, parison moving type, rotary type, accumulation type, horizontal parison type, etc.), cold parison blow molding, injection blow molding, biaxial stretch blow molding (extrusion cold parison biaxial stretch blow molding, injection cold parison biaxial stretch blow molding, injection molding embedded biaxial stretch blow molding, etc.) can be cited. The obtained laminate can be subjected to heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making processing, deep drawing processing, box processing, tube processing, slitting processing, etc. as needed.

[0452] The monolayer film formed from the present EVOH resin composition, the bag formed from the present multilayer structure, and the container and cover material formed from cups, trays, tubes, bottles, etc. are useful as various packaging materials for seasonings such as mayonnaise and dressing, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, and pharmaceuticals, in addition to general foods. In particular, the present EVOH resin composition layer has excellent resistance to hot water treatment and excellent thermal stability, and is therefore particularly useful as a packaging material for hot water sterilization of foods, pharmaceuticals, pesticides, etc.

[0453] << Fifth Method >>

[0454] EVOH resin has excellent transparency, oxygen and other gas barrier properties, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and is molded into films, sheets, bottles, etc. and is widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and pesticide packaging materials.

[0455] However, EVOH resin has a relatively active hydroxyl group in the molecule and therefore tends to be easily degraded by heat, and is prone to coloring during melt molding.

[0456] In order to solve the above-mentioned problems, Patent Document 1 discloses, for example, that EVOH resin contains an unsaturated aldehyde to suppress oxidative degradation during melt molding of the EVOH resin and thereby suppress coloration.

[0457] Patent Document 1: International Publication No. 2013 / 146961

[0458] However, even a trace amount of aldehyde compounds such as the above-mentioned unsaturated aldehydes may sometimes cause bad odors. In particular, there is a concern that the aldehyde compounds may volatilize during the molding process exposed to high temperatures and deteriorate the working environment. In addition, the improvement effects on the long-term operation moldability such as the suppression of oxidative degradation during heating such as melt mixing and melt molding are not sufficient. Therefore, there is a strong need for an EVOH resin composition that does not deteriorate the working environment, is not easily thermally degraded during heating, and can produce high-quality molded products.

[0459] An object of the present invention is to provide an EVOH resin composition in which thermal degradation of the EVOH resin during heating such as melt molding is suppressed.

[0460] In view of the above circumstances, the present inventors have found that by adding a styrene derivative having a substituent at the α-position and a specific trace amount of a titanium compound to an EVOH resin, an EVOH resin composition can be obtained in which thermal degradation of the EVOH resin during heating such as melt molding is suppressed.

[0461] That is, the present invention has the following aspects.

[0462] [5-1] An EVOH resin composition comprising an EVOH resin (A), a styrene derivative (B5) having a substituent at the α-position, and a titanium compound (C),

[0463] The metal-equivalent content of the titanium compound (C) is 0.001 ppm or more and less than 5 ppm based on the mass of the EVOH resin composition.

[0464] [5-2] The EVOH resin composition according to [5-1], wherein the content of the styrene derivative (B5) having a substituent at the α-position is 1 to 10000 ppm based on the mass of the EVOH resin composition.

[0465] [5-3] The EVOH resin composition according to [5-1] or [5-2], wherein the mass ratio of the content of the styrene derivative (B5) having a substituent at the α-position to the metal-equivalent content of the titanium compound (C) is 0.2 to 10,000,000.

[0466] [5-4] The EVOH resin composition according to any one of [5-1] to [5-3], wherein the styrene derivative (B5) having a substituent at the α-position is an α-methylstyrene derivative.

[0467] [5-5] A pellet comprising the EVOH resin composition according to any one of [5-1] to [5-4].

[0468] [5-6] A multilayer structure comprising at least one layer comprising the EVOH resin composition according to any one of [5-1] to [5-4].

[0469] [5-7] A method for producing an EVOH resin composition, the method comprising producing the EVOH resin composition described in any one of [5-1] to [5-4].

[0470] The method comprises the step of melt-mixing a composition raw material containing the EVOH resin and the titanium compound.

[0471] [5-8] A method for producing a multilayer structure, which is a method for producing the multilayer structure described in [5-6], comprising the step of melt-molding a layer composed of the EVOH resin composition.

[0472] The EVOH resin composition of the present invention is excellent in thermal stability and therefore can suppress thermal degradation of the EVOH resin during melt molding.

[0473] Hereinafter, the present invention will be described in more detail based on embodiments of the present invention, but the present invention is not limited to these embodiments.

[0474] <EVOH Resin Composition>

[0475] The EVOH resin composition of one embodiment of the present invention (hereinafter referred to as "this EVOH resin composition") has an EVOH resin (A) as the main component, and contains a styrene derivative (B5) having a substituent at the α-position and a specific trace amount of a titanium compound (C).

[0476] That is, in this EVOH resin composition, the base resin is the EVOH resin (A), and the content of the EVOH resin (A) in this EVOH resin composition is usually 70% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 95% by mass or more.

[0477] Hereinafter, each component will be described.

[0478] [EVOH Resin (A)]

[0479] The EVOH resin (A) used in the present invention is usually a resin obtained by saponifying an ethylene-vinyl ester copolymer which is a copolymer of ethylene and a vinyl ester monomer, and the same resin as the (A) component described in the above first embodiment can be used.

[0480] [Styrene Derivative (B5) Having a Substituent at the α-Position]

[0481] The above styrene derivative having a substituent at the α-position (hereinafter sometimes referred to as "specific styrene derivative") (B5) used in the present invention is a compound having a styrene molecular structure as a molecular skeleton in an aromatic compound having the ability to resonate-stabilize and capture free radicals and having a substituent at the α-position.

[0482] As the above specific styrene derivative (B5), for example, α-methylstyrene derivatives can be cited. Specifically, α-methylstyrene, 4-tert-butylstyrene, 4-methoxystyrene, 2-acetoxystyrene, 2,4-diphenyl-4-methyl-1-pentene, etc. can be cited. Among them, from the aspect of suppressing thermal deterioration as an effect of the present invention, 2,4-diphenyl-4-methyl-1-pentene which stabilizes free radical resonance through having a benzyl position is preferred.

[0483] The molecular weight of the above specific styrene derivative (B5) is usually 100 to 100,000, preferably 100 to 10,000, particularly preferably 100 to 1,000, and especially preferably 130 to 300. When the molecular weight is in the above range, there is a tendency to more effectively obtain the effects of the present invention.

[0484] The content of the specific styrene derivative (B5) is preferably 1 to 10,000 ppm, more preferably 100 to 8,000 ppm, particularly preferably 300 to 5,000 ppm, further preferably 500 to 4,000 ppm, and particularly preferably 1,000 to 3,000 ppm relative to the mass of the EVOH resin composition. If it is too much, productivity tends to decrease, and if it is too little, thermal stability tends to decrease.

[0485] It should be noted that the EVOH resin composition serving as a basis for the content ratio of the above-mentioned specific styrene derivative (B5) is an EVOH resin composition as a final product containing EVOH resin (A), specific styrene derivative (B5), titanium compound (C), and various additives blended as needed.

[0486] The content of the specific styrene derivative (B5) in the present EVOH resin composition can be measured, for example, using thermal extraction-cooling concentration introduction-gas chromatography mass spectrometry (TD-CI-GC / MS) under the following conditions.

[0487] <Method for Determining Content of Styrene Derivative (B5)>

[0488] [TD-CI-GC / MS measurement conditions]

[0489] (TDS section conditions)

[0490] Equipment used: TDS-2 [GERSTEL]

[0491] Sample mode: standby cooling

[0492] Flow mode: splitless

[0493] Standby temperature: 20℃

[0494] Transfer temperature: 250℃

[0495] Initial temperature: 20℃

[0496] Initial time: 4 minutes

[0497] 1 st Rate (1st rate): 60℃ / min

[0498] 1 st Final temperature (1st final temp): 200℃

[0499] 1 st Final time: 60 minutes

[0500] (CIS Department Conditions)

[0501] Equipment used: CIS-4 [GERSTEL]

[0502] Initial temperature: -150℃

[0503] Initial time: 1min

[0504] 1 st Rate (1st rate): 12℃ / sec

[0505] 1 st Final temperature: 250℃

[0506] 1 st Final time: 5 minutes

[0507] Equilib.time: 0.5min

[0508] (Split ratio: 30:1)

[0509] (GC / MS conditions)

[0510] Equipment used: 7890A (GC)-5977 (MS) quadrupole [Agilent Technologies]

[0511] Column: DB-WAX [Agilent Technologies]

[0512] Length × inner diameter × film thickness = 30m × 0.25mm × 0.25μm

[0513] Temperature: OVEN40℃(5min hold)-Rate10℃ / min-250℃(10min hold)

[0514] INJ250℃AUX250℃

[0515] Carrier gas: He (Flow 1mL / min, constant flow)

[0516] Split ratio: 30:1

[0517] Measurement mode: SIM (m / z = 91, 119, 236)

[0518] Solvent waiting time: 10min

[0519] [Titanium compound (C)]

[0520] Examples of the titanium compound (C) used in the present invention include inorganic titanium compounds and organic titanium compounds. As the titanium compound, the same titanium compound as the component (C) described in the first embodiment can be used.

[0521] The metal conversion content of the above-mentioned titanium compound (C) is greater than 0.001ppm and less than 5ppm relative to the mass of the EVOH resin composition. It is preferably 0.01 to 3ppm, more preferably 0.03 to 1ppm, and particularly preferably 0.05 to 0.5ppm. By making the content of the titanium compound (C) within the above range, thermal degradation during melt molding can be suppressed, and long-term operation performance is excellent. In addition, if the content of the titanium compound (C) is too little, the effect of suppressing thermal degradation is reduced. If the content is too much, thermal decomposition of the EVOH resin is likely to occur, and it is easy to color.

[0522] The metal conversion content of the above-mentioned titanium compound (C) can be quantified by the following operation: weigh the EVOH resin composition into a platinum crucible, incinerate it using a burner and an electric furnace in sequence, heat and decompose the ash with nitric acid and hydrofluoric acid, treat it with a mixed acid of dilute nitric acid and dilute hydrofluoric acid and make it constant, and use an ICP mass spectrometer (manufactured by Agilent Technologies, Agilent 8800) to determine the titanium in the obtained constant solution by ICP mass spectrometry.

[0523] The mass ratio of the content of the above-mentioned specific styrene derivative (B5) to the metal conversion content of the above-mentioned titanium compound (C) is preferably 0.2 to 10,000,000, more preferably 0.3 to 1,000,000, further preferably 100 to 270,000, particularly preferably 600 to 100,000, particularly preferably 800 to 50,000, and further preferably 1,000 to 30,000.

[0524] When this value is too large, the ultraviolet absorption ability of the present EVOH resin composition tends to decrease, and when it is too small, the thermal stability tends to decrease.

[0525] Here, it is generally known that EVOH resin deteriorates due to heat. The reason is believed to be as follows. That is, it is believed that the EVOH resin deteriorates due to heat, generating free radicals, and the hydroxyl groups possessed by the EVOH resin undergo a dehydration reaction due to the free radicals, thereby generating a double bond structure in the main chain of the EVOH resin. Moreover, this site becomes a reaction starting point, and further dehydration reaction occurs, etc., forming a polyene structure in the main chain of the EVOH resin.

[0526] Furthermore, generally, when a titanium compound is contained in an EVOH resin composition, it is considered that the EVOH resin composition is colored by titanium ions, and therefore it is common technical knowledge for those skilled in the art to avoid using the titanium compound.

[0527] However, the present invention goes against such common technical knowledge and finds that when a specific styrene derivative (B5) is used in combination with a specific trace amount of a titanium compound (C), an EVOH resin composition in which thermal degradation is significantly suppressed can be obtained.

[0528] That is, it is speculated that titanium is stable as a tetravalent ion, and even in a trace amount, it coordinates to the double bonds of the main chain of the EVOH resin as described above, forms a chelate or the like to stabilize, and thus further suppresses the formation of a polyene structure. In addition, it is speculated that the coexistence of the specific styrene derivative (B5) and the titanium compound (C) can more effectively exert the stabilizing effect based on the titanium compound (C).

[0529] On the other hand, if the content of the titanium compound (C) is too large, it is considered that thermal decomposition of the EVOH resin occurs due to the titanium compound (C). Therefore, in the present invention, the content of the titanium compound (C) is limited to a specific trace amount.

[0530] [Other thermoplastic resins]

[0531] The present EVOH resin composition may contain other thermoplastic resins other than the EVOH resin (A) within a range that does not inhibit the effects of the present invention (e.g., usually 30% by mass or less, preferably 20% by mass or less, particularly preferably 10% by mass or less of the present EVOH resin composition).

[0532] As other thermoplastic resins, known thermoplastic resins can be used, for example, polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more.

[0533] [Other compounding ingredients]

[0534] The EVOH resin composition may contain a compounding agent generally compounded with an EVOH resin within a range that does not inhibit the effects of the present invention. As the compounding agent, the same compounding agent as described in the first embodiment can be used.

[0535] [Method for producing EVOH resin composition]

[0536] The present EVOH resin composition can be produced by mixing the above-mentioned EVOH resin (A), the specific styrene derivative (B5) and the titanium compound (C) by a known method, such as a dry blending method, a melt mixing method, a solution mixing method, an impregnation method, etc. Among these, it is preferably produced by a process of melt mixing the composition raw materials containing the above-mentioned EVOH resin and the titanium compound. In addition, these production methods can also be arbitrarily combined.

[0537] Examples of the dry blending method include (i) a method of dry blending a pelletized EVOH resin (A), a specific styrene derivative (B5), and a titanium compound (C) using a tumbler or the like.

[0538] As the above-mentioned melt mixing method, for example, there can be cited (ii) a method in which a granular EVOH resin (A) is dry-blended with a specific styrene derivative (B5) and a titanium compound (C) and a dry blend is melt-kneaded to obtain granules or other molded products; (iii) a method in which a specific styrene derivative (B5) and / or a titanium compound (C) are added to a molten EVOH resin (A) and the mixture is melt-kneaded to obtain granules or other molded products, etc.

[0539] As the above-mentioned solution mixing method, for example, there can be cited the following method: (iv) a method in which a solution is prepared using a granular EVOH resin (A), a specific styrene derivative (B5) and / or a titanium compound (C) is added thereto, the solution is solidified and granulated, and then the solid-liquid separation and drying are carried out using a known method; (v) a method in which, during the manufacturing process of the EVOH resin (A), a uniform solution of the EVOH resin before saponification (water / alcohol solution, etc.) is made to contain a specific styrene derivative (B5) and / or a titanium compound (C), the solution is solidified and granulated, and then the solid-liquid separation and drying is carried out using a known method, etc.

[0540] As the above-mentioned impregnation method, for example, there can be cited a method of (vi) contacting a granular EVOH resin (A) with an aqueous solution containing a specific styrene derivative (B5) and / or a titanium compound (C), allowing the EVOH resin (A) to contain the above-mentioned specific styrene derivative (B5) and / or titanium compound (C) and then drying the mixture.

[0541] As the aqueous solution containing the titanium compound (C), an aqueous solution of the titanium compound (C) or an aqueous solution obtained by immersing the titanium compound (C) in water containing various chemicals to dissolve titanium ions can be used. The same applies to the aqueous solution containing the specific styrene derivative (B5).

[0542] In addition, it should be noted that in the above-mentioned impregnation method, the content (metal conversion) of the specific styrene derivative (B5) and the titanium compound (C) can be controlled by the concentration of the specific styrene derivative (B5) and the titanium compound (C) in the aqueous solution in which the EVOH resin (A) is impregnated, the impregnation temperature, the impregnation time, etc.

[0543] The immersion time is usually 0.5 to 48 hours, preferably 1 to 36 hours, and the immersion temperature is usually 10 to 40°C, preferably 20 to 35°C.

[0544] In addition, various drying methods can be used as the drying method in each of the above-mentioned production methods, and any of static drying and fluidized drying can be used. In addition, these methods can also be combined.

[0545] In order to obtain the present EVOH resin composition, as described above, these various methods can be combined. Among them, from the perspective of productivity and obtaining a resin composition with a more significant effect of the present invention, the melt mixing method is preferred, and the method (ii) is particularly preferred. In addition, when using the above-mentioned other thermoplastic resins and other compounding agents, they can also be compounded by conventional methods according to the above-mentioned manufacturing method.

[0546] The EVOH resin composition obtained in this manner may be in any shape, but is preferably in the form of pellets.

[0547] As the above-mentioned particles, for example, there are spherical, elliptical, cylindrical, cubic, rectangular parallelepiped, etc., usually elliptical or cylindrical, and its size is considered from the perspective of convenience when used as a molding material later. In the case of an elliptical shape, the short diameter is usually 1 to 10 mm, preferably 2 to 6 mm, and more preferably 2.5 to 5.5 mm, and the long diameter is usually 1.5 to 30 mm, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm. In addition, in the case of a cylindrical shape, the diameter of the bottom surface is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm.

[0548] In addition, it is preferable that the shape and size of the pelletized EVOH resin (A) used in each of the above-mentioned production methods are also the same.

[0549] It should be noted that when the EVOH resin composition is in the form of pellets, it is preferred to attach a known lubricant to the surface of the pellets from the perspective of stabilizing the feeding property during melt molding. Examples of the lubricant include higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters of higher fatty acids, etc.), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, behenic acid amide; unsaturated higher fatty acid amides such as oleic acid amide, erucic acid amide, bis-higher fatty acid amides such as ethylene bisstearic acid amide, ethylene bisoleic acid amide, ethylene biserucic acid amide, ethylene bislauric acid amide, etc.), low molecular weight polyolefins (e.g., low molecular weight polyethylene or low molecular weight polypropylene having a molecular weight of about 500 to 10,000, or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, fluorinated vinyl resins, etc. These compounds can be used alone or in combination of two or more. In addition, the content of the lubricant is usually 5% by mass or less, preferably 1% by mass or less of the EVOH resin composition. It should be noted that the lower limit is usually 0% by mass.

[0550] The EVOH resin composition obtained in this manner can suppress thermal degradation during heating, and the 5% weight loss temperature of the EVOH resin composition is usually 330°C or higher, preferably 331°C or higher. In addition, the 10% weight loss temperature of the EVOH resin composition is usually 351°C or higher, preferably 352°C or higher, and particularly preferably 353°C or higher.

[0551] The upper limits of the 5% weight loss temperature and the 10% weight loss temperature are preferably as high as possible and are usually 450°C.

[0552] A difference of 1° C. in the above-mentioned weight loss temperature represents a significant difference in yield in actual production, and therefore, the difference is very large.

[0553] The above-mentioned "5% weight loss temperature" and "10% weight loss temperature" refer to the temperature (5% weight loss temperature) at which the weight of 5 mg of the present EVOH resin composition is reduced to 95% of the weight before measurement and the temperature (10% weight loss temperature) at which the weight is reduced to 90% of the weight before measurement, measured using a thermogravimetric measuring apparatus (manufactured by Perkin Elmer, Pyris 1TGA) in a nitrogen atmosphere at an air flow rate of 20 mL / min, a heating rate of 10°C / min, and a temperature range of 30 to 550°C.

[0554] The water content of the present EVOH resin composition is usually 0.01 to 0.5% by mass, preferably 0.05 to 0.35% by mass, and particularly preferably 0.1 to 0.3% by mass.

[0555] The water content of the present EVOH resin composition is measured and calculated by the following method.

[0556] The mass (W1) of the EVOH resin composition before drying was measured using an electronic balance, dried in a hot air dryer at 150°C for 5 hours, cooled in the dryer for 30 minutes, and then the mass (W2) was measured and calculated using the following formula.

[0557] <Formula>

[0558] Water content (mass %) = [(W1-W2) / W1] × 100

[0559] The EVOH resin composition can be prepared into various forms such as powder and liquid in addition to pellets, and provided as a molding material for various molded objects. In particular, in the present invention, when provided as a material for melt molding, there is a tendency to more effectively obtain the effect of the present invention, so it is preferred.

[0560] In addition, the present EVOH resin composition also includes a resin composition obtained by mixing a resin other than the EVOH resin (A) used in the present EVOH resin composition.

[0561] Examples of the molded product include a single-layer film molded from the present EVOH resin composition, and a multilayer structure having a layer composed of the present EVOH resin composition.

[0562] [Multilayer structure]

[0563] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the present multilayer structure") comprises a layer composed of the present EVOH resin composition. The layer composed of the present EVOH resin composition (hereinafter referred to as "the present EVOH resin composition layer") can be further provided with strength, or the present EVOH resin composition layer can be protected from the influence of moisture, etc., or other functions can be provided by laminating it with another substrate having a thermoplastic resin other than the EVOH resin composition as a main component (hereinafter, the resin used in the substrate is sometimes referred to as "substrate resin").

[0564] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers, ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polybutene, polypentene, (unmodified) polyolefin resins including polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and these polyolefin resins. Modified olefin resins in a broad sense include unsaturated carboxylic acid-modified polyolefin resins obtained by adhesively grafting hydrocarbons with unsaturated carboxylic acids or their esters, polyolefin resins, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, chlorinated polyethylene, chlorinated polypropylene and other halogenated polyolefins, aromatic or aliphatic polyketones, and the like.

[0565] Among these, polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred as the hydrophobic resin, and polyethylene resins, polypropylene resins, polycyclic olefin resins, and polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins thereof are more preferred. It is particularly preferred to use polycyclic olefin resins as the hydrophobic resin.

[0566] When the EVOH resin composition layer is a (a1, a2, ...) and the substrate resin layer is b (b1, b2, ...), the layer structure of the multilayer structure may be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc. In addition, when the recycled layer including a mixture of the EVOH resin composition and a thermoplastic resin other than the EVOH resin composition obtained by remelting and molding the end portions, defective products, etc. generated in the process of manufacturing the multilayer structure is R, it may be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The number of layers of the multilayer structure is usually 2 to 15 in total, preferably 3 to 10. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be interposed between the layers as necessary.

[0567] As the above-mentioned adhesive resin, a known resin can be used, as long as it is appropriately selected according to the type of thermoplastic resin used in the substrate resin layer "b". Representative examples include modified polyolefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to polyolefin resins using addition reactions, grafting reactions, etc. As the above-mentioned modified polyolefin polymers containing carboxyl groups, for example, maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block and random) copolymers, maleic anhydride grafted modified ethylene-ethyl acrylate copolymers, maleic anhydride grafted modified ethylene-vinyl acetate copolymers, maleic anhydride modified polycyclic olefin resins, maleic anhydride grafted modified polyolefin resins, etc. can be cited. They can be used alone or in combination of two or more.

[0568] In the present multilayer structure, when an adhesive resin layer is used between the present EVOH resin composition layer and the base resin layer, since the adhesive resin layer is located on both sides of the present EVOH resin composition layer, an adhesive resin having excellent hydrophobicity is preferably used.

[0569] The above-mentioned base resin and adhesive resin may also contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, nucleating agents, antiblocking agents, waxes, etc. within a range that does not hinder the purpose of the present invention (for example, 30% by mass or less, preferably 10% by mass or less relative to the entire resin). These may be used alone or in combination of two or more.

[0570] The lamination of the above-mentioned EVOH resin composition layer and the above-mentioned substrate resin layer (including the case where an adhesive resin layer is interposed) can be carried out by a known method. For example, there can be cited a method of melt-extrusion lamination of the substrate resin on a film, sheet, etc. of the present EVOH resin composition; a method of melt-extrusion lamination of the present EVOH resin composition on a substrate resin layer; a method of co-extruding the present EVOH resin composition and the substrate resin; a method of dry lamination of the present EVOH resin composition (layer) and the substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc.; a method of removing the solvent after applying a solution of the present EVOH resin composition on the substrate resin, etc. Among these, from the viewpoint of cost and environment, it is preferred to manufacture by a process of melt-molding the present EVOH resin composition layer, and specifically, a co-extrusion method is preferred.

[0571] The present multilayer structure may also be subjected to (heating) stretching treatment as required. The stretching treatment may be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, it may be simultaneous stretching or sequential stretching. In addition, as a stretching method, a stretching method with a high stretching ratio such as a roller stretching method, a tentering stretching method, a tubular stretching method, a stretch blow molding method, and a vacuum pressure molding method may be adopted. The stretching temperature is a temperature near the melting point of the multilayer structure, usually selected from the range of 40 to 170°C, preferably about 60 to 160°C. When the stretching temperature is too low, the stretchability becomes poor, and when it is too high, it is difficult to maintain a stable stretched state.

[0572] In addition, for the purpose of imparting dimensional stability, the stretched multilayer structure may be heat-fixed. Heat-fixing may be performed by a known method, for example, by heat-treating the stretched multilayer structure at a temperature of usually 80 to 180° C., preferably 100 to 165° C., for usually 2 to 600 seconds while maintaining the stretched multilayer structure in a tensioned state.

[0573] When the stretched multilayer structure is used as a shrink film, in order to impart heat shrinkage, the stretched multilayer structure may be cooled and fixed by blowing cold air instead of the heat setting.

[0574] The thickness of the present multilayer structure (including the stretched multilayer structure), and the thickness of the present EVOH resin composition layer, the base resin layer and the adhesive resin layer constituting the multilayer structure vary depending on the layer constitution, the type of base resin, the type of adhesive resin, the application, the packaging form, the required physical properties, etc., and cannot be generalized. The thickness of the present multilayer structure (including the stretched multilayer structure) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0575] Furthermore, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the substrate resin layer in the present multilayer structure (present EVOH resin composition layer / substrate resin layer) is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60, as a ratio of the thickest layers. In addition, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the adhesive resin layer in the present multilayer structure (present EVOH resin composition layer / adhesive resin layer) is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10, as a ratio of the thickest layers.

[0576] In addition, the present multilayer structure can also be used to obtain a cup or tray-shaped multilayer container. In this case, a deep drawing method is usually used, and specifically, vacuum forming, pressure forming, vacuum pressure forming, plunger-assisted vacuum pressure forming, etc. can be cited. Furthermore, when a tubular or bottle-shaped multilayer container (laminated structure) is obtained from a multilayer parison (a hollow tubular preform before blow molding), a blow molding method can be used. Specifically, extrusion blow molding (double-head type, mold moving type, parison moving type, rotary type, accumulation type, horizontal parison type, etc.), cold parison blow molding, injection blow molding, biaxial stretch blow molding (extrusion cold parison biaxial stretch blow molding, injection cold parison biaxial stretch blow molding, injection molding embedded biaxial stretch blow molding, etc.) can be cited. The obtained laminate can be subjected to heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making processing, deep drawing processing, box processing, tube processing, slitting processing, etc. as needed.

[0577] The single-layer film formed from the present EVOH resin composition, the bag composed of the present multilayer structure, and the container and cover materials composed of cups, trays, tubes, bottles, etc. are useful as various packaging materials for not only general foods but also seasonings such as mayonnaise and sauces, fermented foods such as miso, oily foods such as salad oils, beverages, cosmetics, and pharmaceuticals.

[0578] Example

[0579] The present invention is specifically described below using examples. However, the present invention is not limited to the following examples. It should be noted that "parts" in the examples are based on mass unless otherwise specified.

[0580] <<1st Method>>

[0581] <Example 1-1>

[0582] As the EVOH resin (A), pellets of EVOH resin having an ethylene structural unit content of 29 mol %, a saponification degree of 99.6 mol %, and an MFR of 4 g / 10 min (210° C., a load of 2160 g) were used.

[0583] Zinc stearate (manufactured by Nitto Kasei Kogyo Co., Ltd., Zn—St) was used as the metal compound (B1) belonging to the specific period d-block, and titanium oxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the titanium compound (C).

[0584] The EVOH resin (A) pellets were dry-blended with 45 ppm of zinc stearate in metal conversion relative to the mass of the EVOH resin composition and 0.1 ppm of titanium oxide in metal conversion relative to the mass of the EVOH resin composition to obtain a mixture. The mixture was then supplied to a twin-screw extruder equipped with a twin-hole die. The strands extruded and discharged under the following extrusion conditions were air-cooled and solidified on a belt conveyor. Then, the solidified strands were cut to obtain pellets of the EVOH resin composition.

[0585] [Extrusion conditions]

[0586] Extruder set temperature (℃): C1 / C2 / C3 / C4 / C5 / C6

[0587] =150 / 200 / 210 / 210 / 210 / 210

[0588] <Example 1-2>

[0589] Pellets of an EVOH resin composition were obtained in the same manner as in Example 1-1 except that the amount of titanium oxide blended in Example 1-1 was changed to 1 ppm in terms of metal relative to the mass of the EVOH resin composition.

[0590] <Comparative Example 1-1>

[0591] In Example 1-1, pellets of an EVOH resin composition were obtained in the same manner as in Example 1-1 except that titanium oxide was not used.

[0592] <Comparative Example 1-2>

[0593] Pellets of an EVOH resin composition were obtained in the same manner as in Example 1-1 except that the amount of titanium oxide blended in Example 1-1 was changed to 10 ppm in terms of metal relative to the mass of the EVOH resin composition.

[0594] The following thermal stability evaluation was performed using the obtained pellets of the EVOH resin compositions of Examples 1-1 and 1-2 and Comparative Examples 1-1 and 1-2. The results are shown in Table 1-1 described below.

[0595] 〔Thermal stability evaluation〕

[0596] Using 5 mg of the obtained EVOH resin composition pellets, the weight was measured using a thermogravimetric measuring apparatus (manufactured by PerkinElmer, Pyris 1TGA) under a nitrogen atmosphere at an air flow rate of 20 mL / min, a temperature of 230° C., and a time of 1 hour, and the weight reduction rate was calculated using the following formula. The lower the value, the less decomposed the resin composition is, which means that the resin composition has excellent thermal stability.

[0597] <Formula>

[0598] Weight reduction rate (%) = [(weight before heating - weight after heating) / weight before heating] × 100

[0599] [Table 1-1]

[0600]

[0601] According to the above Table 1-1, the EVOH resin compositions of Examples 1-1 and 1-2 containing a metal compound (B1) belonging to a specific period d zone and a specific trace amount of a titanium compound (C) have a smaller weight loss rate and excellent thermal stability than the EVOH resin composition of Comparative Example 1-1 that does not contain the titanium compound (C) and the EVOH resin composition of Comparative Example 1-2 that contains a larger amount of a titanium compound (C) than the specific range.

[0602] Furthermore, the multilayered structure including the layer composed of the EVOH resin composition of Examples 1-1 and 1-2 was also suppressed from thermal degradation and was excellent in thermal stability.

[0603] <<Method 2>>

[0604] <Example 2-1>

[0605] As the EVOH resin (A), pellets of EVOH resin having an ethylene structural unit content of 29 mol %, a saponification degree of 99.6 mol %, and an MFR of 4 g / 10 min (210° C., a load of 2160 g) were used.

[0606] As the polyolefin resin (B2), polypropylene (manufactured by JAPAN POLYPROPY LENE CORPORATION, EA9, density: 0.90 g / cm 3 ), and titanium oxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the titanium compound (C).

[0607] 150 parts of the pellets of the EVOH resin (A), 2850 parts of the polyolefin resin (B2) and 0.01 ppm of the titanium oxide in terms of metal content relative to the mass of the EVOH resin composition were dry-blended to obtain a mixture. The mixture was then supplied to a twin-screw extruder equipped with a twin-hole die. The strands extruded and discharged under the following extrusion conditions are cooled and solidified in a water tank. Next, air is blown to the solidified strands to remove water droplets on the strand surface, and then the strands are cut to obtain pellets of the EVOH resin composition.

[0608] [Extrusion conditions]

[0609] Extruder set temperature (℃): C1 / C2 / C3 / C4 / C5 / C6

[0610] =150 / 200 / 210 / 210 / 210 / 210

[0611] <Example 2-2>

[0612] Pellets of an EVOH resin composition were obtained in the same manner as in Example 2-1 except that the amount of titanium oxide blended in Example 2-1 was changed to 0.083 ppm in terms of metal relative to the mass of the EVOH resin composition.

[0613] <Comparative Example 2-1>

[0614] In Example 2-1, pellets of an EVOH resin composition were obtained in the same manner as in Example 2-1 except that titanium oxide was not used.

[0615] <Comparative Example 2-2>

[0616] In Example 2-1, pellets of an EVOH resin composition were obtained in the same manner as in Example 2-1 except that the blending amount of titanium oxide was changed to 0.83 ppm in terms of metal relative to the mass of the EVOH resin composition.

[0617] The following thermal stability evaluation was performed using the obtained pellets of the EVOH resin compositions of Examples 2-1 and 2-2 and Comparative Examples 2-1 and 2-2. The results are shown in Table 2-1 described below.

[0618] 〔Thermal stability evaluation〕

[0619] Using 5 mg of the obtained EVOH resin composition pellets, the weight was measured using a thermogravimetric measuring apparatus (manufactured by PerkinElmer, Pyris 1TGA) under a nitrogen atmosphere at an air flow rate of 20 mL / min, a temperature of 230° C., and a time of 1 hour, and the weight reduction rate was calculated using the following formula. The lower the value, the less decomposed the resin composition is, which means that the resin composition has excellent thermal stability.

[0620] <Formula>

[0621] Weight reduction rate (%) = [(weight before heating - weight after heating) / weight before heating] × 100

[0622] [Table 2-1]

[0623]

[0624] According to the above Table 2-1, it can be seen that the EVOH resin compositions of Examples 2-1 and 2-2 containing a polyolefin-based resin (B2) and a specific trace amount of a titanium compound (C) have a smaller weight change and better thermal stability than the EVOH resin composition of Comparative Example 2-1 that does not contain the titanium compound (C) and the EVOH resin composition of Comparative Example 2-2 that contains a larger amount of titanium compound (C) than the specific range.

[0625] Furthermore, the multilayer structure including the layer composed of the EVOH resin composition of Examples 2-1 and 2-2 was also suppressed from thermal degradation and was excellent in thermal stability.

[0626] <<Third Method>>

[0627] <Example 3-1>

[0628] As the EVOH resin (A), pellets of EVOH resin having an ethylene structural unit content of 29 mol %, a saponification degree of 99.6 mol %, and an MFR of 4 g / 10 min (210° C., a load of 2160 g) were used.

[0629] As the olefin polymer (B3), an ethylene-butene random copolymer (manufactured by Mitsui Chemicals, Inc., TAFMERA-4085S: density 0.885 g / cm 3 ) (B3-1) and acid-modified ethylene-butene copolymer (manufactured by Mitsui Chemicals, MA8510: density 0.885 g / cm 3 )(B3-2), titanium oxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the titanium compound (C).

[0630] 2400 parts of the pellets of the EVOH resin (A), 300 parts of (B3-1) and 300 parts of (B3-2) as the olefin polymer (B3), and 0.13 ppm of the titanium oxide in terms of metal content relative to the mass of the EVOH resin composition were dry-blended to obtain a mixture. The mixture was then supplied to a twin-screw extruder equipped with a twin-hole die. The strands extruded and discharged under the following extrusion conditions are cooled and solidified in a water tank. Next, air is blown to the solidified strands to remove water droplets on the strand surface, and then the strands are cut to obtain pellets of the EVOH resin composition.

[0631] [Extrusion conditions]

[0632] Extruder set temperature (℃): C1 / C2 / C3 / C4 / C5 / C6

[0633] =150 / 200 / 210 / 210 / 210 / 210

[0634] <Example 3-2>

[0635] In Example 3-1, pellets of an EVOH resin composition were obtained in the same manner as in Example 3-1 except that the blending amount of titanium oxide was changed to 1.3 ppm in terms of metal relative to the mass of the EVOH resin composition.

[0636] <Comparative Example 3-1>

[0637] In Example 3-1, pellets of an EVOH resin composition were obtained in the same manner as in Example 3-1 except that titanium oxide was not used.

[0638] <Comparative Example 3-2>

[0639] In Example 3-1, pellets of an EVOH resin composition were obtained in the same manner as in Example 3-1 except that the blending amount of titanium oxide was changed to 13 ppm in terms of metal relative to the mass of the EVOH resin composition.

[0640] The following thermal stability evaluation was performed using the obtained pellets of the EVOH resin compositions of Examples 3-1 and 3-2 and Comparative Examples 3-1 and 3-2. The results are shown in Table 3-1 described below.

[0641] 〔Thermal stability evaluation〕

[0642] Using 5 mg of the obtained pellets of the EVOH resin composition, the temperature (5% weight loss temperature) at which the weight decreased to 95% of the weight before the measurement was measured using a thermogravimetric measuring apparatus (manufactured by PerkinElmer, Pyris 1TGA) under a nitrogen atmosphere at an air flow rate of 20 mL / min and a temperature range of 30 to 550° C. The higher the temperature, the better the thermal stability.

[0643] [Table 3-1]

[0644]

[0645] According to the above Table 3-1, it can be seen that the EVOH resin compositions of Examples 3-1 and 3-2 containing a specific olefin-based polymer (B3) and a specific trace amount of a titanium compound (C) have a higher 5% weight loss temperature and excellent thermal stability compared with the EVOH resin composition of Comparative Example 3-1 that does not contain the titanium compound (C) and the EVOH resin composition of Comparative Example 3-2 that contains a titanium compound (C) in an amount greater than the specific range.

[0646] Furthermore, the multilayered structures including the layers composed of the EVOH resin compositions of Examples 3-1 and 3-2 were also suppressed from thermal degradation and were excellent in thermal stability.

[0647] <<Method 4>>

[0648] <Example 4-1>

[0649] As the EVOH resin (A), pellets of EVOH resin having an ethylene structural unit content of 29 mol %, a saponification degree of 99.6 mol %, and an MFR of 4 g / 10 min (210° C., a load of 2160 g) were used.

[0650] In addition, nylon 6 (Novamid 1028EN, manufactured by DSM Engineering Plastics) was used as the polyamide-based resin (B4), and titanium oxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the titanium compound (C).

[0651] 90 parts of the pellets of the EVOH resin (A), 10 parts of the polyamide resin (B4) and 0.1 ppm of the titanium oxide in terms of metal content relative to the mass of the EVOH resin composition were dry-blended to obtain a mixture. The mixture was then supplied to a twin-screw extruder equipped with a twin-hole die. The strands extruded and discharged under the following extrusion conditions are cooled and solidified in a water tank. Next, air is blown to the solidified strands to remove water droplets on the strand surface, and then the strands are cut to obtain pellets of the EVOH resin composition.

[0652] [Extrusion conditions]

[0653] Extruder set temperature (℃): C1 / C2 / C3 / C4 / C5 / C6

[0654] =150 / 200 / 210 / 210 / 210 / 210

[0655] <Example 4-2>

[0656] In Example 4-1, pellets of an EVOH resin composition were obtained in the same manner as in Example 4-1 except that the blending amount of titanium oxide was changed to 1 ppm in terms of metal relative to the mass of the EVOH resin composition.

[0657] <Comparative Example 4-1>

[0658] In Example 4-1, pellets of an EVOH resin composition were obtained in the same manner as in Example 4-1 except that titanium oxide was not used.

[0659] <Comparative Example 4-2>

[0660] In Example 4-1, pellets of an EVOH resin composition were obtained in the same manner as in Example 4-1 except that the blending amount of titanium oxide was changed to 10 ppm in terms of metal relative to the mass of the EVOH resin composition.

[0661] The following thermal stability evaluation was performed using the obtained pellets of the EVOH resin compositions of Examples 4-1 and 4-2 and Comparative Examples 4-1 and 4-2. The results are shown in Table 4-1 described below.

[0662] 〔Thermal stability evaluation〕

[0663] Using 5 mg of the obtained pellets of the EVOH resin composition, a thermogravimetric measuring apparatus (manufactured by PerkinElmer, Pyris 1TGA) was used to measure the temperature at which the weight decreased to 95% of the weight before measurement (5% weight loss temperature) and the temperature at which the weight decreased to 90% of the weight before measurement (10% weight loss temperature) under the conditions of a nitrogen atmosphere, a gas flow rate of 20 mL / min, and a temperature range of 30 to 550° C. The higher the temperature, the better the thermal stability.

[0664] [Table 4-1]

[0665]

[0666] According to the above Table 4-1, it can be seen that the EVOH resin compositions of Examples 4-1 and 4-2 containing a polyamide resin (B4) and a specific trace amount of a titanium compound (C) have higher 5% weight loss temperatures and 10% weight loss temperatures than the EVOH resin composition of Comparative Example 4-1 that does not contain the titanium compound (C) and the EVOH resin composition of Comparative Example 4-2 that contains a titanium compound (C) in an amount greater than the specific range, and have excellent thermal stability.

[0667] Furthermore, the multilayered structures including the layers composed of the EVOH resin compositions of Examples 4-1 and 4-2 were also suppressed from thermal degradation and were excellent in thermal stability.

[0668] << Fifth Method >>

[0669] <Example 5-1>

[0670] As the EVOH resin (A), pellets of EVOH resin having an ethylene structural unit content of 29 mol %, a saponification degree of 99.6 mol %, and an MFR of 4 g / 10 min (210° C., a load of 2160 g) were used.

[0671] In addition, 2,4-diphenyl-4-methyl-1-pentene (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the specific styrene derivative (B5), and titanium oxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the titanium compound (C).

[0672] The above-mentioned specific styrene derivative (B5) in an amount of 2000 ppm based on the mass of the EVOH resin composition and the above-mentioned titanium oxide in an amount of 0.1 ppm based on the mass of the EVOH resin composition in terms of metal conversion were dry-blended with the above-mentioned EVOH resin (A) pellets to obtain a mixture. The above-mentioned mixture was then preheated at 230° C. for 5 minutes using a plasticizer (made by Brabender) and melt-kneaded for 5 minutes to obtain an EVOH resin composition. The obtained EVOH resin composition was pulverized at 650 rpm using a pulverizer (SKR16-240 made by Sometani Industries) to obtain a pulverized product.

[0673] <Example 5-2>

[0674] In Example 5-1, except that the blending amount of titanium oxide was changed to 1 ppm in terms of metal relative to the mass of the EVOH resin composition, a pulverized product of an EVOH resin composition was obtained in the same manner as in Example 5-1.

[0675] <Comparative Example 5-1>

[0676] In Example 5-1, except that titanium oxide was not used, a ground product of an EVOH resin composition was obtained in the same manner as in Example 5-1.

[0677] <Comparative Example 5-2>

[0678] In Example 5-1, except that the blending amount of titanium oxide was changed to 5 ppm in terms of metal relative to the mass of the EVOH resin composition, a pulverized product of an EVOH resin composition was obtained in the same manner as in Example 5-1.

[0679] The pulverized products of the EVOH resin compositions of Examples 5-1 and 5-2 and Comparative Examples 5-1 and 5-2 were used to perform the following thermal stability evaluation. The results are shown in Table 5-1 described below.

[0680] 〔Thermal stability evaluation〕

[0681] Using 5 mg of the pulverized product of the obtained EVOH resin composition, a thermogravimetric measuring apparatus (manufactured by PerkinElmer, Pyris 1TGA) was used to measure the temperature at which the weight decreased to 95% of the weight before measurement (5% weight loss temperature) and the temperature at which the weight decreased to 90% of the weight before measurement (10% weight loss temperature) under the conditions of a nitrogen atmosphere, a gas flow rate of 20 mL / min, and a temperature range of 30 to 550° C. The higher the temperature, the better the thermal stability.

[0682] [Table 5-1]

[0683]

[0684] According to the above Table 5-1, it can be seen that the EVOH resin compositions of Examples 5-1 and 5-2 containing a specific styrene derivative (B5) and a specific trace amount of a titanium compound (C) have higher 5% weight loss temperatures and 10% weight loss temperatures than the EVOH resin composition of Comparative Example 5-1 that does not contain the titanium compound (C) and the EVOH resin composition of Comparative Example 5-2 that contains a titanium compound (C) in an amount greater than the specific range, and have excellent thermal stability.

[0685] Furthermore, the multilayered structures including the layers composed of the EVOH resin compositions of Examples 5-1 and 5-2 were also suppressed from thermal degradation and were excellent in thermal stability.

[0686] It should be noted that the comparative examples of the first to fifth aspects described above are comparative examples of the respective aspects and are not necessarily limited to comparative examples of the present invention.

[0687] The above embodiments show specific aspects of the present invention, but the above embodiments are merely illustrative and are not to be construed as limiting. Various modifications that are obvious to those skilled in the art are intended to be included within the scope of the present invention.

[0688] Industrial Applicability

[0689] The modified EVOH resin composition is inhibited from thermal degradation during melt molding and is therefore useful as packaging materials for various foods, including seasonings such as mayonnaise and sauces, fermented foods such as miso, oily foods such as salad oils, beverages, cosmetics, and pharmaceuticals.

Claims

1. An ethylene-vinyl alcohol copolymer composition comprising: Ethylene-vinyl alcohol copolymer A, At least one compound B selected from the group consisting of a metal compound B1 belonging to the 4th period d-block of the long period periodic table, a polyolefin resin B2, an olefin polymer B3, a polyamide resin B4, and a styrene derivative B5 having a substituent at the α position, wherein the metal compound B1 does not include a titanium compound, and Titanium compound C; The olefin polymer B2 is at least one selected from olefin thermoplastic elastomers, aliphatic rubbers and ionomers, The metal equivalent content of the titanium compound C is 0.00005 ppm or more and less than 5 ppm based on the mass of the ethylene-vinyl alcohol-based copolymer composition.

2. The ethylene-vinyl alcohol copolymer composition according to claim 1, wherein The mass content ratio A / B of the ethylene-vinyl alcohol copolymer A to the component B is 1 / 99 to 99 / 1.

3. The ethylene-vinyl alcohol copolymer composition according to claim 1 or 2, wherein The metal conversion content of the titanium compound C is 0.001 to 3 ppm based on the total mass of the ethylene-vinyl alcohol-based copolymer A and the titanium compound C.

4. The ethylene-vinyl alcohol copolymer composition according to any one of claims 1 to 3, wherein The metal compound B1 belonging to the d-block of the fourth period of the long period periodic table has a metal conversion content of 0.1 to 500 ppm based on the mass of the ethylene-vinyl alcohol copolymer composition.

5. The ethylene-vinyl alcohol copolymer composition according to any one of claims 1 to 4, wherein The metal compound B1 belonging to the 4th period d zone of the long period periodic table is a zinc compound.

6. The ethylene-vinyl alcohol copolymer composition according to any one of claims 1 to 5, wherein The metal compound B1 belonging to the 4th period d zone of the long period periodic table is a carboxylate.

7. The ethylene-vinyl alcohol copolymer composition according to any one of claims 1 to 3, wherein The polyolefin resin B2 has a density of 0.89 g / cm 3 The above polyolefin resins.

8. The ethylene-vinyl alcohol copolymer composition according to any one of claims 1 to 3 and 7, wherein The polyolefin-based resin B2 is polypropylene.

9. The ethylene-vinyl alcohol copolymer composition according to any one of claims 1 to 3, wherein The content of the styrene derivative B5 having a substituent at the α-position is 1 to 10000 ppm based on the mass of the ethylene-vinyl alcohol copolymer composition.

10. The ethylene-vinyl alcohol copolymer composition according to any one of claims 1 to 3 and 9, wherein The styrene derivative B5 having a substituent at the α-position is an α-methylstyrene derivative.

11. A method for producing an ethylene-vinyl alcohol copolymer composition, the method comprising the step of melt-mixing a composition raw material containing the A, the B and the C.

12. A melt molding material, comprising the ethylene-vinyl alcohol copolymer composition according to any one of claims 1 to 10.

13. Pellets comprising the ethylene-vinyl alcohol copolymer composition according to any one of claims 1 to 10. 14 . A multilayer structure comprising at least one layer comprising the ethylene-vinyl alcohol copolymer composition according to claim 1 .

15. A method for producing a multilayer structure, which is the method for producing a multilayer structure according to claim 14, comprising the step of melt-molding a layer composed of the ethylene-vinyl alcohol copolymer composition.