Ethylene-vinyl alcohol copolymer composition, material for melt molding, multilayer structure, thermoformed container, method for producing ethylene-vinyl alcohol copolymer composition, and method for producing multilayer structure
By adding trace amounts of titanium compounds to EVOH resin, the problems of thermal deterioration and color changes during the melt molding process are solved, the long-term operability of the composition is improved, and the color stability of the product is ensured.
Patent Information
- Application Number
- CN202380024933.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-15
AI Technical Summary
Existing EVOH resin compositions are prone to thermal deterioration and coloration changes during the melt molding process, affecting their long-term operability.
Adding specific trace amounts of titanium compounds to EVOH resins containing different ethylene contents forms a stabilized structure through chelation of titanium ions with the resin main chain, inhibiting the formation of polyene structures, thereby reducing color changes caused by thermal deterioration.
It effectively suppresses color changes caused by thermal deterioration, improves the long-term operability of the EVOH resin composition, and ensures the color stability and production performance of the product.
Smart Images

Figure BDA0005022347310000181
Abstract
Description
Technical Field
[0001] The present invention relates to an ethylene-vinyl alcohol copolymer composition, a melt molding material, a multilayer structure, a thermoforming container, a method for producing the ethylene-vinyl alcohol copolymer composition, and a method for producing the multilayer structure. Background Art
[0002] Ethylene-vinyl alcohol copolymers (hereinafter also referred to as "EVOH resins") are excellent in transparency, gas barrier properties such as oxygen, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and are molded into films, sheets, bottles, etc., and are widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and pesticide packaging materials.
[0003] EVOH resin has a tendency that the greater the content of ethylene structural units (hereinafter, also referred to as "ethylene content"), the better the stretchability. On the other hand, the greater the ethylene content (the smaller the content of vinyl alcohol structural units (hereinafter, referred to as "vinyl alcohol content")), the lower the gas barrier properties. In order to achieve both gas barrier properties and stretchability, it is proposed to use EVOH resin with a large vinyl alcohol content (in other words, a small ethylene content and a high saponification degree) and EVOH resin with a small vinyl alcohol content (in other words, a large ethylene content and a low saponification degree) in combination.
[0004] For example, Patent Document 1 discloses a composition in which EVOH resins having different ethylene contents and saponification degrees are used together. Patent Document 1 describes a laminate formed by vacuum pressure molding a laminated body using an EVOH resin composition as an intermediate layer and the laminated body and a polystyrene layer, and the laminated body has excellent transparency and appearance, no cracks, uneven thickness, and excellent gas barrier properties. The difference in ethylene content between the two EVOH resins used together in the EVOH resin composition is 4 mol% or more, and the difference in saponification degree is 3 mol% or more, and further, the difference in solubility parameter is also above a prescribed level.
[0005] In addition, Patent Document 2 discloses an EVOH resin composition comprising two EVOH resins having a difference in ethylene content of 3 to 20 mol % and having a specific boron concentration. Even when the laminated film is heated and stretched (in the order of 4 times in the longitudinal direction and 6 times in the transverse direction) using the EVOH resin composition as an intermediate layer and a polypropylene layer laminated via an adhesive resin layer, no whitening, streaks or other stretching unevenness is observed.
[0006] In order to manufacture various molded products using the above-mentioned technology, melt molding such as extrusion molding and injection molding is performed, but when the EVOH resin composition is melt-molded, thermal degradation is easily generated. In particular, in such a method using different EVOH resins, since EVOH resins having different melting points are melt-molded at a single temperature, the EVOH resin with a low melting point tends to be easily thermally degraded, poor in thermal stability, and easily colored.
[0007] As a method for improving the coloration caused when using different EVOH resins, for example, a technique is known in which an EVOH resin having a molecular weight satisfying a specific condition measured after heat treatment at 220° C. for 50 hours in a nitrogen atmosphere is used (see, for example, Patent Document 3).
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Laid-Open No. 63-230757
[0011] Patent Document 2: Japanese Patent Application Laid-Open No. 8-311276
[0012] Patent Document 3: Japanese Patent Application Publication No. 2016-29157 Summary of the invention
[0013] In recent years, there has been a trend toward higher functionality in molding equipment, with the diversification of feed blocks and mold shapes in molding equipment, thinner multilayer structures in final products, or increased number of layers. However, in molding equipment that has become more complex due to higher functionality, resins may suffer from thermal degradation and coloration, and the productivity (long run performance) of products may decrease.
[0014] The EVOH resin compositions disclosed in Patent Documents 1 to 3 are excellent in gas barrier properties, stretchability and other moldability, but further improvement is required in terms of color change due to thermal degradation during the melt molding process.
[0015] Therefore, under such background, the present invention provides an EVOH resin composition which suppresses color change due to thermal degradation during melt molding and has excellent long-term working properties.
[0016] In view of the above circumstances, the present inventors have found that an EVOH resin composition in which color change due to thermal degradation is suppressed can be obtained by adding a specific trace amount of a titanium compound to an EVOH resin comprising two or more EVOH resins having different ethylene contents.
[0017] That is, the present invention has the following aspects.
[0018] [1] An EVOH resin composition comprising:
[0019] An EVOH resin (A) comprising two or more EVOH resins having different contents of ethylene structural units, and
[0020] A titanium compound (B);
[0021] The metal-equivalent content of the titanium compound (B) is 0.001 ppm or more and less than 5 ppm based on the mass of the EVOH resin composition.
[0022] [2] The EVOH resin composition according to [1], wherein the difference in ethylene structural unit content between the EVOH resin having the highest ethylene structural unit content and the EVOH resin having the lowest ethylene structural unit content in the EVOH resin (A) is 2 mol% or more.
[0023] [3] The EVOH resin composition according to [1] or [2], wherein the EVOH resin (A) comprises at least an EVOH resin (A1) having an ethylene structural unit content of less than 35 mol% and an EVOH resin (A2) having an ethylene structural unit content of 35 mol% or more.
[0024] [4] The EVOH resin composition according to [3], wherein the mass ratio (A1 / A2) of the EVOH resin (A1) having an ethylene structural unit content of less than 35 mol% to the EVOH resin (A2) having an ethylene structural unit content of more than 35 mol% is 1 / 99 to 99 / 1.
[0025] [5] A melt molding material comprising the EVOH resin composition according to any one of [1] to [4].
[0026] [6] A multilayer structure comprising at least one layer comprising the EVOH resin composition according to any one of [1] to [4].
[0027] [7] A thermoformed container, comprising the multilayer structure described in [6].
[0028] [8] A method for producing an EVOH resin composition, which is the method for producing the EVOH resin composition according to any one of [1] to [4], comprising the step of melt-mixing a composition raw material containing the EVOH resin and a titanium compound.
[0029] [9] A method for producing a multilayer structure, which is a method for producing the multilayer structure described in [6], wherein:
[0030] The present invention comprises a step of melt-molding a layer composed of the EVOH resin composition.
[0031] The EVOH resin composition of the present invention is suppressed from undergoing color change due to thermal degradation during melt molding and is excellent in long-term operating properties. DETAILED DESCRIPTION
[0032] Hereinafter, the present invention will be described in more detail based on embodiments of the present invention, but the present invention is not limited to these embodiments.
[0033] In the present invention, when expressed as "X to Y" (X and Y are arbitrary numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", and also includes the meaning of "preferably greater than X" or "preferably less than Y".
[0034] In addition, when expressed as "X or more" (X is an arbitrary number) or "Y or less" (Y is an arbitrary number), it also includes the meaning of "preferably greater than X" or "preferably less than Y".
[0035] <EVOH resin composition>
[0036] The EVOH resin composition according to one embodiment of the present invention (hereinafter also referred to as "the present EVOH resin composition") contains as a main component an EVOH resin (A) comprising two or more EVOH resins having different ethylene contents, and contains a specific trace amount of a titanium compound (B).
[0037] That is, in the present EVOH resin composition, the base resin is EVOH resin (A), and the content of EVOH resin (A) in the present EVOH resin composition is usually 70% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 95% by mass or more.
[0038] Hereinafter, each component will be described.
[0039] 〔EVOH resin (A)〕
[0040] The EVOH resin (A) used in the present invention includes two or more EVOH resins having different ethylene contents. The EVOH resin is generally a water-insoluble thermoplastic resin obtained by saponifying an ethylene-vinyl ester copolymer, which is a copolymer of ethylene and a vinyl ester monomer.
[0041] As the vinyl ester monomer, vinyl acetate can be used representatively from the aspects of market availability and good impurity treatment efficiency during production. As other vinyl ester monomers other than vinyl acetate, for example, aliphatic vinyl esters such as vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, and vinyl versatate, and aromatic vinyl esters such as vinyl benzoate can be mentioned. Usually, aliphatic vinyl esters having 3 to 20 carbon atoms, preferably 4 to 10 carbon atoms, and particularly preferably 4 to 7 carbon atoms can be used. These are usually used alone, but multiple types can also be used simultaneously as needed.
[0042] As the polymerization method for copolymerizing the above-mentioned ethylene and vinyl ester monomers, any known polymerization method can be used, such as solution polymerization, suspension polymerization, emulsion polymerization, etc., but generally, solution polymerization using methanol as a solvent is used. In addition, the saponification of the obtained ethylene-vinyl ester copolymer can also be carried out by a known method.
[0043] The EVOH resin produced in this manner mainly contains structural units derived from ethylene and vinyl alcohol, and also contains a small amount of vinyl ester structural units which remain without being saponified.
[0044] The EVOH resin may further contain a structural unit derived from the following comonomer (for example, 10 mol% or less of the EVOH resin) within a range not inhibiting the effects of the present invention.
[0045] Examples of the comonomer include olefins such as propylene, 1-butene, and isobutylene; α-olefins containing a hydroxyl group such as 3-butene-1-ol, 3-butene-1,2-diol, 4-pentene-1-ol, and 5-hexene-1,2-diol, or derivatives thereof such as esters and acylates; hydroxyalkyl vinylides such as 2-methylenepropane-1,3-diol and 3-methylenepentane-1,5-diol; 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, phthalic acid (anhydride), maleic acid (anhydride), itaconic acid (anhydride) or their salts or mono- or di-alkyl esters having 1 to 18 carbon atoms in the alkyl group; acrylamide, N-alkyl acrylamide having 1 to 18 carbon atoms in the alkyl group, N,N-dimethylacrylamide, 2-acrylamidopropanesulfonic acid or its salts, acrylamidopropyl dimethylamine or Acrylic amides such as their acid salts or quaternary ammonium salts; methacrylamide, N-alkyl methacrylamide with 1 to 18 carbon atoms in the alkyl group, N,N-dimethyl methacrylamide, 2-methacrylamide propanesulfonic acid or its salts, methacrylamide propyl dimethylamine or its acid salts or quaternary ammonium salts; N-vinyl amides such as N-vinyl pyrrolidone, N-vinyl formamide, N-vinyl acetamide; vinyl cyanides such as acrylonitrile and methacrylonitrile; alkyl carbon atoms Vinyl ethers such as alkyl vinyl ethers, hydroxyalkyl vinyl ethers, and alkoxyalkyl vinyl ethers having 1 to 18 moieties; halogenated vinyl compounds such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, and vinyl bromide; vinyl silanes such as trimethoxyvinylsilane; halogenated allyl compounds such as allyl acetate and allyl chloride; allyl alcohols such as allyl alcohol and dimethoxyallyl alcohol; comonomers such as trimethyl-(3-acrylamide-3-dimethylpropyl)-ammonium chloride and acrylamide-2-methylpropanesulfonic acid. These may be used alone or in combination of two or more.
[0046] Among them, α-olefins containing hydroxyl groups are preferred, and 3-butene-1,2-diol and 5-hexene-1,2-diol are particularly preferred. When the above-mentioned α-olefins containing hydroxyl groups are copolymerized, the obtained EVOH resin has a primary hydroxyl group in the side chain. From the perspective of maintaining gas barrier properties while improving secondary moldability, such EVOH resins having primary hydroxyl groups in the side chain, especially EVOH resins having a 1,2-diol structure in the side chain are preferred.
[0047] When the EVOH resin has a primary hydroxyl group in the side chain, the content of the structural unit derived from the monomer having the primary hydroxyl group is usually 0.1 to 20 mol %, preferably 0.5 to 15 mol %, particularly preferably 1 to 10 mol % of the EVOH resin.
[0048] As the EVOH resin, EVOH-based resins that have been “post-modified” by esterification, urethanization, acetalization, cyanoethylation, oxyalkylation, etc. may also be used.
[0049] When the post-modified EVOH resin is used, the modification rate is usually 10 mol% or less, preferably 4 mol% or less. If the modification rate of the EVOH resin is too high, it is easily thermally degraded, and the long-term operating performance tends to decrease.
[0050] As described above, the EVOH resin (A) includes two or more EVOH resins having different ethylene contents. In the present invention, the ethylene content of the EVOH resin refers to a value measured in accordance with ISO 14663.
[0051] The ethylene content of the EVOH resin (A) is usually 20 to 60 mol%, preferably 25 to 50 mol%, and particularly preferably 25 to 45 mol%. If the content is too low, the gas barrier properties and melt moldability at high humidity tend to be reduced in the case of gas barrier applications, while if the content is too high, the gas barrier properties tend to be reduced.
[0052] In the above EVOH resin (A), the difference in ethylene content between the EVOH resin having the largest ethylene content and the EVOH resin having the smallest ethylene content is preferably 2 mol% or more, more preferably 2 to 25 mol%, more preferably 4 to 20 mol%, and particularly preferably 5 to 18 mol%. If the difference in ethylene content is too small, it tends to be difficult to maintain a balance between moldability and gas barrier properties, while if it is too large, the compatibility between the two tends to decrease.
[0053] The difference in ethylene content of the two or more EVOH resins contained in the above-mentioned EVOH resin (A) can also be obtained, for example, by measuring the melting peak temperature. That is, in general, since the ethylene content of the EVOH resin is related to the melting point of the EVOH resin, the ethylene content of the two or more EVOH resins contained in the EVOH resin (A) can be calculated separately by measuring the melting peak temperature of the present EVOH resin composition.
[0054] The melting peak temperature is the peak temperature measured by using a differential scanning calorimeter (DSC) at a temperature increase of 10°C / min from -50 to 230°C, a temperature decrease of 10°C / min from 230 to -50°C, and a temperature increase of 10°C / min from -50 to 230°C.
[0055] The melting peak temperature difference of the EVOH resin (A) obtained by using the DSC is usually 3° C. or more, preferably 3 to 40° C., more preferably 6 to 24° C., and particularly preferably 8 to 16° C. If the temperature difference is too small, it tends to be difficult to maintain a balance between moldability and gas barrier properties, while if it is too large, the compatibility between the two tends to decrease.
[0056] The number of EVOH resins having different ethylene contents contained in the EVOH resin (A) is usually 2 to 4, preferably 2 to 3, and particularly preferably 2. The greater the number of EVOH resins, the lower the productivity and economic efficiency tend to be.
[0057] In addition, the fact that the present EVOH resin composition contains several types of EVOH resins having different ethylene contents can be confirmed from the number of peaks measured by the above-mentioned DSC.
[0058] In addition, from the viewpoint of thermal stability, the above-mentioned EVOH resin (A) preferably has at least an EVOH resin (A1) having an ethylene content of less than 35 mol% (hereinafter also referred to as "EVOH resin (A1)") and an EVOH resin (A2) having an ethylene content of more than 35 mol% (hereinafter also referred to as "EVOH resin (A2)").
[0059] The ethylene content of the EVOH resin (A1) is usually less than 35 mol%, preferably 20 to 34 mol%, more preferably 22 to 34 mol%, and particularly preferably 25 to 33 mol%. When the ethylene content is too low, the decomposition temperature and the melting point are too close, and melt molding of the EVOH resin composition tends to become difficult. On the contrary, when the ethylene content is too high, the effect of imparting gas barrier properties by the EVOH resin (A1) tends to be insufficient.
[0060] The ethylene content of the EVOH resin (A2) is usually 35 mol% or more, preferably 35 to 60 mol%, more preferably 36 to 56 mol%, and particularly preferably 37 to 45 mol%. When the ethylene content is too low, the effect of improving the stretchability of the EVOH resin (A2) is small, and as a result, the secondary moldability tends to decrease. On the contrary, when the ethylene content is too high, in order to make the difference in ethylene content within the specified range, an EVOH resin with a large ethylene content has to be selected as the other EVOH resin, and as a result, the gas barrier properties of the EVOH resin composition layer become insufficient.
[0061] The saponification degree of the EVOH resin (A) is usually 90 to 100 mol%, preferably 95 to 100 mol%, and particularly preferably 99 to 100 mol%. If the saponification degree is too low, gas barrier properties, thermal stability, moisture resistance, etc. tend to decrease.
[0062] The saponification degree of the EVOH resin (A1) is usually 90 mol% or more, preferably 95 to 100 mol%, particularly preferably 98 to 100 mol%. If the saponification degree is too low, the effect of imparting gas barrier properties by the EVOH resin (A1) tends to be insufficient.
[0063] The saponification degree of the EVOH resin (A2) is usually 90 mol% or more, preferably 93 to 100 mol%, particularly preferably 98 to 100 mol%. If the saponification degree is too low, the effect of imparting gas barrier properties by the EVOH resin (A2) tends to be insufficient.
[0064] In addition, the said saponification degree is the value measured based on JIS K 6726 (wherein, EVOH is used as the solution which uniformly dissolved in the water / methanol solvent).
[0065] The melt flow rate (MFR) (210° C., load 2160 g) of the EVOH resin (A) is usually 0.5 to 100 g / 10 min, preferably 1 to 50 g / 10 min, and particularly preferably 2 to 35 g / 10 min. If the MFR is too large, the film-forming property tends to become unstable, while if it is too small, the viscosity tends to become too high and melt extrusion tends to be difficult.
[0066] The melt flow rate (MFR) (210°C, load 2160g) of the EVOH resin (A1) is usually 1 to 100g / 10min, preferably 2 to 50g / 10min, and particularly preferably 3 to 10g / 10min. If the MFR is too large, the mechanical strength of the molded product tends to decrease, and if it is too small, the extrusion processability tends to decrease.
[0067] The melt flow rate (MFR) (210°C, load 2160g) of the EVOH resin (A2) is usually 1 to 100g / 10min, preferably 2 to 50g / 10min, and particularly preferably 3 to 30g / 10min. If the MFR is too large, the mechanical strength of the molded product tends to decrease, and if it is too small, the extrusion processability tends to decrease.
[0068] It should be noted that with respect to the combination of EVOH resin (A1) and EVOH resin (A2), the difference (ΔMFR) in MFR (210°C, load 2160 g) is preferably 5 g / 10 min or less so that the resin fluidity during melt molding is the same, and it is more preferable to adjust the saponification degree of each EVOH resin to 1.5 g / 10 min or less.
[0069] The mass ratio of the EVOH resin (A1) to the EVOH resin (A2) [EVOH resin (A1) / EVOH resin (A2)] is usually 1 / 99 to 99 / 1, preferably 10 / 90 to 90 / 10, more preferably 50 / 50 to 90 / 10, particularly preferably 60 / 40 to 88 / 12, and particularly preferably 70 / 30 to 85 / 15. If the ratio of the EVOH resin (A1) is too small, the gas barrier properties tend to be insufficient, and if it is too large, the stretching improvement effect tends to be reduced.
[0070] [Titanium compound (B)]
[0071] Examples of the titanium compound (B) include inorganic titanium compounds and organic titanium compounds. The titanium compounds may be used alone or in combination of two or more. Among them, inorganic titanium compounds are preferred.
[0072] Examples of the inorganic titanium compound include titanium oxide, titanium hydroxide, titanium chloride, and inorganic titanium salts.
[0073] Examples of the titanium oxide include titanium (II) oxide, titanium (III) oxide, titanium (IV) oxide, and titanium oxyoxide.
[0074] Examples of the titanium hydroxide include titanium hydroxide and titanium hydroxide.
[0075] Examples of the titanium chloride include titanous chloride and titanium chloride.
[0076] Examples of the inorganic salt of titanium include titanium phosphate and titanium sulfate.
[0077] Among them, titanium oxide is preferred, titanium (IV) oxide is more preferred, and rutile titanium (IV) oxide is particularly preferred.
[0078] Examples of the organic titanium compound include titanium acetate, titanium butyrate, titanium stearate and other titanium carboxylates.
[0079] In addition, the titanium compound (B) may be present in the present EVOH resin composition in the form of a titanium compound or in the form of an ionized state or a complex interacting with the EVOH resin or other ligands.
[0080] The average particle size of the titanium compound (B) is usually 0.001 to 100 μm, preferably 0.01 to 50 μm, and more preferably 0.015 to 20 μm. When the average particle size of the titanium compound is within the above range, the coloration suppressing effect tends to be excellent.
[0081] The metal conversion content of the above-mentioned titanium compound (B) is greater than 0.001ppm and less than 5ppm relative to the mass of the EVOH resin composition. It is preferably 0.01 to 3ppm, more preferably 0.03 to 1ppm, and particularly preferably 0.05 to 0.5ppm. By making the content of the titanium compound (B) within the above range, the color change caused by thermal degradation during melt molding can be suppressed, and long-term operation performance is excellent. In addition, if the content of the titanium compound (B) is too little, the effect of suppressing color change is reduced. If the content is too much, it is easy to cause thermal decomposition of the EVOH resin and it is easy to color.
[0082] The metal conversion content of the above-mentioned titanium compound can be quantified by the following operation: the EVOH resin composition is weighed into a platinum crucible, ashed using a burner and an electric furnace in sequence, the ashed is heated and decomposed with nitric acid and hydrofluoric acid, treated with a mixed acid of dilute nitric acid and dilute hydrofluoric acid and fixed to volume, and the titanium in the obtained fixed solution is determined by ICP mass spectrometry using an ICP mass spectrometer (manufactured by Agilent Technologies, Agilent 8800).
[0083] Generally, EVOH resin is colored due to thermal degradation. This is believed to be because EVOH resin is degraded by heat, generating free radicals, which dehydrate the hydroxyl groups of EVOH resin, generate double bonds in the main chain of EVOH resin, and this site becomes the starting point of the reaction, further promoting dehydration and forming a conjugated polyene structure in the main chain of EVOH resin.
[0084] In this regard, the present EVOH resin composition contains a specific trace amount of titanium compound, so that the color change of the EVOH resin due to thermal degradation is suppressed, and the long-term operation performance is excellent. Generally, when a titanium compound is contained in an EVOH resin composition, it is believed that the EVOH resin composition is colored by titanium ions, and it is technical common sense for those skilled in the art to avoid using titanium compounds. However, the present invention violates such technical common sense and finds that when a specific trace amount of titanium compound is used, an EVOH resin composition in which the color change due to thermal degradation is suppressed can be obtained.
[0085] That is, titanium is stable in the form of a tetravalent ion, and it is presumed that even a trace amount coordinates to the double bonds of the main chain of the EVOH resin as described above, stabilizes by forming a chelate or the like, and suppresses the formation of a polyene structure.
[0086] On the other hand, when the content of the titanium compound is too large, it is considered that the EVOH resin is thermally decomposed by the titanium compound and thus is colored.
[0087] [Other thermoplastic resins]
[0088] The present EVOH resin composition may contain a thermoplastic resin other than EVOH resin within a range that does not inhibit the effects of the present invention (for example, generally 30% by mass or less, preferably 20% by mass or less, particularly preferably 10% by mass or less of the present EVOH resin composition).
[0089] As other thermoplastic resins, known thermoplastic resins can be used, for example, polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, ionomers, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more.
[0090] [Other compounding ingredients]
[0091] In addition, the EVOH resin composition may contain a compounding agent generally used in EVOH resin within a range that does not hinder the effect of the present invention. As the above-mentioned compounding agent, for example, inorganic complex salts (such as hydrotalcite), plasticizers (such as aliphatic polyols such as ethylene glycol, glycerol, hexylene glycol, etc.), oxygen absorbers [such as inorganic oxygen absorbers such as aluminum powder and potassium sulfite; ascorbic acid, and its fatty acid esters or metal salts, etc., gallic acid, polyphenols such as phenolic resins containing hydroxyl groups, terpene compounds, blends of resins containing resin hydrogen and transition metals (such as a combination of polypropylene and cobalt), blends of resins containing carbon-carbon unsaturated bonds and transition metals (such as polybutadiene) can be added. Combinations of olefins and cobalt), photo-oxidative degradable resins (e.g., polyketones), anthraquinone polymers (e.g., polyvinyl anthraquinone), etc., or materials obtained by adding photoinitiators (e.g., benzophenone) or antioxidants or deodorants (e.g., activated carbon) other than those mentioned above to these complexes, etc., polymeric oxygen absorbers], heat stabilizers, light stabilizers, ultraviolet absorbers, colorants, antistatic agents, surfactants (excluding surfactants used as lubricants), antibacterial agents, anti-blocking agents, fillers (e.g., inorganic fillers), etc. These compounds may be used alone or in combination of two or more.
[0092] [Method for producing EVOH resin composition]
[0093] The present EVOH resin composition can be produced, for example, by mixing the above-mentioned EVOH resin (A) and the titanium compound (B) by a known method, such as a dry blending method, a melt mixing method, a solution mixing method, an impregnation method, etc. Among these, it is preferably produced by a method having a step of melt mixing a composition raw material containing the above-mentioned EVOH resin and the titanium compound. In addition, these production methods can also be arbitrarily combined.
[0094] Examples of the dry blending method include (i) a method of dry blending one EVOH resin constituting the pelletized EVOH resin (A) or the pelletized EVOH resin (A) and the titanium compound (B) using a tumbler or the like.
[0095] Examples of the melt mixing method include (ii) a method of melt-kneading a dry mixture obtained by dry-blending a type of EVOH resin constituting a granular EVOH resin (A) or a granular EVOH resin (A) with a titanium compound (B); and (iii) a method of melt-kneading a type of EVOH resin constituting the EVOH resin (A) or a molten EVOH resin (A).
[0096] As the above-mentioned solution mixing method, for example, there can be cited the following methods: (iv) a method in which a solution is prepared using one EVOH resin constituting a granular EVOH resin (A) or a granular EVOH resin (A), a titanium compound (B) is added thereto, the solution is solidified and formed, and then the solution is separated into solid and liquid and dried by a known method; (v) in the manufacturing process of the EVOH resin, a titanium compound (B) is added to an ethylene-vinyl ester copolymer solution before saponification or a uniform solution of the EVOH resin (water / alcohol solution, etc.), and then the solution is solidified and formed, and then the solution is separated into solid and liquid and dried by a known method, etc.
[0097] As the above-mentioned impregnation method, for example, there can be cited a method of (vi) contacting one EVOH resin constituting a granular EVOH resin (A) or a granular EVOH resin (A) with an aqueous solution containing a titanium compound (B), allowing the EVOH resin or the EVOH resin (A) to contain the titanium compound (B), and then drying the resultant.
[0098] As the aqueous solution containing the titanium compound (B), an aqueous solution of the titanium compound (B) or an aqueous solution obtained by immersing the titanium compound (B) in water containing various chemicals to dissolve titanium ions can be used.
[0099] In the above impregnation method, the content (metal conversion) of the titanium compound (B) can be controlled by the concentration of the titanium compound (B) in the aqueous solution in which the EVOH resin or EVOH resin (A) is impregnated, the impregnation temperature, the impregnation time, etc.
[0100] Regarding the immersion temperature and immersion time, the immersion time is usually 0.5 to 48 hours, preferably 1 to 36 hours, and the immersion temperature is usually 10 to 40°C, preferably 20 to 35°C.
[0101] As the drying method in each of the above-mentioned production methods, various drying methods can be adopted, and any of static drying and fluidized drying can be adopted. In addition, these methods can also be combined.
[0102] As described above, in the present invention, the above-mentioned different methods can be combined. Among them, from the perspective of productivity and the ability to obtain a resin composition with a more significant effect of the present invention, the melt mixing method is preferred, and the method (ii) is particularly preferred. In addition, when mixing EVOH resins with different ethylene contents, it is sufficient to mix them by the above-mentioned dry blending method, melt kneading method, solution mixing method, etc. Furthermore, when using the above-mentioned other thermoplastic resins and other compounding agents, it is sufficient to mix them by conventional methods according to the above-mentioned manufacturing method.
[0103] The present EVOH resin composition obtained by the above-mentioned production methods may be in any shape, but is preferably in the form of pellets.
[0104] As the above-mentioned particles, for example, there are spherical, elliptical, cylindrical, cubic, rectangular parallelepiped, etc., but they are usually elliptical or cylindrical. Regarding their size, from the perspective of convenience when used as a molding material later, in the case of an elliptical shape, the short diameter is usually 1 to 10 mm, preferably 2 to 6 mm, and more preferably 2.5 to 5.5 mm, and the long diameter is usually 1.5 to 30 mm, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm. In addition, in the case of a cylindrical shape, the diameter of the bottom surface is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm.
[0105] In addition, it is preferable that the shape and size of the pelletized EVOH resin used in each of the above-mentioned production methods are also the same.
[0106] Even when the EVOH resin composition is heated during melt molding, the color change is suppressed, and the long-term operation performance is excellent. The ratio of the YI value (yellow index) after heating to the YI value before heating (YI value after heating / YI value before heating) is usually 6.4 or less, preferably 6.2 or less, and particularly preferably 5.9 or less. If the ratio of the YI value after heating to the YI value before heating is within the above range, there is a tendency to further suppress the color change. It should be noted that the lower limit of the ratio of the YI value after heating to the YI value before heating is usually 1.
[0107] The YI value before heating can be obtained by grinding the EVOH resin composition into 1-5 mm square pieces, filling the pieces into a cylinder with an inner diameter of 32 mm and a height of 30 mm, and measuring the pieces with a spectrocolorimeter SE6000 (manufactured by Nippon Denshoku Industries) in a flattened state.
[0108] The YI value after heating can be obtained by heating the present EVOH resin composition crushed into 1 to 5 mm square pieces in an oven under air atmosphere at 150° C. for 5 hours and measuring the resulting EVOH resin composition in the same manner.
[0109] The water content of the present EVOH resin composition is usually 0.01 to 0.5% by mass, preferably 0.05 to 0.35% by mass, and particularly preferably 0.1 to 0.3% by mass.
[0110] In addition, the water content of this EVOH resin composition is measured and calculated by the following method.
[0111] The mass (W1) of the EVOH resin composition before drying was measured using an electronic balance, dried in a hot air dryer at 150°C for 5 hours, and the mass (W2) after cooling in the dryer for 30 minutes was measured and calculated using the following formula.
[0112] Water content (mass %) = [(W1-W2) / W1] × 100
[0113] In addition, when the EVOH resin composition is in the form of pellets, it is also preferred to attach a known lubricant to the surface of the pellets from the perspective of stabilizing the feeding property during melt molding. Examples of the lubricant include higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters of higher fatty acids, etc.), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, behenic acid amide; unsaturated higher fatty acid amides such as oleic acid amide, erucic acid amide, bis-higher fatty acid amides such as ethylene bis-stearic acid amide, ethylene bis-oleic acid amide, ethylene bis-erucic acid amide, ethylene bis-lauric acid amide, etc.), low molecular weight polyolefins (e.g., low molecular weight polyethylene or low molecular weight polypropylene having a molecular weight of about 500 to 10,000, or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, fluorinated vinyl resins, etc. These compounds can be used alone or in combination of two or more. In addition, the content of the lubricant is usually 5% by mass or less, preferably 1% by mass or less of the EVOH resin composition. It should be noted that the lower limit is usually 0% by mass.
[0114] The EVOH resin composition obtained in this way is prepared into various forms such as granules, powders or liquids, and is provided as a molding material for various molded objects. In particular, in the present invention, when provided as a material for melt molding, there is a tendency to more effectively obtain the effect of the present invention, so it is preferred.
[0115] In addition, the present EVOH resin composition also includes a resin composition obtained by mixing a resin other than the EVOH resin used in the present EVOH resin composition.
[0116] Examples of the molded product include a single-layer film molded from the present EVOH resin composition, and a multilayer structure having a layer composed of the present EVOH resin composition.
[0117] [Multilayer structure]
[0118] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the present multilayer structure") comprises a layer composed of the present EVOH resin composition. The layer composed of the present EVOH resin composition (hereinafter referred to as "the present EVOH resin composition layer") can be further provided with strength, or the present EVOH resin composition layer can be protected from moisture or the like, or other functions can be provided by laminating with another substrate having a thermoplastic resin other than the present EVOH resin composition as a main component (hereinafter, the resin used for the substrate is sometimes referred to as "substrate resin").
[0119] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers and ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, (unmodified) polyolefin resins such as polybutene, polypentene, and polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and mixtures of these polyolefin resins. The polyolefin resins in a broad sense of modified olefin resins such as unsaturated carboxylic acid-modified polyolefin resins obtained by graft-modifying hydrocarbons with unsaturated carboxylic acids or their esters, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, halogenated polyolefins such as chlorinated polyethylene and chlorinated polypropylene, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.
[0120] Among these, polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred as hydrophobic resins, and polyethylene resins, polypropylene resins, polycyclic olefin resins, and polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins thereof are more preferred.
[0121] When the EVOH resin composition layer is a (a1, a2, ...) and the substrate resin layer is b (b1, b2, ...), the layer structure of the multilayer structure may be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc. In addition, when the recycled layer including a mixture of the EVOH resin composition obtained by remelting and molding the end or defective products generated in the process of manufacturing the multilayer structure and a thermoplastic resin other than the EVOH resin composition is R, it may be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The number of layers of the multilayer structure is usually 2 to 15 in total, preferably 3 to 10. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be interposed between the layers as necessary.
[0122] As the above-mentioned adhesive resin, a known adhesive resin can be used, as long as it is appropriately selected according to the type of thermoplastic resin used in the substrate resin layer "b". Representative examples include modified polyolefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to polyolefin resins through addition reactions or grafting reactions. As the above-mentioned modified polyolefin polymers containing carboxyl groups, for example, maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block and random) copolymers, maleic anhydride grafted modified ethylene-ethyl acrylate copolymers, maleic anhydride grafted modified ethylene-vinyl acetate copolymers, maleic anhydride modified polycyclic olefin resins, maleic anhydride grafted modified polyolefin resins, etc. can be cited. These can be used alone or in combination of two or more.
[0123] In the present multilayer structure, when an adhesive resin layer is used between the present EVOH resin composition layer and the base resin layer, since the adhesive resin layer is located on both sides of the present EVOH resin composition layer, it is preferred to use an adhesive resin having excellent hydrophobicity.
[0124] The above-mentioned base resin and adhesive resin may also contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, nucleating agents, antiblocking agents, waxes, etc. within a range that does not hinder the gist of the present invention (e.g., 30% by mass or less, preferably 10% by mass or less relative to the entire resin). These may be used alone or in combination of two or more.
[0125] The lamination of the above-mentioned EVOH resin composition layer and the above-mentioned substrate resin layer (including the case where an adhesive resin layer is interposed) can be carried out by a known method. For example, there can be cited a method of melt-extrusion lamination of the substrate resin on a film, sheet, etc. of the present EVOH resin composition; a method of melt-extrusion lamination of the present EVOH resin composition on a substrate resin layer; a method of co-extruding the present EVOH resin composition and the substrate resin; a method of dry lamination of the present EVOH resin composition (layer) and the substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc.; a method of removing the solvent after applying a solution of the present EVOH resin composition on the substrate resin, etc. Among these, from the viewpoint of cost and environment, it is preferred to manufacture by a process of melt-molding the present EVOH resin composition layer, and specifically, a co-extrusion method is preferred.
[0126] Since the EVOH resin composition has thermoformability, the multilayer structure can be applied to thermoforming such as stretching or deep drawing. The EVOH resin composition and the multilayer structure are preferably used as materials for thermoforming containers such as cups, trays, tubes, and bottles by thermoforming.
[0127] The present multilayer structure may also be subjected to (heating) stretching treatment as required. The stretching treatment may be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, it may be simultaneous stretching or sequential stretching. In addition, as a stretching method, a stretching method with a high stretching ratio such as a roller stretching method, a tentering stretching method, a tubular stretching method, a stretch blow molding method, and a vacuum pressure forming method may be adopted. The stretching temperature is a temperature near the melting point of the multilayer structure, usually selected from a range of 40 to 170°C, preferably about 60 to 160°C. When the stretching temperature is too low, the stretchability becomes poor, and when it is too high, it is difficult to maintain a stable stretched state.
[0128] In addition, for the purpose of imparting dimensional stability, the stretched multilayer structure is heat-fixed. Heat-fixing can be implemented by a known method, for example, while maintaining the stretched multilayer structure in a tensile state, heat-treating it at a temperature of usually 80 to 180° C., preferably 100 to 165° C., for usually 2 to 600 seconds.
[0129] When the stretched multilayer structure is used as a shrink film, in order to impart heat shrinkage, the stretched multilayer structure may be cooled and fixed by blowing cold air instead of the heat setting.
[0130] The thickness of the present multilayer structure (including the stretched multilayer structure) and the thickness of the present EVOH resin composition layer, substrate resin layer and adhesive resin layer constituting the multilayer structure vary depending on the layer constitution, the type of substrate resin, the type of adhesive resin, the application and packaging form, the required physical properties, etc., and cannot be generalized, but the thickness of the present multilayer structure (including the stretched multilayer structure) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the substrate resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.
[0131] Furthermore, when the layers are multiple, the thickness ratio of the present EVOH resin composition layer to the substrate resin layer in the present multilayer structure (present EVOH resin composition layer / substrate resin layer) is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60, as a ratio of the thickest layers. In addition, when the layers are multiple, the thickness ratio of the present EVOH resin composition layer to the adhesive resin layer in the present multilayer structure (present EVOH resin composition layer / adhesive resin layer) is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10, as a ratio of the thickest layers.
[0132] In addition, the present multilayer structure can also be used to obtain a multilayer container in the shape of a cup or tray. In this case, a deep drawing method can usually be used, specifically, vacuum forming, pressure forming, vacuum pressure forming, plug-assisted vacuum pressure forming, etc. can be cited. Furthermore, in the case of obtaining a tube or bottle-shaped multilayer container (laminated structure) from a multilayer parison (a hollow tubular preform before blow molding), a blow molding method can be used. Specifically, extrusion blow molding (double-head type, mold moving type, parison moving type, rotary type, accumulator type, horizontal parison type, etc.), cold parison blow molding, injection blow molding, biaxial stretch blow molding (extrusion cold parison biaxial stretch blow molding, injection cold parison biaxial stretch blow molding, injection molding embedded biaxial stretch blow molding, etc.) can be cited. The obtained laminate can be subjected to heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making processing, deep drawing processing, box processing, tube processing, slitting processing, etc. as needed.
[0133] The monolayer film formed from the present EVOH resin composition, the container or cover material composed of the bag, cup, tray, tube, bottle, etc. composed of the present multilayer structure is useful as various packaging material containers for seasonings such as mayonnaise and sauce, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, pharmaceuticals, etc., in addition to general foods. In particular, since the present multilayer structure has thermoformability and coloration is suppressed, it is particularly useful as a thermoformed container system for food, medicine, pesticides, etc.
[0134] Example
[0135] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to the following examples in any way.
[0136] It should be noted that "parts" in the examples are based on mass unless otherwise specified.
[0137] <Example 1>
[0138] As EVOH resin (A1), particles of EVOH resin with an ethylene content of 29 mol%, a saponification degree of 99.6 mol%, and an MFR of 4 g / 10 min (210°C, a load of 2160 g) were used. As EVOH resin (A2), particles of EVOH resin with an ethylene content of 44 mol%, a saponification degree of 99.6 mol%, and an MFR of 4 g / 10 min (210°C, a load of 2160 g) were used.
[0139] In addition, titanium oxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the titanium compound.
[0140] 80 parts of the pellets of the EVOH resin (A1), 20 parts of the pellets of the EVOH resin (A2), and 0.1 ppm of the titanium oxide in terms of metal content relative to the mass of the EVOH resin composition were dry-blended to obtain a mixture.
[0141] The mixture is fed to a twin-screw extruder equipped with a double-hole die. The strands extruded and discharged under the following extrusion conditions were air-cooled and solidified on a belt conveyor. Then, the solidified strands were cut to obtain pellets of the EVOH resin composition.
[0142] [Extrusion conditions]
[0143] Extruder set temperature (℃): C1 / C2 / C3 / C4 / C5 / C6
[0144] =150 / 200 / 210 / 210 / 210 / 210
[0145] <Example 2>
[0146] Pellets of an EVOH resin composition were obtained in the same manner as in Example 1 except that the amount of titanium oxide blended in Example 1 was changed to 1 ppm in terms of metal relative to the mass of the EVOH resin composition.
[0147] <Comparative Example 1>
[0148] Pellets of an EVOH resin composition were obtained in the same manner as in Example 1 except that the titanium oxide was not used.
[0149] <Comparative Example 2>
[0150] Pellets of an EVOH resin composition were obtained in the same manner as in Example 1 except that the amount of titanium oxide blended in Example 1 was changed to 10 ppm in terms of metal relative to the mass of the EVOH resin composition.
[0151] The following long-term running performance evaluation was performed using the obtained pellets of the EVOH resin compositions of Examples 1 and 2 and Comparative Examples 1 and 2. The results are shown in Table 1 described below.
[0152] 〔Long-term operability evaluation〕
[0153] The obtained pellets of the EVOH resin composition were pulverized at 650 rpm using a pulverizer (SKR16-240 manufactured by Sometani Industries, Ltd.) to prepare pulverized products having a size of 1 to 5 mm square.
[0154] The obtained pulverized product was filled in a cylinder having an inner diameter of 32 mm and a height of 30 mm, and the YI value was measured with a spectrocolorimeter SE6000 (manufactured by Nippon Denshoku Industries) in a smoothed state.
[0155] In addition, the YI value of the pulverized product was similarly measured after the pulverized product was heat-treated in an oven at 150° C. for 5 hours.
[0156] Then, the ratio of the YI value after heating to the YI value before heating was calculated.
[0157] A larger ratio of the YI value after heating to the YI value before heating means that the EVOH resin composition changes color to yellow after heating.
[0158] [Table 1]
[0159]
[0160] According to Table 1, the EVOH resin compositions of Examples 1 and 2 containing a specific trace amount of titanium compound have a smaller ratio of YI values than the EVOH resin composition of Comparative Example 1 containing no titanium compound and the EVOH resin composition of Comparative Example 2 containing a titanium compound exceeding a specific range, and the color change due to heating is suppressed, so the long-term running property is excellent. In addition, the multilayer structure and thermoformed container having a layer composed of the EVOH resin composition of Examples 1 and 2 can also obtain the effect of suppressing the color change and excellent long-term running property.
[0161] The above embodiments show specific aspects of the present invention, but the above embodiments are merely illustrative and are not to be construed as limiting. Various modifications that are obvious to those skilled in the art are intended to be included within the scope of the present invention.
[0162] Industrial Applicability
[0163] Since the EVOH resin composition is suppressed from coloring changes due to thermal degradation during melt molding and has excellent long-term operability, it is useful as various packaging materials for various foods, such as mayonnaise, seasonings such as sauces, fermented foods such as miso, oily foods such as salad oils, beverages, cosmetics, and pharmaceuticals.
Claims
1. An ethylene-vinyl alcohol copolymer composition comprising: an ethylene-vinyl alcohol copolymer A comprising two or more ethylene-vinyl alcohol copolymers having different contents of ethylene structural units, and Titanium compound B; The metal equivalent content of the titanium compound B is 0.001 ppm or more and less than 5 ppm based on the mass of the ethylene-vinyl alcohol-based copolymer composition.
2. The ethylene-vinyl alcohol copolymer composition according to claim 1, wherein The difference in ethylene structural unit content between the ethylene-vinyl alcohol copolymer having the largest ethylene structural unit content and the ethylene-vinyl alcohol copolymer having the smallest ethylene structural unit content in the ethylene-vinyl alcohol copolymer A is 2 mol% or more.
3. The ethylene-vinyl alcohol copolymer composition according to claim 1 or 2, wherein The ethylene-vinyl alcohol copolymer A at least includes an ethylene-vinyl alcohol copolymer A1 having an ethylene structural unit content of less than 35 mol % and an ethylene-vinyl alcohol copolymer A2 having an ethylene structural unit content of 35 mol % or more.
4. The ethylene-vinyl alcohol copolymer composition according to claim 3, wherein The mass ratio of the ethylene-vinyl alcohol copolymer A1 having an ethylene structural unit content of less than 35 mol % to the ethylene-vinyl alcohol copolymer A2 having an ethylene structural unit content of 35 mol % or more, i.e., A1 / A2, is 1 / 99 to 99 / 1.
5. A melt molding material, comprising the ethylene-vinyl alcohol copolymer composition according to any one of claims 1 to 4. 6 . A multilayer structure comprising at least one layer comprising the ethylene-vinyl alcohol copolymer composition according to claim 1 .
7. A thermoformed container, comprising the multilayer structure according to claim 6.
8. A method for producing an ethylene-vinyl alcohol copolymer composition, which is a method for producing the ethylene-vinyl alcohol copolymer composition according to any one of claims 1 to 4, The method comprises the step of melt-mixing a composition raw material containing the ethylene-vinyl alcohol copolymer and a titanium compound.
9. A method for producing a multilayer structure, which is a method for producing the multilayer structure according to claim 6, The method comprises the step of melt-molding a layer composed of the ethylene-vinyl alcohol copolymer composition.