Resin composition
By using a specific amount of Fe-Ni-Si alloy magnetic powder combined with thermosetting resin in the resin composition, the balance between high relative permeability and low magnetic loss of the inductor element core material is solved, thereby improving the performance of the inductor element.
Patent Information
- Application Number
- CN202380022718.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-24
- Filing Date
- 2023-01-17
- Publication Date
- 2024-10-15
AI Technical Summary
In the prior art, it is difficult for core materials used in inductor elements to simultaneously achieve high relative permeability and low magnetic loss, especially in applications where inductor elements are placed inside the substrate. Resin compositions of magnetic powders have failed to effectively improve this problem.
A resin composition is formed by combining Fe-Ni-Si alloy magnetic powder with a Si content ranging from 1% to 8% by mass with a thermosetting resin. The particle size and ratio of the magnetic powder are optimized to improve the relative permeability and reduce the magnetic loss.
This study achieved a balanced improvement in relative permeability and magnetic loss of the cured resin composition, thereby enhancing the performance of inductor components.
Smart Images

Figure BDA0005001253390000421 
Figure HDA0005001253400000011 
Figure HDA0005001253400000012
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition, and a cured product, a magnetic paste, a resin sheet, a circuit board, and an inductor board using the resin composition. Background Art
[0002] As a core material of an inductor component, a cured product obtained by curing a resin composition containing magnetic powder may be used. As the magnetic powder, FeNi alloy powder may be used (Patent Document 1).
[0003] Prior art literature Patent Document 1: Japanese Patent Application Publication No. 2018-178254 Summary of the invention
[0004] Technical problem to be solved by the invention In the past, independent inductor components were generally installed on the substrate of the semiconductor device. However, in recent years, the following method is sometimes used: a coil is formed using the conductor pattern of the substrate, and an inductor element is arranged inside the substrate. In order to further improve the performance of the inductor element used for such purposes, it is required to further improve the magnetic properties of the core material. Specifically, it is necessary to develop a technology that can realize a core material with high relative magnetic permeability and low magnetic loss using a cured product of a resin composition containing magnetic powder.
[0005] The present invention is proposed in view of the above-mentioned problems, and its purpose is to provide: a resin composition that can obtain a cured product with improved relative magnetic permeability and magnetic loss; a cured product of the above-mentioned resin composition; a magnetic paste and a resin sheet containing the above-mentioned resin composition; and a circuit substrate and an inductor substrate containing the cured product of the above-mentioned resin composition.
[0006] Means of solving technical problems The present inventors have conducted intensive research to solve the above-mentioned problems. As a result, the present inventors have found that a resin composition comprising (A) Fe-Ni-Si alloy magnetic powder containing a specific amount of Si and (B) a thermosetting resin in combination can solve the above-mentioned problems, thereby completing the present invention. That is, the present invention includes the following contents.
[0007] <1> A resin composition comprising (A) Fe-Ni-Si alloy magnetic powder and (B) a thermosetting resin, wherein the amount of Si contained in the component (A) is 1% to 8% by mass relative to 100% by mass of the component (A). <2> according to <1> The resin composition, wherein the amount of the component (A) is 40% by mass or more relative to 100% by mass of the non-volatile components in the resin composition. <3> according to <1> or <2> The resin composition, wherein the amount of the component (A) is 30% by volume or more relative to 100% by volume of the non-volatile components in the resin composition. <4> according to <1> ~ <3> The resin composition described above, wherein the component (A) has an average particle size of 1 μm or more. <5> according to <1> ~ <4> The resin composition described above, wherein the component (A) has an average particle size of 10 μm or less. <6> according to <1> ~ <5> The resin composition described in any one of the above claims further comprises (C) a magnetic powder other than the Fe-Ni-Si alloy magnetic powder. <7> according to <6> The resin composition, wherein the component (C) contains alloy magnetic powder other than Fe-Ni-Si alloy magnetic powder. <8> according to <6> or <7> In the resin composition, component (C) comprises ferrite-based magnetic powder. <9> according to <6> ~ <8> The resin composition described above, wherein the component (C) comprises a ferrite-based magnetic powder, and the ferrite-based magnetic powder comprises at least one element selected from the group consisting of Mn, Zn, Ni and Cu. <10> according to <6> ~ <9> The resin composition described above, wherein the component (C) has an average particle size smaller than that of the component (A). <11> according to <6> ~ <10> The resin composition described above, wherein the ratio of the average particle size of the component (C) to the average particle size of the component (A) (average particle size of the component (C) / average particle size of the component (A)) is 0.001 to 0.9. <12> according to <6> ~ <11> The resin composition described above, wherein the volume ratio of the component (C) to the component (A) (component (C) / component (A)) is 0.01 to 0.9. <13> according to <6> ~ <12> The resin composition described in any one of the preceding claims, wherein the total amount of the component (A) and the component (C) is 70% by mass or more based on 100% by mass of the nonvolatile matter in the resin composition. <14> according to <6> ~ <13> The resin composition described in any one of the preceding claims, wherein the total amount of the component (A) and the component (C) is 50% by volume or more based on 100% by volume of a nonvolatile component in the resin composition. <15> according to <1> ~ <14> The resin composition described in any one of the preceding claims, wherein the component (B) comprises an epoxy resin. <16> according to <1> ~ <15> The resin composition described above further comprises (D) a thermoplastic resin. <17> according to <1> ~ <16> The resin composition as described above, which is used for filling holes. <18> <1> ~ <17> A cured product of any one of the resin compositions. <19> A magnetic paste comprising <1> ~ <17> The resin composition described above. <20> A resin sheet comprising a support and a resin composition layer provided on the support, wherein the resin composition layer comprises <1> ~ <17> The resin composition described above. <21> A circuit board comprising a substrate having a hole and a <1> ~ <17> A cured product of any one of the resin compositions. <22> A circuit substrate comprising <1> ~ <17> A cured material layer of a cured material of any one of the resin compositions. <23> An inductor substrate having <21> or <22> The circuit substrate. Effects of the Invention
[0008] According to the present invention, there can be provided: a resin composition that can obtain a cured product with improved relative magnetic permeability and magnetic loss; a cured product of the above resin composition; a magnetic paste and a resin sheet containing the above resin composition; and a circuit substrate and an inductor substrate containing the cured product of the above resin composition. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1 It is a cross-sectional view schematically showing a core substrate prepared in the method for manufacturing a circuit substrate according to the first example of one embodiment of the present invention. Figure 2 It is a cross-sectional view schematically showing a core substrate in which a through hole is formed in a method for manufacturing a circuit substrate according to a first example of an embodiment of the present invention. Figure 3 It is a cross-sectional view schematically showing a core substrate in which a plating layer is formed in a through hole in a method for manufacturing a circuit substrate according to a first example of one embodiment of the present invention. Figure 4 This is a cross-sectional view schematically showing a state in which a through hole of a core substrate is filled with a resin composition in a method for producing a circuit substrate according to a first example of one embodiment of the present invention. Figure 5 This is a schematic cross-sectional view for explaining step (2) of the method for manufacturing a circuit board according to the first example of one embodiment of the present invention. Figure 6 This is a schematic cross-sectional view for explaining step (3) of the method for manufacturing a circuit board according to the first example of one embodiment of the present invention. Figure 7 This is a schematic cross-sectional view for explaining step (5) of the method for manufacturing a circuit board according to the first example of one embodiment of the present invention. Figure 8 This is a schematic cross-sectional view for explaining step (5) of the method for manufacturing a circuit board according to the first example of one embodiment of the present invention. Fig. 9 This is a schematic cross-sectional view for explaining step (i) in the method for manufacturing a circuit board according to the second example of one embodiment of the present invention. Fig.10 This is a schematic cross-sectional view for explaining step (i) in the method for manufacturing a circuit board according to the second example of one embodiment of the present invention. Fig.11 This is a schematic cross-sectional view for explaining the step (ii) in the method for manufacturing a circuit board according to the second example of one embodiment of the present invention. Fig.12 This is a schematic cross-sectional view for explaining step (iv) in the method for manufacturing a circuit board according to the second example of one embodiment of the present invention. Fig.13 This is a schematic plan view of a circuit board included in an inductor substrate when viewed from one side in the thickness direction thereof. Fig.14 It means in Fig.13 The schematic diagram of the cut end surface of the circuit substrate cut at the position indicated by the II-II dot-dash line shown. Fig.15 This is a schematic plan view for explaining the structure of a first conductive layer of a circuit substrate including an inductor substrate. DETAILED DESCRIPTION
[0010] Hereinafter, the present invention will be described in detail based on its preferred embodiments. However, the present invention is not limited to the following embodiments and examples, and can be implemented with arbitrary modifications within the scope of the claims and their equivalents.
[0011] In the following description, the "resin component" of the resin composition means a component excluding inorganic particles such as magnetic powder, among non-volatile components contained in the resin composition.
[0012] In the following description, “magnetic permeability” means “relative magnetic permeability” unless otherwise specified.
[0013] <Overview of Resin Composition> A resin composition according to one embodiment of the present invention comprises (A) Fe-Ni-Si alloy magnetic powder and (B) a thermosetting resin. (A) Fe-Ni-Si alloy magnetic powder refers to a powder of an alloy comprising Fe, Ni and Si. In addition, (A) Fe-Ni-Si alloy magnetic powder comprises Si in a specific range of 1% to 8% by mass relative to 100% by mass of the (A) Fe-Ni-Si alloy magnetic powder. According to the resin composition, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be improved. Specifically, the relative magnetic permeability of the cured product can be increased, and the magnetic loss can be reduced.
[0014] The present inventors have estimated the mechanism by which such excellent effects can be obtained by the resin composition according to the present embodiment as follows. Generally, FeNi alloy has a crystal structure formed by Fe and Ni, and therefore has high crystallinity. Therefore, FeNi alloy has high relative magnetic permeability, but on the other hand, it tends to have high magnetic loss. In contrast, when Si is introduced into FeNi alloy, the crystal structure of Fe and Ni is distorted. Therefore, the greater the amount of Si introduced, the greater the distortion of the crystal structure of Fe and Ni, so it can be predicted that the relative magnetic permeability and magnetic loss will be greatly reduced. However, the inventors have conducted research and found that when the amount of Si introduced is in a specific range of 1% to 8% by mass, the reduction in magnetic loss can be increased, while the reduction in relative magnetic permeability can be reduced. Therefore, the (A) Fe-Ni-Si alloy magnetic powder containing Si in the above-mentioned specific range can exert the high relative magnetic permeability brought about by the crystal structure of Fe and Ni, and at the same time can exert the specific effect of Si that can effectively reduce magnetic loss. Therefore, the cured product of the resin composition can improve the relative magnetic permeability and magnetic loss in a balanced manner compared to a cured product of a conventional resin composition containing magnetic powder, by utilizing the above-mentioned specific action of the (A) Fe-Ni-Si alloy magnetic powder.
[0015] However, the technical scope of the present invention is not limited to the above mechanism. In addition, in the description of the above mechanism, the case of introducing Si into the FeNi alloy is taken as an example, but the method for producing the (A) Fe-Ni-Si alloy magnetic powder is not limited, and therefore, the powder produced by a method other than introducing Si into the FeNi alloy is also included in the (A) Fe-Ni-Si alloy magnetic powder.
[0016] <(A)Fe-Ni-Si alloy magnetic powder> The resin composition according to the present embodiment includes (A) Fe-Ni-Si alloy magnetic powder as the component (A). Therefore, the (A) Fe-Ni-Si alloy magnetic powder includes Fe, Ni, and Si in combination.
[0017] The amount of Si contained in the (A) Fe-Ni-Si alloy magnetic powder is usually 1% by mass or more, preferably 2% by mass or more, particularly preferably 3% by mass or more, and usually 8% by mass or less, more preferably 7% by mass or less, particularly preferably 6% by mass or less, relative to 100% by mass of the (A) Fe-Ni-Si alloy magnetic powder. When the amount of Si is within the above range, the relative permeability of the cured product of the resin composition can be improved and the magnetic loss can be reduced in a balanced manner.
[0018] (A) The mass ratio of the amount of Si to the amount of Fe contained in the Fe-Ni-Si alloy magnetic powder (Si / Fe) is preferably 0.01 or more, more preferably 0.02 or more, particularly preferably 0.04 or more, preferably 0.17 or less, more preferably 0.16 or less, and particularly preferably 0.14 or less. When the mass ratio of the amount of Si to the amount of Fe (Si / Fe) is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0019] (A) The mass ratio of the amount of Si to the amount of Ni contained in the Fe-Ni-Si alloy magnetic powder (Si / Ni) is preferably 0.01 or more, more preferably 0.02 or more, particularly preferably 0.04 or more, preferably 0.21 or less, more preferably 0.20 or less, and particularly preferably 0.18 or less. When the ratio of the amount of Si to the amount of Ni (Si / Ni) is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0020] The amount of Fe contained in the (A) Fe-Ni-Si alloy magnetic powder is preferably 33.00% by mass or more, more preferably 38.00% by mass or more, further preferably 43.00% by mass or more, particularly preferably 48.00% by mass or more, preferably 65.00% by mass or less, more preferably 60.00% by mass or less, further preferably 55.00% by mass or less, and particularly preferably 52.00% by mass or less, relative to 100% by mass of the (A) Fe-Ni-Si alloy magnetic powder. When the amount of Fe is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0021] Relative to 100% by mass of the (A) Fe-Ni-Si alloy magnetic powder, the amount of Ni contained in the (A) Fe-Ni-Si alloy magnetic powder is preferably 33.00% by mass or more, more preferably 38.00% by mass or more, further preferably 40.00% by mass or more, particularly preferably 42.00% by mass or more, preferably 65.00% by mass or less, more preferably 60.00% by mass or less, further preferably 54.00% by mass or less, particularly preferably 49.00% by mass or less. When the amount of Ni is within the above range, the relative permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0022] The total amount of Fe and Ni contained in the (A) Fe-Ni-Si alloy magnetic powder is preferably 85% by mass or more, more preferably 87% by mass or more, particularly preferably 92% by mass or more, preferably 99% by mass or less, more preferably 98.5% by mass or less, and particularly preferably 98% by mass or less, relative to 100% by mass of the (A) Fe-Ni-Si alloy magnetic powder. When the total amount of Fe and Ni is within the above range, the relative permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0023] (A) The mass ratio of the amount of Fe to the amount of Ni contained in the Fe-Ni-Si alloy magnetic powder (Fe / Ni) is preferably 0.5 or more, more preferably 0.7 or more, particularly preferably 1.0 or more, preferably 1.21 or less, more preferably 1.20 or less, and particularly preferably 1.19 or less. When the ratio of the amount of Fe to the amount of Ni (Fe / Ni) is within the above range, the relative permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0024] (A) Fe-Ni-Si alloy magnetic powder may also contain any element other than Fe, Ni and Si. As the arbitrary element, for example, an element from impurities that may inevitably be mixed according to the manufacturing method of (A) Fe-Ni-Si alloy magnetic powder can be cited. As specific examples of the arbitrary element, P, S, Mn, Cr, Mo, Cu and Co can be cited. However, from the viewpoint of significantly exerting the effect of the present invention, (A) Fe-Ni-Si alloy magnetic powder preferably does not contain any element other than Fe, Ni and Si. Therefore, (A) Fe-Ni-Si alloy magnetic powder preferably contains only Fe, Ni and Si.
[0025] (A) The amounts of Fe, Ni, and Si contained in the Fe—Ni—Si alloy magnetic powder can be measured by an inductively coupled plasma optical emission spectrometer (for example, “ICP-OES 720ES” manufactured by Agilent Technologies).
[0026] The average particle size D50 of the (A) Fe-Ni-Si alloy magnetic powder is preferably 1 μm or more, more preferably 2 μm or more, and particularly preferably 3 μm or more. When the average particle size D50 of the (A) Fe-Ni-Si alloy magnetic powder is above the aforementioned lower limit, it is preferred from the perspective of safety in handling the (A) Fe-Ni-Si alloy magnetic powder. Furthermore, when the average particle size D50 of the (A) Fe-Ni-Si alloy magnetic powder is above the aforementioned lower limit, the (A) Fe-Ni-Si alloy magnetic powder and the resin component containing the (B) thermosetting resin can be mixed with high uniformity, thereby effectively suppressing the localization of the (A) Fe-Ni-Si alloy magnetic powder caused by agglomeration. Therefore, the relative magnetic permeability and magnetic loss of the solidified material can be effectively improved. The upper limit of the average particle size D50 of the (A) Fe-Ni-Si alloy magnetic powder is preferably 10 μm or less, more preferably 9 μm or less, and particularly preferably 7 μm or less. When the average particle size D50 of the (A) Fe-Ni-Si alloy magnetic powder is below the above upper limit, the particles of the (A) Fe-Ni-Si alloy magnetic powder can be made smaller. Therefore, the generation of large eddy current losses caused by giant particles can be suppressed, thereby effectively suppressing magnetic losses. This effect is particularly effective when the amount of the (A) Fe-Ni-Si alloy magnetic powder is large.
[0027] (A) The average particle size D50 of the Fe-Ni-Si alloy magnetic powder, unless otherwise stated, represents the median particle size on a volume basis. The average particle size D50 can be measured by a laser diffraction / scattering method based on Mie scattering theory. Specifically, a particle size distribution can be prepared on a volume basis by a laser diffraction scattering particle size distribution measuring device, and the median particle size can be measured as the average particle size D50. The measured sample can preferably use a sample obtained by dispersing the powder in water by ultrasound. As a laser diffraction scattering particle size distribution measuring device, "LA-500" manufactured by Horiba, Ltd., "SALD-2200" manufactured by Shimadzu Corporation, etc. can be used.
[0028] (A) The specific surface area of the Fe-Ni-Si alloy magnetic powder is preferably 0.05 m 2 / g or more, more preferably 0.1m 2 / g or more, more preferably 0.5m 2 / g or more. Preferably 20m 2 / g or less, more preferably 10m 2 / g or less, more preferably 5m 2 / g or less. (A) When the specific surface area of the Fe-Ni-Si alloy magnetic powder is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved. The specific surface area of the magnetic powder can be measured by the BET method. Specifically, the specific surface area can be measured by the BET multi-point method using a specific surface area measuring device ("Macsorb HMModel 1210" manufactured by Mountech) to adsorb nitrogen on the surface of the sample according to the BET method.
[0029] The particles of the (A) Fe-Ni-Si alloy magnetic powder are preferably spherical. According to the research of the present inventors, the particles of the (A) Fe-Ni-Si alloy magnetic powder containing Si can generally have a shape with fewer bumps on the surface compared to the particles of the FeNi alloy powder not containing Si, and thus can have a shape close to a sphere.
[0030] The value obtained by dividing the major axis length of the particles of the (A) Fe-Ni-Si alloy magnetic powder by the minor axis length (aspect ratio) is preferably 2 or less, more preferably 1.6 or less, and further preferably 1.4 or less. When the (A) Fe-Ni-Si alloy magnetic powder has an aspect ratio within the above range, magnetic loss can be suppressed or the viscosity of the resin composition can be reduced.
[0031] There is no limitation on the method for manufacturing (A)Fe-Ni-Si alloy magnetic powder. (A)Fe-Ni-Si alloy magnetic powder can be manufactured, for example, using an atomization method. In the atomization method, (A)Fe-Ni-Si alloy magnetic powder is usually obtained by a method including the following steps, wherein a liquid stream containing molten iron, nickel and Si is allowed to fall while high-pressure water or gas is sprayed to rapidly solidify it. In the above-mentioned atomization method, a water atomization method of spraying water into the falling liquid stream is preferred. As such an atomization method, for example, the method described in Japanese Patent Gazette No. 2018-178254 can be used.
[0032] Relative to 100 volume % of the non-volatile components contained in the resin composition, the amount (volume %) of the (A) Fe-Ni-Si alloy magnetic powder contained in the resin composition is preferably 30 volume % or more, more preferably 40 volume % or more, particularly preferably 50 volume % or more, preferably 90 volume % or less, more preferably 80 volume % or less, and particularly preferably 70 volume % or less. When the amount of the (A) Fe-Ni-Si alloy magnetic powder is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved. In addition, when the amount of the (A) Fe-Ni-Si alloy magnetic powder is below the upper limit of the above range, the viscosity of the resin composition can usually be effectively reduced, and it is easy to make it into a paste.
[0033] The volume-based amount (volume %) of each component contained in the resin composition is calculated from the mass of the components contained in the resin composition. Specifically, the volume of each component can be obtained by dividing the mass by the specific gravity, and then the volume-based amount (volume %) can be calculated from the obtained volume of each component.
[0034] Relative to 100% by mass of the non-volatile components contained in the resin composition, the amount (mass %) of the (A) Fe-Ni-Si alloy magnetic powder contained in the resin composition is preferably 40% by mass or more, more preferably 50% by mass or more, particularly preferably 60% by mass or more, preferably 95% by mass or less, more preferably 90% by mass or less, and particularly preferably 80% by mass or less. When the amount of the (A) Fe-Ni-Si alloy magnetic powder is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved. In addition, when the amount of the (A) Fe-Ni-Si alloy magnetic powder is below the upper limit of the above range, the viscosity of the resin composition can usually be effectively reduced, and it is easy to make it into a paste.
[0035] The total amount of magnetic powder contained in the resin composition is usually expressed as the total amount of (A) Fe-Ni-Si alloy magnetic powder and (C) any magnetic powder described later. The total amount (volume %) of the magnetic powder contained in the resin composition is preferably 50% by volume or more, more preferably 60% by volume or more, further preferably 65% by volume or more, particularly preferably 70% by volume or more, preferably 90% by volume or less, more preferably 86% by volume or less, and particularly preferably 82% by volume or less, relative to 100% by volume of the non-volatile component in the resin composition. When the total amount of magnetic powder is within the above range, the relative permeability and magnetic loss of the cured product of the resin composition can be effectively improved. In addition, when the total amount of magnetic powder is below the upper limit of the above range, the viscosity of the resin composition can usually be effectively reduced, and it is easy to make a paste.
[0036] The total amount of magnetic powder contained in the resin composition is usually represented by the total amount of (A) Fe-Ni-Si alloy magnetic powder and (C) any magnetic powder described later. The total amount (mass %) of the magnetic powder contained in the resin composition is preferably 70 mass % or more, more preferably 80 mass % or more, further preferably 85 mass % or more, particularly preferably 90 mass % or more, preferably 99 mass % or less, more preferably 98 mass % or less, and particularly preferably 97 mass % or less, relative to 100 mass % of the non-volatile components in the resin composition. When the total amount of magnetic powder is within the above range, the relative permeability and magnetic loss of the cured product of the resin composition can be effectively improved. In addition, when the total amount of magnetic powder is below the upper limit value of the above range, the viscosity of the resin composition can usually be effectively reduced and it is easy to make a paste.
[0037] <(B) Thermosetting resin> The resin composition involved in one embodiment of the present invention includes (B) a thermosetting resin as the (B) component. The (B) thermosetting resin can usually bind magnetic powders such as (A) Fe-Ni-Si alloy magnetic powder. In addition, the (B) thermosetting resin usually reacts by heat to produce bonding and can be cured. Therefore, by curing the resin composition comprising the (A) Fe-Ni-Si alloy magnetic powder and the (B) thermosetting resin, a cured product can be obtained. The cured product has excellent relative permeability and magnetic loss, and thus can form an excellent magnetic layer.
[0038] Examples of the thermosetting resin (B) include epoxy resins, phenolic resins, active ester resins, amine resins, acid anhydride resins, benzoxazine resins, cyanate resins, and carbodiimide resins. The thermosetting resin (B) may be used alone or in combination of two or more.
[0039] The (B) thermosetting resin preferably includes the (B-1) epoxy resin. The (B-1) epoxy resin refers to a resin having one or more epoxy groups in the molecule. When the (B) thermosetting resin includes the (B-1) epoxy resin, the dispersibility of the (A) Fe-Ni-Si alloy magnetic powder can be improved, or the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0040] Examples of the epoxy resin (B-1) include biphenyl epoxy resins, bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, bisphenol AF epoxy resins, dicyclopentadiene epoxy resins, trisphenol epoxy resins, phenol novolac epoxy resins, glycidylamine epoxy resins, glycidyl ester epoxy resins, cresol novolac epoxy resins, biphenyl epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, alicyclic epoxy resins having an ester skeleton, Epoxy resin; heterocyclic epoxy resin; epoxy resin containing spiro ring; cyclohexane epoxy resin; cyclohexanedimethanol epoxy resin; trimethylol epoxy resin; tetraphenylethane epoxy resin; epoxy resin containing condensed ring skeleton such as naphthyl ether epoxy resin, tert-butyl-catechol epoxy resin, naphthalene epoxy resin, naphthol epoxy resin, anthracene epoxy resin, naphthol novolac epoxy resin; isocyanurate epoxy resin; epoxy resin containing alkylene oxide skeleton and butadiene skeleton; epoxy resin containing fluorene structure; etc. (B-1) Epoxy resin can be used alone or in combination of two or more.
[0041] The epoxy resin (B-1) preferably contains an epoxy resin having two or more epoxy groups in one molecule. The proportion of the epoxy resin having two or more epoxy groups in one molecule is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more, relative to 100% by mass of the total amount of the epoxy resin (B-1).
[0042] (B-1) The epoxy resin preferably has an aromatic structure. When two or more epoxy resins are used, preferably one or more epoxy resins have an aromatic structure. The aromatic structure is a chemical structure generally defined as an aromatic structure, and also includes polycyclic aromatics and aromatic heterocycles.
[0043] The epoxy resin (B-1) includes an epoxy resin that is liquid at a temperature of 20°C (hereinafter sometimes referred to as "liquid epoxy resin") and an epoxy resin that is solid at a temperature of 20°C (hereinafter sometimes referred to as "solid epoxy resin"). The epoxy resin (B-1) may be only a liquid epoxy resin, only a solid epoxy resin, or a combination of a liquid epoxy resin and a solid epoxy resin. Among them, the epoxy resin (B-1) preferably includes a liquid epoxy resin, and particularly preferably includes only a liquid epoxy resin.
[0044] As the liquid epoxy resin, a liquid epoxy resin having two or more epoxy groups in one molecule is preferred. As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane type epoxy resin, cyclohexanedimethanol type epoxy resin, epoxy resin having a butadiene structure, epoxy resin containing an alkylene oxide skeleton and a butadiene skeleton, epoxy resin containing a fluorene structure, and dicyclopentadiene type epoxy resin are preferred. Among them, bisphenol A type epoxy resin and bisphenol F type epoxy resin are particularly preferred.
[0045] Specific examples of liquid epoxy resins include "YX7400" manufactured by Mitsubishi Chemical Corporation; "HP4032", "HP4032D", and "HP4032SS" (naphthalene-type epoxy resins) manufactured by DIC Corporation; "828US", "828EL", "jER828EL", "825", and "EPIKOTE "828EL" (bisphenol A type epoxy resin); "jER807", "1750" (bisphenol F type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630", "630LSD", "604" (glycidylamine type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "ED-523T" (GLYCIROL type epoxy resin) manufactured by ADEKA Corporation; "EP-3950L", "EP-3980S" (glycidylamine type epoxy resin) manufactured by ADEKA Corporation; "EP-4088S" (dicyclopentadiene type epoxy resin) manufactured by ADEKA Corporation; "ZX-1059" (a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin) manufactured by Nippon Steel Chemical Materials Co., Ltd.; Nagase "EX-721" (glycidyl ester type epoxy resin) manufactured by ChemteX; "EX-991L" (epoxy resin containing an alkylene oxide skeleton) manufactured by Nagase ChemteX; "CELLOXIDE 2021P" and "CELLOXIDE 2081" (alicyclic epoxy resins having an ester skeleton) manufactured by Daicel; "PB-3600" manufactured by Daicel, "JP-100" and "JP-200" manufactured by Nippon Soda Co., Ltd. (epoxy resins having a butadiene structure); "ZX-1658" and "ZX-1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resins) manufactured by Nippon Steel Chemicals Co., Ltd.; "EG-280" (epoxy resin containing a fluorene structure) manufactured by Osaka Gas Chemical Co., Ltd.; etc. The liquid epoxy resins may be used alone or in combination of two or more.
[0046] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferred, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferred. As the solid epoxy resin, a biphenylol type epoxy resin, a naphthalene type epoxy resin, a naphthalene type tetrafunctional epoxy resin, a cresol novolac type epoxy resin, a dicyclopentadiene type epoxy resin, a trisphenol type epoxy resin, a naphthol type epoxy resin, a biphenyl type epoxy resin, a naphthyl ether type epoxy resin, anthracene type epoxy resin, a bisphenol A type epoxy resin, a bisphenol AF type epoxy resin, a tetraphenylethane type epoxy resin is preferred, and a dicyclopentadiene type epoxy resin is particularly preferred.
[0047] Specific examples of solid epoxy resins include "HP4032H" (naphthalene-type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene-type tetrafunctional epoxy resin) manufactured by DIC Corporation; "N-690" (cresol novolac-type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac-type epoxy resin) manufactured by DIC Corporation; "HP-7200", "HP-7200HH", and "HP-7200H" (dicyclopentadiene epoxy resin) manufactured by DIC Corporation; "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000" (naphthyl ether type epoxy resin) manufactured by DIC Corporation; "EPPN-502H" (trisphenol type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC7000L" (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC3000H", "NC3000", "NC3000 L", "NC3100" (biphenyl type epoxy resin); "ESN475V" (naphthol type epoxy resin) manufactured by Nippon Steel Chemicals; "ESN485" (naphthol novolac type epoxy resin) manufactured by Nippon Steel Chemicals; "YX4000H", "YX4000", "YL6121" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical; "YX4000HK" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical; "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical ); "YX7700" manufactured by Mitsubishi Chemical Corporation (a novolac epoxy resin containing a xylene structure); "PG-100" and "CG-500" manufactured by Osaka Gas Chemical Co., Ltd.; "YL7760" manufactured by Mitsubishi Chemical Corporation (a bisphenol AF epoxy resin); "YL7800" manufactured by Mitsubishi Chemical Corporation (a fluorene epoxy resin); "jER1010" manufactured by Mitsubishi Chemical Corporation (a solid bisphenol A epoxy resin); "jER1031S" manufactured by Mitsubishi Chemical Corporation (a tetraphenylethane epoxy resin), etc. The solid epoxy resin may be used alone or in combination of two or more.
[0048] When a liquid epoxy resin and a solid epoxy resin are used in combination as the epoxy resin, the mass ratio of the liquid epoxy resin to the solid epoxy resin (liquid epoxy resin / solid epoxy resin) is preferably 0.5 or more, more preferably 1 or more, further preferably 5 or more, and particularly preferably 10 or more.
[0049] The epoxy equivalent of the epoxy resin (B-1) is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., further preferably 80 g / eq. to 2000 g / eq., and further more preferably 110 g / eq. to 1000 g / eq. The epoxy equivalent is the mass of the resin containing 1 equivalent of epoxy groups. The epoxy equivalent can be measured according to JIS K 7236.
[0050] The weight average molecular weight (Mw) of the (B-1) epoxy resin is preferably 100 to 5000, more preferably 250 to 3000, and even more preferably 400 to 1500. The weight average molecular weight of the resin can be measured as a value in terms of polystyrene by gel permeation chromatography (GPC).
[0051] The amount (mass %) of the epoxy resin (B-1) contained in the resin composition is preferably 0.1 mass % or more, more preferably 0.5 mass % or more, particularly preferably 1 mass % or more, preferably 30 mass % or less, more preferably 20 mass % or less, particularly preferably 10 mass % or less, relative to 100 mass % of the non-volatile components of the resin composition. When the amount of the epoxy resin (B-1) is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0052] The amount (mass %) of the epoxy resin (B-1) contained in the resin composition is preferably 10 mass % or more, more preferably 20 mass % or more, particularly preferably 30 mass % or more, preferably 90 mass % or less, more preferably 80 mass % or less, particularly preferably 70 mass % or less, relative to 100 mass % of the resin component of the resin composition. When the amount of the epoxy resin (B-1) is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0053] When (B) thermosetting resin includes (B-1) epoxy resin, (B) thermosetting resin may also include a resin capable of reacting and combining with (B-1) epoxy resin. Hereinafter, the resin capable of reacting and combining with (B-1) epoxy resin is sometimes referred to as "(B-2) curing agent". Examples of (B-2) curing agents include phenolic resins, active ester resins, amine resins, carbodiimide resins, anhydride resins, benzoxazine resins, cyanate resins, thiol resins, and the like. (B-2) curing agents may be used alone or in combination of two or more. Among them, phenolic resins are preferred.
[0054] As the phenolic resin, a resin having one or more, preferably two or more, hydroxyl groups bonded to aromatic rings such as a benzene ring and a naphthalene ring in one molecule can be used. From the viewpoint of heat resistance and water resistance, a phenolic resin having a phenolic structure is preferred. In addition, from the viewpoint of adhesion, a nitrogen-containing phenolic resin is preferred, and a phenolic resin containing a triazine skeleton is more preferred. Among them, from the viewpoint of highly satisfying heat resistance, water resistance and adhesion, a linear phenolic resin containing a triazine skeleton is preferred.
[0055] Specific examples of phenolic resins include "MEH-7700", "MEH-7810", "MEH-7851", and "MEH-8000H" manufactured by Meiwa Chemicals; "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd.; "SN-170", "SN-180", "SN-190", "SN-475", "SN-485", "SN-495", "SN-495V", "SN-375", and "SN-475" manufactured by Nippon Steel Chemicals Co., Ltd. N-395"; "TD-2090", "TD-2090-60M", "LA-7052", "LA-7054", "LA-1356", "LA-3018", "LA-3018-50P", "EXB-9500", "HPC-9500", "KA-1160", "KA-1163", "KA-1165" manufactured by DIC Corporation; "GDP-6115L", "GDP-6115H", "ELPC 75" and other products manufactured by Qun Rong Chemical Co., Ltd.
[0056] As active ester resin, compounds having more than one, preferably more than two active ester groups in one molecule can be used. Among them, as active ester resin, preferably phenolic esters, thiophenolic esters, N-hydroxylamine esters, esters of heterocyclic hydroxy compounds, etc. have more than two ester groups with high reactive activity in one molecule. The active ester resin is preferably obtained by the condensation reaction of carboxylic acid compounds and / or thiocarboxylic acid compounds with hydroxy compounds and / or thiol compounds. In particular, from the viewpoint of improving heat resistance, active ester resins obtained from carboxylic acid compounds and hydroxy compounds are preferably obtained, and active ester resins obtained from carboxylic acid compounds and phenolic compounds and / or naphthol compounds are more preferably obtained. As carboxylic acid compounds, for example benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, pyromellitic acid, etc. can be cited. Examples of the phenol compound or naphthol compound include hydroquinone, resorcinol, bisphenol A, bisphenol F, bisphenol S, phenolphthalein, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucinol, pyrogallol, dicyclopentadiene-type diphenol compounds, and novolac resins. Here, the “dicyclopentadiene-type diphenol compound” refers to a diphenol compound obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.
[0057] Preferred specific examples of active ester resins include active ester resins containing a dicyclopentadiene diphenol structure, active ester resins containing a naphthalene structure, active ester resins containing acetylated products of novolac resins, and active ester resins containing benzoylated products of novolac resins. Among them, active ester resins containing a naphthalene structure and active ester resins containing a dicyclopentadiene diphenol structure are more preferred. "Dicyclopentadiene diphenol structure" means a divalent structural unit formed of phenylene-dicyclopentylene-phenylene.
[0058] As commercially available active ester resins, examples of active ester resins containing a dicyclopentadiene-type diphenol structure include "EXB9451", "EXB9460", "EXB9460S", "HPC-8000-65T", "HPC-8000H-65TM", and "EXB-8000L-65TM" (manufactured by DIC Corporation); examples of active ester resins containing a naphthalene structure include "EXB-9416-70BK", "EXB-8150-65T", "EXB-8100L-65T", and "EXB-8150L-65T" (manufactured by DIC Corporation); Examples of active ester resins comprising acetylated products of linear phenolic resins include "DC808" (manufactured by Mitsubishi Chemical Corporation); examples of active ester resins comprising benzoylated products of linear phenolic resins include "YLH1026" (manufactured by Mitsubishi Chemical Corporation); examples of active ester resins that are acetylated products of linear phenolic resins include "DC808" (manufactured by Mitsubishi Chemical Corporation); examples of active ester resins that are benzoylated products of linear phenolic resins include "YLH1026" (manufactured by Mitsubishi Chemical Corporation), "YLH1030" (manufactured by Mitsubishi Chemical Corporation), and "YLH1048" (manufactured by Mitsubishi Chemical Corporation), etc.
[0059] As the amine resin, a resin having one or more, preferably two or more, amino groups in one molecule can be used. Examples of the amine resin include aliphatic amines, polyether amines, alicyclic amines, aromatic amines, and the like. Among them, aromatic amines are preferred. The amine resin is preferably a primary amine or a secondary amine, and a primary amine is more preferred. Specific examples of the amine resin include 4,4'-methylenebis(2,6-dimethylaniline), diphenyldiaminosulfone, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, metaphenylenediamine, metaxylene diamine, diethyltoluene diamine, 4,4'-diaminodiphenyl ether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, 2,2-bis(3-amino- 4-hydroxyphenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, etc. Amine resins can also be commercially available products, for example, "KAYABOND C-200S", "KAYABOND C-100", "KAYAHARD AA", "KAYAHARD AB", "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd., "Epicure W" manufactured by Mitsubishi Chemical Corporation, etc.
[0060] As the carbodiimide resin, a resin having one or more, preferably two or more, carbodiimide structures in one molecule can be used. Specific examples of the carbodiimide resin include aliphatic biscarbodiimides such as tetramethylene-bis(tert-butylcarbodiimide) and cyclohexanebis(methylene-tert-butylcarbodiimide); aromatic biscarbodiimides such as phenylene-bis(xylylcarbodiimide); aliphatic polycarbodiimides such as polyhexamethylenecarbodiimide, polytrimethylhexamethylenecarbodiimide, polycyclohexylenecarbodiimide, poly(methylenebiscyclohexylenecarbodiimide), poly(isophoronecarbodiimide); poly(phenylenecarbodiimide), poly(
[0043] Polycarbodiimides include aromatic polycarbodiimides such as naphthylene carbodiimide), poly(tolylene carbodiimide), poly(methyl diisopropyl phenylene carbodiimide), poly(triethyl phenylene carbodiimide), poly(diethyl phenylene carbodiimide), poly(triisopropyl phenylene carbodiimide), poly(diisopropyl phenylene carbodiimide), poly(xylylene carbodiimide), poly(tetramethyl xylylene carbodiimide), poly(methylene diphenylene carbodiimide), and poly[methylene bis(methyl phenylene) carbodiimide]. Examples of commercially available carbodiimide resins include "CARBODILITE V-02B", "CARBODILITE V-03", "CARBODILITE V-04K", "CARBODILITE V-07" and "CARBODILITE V-09" manufactured by Nisshinbo Chemical Co., Ltd.; and "Stabaxol P", "Stabaxol P400" and "Hycasyl 510" manufactured by Rhein-Chemie.
[0061] As the anhydride resin, a resin having one or more anhydride groups in one molecule can be used, preferably a resin having two or more anhydride groups in one molecule. Specific examples of the anhydride resin include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenylsuccinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, diphenyl Acid anhydrides of polymer type such as ketone tetracarboxylic dianhydride, biphenyl tetracarboxylic dianhydride, naphthalene tetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfone tetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), styrene-maleic acid resin obtained by copolymerization of styrene and maleic acid, etc. Commercially available products of anhydride-based resins include, for example, "HNA-100", "MH-700", "MTA-15", "DDSA", and "OSA" manufactured by Shin Nippon Chemical Co., Ltd.; "YH-306" and "YH-307" manufactured by Mitsubishi Chemical Corporation; "HN-2200" and "HN-5500" manufactured by Hitachi Chemical Co., Ltd.; and "EF-30", "EF-40", "EF-60", and "EF-80" manufactured by Cray Valley Corporation.
[0062] Specific examples of the benzoxazine resin include "JBZ-OD100", "JBZ-OP100D", and "ODA-BOZ" manufactured by JFE Chemical Co., Ltd.; "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.; and "HFB2006M" manufactured by Showa High Molecular Co., Ltd.
[0063] Examples of cyanate resins include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenylcyanate), 4,4'-ethylenediphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanatephenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanatephenyl-1-(methylethylene))benzene, bis(4-cyanatephenyl)sulfide, and bis(4-cyanatephenyl)ether; polyfunctional cyanate resins derived from phenol novolac resins and cresol novolac resins; prepolymers obtained by partially triazinizing these cyanate resins; and the like. Specific examples of cyanate ester resins include "PT30" and "PT60" manufactured by Lonza Japan Co., Ltd. (both are phenol novolac-type multifunctional cyanate resins), "BA230" and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate is triazine-formed to become trimers), etc.
[0064] Examples of the thiol resin include trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), and tris(3-mercaptopropyl)isocyanurate.
[0065] The active group equivalent of the curing agent (B-2) is preferably 50 g / eq. to 3000 g / eq., more preferably 100 g / eq. to 1000 g / eq., further preferably 100 g / eq. to 500 g / eq., and particularly preferably 100 g / eq. to 300 g / eq. The active group equivalent represents the mass of the curing agent (B-2) per 1 equivalent of active groups.
[0066] When the number of epoxy groups of the epoxy resin (B-1) is set to 1, the number of active groups of the curing agent (B-2) is preferably 0.01 or more, more preferably 0.1 or more, particularly preferably 0.5 or more, preferably 10 or less, more preferably 5 or less, and particularly preferably 3 or less. The active group of the curing agent (B-2) is an active hydroxyl group, etc., which varies depending on the type of curing agent. In addition, the number of epoxy groups of the epoxy resin (B-1) refers to the value obtained by adding the mass of the non-volatile components of each epoxy resin divided by the epoxy equivalent for all epoxy resins. Furthermore, the number of active groups of the curing agent (B-2) refers to the value obtained by adding the mass of the non-volatile components of each curing agent divided by the active group equivalent for all curing agents.
[0067] The amount (mass %) of the (B-2) curing agent contained in the resin composition is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, particularly preferably 1% by mass or more, preferably 20% by mass or less, more preferably 10% by mass or less, particularly preferably 5% by mass or less, relative to 100% by mass of the non-volatile component of the resin composition. When the amount of the (B-2) curing agent is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0068] The amount (mass %) of the (B-2) curing agent contained in the resin composition is preferably 1 mass % or more, more preferably 5 mass % or more, particularly preferably 10 mass % or more, preferably 50 mass % or less, more preferably 40 mass % or less, particularly preferably 30 mass % or less, relative to 100 mass % of the resin component of the resin composition. When the amount of the (B-2) curing agent is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0069] The weight average molecular weight (Mw) of the (B) thermosetting resin may generally be in the same range as the weight average molecular weight of the (B-1) epoxy resin described above.
[0070] The amount (mass %) of the (B) thermosetting resin contained in the resin composition is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, particularly preferably 1% by mass or more, preferably 30% by mass or less, more preferably 20% by mass or less, particularly preferably 10% by mass or less, relative to 100% by mass of the non-volatile components of the resin composition. When the amount of the (B) thermosetting resin is within the above range, the relative permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0071] The amount (mass %) of the (B) thermosetting resin contained in the resin composition is preferably 10 mass % or more, more preferably 30 mass % or more, particularly preferably 50 mass % or more, preferably 99 mass % or less, more preferably 90 mass % or less, particularly preferably 80 mass % or less, relative to 100 mass % of the resin component of the resin composition. When the amount of the (B) thermosetting resin is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0072] <(C) Any magnetic powder (magnetic powder other than Fe-Ni-Si alloy magnetic powder)> The resin composition according to one embodiment of the present invention may further include (C) a magnetic powder other than the Fe-Ni-Si alloy magnetic powder as an arbitrary component in combination with the above-mentioned (A) to (B) components. The "(C) magnetic powder other than the Fe-Ni-Si alloy magnetic powder" as the (C) component may be appropriately referred to as "(C) arbitrary magnetic powder".
[0073] As (C) any magnetic powder, particles of a material having a relative magnetic permeability greater than 1 can be used. The material of (C) any magnetic powder is generally an inorganic material, and can be a soft magnetic material or a hard magnetic material. In addition, the material of (C) any magnetic powder can be used alone or in combination of two or more. Therefore, (C) any magnetic powder can be a soft magnetic powder, a hard magnetic powder, or a combination of a soft magnetic powder and a hard magnetic powder. In addition, (C) any magnetic powder can be used alone or in combination of two or more. Among them, (C) any magnetic powder preferably contains soft magnetic powder, and more preferably contains only soft magnetic powder.
[0074] (C) As an optional magnetic powder, a magnetic metal oxide powder and a magnetic metal powder are mentioned, for example.
[0075] As magnetic metal oxide powders, for example: ferrite-based magnetic powders; and iron oxide powders such as iron oxide powder (III) and iron oxide powder; etc. Among them, ferrite-based magnetic powders are preferred. Therefore, (C) any magnetic powder preferably includes ferrite-based magnetic powders. In one example, as (C) any magnetic powder, only ferrite-based magnetic powders may be used. Ferrite-based magnetic powders are generally formed of composite oxides having iron oxide as a main component and are chemically stable. Therefore, according to the ferrite-based magnetic powders, advantages such as high corrosion resistance, low risk of fire, and difficulty in demagnetization can be obtained.
[0076] Examples of ferrite-based magnetic powders include Fe-Mn ferrite powder, Fe-Mn-Mg ferrite powder, Fe-Mn-Mg-Sr ferrite powder, Fe-Mg-Zn ferrite powder, Fe-Mg-Sr ferrite powder, Fe-Zn-Mn ferrite powder, Fe-Cu-Zn ferrite powder, Fe-Ni-Zn ferrite powder, Fe-Ni-Zn-Cu ferrite powder, Fe-Ba-Zn ferrite powder, Fe-Ba-Mg ferrite powder, Fe-Ba-Ni ferrite powder, Fe-Ba-Co ferrite powder, Fe-Ba-Ni-Co ferrite powder, and Fe-Y ferrite powder.
[0077] Among the ferrite-based magnetic powders, ferrite-based magnetic powders containing at least one element selected from Mn, Zn, Ni and Cu are preferred. Therefore, (C) any magnetic powder preferably contains ferrite-based magnetic powders containing at least one element selected from Mn, Zn, Ni and Cu. In one example, as (C) any magnetic powder, only ferrite-based magnetic powders containing at least one element selected from Mn, Zn, Ni and Cu can be used. As such preferred ferrite magnetic powders, for example, Fe-Mn ferrite powders, Fe-Mn-Mg ferrite powders, Fe-Mn-Mg-Sr ferrite powders, Fe-Mg-Zn ferrite powders, Fe-Zn-Mn ferrite powders, Fe-Cu-Zn ferrite powders, Fe-Ni-Zn ferrite powders, Fe-Ni-Zn-Cu ferrite powders, Fe-Ba-Zn ferrite powders, Fe-Ba-Ni ferrite powders, and Fe-Ba-Ni-Co ferrite powders can be cited. Among them, ferrite magnetic powders containing at least one element selected from Zn and Mn are more preferred, and ferrite magnetic powders containing Zn and Mn are particularly preferred. Therefore, as ferrite magnetic powders, Fe-Zn-Mn ferrite powders are particularly preferred. Fe—Zn—Mn-based ferrite powder refers to ferrite powder containing Fe, Zn, and Mn.
[0078] As magnetic metal powders, for example, pure iron powders; Fe-Si alloy powders, Fe-Si-Al alloy powders, Fe-Cr alloy powders, Fe-Cr-Si alloy powders, Fe-Ni-Cr alloy powders, Fe-Cr-Al alloy powders, Fe-Ni alloy powders, Fe-Ni-B alloy powders, Fe-Ni-Mo alloy powders, Fe-Ni-Mo-Cu alloy powders, Fe-Co alloy powders, Fe-Ni-Co alloy powders, Co-based amorphous alloy powders, and the like, crystalline or amorphous alloy magnetic powders; and the like. Among them, alloy magnetic powders other than Fe-Ni-Si alloy magnetic powders are preferred. Therefore, (C) any magnetic powder preferably includes alloy magnetic powders other than Fe-Ni-Si alloy magnetic powders. In one example, as (C) any magnetic powder, only alloy magnetic powders other than Fe-Ni-Si alloy magnetic powders may be used. Furthermore, among alloy magnetic powders, iron alloy powders are more preferred.
[0079] As particularly preferred magnetic metal powders, iron alloy magnetic powders containing Fe and at least one element selected from Si and Cr are preferred, and Fe-Cr-Si alloy powders are particularly preferred. Fe-Cr-Si alloy powders refer to alloy powders containing Fe, Cr, and Si.
[0080] As (C) any magnetic powder, commercially available magnetic powder can be used. Specific examples of commercially available magnetic powder include "MZ03S", "M05S", "M001", and "MZ05S" manufactured by Powdertech; "PST-S" manufactured by Sanyo Special Steel Co., Ltd.; "AW2-08", "AW2-08PF20F", "AW2-08PF10F", "AW2-08PF3F", "Fe-3.5Si-4.5CrPF20F", "Fe-50NiPF20F", and "Fe-80Ni-4MoPF20F" manufactured by EPSON ATMIX; "CVD iron powder 0.7 μm", "LD-M", "LD-MH", "KNI-106", "KNI-106GSM", "KNI-106GS", and "K "NI-109", "KNI-109GSM", "KNI-109GS" manufactured by Toda Industry Co., Ltd.; "KNS-415", "BSF-547", "BSF-029", "BSN-125", "BSN-125", "BSN-714", "BSN-828", "S-1281", "S-1641", "S-1651", "S-1470", "S-1511", "S-2430" manufactured by Nippon Heavy Chemical Industry Co., Ltd.; "Nanotek" manufactured by CIK NanoTek; "JEMK-S", "JEMK-H" manufactured by KINSEIMATEC; "Yttrium iron oxide (yttrium iron oxide)" manufactured by ALDRICH; "MA-RCO-5" manufactured by DOWA Electronics Co., Ltd.; etc. (C) Any magnetic powder may be used alone or in combination of two or more.
[0081] (C) Any magnetic powder preferably has a smaller average particle size than (A) Fe-Ni-Si alloy magnetic powder. When (C) Any magnetic powder has a smaller average particle size than (A) Fe-Ni-Si alloy magnetic powder, (C) Any magnetic powder can enter the gaps between the particles of (A) Fe-Ni-Si alloy magnetic powder, so that the magnetic powder can be highly filled, and thus the magnetic properties such as relative magnetic permeability can be improved.
[0082] The ratio of the average particle size of (C) any magnetic powder to the average particle size of (A) Fe-Ni-Si alloy magnetic powder ((C) average particle size of any magnetic powder / (A) average particle size of Fe-Ni-Si alloy magnetic powder) is preferably within a specific range. Specifically, the above ratio ((C) average particle size of any magnetic powder / (A) average particle size of Fe-Ni-Si alloy magnetic powder) is preferably greater than 0.001, more preferably greater than 0.01, particularly preferably greater than 0.1, preferably less than 0.9, more preferably less than 0.6, and particularly preferably less than 0.3. When the ratio ((C) average particle size of any magnetic powder / (A) average particle size of Fe-Ni-Si alloy magnetic powder) is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0083] (C) The specific range of the average particle size of any magnetic powder is preferably 0.05 μm or more, more preferably 0.1 μm or more, particularly preferably 0.2 μm or more, preferably 3 μm or less, more preferably 2 μm or less, and particularly preferably 1.5 μm or less. (C) When the average particle size of any magnetic powder is above the lower limit, the viscosity of the resin composition can be reduced. In addition, when it is below the upper limit, the relative permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0084] (C) The average particle size of any magnetic powder can be measured by the same method as (A) the average particle size of the Fe—Ni—Si alloy magnetic powder.
[0085] (C) The specific surface area of any magnetic powder is preferably larger than the specific surface area of (A) the Fe-Ni-Si alloy magnetic powder. The specific range of the specific surface area of any magnetic powder is preferably 0.1 m 2 / g or more, more preferably 1.0 m 2 / g or more, particularly preferably 2m 2 / g or more, preferably 40m 2 / g or less, more preferably 30m 2 / g or less, particularly preferably 20m 2 / g or less.
[0086] (C) The particles of any magnetic powder are preferably spherical or ellipsoidal particles. The ratio (aspect ratio) calculated by dividing the major axis length of the particles of any magnetic powder (C) by the minor axis length is preferably less than 2, more preferably less than 1.5, further preferably less than 1.2, and usually greater than 1.0. Generally, if the shape of the particles of the magnetic powder is not spherical but flat, it is easy to increase the relative magnetic permeability. On the other hand, if the shape of the particles of the magnetic powder is close to spherical, it is easy to reduce the magnetic loss.
[0087] (C) The true specific gravity of any magnetic powder can be, for example, 4 g / cm 3 ~10g / cm 3 .
[0088] The amount (volume %) of the arbitrary magnetic powder (C) contained in the resin composition may be 0 volume % or more than 0 volume % relative to 100 volume % of the non-volatile components of the resin composition, preferably 1 volume % or more, more preferably 5 volume % or more, particularly preferably 10 volume % or more, preferably 40 volume % or less, more preferably 35 volume % or less, particularly preferably 30 volume % or less. When the amount (volume %) of the arbitrary magnetic powder (C) is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0089] The amount (mass %) of any magnetic powder (C) contained in the resin composition may be 0 mass % or more than 0 mass % relative to 100 mass % of the non-volatile components of the resin composition, preferably 1 mass % or more, more preferably 5 mass % or more, particularly preferably 10 mass % or more, preferably 40 mass % or less, more preferably 35 mass % or less, particularly preferably 30 mass % or less. When the amount (mass %) of any magnetic powder (C) is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0090] When (A) Fe-Ni-Si alloy magnetic powder and (C) any magnetic powder are used in combination, the volume ratio of (C) any magnetic powder to (A) Fe-Ni-Si alloy magnetic powder ((C) component / (A) component) is preferably within a specific range. The above-mentioned volume ratio ((C) component / (A) component) is specifically preferably greater than 0.01, more preferably greater than 0.1, further preferably greater than 0.2, particularly preferably greater than 0.3, preferably less than 0.9, more preferably less than 0.8, and particularly preferably less than 0.7. When the volume ratio ((C) component / (A) component) is within the above-mentioned range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0091] When (A) Fe-Ni-Si alloy magnetic powder and (C) any magnetic powder are used in combination, the mass ratio of (C) any magnetic powder to (A) Fe-Ni-Si alloy magnetic powder ((C) component / (A) component) is preferably within a specific range. The above-mentioned mass ratio ((C) component / (A) component) is specifically preferably greater than 0.1, more preferably greater than 0.2, particularly preferably greater than 0.3, preferably less than 0.7, more preferably less than 0.6, and particularly preferably less than 0.5. When the mass ratio ((C) component / (A) component) is within the above-mentioned range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0092] <(D) Thermoplastic resin> In the resin composition involved in one embodiment of the present invention, the above-mentioned (A) to (C) components can be combined to further include (D) thermoplastic resin as an arbitrary component. The (D) thermoplastic resin as the (D) component does not contain substances belonging to the above-mentioned (A) to (C) components. According to the (D) thermoplastic resin, the mechanical properties of the cured product of the resin composition can be effectively improved.
[0093] Examples of the (D) thermoplastic resin include phenoxy resins, polyimide resins, polyvinyl acetal resins, polyolefin resins, polybutadiene resins, polyamide-imide resins, polyetherimide resins, polysulfone resins, polyethersulfone resins, polyphenylene ether resins, polycarbonate resins, polyetheretherketone resins, polyester resins, etc. The (D) thermoplastic resin may be used alone or in combination of two or more.
[0094] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenol acetophenone skeleton, phenolic skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group. Specific examples of phenoxy resins include "1256" and "4250" manufactured by Mitsubishi Chemical Corporation (both are phenoxy resins containing a bisphenol A skeleton); "YX8100" manufactured by Mitsubishi Chemical Corporation (a phenoxy resin containing a bisphenol S skeleton); "YX6954" manufactured by Mitsubishi Chemical Corporation (a phenoxy resin containing a bisphenol acetophenone skeleton); "FX280" and "FX293" manufactured by Nippon Steel Chemical Materials Co., Ltd.; "YL7500BH30", "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", "YL7482" and "YL7891BH30" manufactured by Mitsubishi Chemical Corporation.
[0095] Specific examples of polyimide resins include "SLK-6100" manufactured by Shin-Etsu Chemical Co., Ltd., "RIKACOAT SN20" and "RIKACOAT PN20" manufactured by Shin-Nippon Chemical Co., Ltd. Specific examples of polyimide resins include linear polyimides obtained by reacting difunctional hydroxyl-terminated polybutadiene, a diisocyanate compound and a tetrabasic acid anhydride (polyimides described in Japanese Unexamined Patent Publication No. 2006-37083), polyimides containing a polysiloxane skeleton (polyimides described in Japanese Unexamined Patent Publication No. 2002-12667 and Japanese Unexamined Patent Publication No. 2000-319386), and the like.
[0096] Examples of the polyvinyl acetal resin include polyvinyl formal resin and polyvinyl butyral resin, and polyvinyl butyral resin is preferred. Specific examples of the polyvinyl acetal resin include "Denka Butyral 4000-2", "Denka Butyral 5000-A", "Denka Butyral 6000-C", and "Denka Butyral 6000-EP" manufactured by Denki Kagaku Kogyo Co., Ltd.; and S-LEC BH series, BX series (e.g., BX-5Z), KS series (e.g., KS-1), BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.
[0097] Examples of the polyolefin resin include ethylene copolymer resins such as low-density polyethylene, ultra-low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymers, ethylene-ethyl acrylate copolymers, and ethylene-methyl acrylate copolymers; and polyolefin polymers such as polypropylene and ethylene-propylene block copolymers.
[0098] Examples of the polybutadiene resin include a resin containing a hydrogenated polybutadiene skeleton, a polybutadiene resin containing a hydroxyl group, a polybutadiene resin containing a phenolic hydroxyl group, a polybutadiene resin containing a carboxyl group, a polybutadiene resin containing an acid anhydride group, a polybutadiene resin containing an epoxy group, a polybutadiene resin containing an isocyanate group, a polybutadiene resin containing a urethane group, and a polyphenylene ether-polybutadiene resin.
[0099] Specific examples of polyamideimide resins include "VYLOMAX HR11NN" and "VYLOMAX HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamideimide resins include modified polyamideimides such as "KS9100" and "KS9300" (polyamideimide containing a polysiloxane skeleton) manufactured by Hitachi Chemical Co., Ltd.
[0100] Specific examples of the polyethersulfone resin include "PES5003P" manufactured by Sumitomo Chemical Co., Ltd. and the like.
[0101] Specific examples of the polysulfone resin include polysulfone "P1700" and "P3500" manufactured by Solvay Performance Polymers.
[0102] Specific examples of the polyphenylene ether resin include "NORYL SA90" manufactured by SABIC, etc. Specific examples of the polyetherimide resin include "Ultem" manufactured by GE, etc.
[0103] As polycarbonate resins, for example, carbonate resins containing hydroxyl groups, carbonate resins containing phenolic hydroxyl groups, carbonate resins containing carboxyl groups, carbonate resins containing acid anhydride groups, carbonate resins containing isocyanate groups, carbonate resins containing urethane groups, etc. Specific examples of polycarbonate resins include "FPC0220" manufactured by Mitsubishi Gas Chemical Co., Ltd., "T6002", "T6001" (polycarbonate diol) manufactured by Asahi Kasei Chemicals Co., Ltd., "C-1090", "C-2090", "C-3090" (polycarbonate diol) manufactured by Kuraray Co., Ltd., etc. Specific examples of polyetheretherketone resins include "Sumiploy K" manufactured by Sumitomo Chemical Co., Ltd., etc.
[0104] Examples of the polyester resin include polyethylene terephthalate resin, polyethylene naphthalate resin, polybutylene terephthalate resin, polybutylene naphthalate resin, polytrimethylene terephthalate resin, polytrimethylene naphthalate resin, and polycyclohexane dimethyl terephthalate resin.
[0105] The weight average molecular weight (Mw) of the (D) thermoplastic resin is preferably greater than 5,000, more preferably 8,000 or more, further preferably 10,000 or more, and particularly preferably 20,000 or more. The upper limit is not particularly limited, and may be, for example, 1,000,000 or less, 500,000 or less, or 100,000 or less.
[0106] The amount (mass %) of the (D) thermoplastic resin contained in the resin composition relative to 100% by mass of the non-volatile component of the resin composition may be 0% by mass, or may be greater than 0% by mass, preferably 0.01% by mass or more, more preferably 0.05% by mass or more, particularly preferably 0.1% by mass or more, preferably 5% by mass or less, more preferably 3% by mass or less, and particularly preferably 2% by mass or less. When the amount of the (D) thermoplastic resin is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0107] The amount (mass %) of the (D) thermoplastic resin contained in the resin composition may be 0 mass % or more than 0 mass % relative to 100 mass % of the resin component of the resin composition, preferably 1 mass % or more, more preferably 5 mass % or more, particularly preferably 10 mass % or more, preferably 40 mass % or less, more preferably 30 mass % or less, particularly preferably 20 mass % or less. When the amount of the (D) thermoplastic resin is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0108] <(E) Dispersant> In the resin composition involved in one embodiment of the present invention, the above-mentioned (A) to (D) components can be combined to further include (E) a dispersant as an arbitrary component. The (E) dispersant as the (E) component does not contain substances belonging to the above-mentioned (A) to (D) components. The (E) dispersant can improve the dispersibility of magnetic powders such as (A) Fe-Ni-Si alloy magnetic powder and (C) arbitrary magnetic powder.
[0109] There is no limitation on the type of (E) dispersant. For example, as the (E) dispersant, there can be used a dispersant that contains a functional group capable of adsorbing magnetic powder and disperses the magnetic powder due to repulsion (e.g., electrostatic repulsion, steric repulsion, etc.) between the (E) dispersants when adsorbed on the magnetic powder. Examples of such (E) dispersants include acidic dispersants and alkaline dispersants.
[0110] Acidic dispersants usually contain acidic functional groups such as carboxyl, sulfonyl (-SO3H), sulfate (-OSO3H), phosphonyl (-PO(OH)2), phosphonyloxy (-OPO(OH)2), hydroxyphosphoryl (-PO(OH)-), and sulfhydryl (-SH). Acidic functional groups usually have dissociated protons and can be neutralized with bases such as amines and hydroxide ions. Preferred acidic dispersants include acidic polymer dispersants containing polymer chains such as polyoxyalkylene chains and polyether chains. Preferred examples of acidic dispersants include "C-2093I" and "SC-1015F (a multifunctional comb-type functional polymer having an ionic group in the main chain and a polyoxyalkylene chain in the graft chain)" manufactured by NOF Corporation; "ED152", "ED153", "ED154", "ED118", "ED174", "ED251", and "DA-375" (polyether-type phosphate-based dispersants) manufactured by Kusumoto Chemicals Co., Ltd.; "RS-410", "RS-610", and "RS-710" (pH 1.9) of the "Phosphanol" series manufactured by Toho Chemical Industry Co., Ltd. (phosphate-based dispersants); and "AKM-0531", "AFB-1521", "SC-0505K", and "SC-0708A" of the "MALIALIM" series manufactured by NOF Corporation.
[0111] The alkaline dispersant usually contains basic functional groups such as primary, secondary and tertiary amino groups; ammonium groups; imino groups; and nitrogen-containing heterocyclic groups such as pyridine, pyrimidine, pyrazine, imidazole, and triazole. The basic functional groups can be neutralized with acids such as organic acids and inorganic acids. As preferred alkaline dispersants, there can be mentioned alkaline polymer dispersants containing polymer chains such as polyester chains. As preferred examples of alkaline dispersants, there can be mentioned "PB-881" (polyamine dispersant containing polyester chains) manufactured by Ajinomoto Fine-Techno Co., Ltd.
[0112] (E) The dispersant may be used alone or in combination of two or more.
[0113] The amount (mass %) of the (E) dispersant contained in the resin composition may be 0 mass % or more than 0 mass % relative to 100 mass % of the non-volatile component of the resin composition, preferably 0.01 mass % or more, more preferably 0.1 mass % or more, particularly preferably 0.2 mass % or more, preferably 5 mass % or less, more preferably 3 mass % or less, particularly preferably 2 mass % or less. When the amount of the (E) dispersant is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0114] The amount (mass %) of the (E) dispersant contained in the resin composition may be 0 mass % or more than 0 mass % relative to 100 mass % of the resin component of the resin composition, preferably 0.1 mass % or more, more preferably 1 mass % or more, particularly preferably 2 mass % or more, preferably 30 mass % or less, more preferably 25 mass % or less, particularly preferably 20 mass % or less. When the amount of the (E) dispersant is within the above range, the relative magnetic permeability and magnetic loss of the cured product of the resin composition can be effectively improved.
[0115] <(F) Curing accelerator> In the resin composition involved in one embodiment of the present invention, it is possible to combine with the above-mentioned (A) to (E) components and further include (F) a curing accelerator as an arbitrary component. The (F) curing accelerator as the (F) component does not contain substances belonging to the above-mentioned (A) to (E) components. The (F) curing accelerator has a function as a catalyst for the reaction of the (B) thermosetting resin, and thus can promote the curing of the resin composition.
[0116] Examples of the (F) curing accelerator include phosphorus curing accelerators, imidazole curing accelerators, amine curing accelerators, guanidine curing accelerators, metal curing accelerators, and urea curing accelerators. The (F) curing accelerator may be used alone or in combination of two or more. Among them, the (F) curing accelerator is preferably a phosphorus curing accelerator and an imidazole curing accelerator, and more preferably a phosphorus curing accelerator.
[0117] Phosphorus-based curing accelerators include, for example, phosphonium salts and phosphines. Phosphonium salts include, for example, tetrabutylphosphonium bromide, tetrabutylphosphonium chloride, tetrabutylphosphonium acetate, tetrabutylphosphonium decanoate, tetrabutylphosphonium laurate, n-butylphosphonium tetraphenylborate, bis(tetrabutylphosphonium)pyromellitic acid salt, tetrabutylphosphonium hexahydrophthalate, tetrabutylphosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate, di-tert-butylmethylphosphonium tetraphenylborate and other aliphatic phosphonium salts; methyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, propyltriphenylphosphonium bromide and the like. Aromatic phosphonium salts such as phosphonium bromide, butyltriphenylphosphonium bromide, benzyltriphenylphosphonium chloride, tetraphenylphosphonium bromide, p-tolyltriphenylphosphonium tetra-p-tolylborate, tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, triphenylethylphosphonium tetraphenylborate, tris(3-methylphenyl)ethylphosphonium tetraphenylborate, tris(2-methoxyphenyl)ethylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate.
[0118] Examples of the phosphine include aliphatic phosphines such as tributylphosphine, tri-tert-butylphosphine, trioctylphosphine, di-tert-butyl(2-butenyl)phosphine, di-tert-butyl(3-methyl-2-butenyl)phosphine, and tricyclohexylphosphine; and dibutylphenylphosphine, di-tert-butylphenylphosphine, methyldiphenylphosphine, ethyldiphenylphosphine, butyldiphenylphosphine, diphenylcyclohexylphosphine, triphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, tri(4-ethylphenyl)phosphine, tri(4-propylphenyl)phosphine, tri(4-isopropylphenyl)phosphine, tri(4-butylphenyl)phosphine, tri(4-tert-butylphenyl)phosphine, tri(2,4-dimethylphenyl)phosphine, tri(2,5-dimethylphenyl)phosphine, tri(2,6-dimethylphenyl)phosphine, tri(3 Aromatic phosphines such as 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,2-bis(diphenylphosphino)acetylene and 2,2'-bis(diphenylphosphino)diphenyl ether; aromatic phosphine-borane complexes such as triphenylphosphine-triphenylborane; aromatic phosphine-quinone addition reactants such as triphenylphosphine-p-benzoquinone addition reactants, etc.
[0119] As the phosphorus-based curing accelerator, a commercially available item may be used, and examples thereof include "TBP-DA" manufactured by Hokko Chemical Industry Co., Ltd. and the like.
[0120] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazole trimellitate, 2,4-diamino-6-[2′-methylimidazolyl-(1′)]-ethyl-s-triazine, 2,4-diamino-6-[2′-methylimidazolyl-(1′)]-ethyl-s-triazine, and 2,4-diamino-6-[2′-methylimidazolyl-(1′)]-ethyl-s-triazine. Imidazole compounds such as amino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, 2-phenylimidazoline, and adducts of imidazole compounds with epoxy resins are preferred, and 2-ethyl-4-methylimidazole and 1-benzyl-2-phenylimidazole are preferred. As the imidazole-based curing accelerator, commercially available products may also be used, for example, "P200-H50" manufactured by Mitsubishi Chemical Corporation; "CUREZOL 2MZ", "2E4MZ", "Cl1Z", "Cl1Z-CN", "Cl1Z-CNS", "Cl1Z-A", "2MZ-OK", "2MA-OK", "2MA-OK-PW", "2MZA-PW", "2PHZ", "2PHZ-PW", "1B2PZ", "1B2PZ-10M", etc. manufactured by Shikoku Chemical Industries, Ltd.
[0121] As the amine-based curing accelerator, for example, trialkylamines such as triethylamine and tributylamine; 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, 1,8-diazabicyclo(5,4,0)-undecene, 1,8-diazabicyclo[5,4,0]undecene-7,4-dimethylaminopyridine, 2,4,6-tris(dimethylaminomethyl)phenol, etc., preferably 4-dimethylaminopyridine. As the amine-based curing accelerator, commercially available products can be used, for example, "PN-50", "PN-23", "MY-25" manufactured by Ajinomoto Fine Technologies Co., Ltd., etc. can be mentioned.
[0122] Examples of the guanidine-based curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanidine, 1-ethylbiguanidine, 1-n-butylbiguanidine, 1-n-octadecylbiguanidine, 1,1-dimethylbiguanidine, 1,1-diethylbiguanidine, 1-cyclohexylbiguanidine, 1-allylbiguanidine, 1-phenylbiguanidine, and 1-(o-tolyl)biguanidine. Preferred examples include dicyandiamide and 1,5,7-triazabicyclo[4.4.0]dec-5-ene.
[0125] As metal curing accelerators, organic metal complexes or organic metal salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin can be cited. Specific examples of organic metal complexes include organic cobalt complexes such as cobalt acetylacetonate (II) and cobalt acetylacetonate (III); organic copper complexes such as copper acetylacetonate (II); organic zinc complexes such as zinc acetylacetonate (II); organic iron complexes such as iron acetylacetonate (III); organic nickel complexes such as nickel acetylacetonate (II); organic manganese complexes such as manganese acetylacetonate (II). As organic metal salts, for example, zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, zinc stearate, etc. can be cited.
[0124] Examples of the urea curing accelerator include 1,1-dimethylurea; aliphatic dimethylureas such as 1,1,3-trimethylurea, 3-ethyl-1,1-dimethylurea, 3-cyclohexyl-1,1-dimethylurea, and 3-cyclooctyl-1,1-dimethylurea; 3-phenyl-1,1-dimethylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(2-methylphenyl)-1,1-dimethylurea, 3-(4-methylphenyl)-1,1-dimethylurea, 3-(3,4-dimethylphenyl)-1,1 -dimethylurea, 3-(4-isopropylphenyl)-1,1-dimethylurea, 3-(4-methoxyphenyl)-1,1-dimethylurea, 3-(4-nitrophenyl)-1,1-dimethylurea, 3-[4-(4-methoxyphenoxy)phenyl]-1,1-dimethylurea, 3-[4-(4-chlorophenoxy)phenyl]-1,1-dimethylurea, 3-[3-(trifluoromethyl)phenyl]-1,1-dimethylurea, N,N-(1,4-phenylene)bis(N',N'-dimethylurea), N,N-(4-methyl-1,3-phenylene)bis(N',N'-dimethylurea) [toluenebisdimethylurea] and the like.
[0125] The amount (mass %) of the (F) curing accelerator contained in the resin composition relative to 100 mass % of the non-volatile components of the resin composition can be 0 mass % or greater than 0 mass %, preferably 0.001 mass % or more, more preferably 0.005 mass % or more, particularly preferably 0.01 mass % or more, preferably 3 mass % or less, more preferably 2 mass % or less, particularly preferably 1 mass % or less.
[0126] The amount (mass %) of the (F) curing accelerator contained in the resin composition relative to 100 mass % of the resin component of the resin composition can be 0 mass % or greater than 0 mass %, and is preferably 0.01 mass % or more, more preferably 0.05 mass % or more, particularly preferably 0.1 mass % or more, preferably 5 mass % or less, more preferably 2 mass % or less, and particularly preferably 1 mass % or less.
[0127] <(G) Optional additives> The resin composition according to one embodiment of the present invention may further include (G) an optional additive as an optional component in combination with the above-mentioned components (A) to (F). The (G) optional additive as the component (G) does not include any substance belonging to the above-mentioned components (A) to (F).
[0128] (G) As optional additives, for example, free radical polymerizable compounds such as maleimide free radical polymerizable compounds, vinylphenyl free radical polymerizable compounds, (meth) acrylic free radical polymerizable compounds, allyl free radical polymerizable compounds, and polybutadiene free radical polymerizable compounds; free radical polymerization initiators such as peroxide free radical polymerization initiators and azo free radical polymerization initiators; inorganic particles (inorganic fillers) such as silica particles; organic fillers such as rubber particles; organic metal compounds such as organic copper compounds and organic zinc compounds; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as silicone-based leveling agents and acrylic polymer-based leveling agents; thickeners such as bentonite and montmorillonite; Defoamers such as silicone defoamers, acrylic defoamers, fluorine defoamers, and vinyl resin defoamers; UV absorbers such as benzotriazole UV absorbers; adhesion enhancers such as urea silane; adhesion imparting agents such as triazole adhesion imparting agents, tetrazole adhesion imparting agents, and triazine adhesion imparting agents; antioxidants such as hindered phenol antioxidants; flame retardants such as phosphorus flame retardants (such as phosphate compounds, phosphazene compounds, phosphinic acid compounds, and red phosphorus), nitrogen flame retardants (such as melamine sulfate), halogen flame retardants, and inorganic flame retardants (such as antimony trioxide); stabilizers such as borate stabilizers, titanate stabilizers, aluminate stabilizers, zirconate stabilizers, isocyanate stabilizers, carboxylic acid stabilizers, and carboxylic anhydride stabilizers, etc. (G) Any additive may be used alone or in combination of two or more.
[0129] <(H)Solvent> The resin composition according to one embodiment of the present invention may further contain (H) a solvent as a volatile component in combination with the nonvolatile components such as the above-mentioned (A) to (G) components.
[0130] As the (H) solvent, an organic solvent is generally used. Examples of the (H) solvent include ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; ether solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, and diphenyl ether; alcohol solvents such as methanol, ethanol, propanol, butanol, and ethylene glycol; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, and carbitol acetate. Ether ester solvents such as acetate, γ-butyrolactone, and methyl methoxypropionate; ester alcohol solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate; ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butyl carbitol); amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone; sulfoxide solvents such as dimethyl sulfoxide; nitrile solvents such as acetonitrile and propionitrile; aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. (H) The solvent may be used alone or in combination of two or more.
[0131] The amount of (H) solvent is preferably set to be able to adjust the melt viscosity of the resin composition to an appropriate range. Relative to 100% by mass of the non-volatile component in the resin composition, the amount of (H) solvent can be, for example, 3% by mass or less, 1% by mass or less, 0.5% by mass or less, 0.1% by mass or less, or 0.01% by mass or less. Among them, the resin composition is particularly preferably free of (H) solvent. When the amount of (H) solvent is small, the generation of voids caused by the volatilization of (H) solvent can be suppressed. Furthermore, the handling and operability of the resin composition can be improved.
[0132] <Characteristics of Resin Composition> The above-mentioned resin composition can be cured by heat. Therefore, by thermally curing the resin composition, a cured product of the resin composition can be obtained. Generally, among the components contained in the resin composition, volatile components such as (H) solvent can be volatilized by heat during thermal curing, while non-volatile components such as (A) to (G) components will not be volatilized by heat during thermal curing. Therefore, the cured product of the resin composition can contain the non-volatile components of the resin composition or their reaction products.
[0133] According to the resin composition involved in the present embodiment, a cured product with improved relative magnetic permeability and magnetic loss can be obtained. Generally, the cured product of the resin composition involved in the present embodiment can have high magnetic permeability and low magnetic loss compared with the cured product of the conventional resin composition containing Fe-Ni alloy magnetic powder without Si, the cured product of the conventional resin composition containing Ni alloy magnetic powder, and the cured product of the conventional resin composition containing Fe-Si-Cr alloy magnetic powder.
[0134] Therefore, according to the above-mentioned resin composition, a cured product with high relative magnetic permeability can be obtained. For example, when the relative magnetic permeability of the cured product of the resin composition is measured under the conditions of a measurement frequency of 20 MHz and a room temperature of 23°C, the relative magnetic permeability is preferably 14.8 or more, more preferably 15.0 or more, and particularly preferably 15.1 or more. There is no particular restriction on the upper limit of the relative magnetic permeability, and for example, it may be 35.0 or less, 30.0 or less, 25.0 or less, 23.0 or less, etc. The relative magnetic permeability of the cured product can be measured, for example, using a cured product obtained by curing the resin composition at 190°C for 90 minutes, using the method described in the examples.
[0135] In addition, according to the above-mentioned resin composition, a cured product with low magnetic loss can be obtained. The magnetic loss can be represented by the loss coefficient tanδ. Generally, the smaller the loss coefficient tanδ, the smaller the magnetic loss. For example, when the loss coefficient tanδ of the cured product of the resin composition is measured under the conditions of a measurement frequency of 20 MHz and a room temperature of 23°C, the loss coefficient tanδ is preferably less than 0.020, more preferably less than 0.017, and particularly preferably less than 0.015. The loss coefficient tanδ of the cured product can be measured, for example, by using a cured product obtained by curing the resin composition at 190°C for 90 minutes, using the method described in the examples.
[0136] Crystalline alloy powders such as alloy powders containing Fe and Ni can generally have high relative magnetic permeability, but on the other hand tend to have large magnetic loss. Therefore, it was difficult to obtain a cured product with high relative magnetic permeability and low magnetic loss in the past. In view of such past situations, the effect of the above-mentioned resin composition that can improve both relative magnetic permeability and magnetic loss is industrially beneficial.
[0137] There is no particular restriction on the properties of the resin composition. Therefore, the resin composition may be solid or in a fluid paste state. For example, the resin composition may be a paste-like resin composition using a solvent, or may be a paste-like resin composition without a solvent by using a liquid thermosetting resin such as a liquid epoxy resin. In the case where the solvent content in the resin composition is small or the resin composition does not contain a solvent, the generation of voids caused by solvent volatilization can be suppressed, and the handling and operability are also excellent.
[0138] Utilizing the above-mentioned excellent properties, the resin composition is preferably used as a resin composition for inductor manufacturing. For example, the above-mentioned resin composition is preferably used as a resin composition for hole filling for filling holes of a substrate provided on a circuit substrate. In addition, for example, the above-mentioned resin composition is also preferably used to form a cured layer on a circuit substrate. In order to be easily applied to these uses, the resin composition can be used in the form of a paste or in the form of a resin sheet containing a layer of the resin composition.
[0139] <Method for producing resin composition> The resin composition involved in one embodiment of the present invention can be manufactured by mixing the above-mentioned components, for example. The above-mentioned components can be mixed in part or in whole at the same time, or can be mixed in sequence. In the process of mixing the components, the temperature can be appropriately set, so heating and / or cooling can be performed temporarily or all the time. In addition, in the process of mixing the components, stirring or vibration can also be performed. Furthermore, degassing can also be performed under low pressure conditions such as vacuum.
[0140] <Magnetic paste> The magnetic paste involved in one embodiment of the present invention includes the above-mentioned resin composition. The magnetic paste is usually a fluid paste containing a resin composition, and therefore can be preferably used for filling holes using a printing method. The magnetic paste can only contain the above-mentioned resin composition, or it can be combined with a resin composition to contain any component. Preferably, the paste-like resin composition itself can be used as a magnetic paste.
[0141] The magnetic paste is preferably in a paste state at 23° C. The viscosity of the magnetic paste is preferably 20 Pa·s or more, more preferably 25 Pa·s or more, further preferably 30 Pa·s or more, particularly preferably 50 Pa·s or more, preferably 200 Pa·s or less, more preferably 180 Pa·s or less, and further preferably 160 Pa·s or less at 23° C. The viscosity can be measured, for example, using an E-type viscometer (“RE-80U” manufactured by Toki Sangyo Co., Ltd., 3°×R9.7 rotor) under the measurement conditions of a measurement sample amount of 0.22 ml and a rotation speed of 5 rpm.
[0142] <Resin Sheet> The resin sheet according to one embodiment of the present invention includes a support and a resin composition layer provided on the support. The resin composition layer includes the above-mentioned resin composition, and preferably includes only the resin composition.
[0143] From the viewpoint of thinning, the thickness of the resin composition layer is preferably 250 μm or less, and more preferably 200 μm or less. The lower limit of the thickness of the resin composition layer may be, for example, 5 μm or more, 10 μm or more, or the like.
[0144] Examples of the support include films made of plastic materials, metal foils, and release papers, and films made of plastic materials and metal foils are preferred.
[0145] When a film formed of a plastic material is used as a support, the plastic material includes polyesters such as polyethylene terephthalate (hereinafter sometimes referred to as "PET") and polyethylene naphthalate (hereinafter sometimes referred to as "PEN"), polycarbonate (hereinafter sometimes referred to as "PC"), acrylic polymers such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among them, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.
[0146] When a metal foil is used as a support, examples of the metal foil include copper foil and aluminum foil, preferably copper foil. The copper foil may be a foil made of a single metal such as copper or an alloy of copper and other metals (such as tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.).
[0147] The support may be subjected to matte treatment or corona treatment on the surface to be bonded to the resin composition layer.
[0148] In addition, as the support, a support with a release layer having a release layer on the surface bonded to the resin composition layer can also be used. As the release agent used in the release layer of the support with a release layer, for example, one or more release agents selected from alkyd release agents, polyolefin release agents, polyurethane release agents and silicone release agents can be cited. The support with a release layer can use a commercial product, for example, it can be a PET film having a release layer with a silicone release agent or an alkyd resin release agent as the main component, that is, "PET501010", "SK-1", "AL-5", "AL-7" manufactured by Lintec; "Lumirror T60" manufactured by Toray Industries; "Purex" manufactured by Teijin; "Unipeel" manufactured by Unitika, etc.
[0149] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, the thickness of the entire support with a release layer is preferably in the above range.
[0150] In the resin sheet, a protective film selected based on the support can be further laminated on the surface of the resin composition layer that is not bonded to the support (i.e., the surface on the side opposite to the support). The thickness of the protective film is not particularly limited, and can be, for example, 1 μm to 40 μm. By providing the protective film, it is possible to suppress the adhesion of garbage or the like on the surface of the resin composition layer or the generation of damage.
[0151] The resin sheet can be, for example, coated on a support by a die coater etc. to form a resin composition layer. As required, an organic solvent can also be mixed in the resin composition and then coated on a support. When using an organic solvent, drying can be performed after coating as required.
[0152] Drying can be carried out, for example, by heating, hot air blowing, etc. The drying conditions are not particularly limited, and the drying is carried out in a manner such that the content of the organic solvent in the resin composition layer is 10% by mass or less, preferably 5% by mass or less. Depending on the components contained in the resin composition, for example, the resin composition layer can be formed by drying at 50° C. to 150° C. for 3 minutes to 10 minutes.
[0153] The resin sheet can be stored in a roll shape. When the resin sheet has a protective film, it can usually be used by peeling off the protective film.
[0154] <Circuit board and method for manufacturing the same> The circuit substrate includes a cured product of the above-mentioned resin composition. The specific structure of the circuit substrate is not limited as long as it includes a cured product of the resin composition. The circuit substrate involved in the first example has a substrate with a hole and a cured product of the resin composition filled in the hole. In addition, the circuit substrate involved in the second example has a cured product layer including a cured product of the resin composition. Hereinafter, the manufacturing method of the circuit substrate involved in these first and second examples is described. However, the circuit substrate and its manufacturing method are not limited to the first and second examples exemplified below.
[0155] <Circuit Board According to the First Example> The circuit substrate involved in the first example comprises a substrate having holes formed therein and a cured product of a resin composition filled in the holes. The circuit substrate can be manufactured, for example, by a manufacturing method comprising the following steps (1) and (2): (1) a step of filling the holes of the substrate with a resin composition, and (2) A step of thermally curing the resin composition to obtain a cured product. In addition, the method for manufacturing a circuit board according to the first example may further include the following steps (3) to (5): (3) Step of polishing the surface of the cured product or resin composition (4) performing a roughening treatment step on the cured product, and (5) A step of forming a conductor layer on the cured product. Usually, the above steps (1) to (5) can be carried out in the order of step (1), step (2), step (3), step (4) and step (5), or step (2) can be carried out after step (3). In the method for manufacturing a circuit substrate according to the first example, it is preferred to use a paste-like resin composition to form a cured product. In the following description, an example of a substrate having a through hole formed therein as a hole penetrating the substrate in the thickness direction is used for description.
[0156] <Process (1)> Step (1) generally includes the step of preparing a substrate having a through hole. The substrate can be purchased from the market. Alternatively, the substrate can be prepared by manufacturing using an appropriate material. The following describes a method for manufacturing a substrate according to an example.
[0157] Figure 1 1 is a cross-sectional view schematically showing a core substrate 10 prepared in a method for manufacturing a circuit substrate according to a first example of an embodiment of the present invention. Figure 1 As shown in the example, a process of preparing a core substrate 10 may be included. The core substrate 10 usually includes a supporting substrate 11. As the supporting substrate 11, insulating substrates such as glass epoxy substrates, metal substrates, polyester substrates, polyimide substrates, BT resin substrates, and thermosetting polyphenylene ether substrates can be cited. In addition, a metal layer can be provided on the supporting substrate 11. The metal layer can be provided on a single surface of the supporting substrate 11, or on both surfaces. Here, an example in which metal layers 12 and 13 are provided on both surfaces of the supporting substrate 11 is shown. As the metal layers 12 and 13, layers formed of metals such as copper can be cited. The metal layers 12 and 13 can be, for example, copper foils such as copper foils with carriers, or metal layers formed of the material of the conductor layer described later.
[0158] Figure 2 1 is a cross-sectional view schematically showing a core substrate 10 having a through hole 14 formed therein in a method for manufacturing a circuit substrate according to a first example of an embodiment of the present invention. Figure 2As shown in the example, a process of forming a through hole 14 in the core substrate 10 may be included. The through hole 14 can be formed, for example, by drilling, laser irradiation, plasma irradiation, etc. Usually, the through hole 14 can be formed by forming a through hole in the core substrate 10. If a specific example is given, the formation of the through hole 14 can be implemented using a commercially available drilling device. As a commercially available drilling device, for example, "ND-1S211" manufactured by Hitachi Via Machinery Co., Ltd. can be cited.
[0159] Figure 3 1 is a schematic cross-sectional view of a core substrate 10 having a plating layer 20 formed in a through hole 14 in a method for manufacturing a circuit substrate according to a first example of an embodiment of the present invention. The step of preparing the substrate may include roughening the core substrate 10 as required, such as Figure 3 The process of forming the plating layer 20 as shown. As the above-mentioned roughening treatment, any roughening treatment of dry type and wet type can be performed. As an example of dry roughening treatment, plasma treatment and the like can be cited. In addition, as an example of wet roughening treatment, a method of sequentially performing swelling treatment using a swelling solution, roughening treatment using an oxidant, and neutralization treatment using a neutralizing solution can be cited. The plating layer 20 can be formed by a plating method. The step of forming the plating layer 20 by the plating method can be the same as the formation of the conductor layer in the step (5) described later. Here, an example of a plating layer 20 formed in the through hole 14, on the surface of the metal layer 12, and on the surface of the metal layer 13 is shown.
[0160] Figure 4 1 is a cross-sectional view schematically showing a state in which a resin composition 30a is filled in a through hole of a core substrate 10 in a method for manufacturing a circuit substrate according to a first example of an embodiment of the present invention. Step (1) includes: after preparing a core substrate 10 having a through hole 14 formed therein as described above, Figure 4 As shown, the resin composition 30a is filled in the through hole 14 of the core substrate 10. The filling can be performed by printing, for example. As the printing method, for example, a method of printing the resin composition 30a into the through hole 14 via a squeegee, a method of printing the resin composition 30a via a cartridge, a method of printing the resin composition 30a by mask printing, a roller coating method, an inkjet method, etc. can be cited.
[0161] <Process (2)> Figure 5 1 is a schematic cross-sectional view for explaining step (2) of the method for manufacturing a circuit board according to the first example of one embodiment of the present invention. Step (2) includes: after filling the through hole 14 with a resin composition 30a, curing the resin composition 30a, such as Figure 5 As shown, a cured product 30 is formed.
[0162] The curing of the resin composition 30a is usually performed by thermal curing. The thermal curing conditions of the resin composition 30a can be appropriately set within the range of the curing of the resin composition 30a. The curing temperature is preferably 120°C or more, more preferably 130°C or more, more preferably 150°C or more, preferably 245°C or less, more preferably 220°C or less, and more preferably 200°C or less. The curing time is preferably 5 minutes or more, more preferably 10 minutes or more, more preferably 15 minutes or more, preferably 120 minutes or less, more preferably 110 minutes or less, and more preferably 100 minutes or less.
[0163] The degree of curing of the cured product 30 obtained in step (2) is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. The degree of curing can be measured using, for example, a differential scanning calorimeter.
[0164] The manufacturing method of the circuit board involved in the first example may include: after filling the resin composition 30a into the through hole 14, before curing the resin composition 30a, the resin composition 30a is heated at a temperature lower than the curing temperature (preheating process). For example, before curing the resin composition 30a, the resin composition 30a may be preheated at a temperature of 50°C or more and less than 120°C (preferably 60°C or more and 110°C or less, more preferably 70°C or more and 100°C or less) for usually 5 minutes or more (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes).
[0165] <Step (3)> Figure 6 1 is a schematic cross-sectional view for explaining step (3) of the method for manufacturing a circuit substrate according to the first example of one embodiment of the present invention. When the resin composition 30a is filled into the through hole 14 in step (1), the remaining resin composition 30a may protrude or adhere to the outside of the through hole 14. Therefore, the resin composition 30a may be disposed not only in the through hole 14 but also outside the through hole 14. Therefore, Figure 6 As shown, step (3) includes grinding the remaining solidified material 30 protruding from or attached to the core substrate 10. Since the remaining solidified material 30 is removed by grinding, the surface of the solidified material 30 can be flattened. In addition, the surface (ground surface) 31 of the solidified material 30 flattened by grinding can usually form a flush plane with the surface 21 around the ground surface 31 (for example, the surface of the core substrate 10, the surface of the plating layer 20).
[0166] As a method for grinding the solidified material 30, a method that can remove the excess solidified material 30 protruding from or attached to the core substrate 10 can be adopted. As such a grinding method, for example, polishing grinding, belt grinding, ceramic grinding, etc. can be cited. As a commercially available polishing grinding device, for example, "NT-700IM" manufactured by Ishii Hyoki Co., Ltd. can be cited.
[0167] The arithmetic mean roughness (Ra) of the polished surface 31 (cured surface) of the cured product 30 is preferably 300 nm or more, more preferably 350 nm or more, and further preferably 400 nm or more from the viewpoint of improving the adhesion between the conductor layer. The upper limit is preferably 1000 nm or less, more preferably 900 nm or less, and further preferably 800 nm or less. The surface roughness (Ra) can be measured using, for example, a non-contact surface roughness meter.
[0168] The method for manufacturing a circuit substrate according to the first example may include, after step (3), a step of heat treating the cured product 30 in order to further improve the degree of cure of the cured product 30. The temperature in the heat treatment may be based on the above-mentioned curing temperature. The specific heat treatment temperature is preferably 120°C or more, more preferably 130°C or more, more preferably 150°C or more, preferably 245°C or less, more preferably 220°C or less, and more preferably 200°C or less. The heat treatment time is preferably 5 minutes or more, more preferably 10 minutes or more, more preferably 15 minutes or more, preferably 90 minutes or less, more preferably 70 minutes or less, and more preferably 60 minutes or less.
[0169] In addition, when step (3) is performed before step (2), a preheating treatment at a temperature lower than the curing temperature of the resin composition may be performed before step (3). The temperature in the preheating treatment is preferably 100° C. or higher, more preferably 110° C. or higher, and further preferably 120° C. or higher, preferably 245° C. or lower, more preferably 220° C. or lower, and further preferably 200° C. or lower. The heat treatment time is preferably 5 minutes or longer, more preferably 10 minutes or longer, further preferably 15 minutes or longer, preferably 90 minutes or shorter, more preferably 70 minutes or shorter, and further preferably 60 minutes or shorter.
[0170] <Step (4)> Step (4) includes roughening the cured product 30 (decontamination treatment). The surface of the cured product 30 is roughened by the roughening treatment. When the surface of the cured product 30 is ground, it usually includes roughening the ground surface 31 (decontamination treatment). The steps and conditions of the roughening treatment are not particularly limited. For example, the steps and conditions used in the method for manufacturing a multilayer printed wiring board can be used. If a specific example is given, the cured product 30 can be roughened by sequentially performing a swelling treatment using a swelling solution, a roughening treatment using an oxidant, and a neutralization treatment using a neutralizing solution.
[0171] As the swelling liquid that can be used in the roughening process, for example, an alkaline solution, a surfactant solution, etc. can be cited, and an alkaline solution is preferred. As for the alkaline solution as the swelling liquid, a sodium hydroxide solution or a potassium hydroxide solution is more preferred. As commercially available swelling liquids, for example, "Swelling Dip Securiganth P" and "Swelling Dip Securiganth SBU" manufactured by Atotech Japan Co., Ltd. can be cited.
[0172] The swelling treatment using the swelling liquid can be performed, for example, by immersing the cured product 30 in a swelling liquid at 30° C. to 90° C. for 1 to 20 minutes. From the viewpoint of suppressing the swelling of the resin contained in the cured product 30 to an appropriate level, it is preferred that the cured product 30 be immersed in a swelling liquid at 40° C. to 80° C. for 5 to 15 minutes.
[0173] As the oxidant used in the roughening treatment using the oxidant, an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide can be cited. The roughening treatment using an oxidant such as an alkaline permanganate solution is preferably performed by immersing the cured product 30 in a solution of an oxidant heated to 60° C. to 80° C. for 10 to 30 minutes. In addition, the concentration of permanganate in the alkaline permanganate solution is preferably 5% to 10% by mass. As a commercially available oxidant, an alkaline permanganate solution such as "Concentrate Compact P" and "Dosing Solution Securiganth P" manufactured by Atotech Japan Co., Ltd. can be cited.
[0174] As a neutralizing solution that can be used in the neutralization treatment, an acidic aqueous solution is preferred. As a commercially available neutralizing solution, for example, "Reduction Solution Securiganth P" manufactured by Atotech Japan Co., Ltd. can be cited. The neutralization treatment using the neutralizing solution can be performed by immersing the treated surface that has been roughened using the oxidant solution in a neutralizing solution at 30°C to 80°C for 5 minutes to 30 minutes. In terms of operability, etc., it is preferred to immerse the cured product 30 that has been roughened using the oxidant solution in a neutralizing solution at 40°C to 70°C for 5 minutes to 20 minutes.
[0175] The arithmetic mean roughness (Ra) of the surface of the cured product 30 after the roughening treatment is preferably 300 nm or more, more preferably 350 nm or more, and further preferably 400 nm or more from the viewpoint of improving the adhesion with the conductor layer. The upper limit is preferably 1500 nm or less, more preferably 1200 nm or less, and further preferably 1000 nm or less. The surface roughness (Ra) can be measured, for example, using a non-contact surface roughness meter.
[0176] <Step (5)> Figure 7 Schematic cross-sectional view for explaining step (5) of the method for manufacturing a circuit substrate according to the first example of one embodiment of the present invention. Figure 7 As shown, step (5) includes forming a conductor layer 40 on the polished surface 31 of the cured product 30. Here, an example is shown in which the conductor layer 40 is formed not only on the polished surface 31 of the cured product 30 but also on the surrounding surface 21 (for example, the surface of the core substrate 10, the surface of the plating layer 20). In addition, Figure 7 2 shows an example in which the conductor layer 40 is formed on both sides of the core substrate 10 , but the conductor layer 40 may be formed only on one side of the core substrate 10 .
[0177] Figure 8 Schematic cross-sectional view for explaining step (5) of the method for manufacturing a circuit substrate according to the first example of one embodiment of the present invention. Figure 8 As shown, step (5) may include: after forming the conductor layer 40, removing a portion of the conductor layer 40, the metal layer 12, the metal layer 13 and the plating layer 20 by etching or the like to form a pattern conductor layer 41.
[0178] The formation method of the conductor layer 40 can include, for example, plating, sputtering, and evaporation, among which plating is preferred. In a preferred embodiment, the surface of the solidified material 30 (and the plated layer 20) can be plated by an appropriate method such as a semi-additive method and a full-additive method to form a pattern conductor layer 41 having a desired wiring pattern. As the material of the conductor layer 40, for example, single metals such as gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin, and indium can be included; alloys of two or more metals selected from gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin, and indium. Among them, from the viewpoints of versatility, cost, ease of patterning, etc., it is preferred to use chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or nickel-chromium alloy, copper-nickel alloy, and copper-titanium alloy, more preferably chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or nickel-chromium alloy, and further preferably copper.
[0179] Here, an example of a method for forming a pattern conductor layer 41 on the polished surface 31 of the cured product 30 is described in detail. A plating seed layer is formed on the polished surface 31 of the cured product 30 by electroless plating. Next, an electrolytic plating layer is formed on the formed plating seed layer by electrolytic plating. Then, as needed, the unnecessary plating seed layer is removed by etching or the like, and a pattern conductor layer 41 having a desired wiring pattern can be formed. After the pattern conductor layer 41 is formed, an annealing treatment can be performed as needed to improve the adhesion strength of the pattern conductor layer 41. The annealing treatment can be performed, for example, by heating at 150°C to 200°C for 20 minutes to 90 minutes.
[0180] From the viewpoint of thinning, the thickness of the pattern conductor layer 41 is preferably 70 μm or less, more preferably 60 μm or less, further preferably 50 μm or less, further more preferably 40 μm or less, particularly preferably 30 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less. The lower limit is preferably 1 μm or more, more preferably 3 μm or more, and further preferably 5 μm or more.
[0181] By the above method, the circuit board 1 including the cured product 30 of the resin composition 30 a can be manufactured.
[0182] <Circuit Board According to Second Example> The circuit substrate involved in the second example includes a cured product layer containing a cured product of a resin composition. The cured product layer preferably only contains a cured product of the resin composition. The cured product layer is preferably formed using a resin sheet. The circuit substrate can be manufactured, for example, by a manufacturing method comprising the following steps (i) to (iv): (i) forming a cured product layer on the inner substrate, (ii) a step of drilling holes in the cured layer, (iii) a step of roughening the surface of the cured material layer, and (iv) a step of forming a conductive layer on the surface of the cured material layer.
[0183] <Step (i)> Step (i) includes forming a cured product layer on the inner substrate. Preferably, step (i) includes laminating a resin sheet on the inner substrate in a manner such that the resin composition layer is bonded to the inner substrate to form a cured product layer. For example, laminating a resin sheet on the inner substrate in a manner such that the resin composition layer is bonded to the inner substrate, and thermally curing the resin composition layer to form a cured product layer.
[0184] Fig. 9 Schematic cross-sectional view for explaining step (i) in the method for manufacturing a circuit substrate according to the second example of one embodiment of the present invention. Fig. 9 As shown in FIG. 1 , a resin sheet 310 including a support 330 and a resin composition layer 320a provided on the support 330 is prepared. Then, the resin sheet 310 and the inner substrate 200 are laminated so that the resin composition layer 320a and the inner substrate 200 are bonded to each other.
[0185] An insulating substrate can be used as the inner substrate 200. Examples of the inner substrate 200 include insulating substrates such as glass epoxy substrates, metal substrates, polyester substrates, polyimide substrates, BT resin substrates, and thermosetting polyphenylene ether substrates. The inner substrate 200 can be an inner circuit substrate having wiring and the like built into its thickness.
[0186] The inner substrate 200 shown in this example includes a first conductor layer 420 provided on the first main surface 200a and an external terminal 240 provided on the second main surface 200b. The first conductor layer 420 may include a plurality of wirings. Fig. 9 In the example shown, only the coil-shaped conductive structure 400 (see Fig.12 The external terminal 240 may be a terminal for electrically connecting to an external device (not shown) or the like. The external terminal 240 may be configured as a part of a conductor layer provided on the second main surface 200b.
[0187] Examples of the conductive material that can constitute the first conductive layer 420 and the external terminal 240 include the same materials as those for the conductive layer described in the first example.
[0188] The first conductor layer 420 and the external terminal 240 may be a single-layer structure or a multi-layer structure in which two or more single metal layers or alloy layers formed of different types of metals or alloys are stacked. In addition, the thickness of the first conductor layer 420 and the external terminal 240 may be the same as that of the second conductor layer 440 described later.
[0189] The line width (L) / line spacing (S) ratio of the first conductor layer 420 and the external terminal 240 is not particularly limited, but from the viewpoint of reducing the surface unevenness and obtaining a cured layer with excellent smoothness, it is usually 900 μm / 900 μm or less, preferably 700 μm / 700 μm or less, more preferably 500 μm / 500 μm or less, further preferably 300 μm / 300 μm or less, and further more preferably 200 μm / 200 μm or less. The lower limit of the line width / line spacing ratio is not particularly limited, but from the viewpoint of making the embedding property of the resin composition layer in the line spacing (space) good, it is preferably 1 μm / 1 μm or more.
[0190] The inner substrate 200 may have a plurality of through holes 220 penetrating the inner substrate 200 from the first main surface 200a to the second main surface 200b. Through-hole wiring 220a is provided in the through hole 220. The through-hole wiring 220a electrically connects the first conductor layer 420 and the external terminal 240.
[0191] The resin composition layer 320a and the inner substrate 200 can be bonded by, for example, heat-pressing the resin sheet 310 to the inner substrate 200 from the support 330 side. As a member for heat-pressing the resin sheet 310 to the inner substrate 200 (hereinafter also referred to as a "heat-pressing member"), for example, a heated metal plate (stainless steel (SUS) end plate, etc.) or a metal roller (SUS roller) can be cited. It should be noted that it is preferred that the heat-pressing member is not pressed by directly contacting the resin sheet 310, but is pressed via a sheet formed of an elastic material such as heat-resistant rubber, so that the resin sheet 310 fully follows the surface unevenness of the inner substrate 200.
[0192] The temperature during the heat pressing is preferably 80°C to 160°C, more preferably 90°C to 140°C, and further preferably in the range of 100°C to 120°C. The pressure during the heat pressing is preferably 0.098MPa to 1.77MPa, and more preferably in the range of 0.29MPa to 1.47MPa. The time during the heat pressing is preferably 20 seconds to 400 seconds, and more preferably in the range of 30 seconds to 300 seconds. The bonding of the resin sheet and the inner substrate is preferably carried out under reduced pressure conditions of 26.7hPa or less.
[0193] The resin composition layer 320a of the resin sheet 310 and the inner substrate 200 can be bonded by a commercially available vacuum laminator. Examples of commercially available vacuum laminators include a vacuum pressure laminator manufactured by Meiki Mfg. Co., Ltd. and a vacuum laminator manufactured by Nikko-Materials.
[0194] After the resin sheet 310 is bonded to the inner substrate 200, the laminated resin sheet 310 may be smoothed by, for example, pressing the heating and pressing member from the support 330 side under normal pressure (under atmospheric pressure). The pressing conditions for the smoothing treatment may be the same as the heating and pressing conditions for the above-mentioned lamination. The smoothing treatment may be performed using a commercially available laminator. It should be noted that the lamination and smoothing treatment may also be performed continuously using the above-mentioned commercially available vacuum laminator.
[0195] Fig.10 Schematic cross-sectional view for explaining step (i) in the method for manufacturing a circuit substrate according to the second example of one embodiment of the present invention. After the resin sheet 310 is laminated on the inner substrate 200, the resin composition layer 320a is cured to form a cured product layer. Fig.10 As shown, the resin composition layer 320 a bonded to the inner substrate 200 is thermally cured to form the first cured material layer 320 .
[0196] The heat curing conditions of the resin composition layer 320a can be appropriately set within the range of curing of the resin composition. The curing temperature is preferably 120°C or more, more preferably 130°C or more, more preferably 150°C or more, preferably 245°C or less, more preferably 220°C or less, and more preferably 200°C or less. The curing time is preferably 5 minutes or more, more preferably 10 minutes or more, more preferably 15 minutes or more, preferably 120 minutes or less, more preferably 110 minutes or less, and more preferably 100 minutes or less.
[0197] The support body 330 may be removed after the thermal curing in step (i) and between step (ii), or may be peeled off after step (ii).
[0198] The arithmetic mean roughness (Ra) before the roughening treatment of the cured product layer is preferably 300 nm or more, more preferably 350 nm or more, and further preferably 400 nm or more from the viewpoint of improving the adhesion between the coating. The upper limit is preferably 1000 nm or less, more preferably 900 nm or less, and further preferably 800 nm or less. The surface roughness (Ra) can be measured, for example, using a non-contact surface roughness meter.
[0199] In step (i), instead of using a resin sheet, a resin composition may be applied onto the inner substrate 200 using a die coater or the like, and then thermally cured to form a cured product layer.
[0200] <Step (ii)> Fig.11 Schematic cross-sectional view for explaining step (ii) in the method for manufacturing a circuit substrate according to the second example of one embodiment of the present invention. Fig.11 As shown, step (ii) includes drilling the first cured material layer 320 to form a via hole 360. The via hole 360 forms a path for electrically connecting the first conductor layer 420 to the second conductor layer 440 described later. The formation of the via hole 360 can be performed, for example, using a drill, laser, plasma, etc. The size and shape of the hole can be appropriately determined according to the design of the printed wiring board.
[0201] <Process (iii)> In step (iii), the surface of the cured layer having the via hole formed therein is subjected to a roughening treatment. The roughening treatment in step (iii) can be performed by the same method as that described in step (4) of the first example.
[0202] The arithmetic mean roughness (Ra) after the roughening treatment of the cured product layer is preferably 300 nm or more, more preferably 350 nm or more, and further preferably 400 nm or more from the viewpoint of improving the adhesion between the coating. The upper limit is preferably 1500 nm or less, more preferably 1200 nm or less, and further preferably 1000 nm or less. The surface roughness (Ra) can be measured, for example, using a non-contact surface roughness meter.
[0203] <Step (iv)> Fig.12 Schematic cross-sectional view for explaining step (iv) in the method for manufacturing a circuit substrate according to the second example of one embodiment of the present invention. Fig.12 As shown, in step (iv), the second conductor layer 440 is formed on the first cured material layer 320 .
[0204] Examples of the conductive material that can constitute the second conductive layer 440 include the same materials as those for the conductive layer described in the first example.
[0205] From the viewpoint of thinning, the thickness of the second conductor layer 440 is preferably 70 μm or less, more preferably 60 μm or less, further preferably 50 μm or less, further more preferably 40 μm or less, particularly preferably 30 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less. The lower limit is preferably 1 μm or more, more preferably 3 μm or more, and further preferably 5 μm or more.
[0206] The second conductor layer 440 can be formed by plating. The second conductor layer 440 is preferably formed by a wet plating method such as a semi-additive method or a full-additive method including an electroless plating process, a mask pattern forming process, an electrolytic plating process, and a flash etching process. By forming the second conductor layer 440 by the wet plating method, the second conductor layer 440 including a desired wiring pattern can be formed. It should be noted that, through this process, the via hole wiring 360a is formed in the via hole 360 at the same time.
[0207] For example, as described below Figures 13-15 In one example shown in , the first conductor layer 420 and the second conductor layer 440 can be arranged in a spiral shape. In one example, one end of the center side of the spiral wiring portion of the second conductor layer 440 is electrically connected to one end of the center side of the spiral wiring portion of the first conductor layer 420 by the via-hole wiring 360a. The other end of the outer peripheral side of the spiral wiring portion of the second conductor layer 440 is electrically connected to the pad 420a of the first conductor layer 420 by the via-hole wiring 360a. Therefore, the other end of the outer peripheral side of the spiral wiring portion of the second conductor layer 440 is electrically connected to the external terminal 240 via the via-hole wiring 360a, the pad 420a, and the through-hole wiring 220a.
[0208] The coil-shaped conductive structure 400 is composed of a spiral wiring portion as a part of the first conductor layer 420, a spiral wiring portion as a part of the second conductor layer 440, and an intra-via wiring 360a that electrically connects the spiral wiring portion of the first conductor layer 420 and the spiral wiring portion of the second conductor layer 440.
[0209] After step (iv), a step of forming a cured product layer on the conductor layer may be further performed. Fig.14 In the example shown, the second cured material layer 340 is formed on the first cured material layer 320 having the second conductor layer 440 and the via-hole wiring 360a. The second cured material layer can be formed by the same process as the process already described. By the above method, the circuit substrate 100 including the first cured material layer 320 and the second cured material layer 340 formed by the cured material of the resin composition can be manufactured.
[0210] <Inductor substrate> The inductor substrate includes the above-mentioned circuit substrate. When such an inductor substrate includes a circuit substrate obtained by the manufacturing method of the circuit substrate involved in the first example, at least a portion around the cured product of the resin composition may have an inductor pattern formed by a conductor. In this case, the inductor substrate may include, for example, an inductor pattern formed by at least a portion of the metal layer 12, the metal layer 13, the plating layer 20, and the pattern conductor layer 41, and an inductor element consisting of a core formed by the cured product 30 surrounded by the inductor pattern. Such an inductor substrate may be applied to the inductor substrate described in Japanese Patent Publication No. 2016-197624, for example.
[0211] In addition, when including a circuit substrate obtained by the method for manufacturing a circuit substrate according to the second example, the inductor substrate may include a cured material layer and a conductive structure at least a portion of which is embedded in the cured material layer. Furthermore, the inductor substrate may include an inductor element composed of a conductive structure and a portion of the cured material layer extending in the thickness direction of the cured material layer and surrounded by the conductive structure.
[0212] Fig.13 This is a schematic plan view of the circuit substrate 100 included in the inductor substrate as viewed from one side in the thickness direction thereof. Fig.14 It means in Fig.13 FIG. 1 is a schematic diagram of a cut end surface of the circuit substrate 100 cut at a position indicated by a II-II dot-dash line. Fig.15 It is a schematic plan view for explaining the structure of the first conductive layer 420 of the circuit substrate 100 including the inductor substrate.
[0213] like Fig.13 and Fig.14 As shown as an example in FIG. 1 , the circuit substrate 100 may be a substrate having a plurality of cured layers (a first cured layer 320, a second cured layer 340) and a plurality of conductor layers (a first conductor layer 420, a second conductor layer 440). Therefore, in the example shown here, the circuit substrate 100 may be a stacked wiring board having stacked cured layers and stacked conductor layers. In addition, the circuit substrate 100 includes an inner substrate 200.
[0214] like Fig.14 As shown in the example, the first cured material layer 320 and the second cured material layer 340 constitute the magnetic part 300 which can be regarded as a solidified material layer. Therefore, the coil-shaped conductive structure 400 is provided in a manner that at least a part is buried in the magnetic part 300. That is, in the circuit substrate 100 shown in this example, the inductor element is composed of the coil-shaped conductive structure 400 and a part of the magnetic part 300 extending in the thickness direction of the magnetic part 300 and surrounded by the coil-shaped conductive structure 400, that is, the core part.
[0215] like Fig.15 As shown as an example in FIG. 4 , the first conductor layer 420 includes: a spiral wiring portion for constituting the coil-shaped conductive structure 400, and a rectangular pad 420a electrically connected to the through-hole wiring 220a. In the example shown here, the spiral wiring portion includes: a straight portion, a bent portion bent at a right angle, and a detour portion detour at the pad 420a. In addition, the spiral wiring portion of the first conductor layer 420 has a shape with an overall outline of a substantially rectangular shape and is wound in a counterclockwise direction from the center side to the outside thereof.
[0216] Similarly, the second conductor layer 440 is provided on the first cured material layer 320. The second conductor layer 440 includes a spiral wiring portion for constituting the coil-shaped conductive structure 400. Fig.13 or Fig.14 In the embodiment, the spiral wiring portion includes a straight portion and a curved portion bent at a right angle. Fig.13 or Fig.14 In the figure, the spiral wiring portion of the second conductor layer 440 has a shape whose overall outline is substantially rectangular and is wound in a clockwise direction from the center to the outside.
[0217] The inductor substrate can be used as a wiring board for mounting electronic components such as semiconductor chips, or as a (multi-layer) printed wiring board using the wiring board as an inner substrate. In addition, it can be used as a chip inductor component obtained by monolithicizing the wiring board, or as a printed wiring board with the chip inductor component mounted on the surface.
[0218] In addition, various forms of semiconductor devices can be manufactured using the wiring board. The semiconductor device including the wiring board can be suitably used in electrical products (e.g., computers, mobile phones, digital cameras, and televisions) and transportation tools (e.g., motorcycles, cars, trains, ships, and aircrafts). Example
[0219] Hereinafter, the present invention will be specifically described by way of examples. The present invention is not limited to these examples. It should be noted that, hereinafter, "%" and "parts" indicating amounts refer to "mass %" and "mass parts" unless otherwise expressly stated. In addition, the temperature condition when no temperature is particularly specified is room temperature (23° C.). Furthermore, the pressure condition when no pressure is particularly specified is normal pressure (1 atm).
[0220] <Example 1: Production of varnish-like resin composition 1> Fe-Ni-Si alloy magnetic powder ("AKT-PB-3Si" manufactured by Mitsubishi Steel Corporation, alloy of 50% Fe, 47% Ni, 3% Si, average particle size (D50 )5μm, true density 8.0g / cm 3 ) 55.09 parts by mass, magnetic powder ("CVD iron powder 0.7 μm" manufactured by JFE Chemical Co., Ltd.), Fe-Si-Cr alloy powder, average particle size (D 50 )0.7μm, true density 6.9g / cm 3 ) 21 parts by mass, epoxy resin ("ZX-1059" manufactured by Nippon Steel Chemical Materials, a mixture of bisphenol A epoxy resin and bisphenol F epoxy resin, epoxy equivalent 169 g / eq., true density 1.2 g / cm 3 ) 1.63 parts by mass, phenolic resin ("LA-7054" manufactured by DIC Corporation, aminotriazine-modified linear phenolic resin, MEK solution containing 60% nonvolatile components, hydroxyl equivalent of 125 g / eq., true density of nonvolatile components of 1.2 g / cm 3 ) 1.85 parts by mass, phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation, a solution of methyl ethyl ketone and cyclohexanone with a non-volatile content of 30% in a ratio of 1:1, special skeleton phenoxy resin, true density of the non-volatile content of 1.2 g / cm 3 ) 1.61 parts by mass, dispersant ("ED-152" manufactured by Kusumoto Chemicals Co., Ltd., polyether phosphate dispersant, true density 1.2 g / cm 3 ) 0.67 parts by mass, and a curing accelerator ("TBP-DA" manufactured by Hokko Chemical Industry Co., Ltd., a phosphorus-based curing accelerator, true density 1.2 g / cm 3 ) were mixed with 0.01 parts by mass and uniformly dispersed using a high-speed rotary mixer to prepare a varnish-like resin composition 1.
[0221] <Example 2: Preparation of varnish-like resin composition 2> In addition to using Fe-Ni-Si alloy magnetic powder (Mitsubishi Steel Corporation "AKT-PB-6Si", Fe50%, Ni44%, Si6% alloy, average particle size (D 50 )5μm, true density 7.8g / cm 3 ) 53.52 parts by mass instead of Fe-Ni-Si alloy magnetic powder ("AKT-PB-3Si" manufactured by Mitsubishi Steel, Ltd., alloy of Fe50%, Ni47%, Si3%, average particle size (D 50 )5μm, true density 8.0g / cm 3 A varnish-like resin composition 2 was prepared in the same manner as in Example 1 except that ) was 55.09 parts by mass.
[0222] <Example 3: Preparation of varnish-like resin composition 3> Fe-Ni-Si alloy magnetic powder ("AKT-PB-3Si" manufactured by Mitsubishi Steel Corporation, alloy of 50% Fe, 47% Ni, 3% Si, average particle size (D 50 )5μm, true density 8.0g / cm 3 ) 93.33 parts by mass, magnetic powder ("MZ03S" manufactured by Powdertech Co., Ltd., Mn-Zn ferrite powder, average particle size (D 50 )1.0μm, true density5.1g / cm 3 ) 27.95 parts by mass, epoxy resin ("ZX-1059" manufactured by Nippon Steel Chemical Materials, a mixture of bisphenol A epoxy resin and bisphenol F epoxy resin, epoxy equivalent 169 g / eq., true density 1.2 g / cm 3 ) 2.31 parts by mass, phenolic resin ("LA-7054" manufactured by DIC Corporation, aminotriazine-modified linear phenolic resin, MEK solution containing 60% nonvolatile components, hydroxyl equivalent of 125 g / eq., true density of nonvolatile components of 1.2 g / cm 3 ) 2.63 parts by mass, phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation, a solution of methyl ethyl ketone and cyclohexanone with a non-volatile content of 30% in a ratio of 1:1, special skeleton phenoxy resin, true density of the non-volatile content of 1.2 g / cm 3 ) 2.02 parts by mass, dispersant (“PB-881” manufactured by Ajinomoto Fine Technology Co., Ltd., polyester dispersant, true density 1.2 g / cm 3 ) 0.54 parts by mass, and a curing accelerator ("TBP-DA" manufactured by Hokko Chemical Industry Co., Ltd., a phosphorus-based curing accelerator, true density 1.2 g / cm 3 ) and 0.02 parts by mass were mixed and uniformly dispersed using a high-speed rotary mixer to prepare a varnish-like resin composition 3.
[0223] <Comparative Example 1: Preparation of Varnish-like Resin Composition 4> In addition to using Fe-Ni-Si alloy magnetic powder (Mitsubishi Steel Corporation "AKT-PB-9Si", Fe50%, Ni41%, Si9% alloy, average particle size (D 50 )5μm, true density 7.6g / cm 3 ) 51.8 parts by mass instead of Fe-Ni-Si alloy magnetic powder ("AKT-PB-3Si" manufactured by Mitsubishi Steel, Ltd., alloy of Fe50%, Ni47%, Si3%, average particle size (D 50 )5μm, true density 8.0g / cm 3 A varnish-like resin composition 4 was prepared in the same manner as in Example 1 except that ) was 55.09 parts by mass.
[0224] <Comparative Example 2: Preparation of Varnish-like Resin Composition 5> In addition to using Fe-Ni alloy magnetic powder (Mitsubishi Steel Corporation "AKT-PB", Fe50%, Ni50% alloy, average particle size (D 50 )5μm, true density 8.2g / cm 3 ) 54.82 parts by mass instead of Fe-Ni-Si alloy magnetic powder ("AKT-PB-3Si" manufactured by Mitsubishi Steel, Ltd., alloy of Fe50%, Ni47%, Si3%, average particle size (D 50 )5μm, true density 8.0g / cm 3 A varnish-like resin composition 5 was prepared in the same manner as in Example 1 except that ) was 55.09 parts by mass.
[0225] <Comparative Example 3: Preparation of Varnish-like Resin Composition 6> In addition to using Ni alloy magnetic powder (Mitsubishi Steel Corporation "AKT-78Ni-5Mo", Fe17%, Ni78%, Mo5% alloy, average particle size (D 50 )5μm, true density 8.9g / cm 3 ) 60.16 parts by mass instead of Fe-Ni-Si alloy magnetic powder ("AKT-PB-3Si" manufactured by Mitsubishi Steel, Ltd., alloy of Fe50%, Ni47%, Si3%, average particle size (D 50 )5μm, true density 8.0g / cm 3 A varnish-like resin composition 6 was prepared in the same manner as in Example 1 except that ) was 55.09 parts by mass.
[0226] <Comparative Example 4: Preparation of Varnish-like Resin Composition 7> In addition to using Fe-Si-Cr alloy magnetic powder (EPSON ATMIX "AW2-08PF3F", Fe-Si-Cr alloy, average particle size (D 50 )3.5μm, true density7.0g / cm 3 ) 47 parts by mass instead of Fe-Ni-Si alloy magnetic powder ("AKT-PB-3Si" manufactured by Mitsubishi Steel, Ltd., alloy of Fe50%, Ni47%, Si3%, average particle size (D 50 )5μm, true density 8.0g / cm 3 A varnish-like resin composition 7 was prepared in the same manner as in Example 1 except that ) was 55.09 parts by mass.
[0227] <Comparative Example 5: Preparation of Varnish-like Resin Composition 8> In addition to using Fe-Si-Cr alloy magnetic powder (EPSON ATMIX "AW2-08PF3F", Fe-Si-Cr alloy, average particle size (D 50 )3.5μm, true density7.0g / cm 3 ) 69 parts by mass instead of Fe-Ni-Si alloy magnetic powder ("AKT-PB-3Si" manufactured by Mitsubishi Steel, Ltd., alloy of Fe50%, Ni47%, Si3%, average particle size (D 50 )5μm, true density 8.0g / cm 3 A varnish-like resin composition 8 was prepared in the same manner as in Example 1 except that ) was 55.09 parts by mass.
[0228] <Production of Resin Sheet> The varnish-like resin composition prepared in each example and comparative example was coated on a polyethylene terephthalate (hereinafter referred to as "PET") film (thickness 38 μm) as a support using a die coater so that the thickness of the resin composition layer after drying was 100 μm to form a resin composition layer. The resin composition layer was dried at 75° C. to 120° C. (average 100° C.) for 7 minutes to reduce the amount of residual solvent in the resin composition layer to about 0.4% by mass or less to obtain a resin sheet.
[0229] <Production of Sheet-Shaped Cured Product> The resin sheet prepared using the varnish-like resin composition prepared in each of Examples and Comparative Examples was heated at 190° C. for 90 minutes to thermally cure the resin composition layer. The PET film as a support was peeled off to obtain a sheet-like cured product.
[0230] <Test Example: Evaluation of Magnetic Properties> The obtained sheet-shaped cured product was cut to obtain an evaluation sample with a width of 5 mm and a length of 18 mm. For this evaluation sample, the relative magnetic permeability (μ') and magnetic loss (μ") were measured at a measurement frequency of 20 MHz and a room temperature of 23°C using an Agilent Technologies ("HP8362B") three-turn coil method. The loss coefficient tanδ was calculated by the formula "tanδ=μ" / μ'".
[0231] The evaluation criteria of the relative magnetic permeability are as follows. “0”: Relative magnetic permeability is greater than 15. “×”: Relative magnetic permeability is less than 15.
[0232] The evaluation criteria of the loss factor are as follows. “○”: The loss coefficient is less than 0.02. “×”: The loss coefficient exceeds 0.02.
[0233] [result] The results of the above-mentioned Examples and Comparative Examples are shown in the following tables.
[0234] [Table 1] [Table 1. Results of Examples and Comparative Examples] Explanation of symbols
[0235] 1 Circuit board 10-core substrate 11 Support base plate 12 Metal Layer 13 Metal layer 14 Through Holes 20 Plating layer 21 The surface around the grinding surface 30 solids 30a Resin composition 31 Surface of the ground solidified material (ground surface) 40 conductor layers 41 pattern conductor layer 100 circuit board 200 inner substrate 200a first main surface 200b Second main surface 220 through hole 220a through-hole wiring 240 external terminal 310 resin sheet 320 first cured material layer 320a Resin composition layer 330 support body 360 Vias 360a via wiring 400 Coil-shaped conductive structure 420 first conductor layer 420a pad 440 second conductor layer.
Claims
1. A resin composition comprising (A) Fe-Ni-Si alloy magnetic powder and (B) a thermosetting resin, The amount of Si contained in the component (A) is 1 to 8 mass % relative to 100 mass % of the component (A).
2. The resin composition according to claim 1, wherein The amount of the component (A) is 40% by mass or more relative to 100% by mass of the nonvolatile matter in the resin composition.
3. The resin composition according to claim 1, wherein The amount of the component (A) is 30% by volume or more relative to 100% by volume of the nonvolatile matter in the resin composition.
4. The resin composition according to claim 1, wherein The average particle size of the component (A) is 1 μm or more.
5. The resin composition according to claim 1, wherein The average particle size of the component (A) is 10 μm or less.
6. The resin composition according to claim 1, wherein The invention further includes (C) magnetic powder other than Fe-Ni-Si alloy magnetic powder.
7. The resin composition according to claim 6, wherein The component (C) contains alloy magnetic powder other than Fe-Ni-Si alloy magnetic powder.
8. The resin composition according to claim 6, wherein The component (C) contains ferrite-based magnetic powder.
9. The resin composition according to claim 6, wherein The component (C) includes a ferrite-based magnetic powder containing at least one element selected from the group consisting of Mn, Zn, Ni, and Cu.
10. The resin composition according to claim 6, wherein The component (C) has an average particle size smaller than that of the component (A).
11. The resin composition according to claim 6, wherein The ratio of the average particle size of the component (C) to the average particle size of the component (A) (average particle size of the component (C) / average particle size of the component (A)) is 0.001 to 0.
9.
12. The resin composition according to claim 6, wherein The volume ratio of the component (C) to the component (A) (component (C) / component (A)) is 0.01 to 0.
9.
13. The resin composition according to claim 6, wherein The total amount of the component (A) and the component (C) is 70% by mass or more based on 100% by mass of the nonvolatile matter in the resin composition.
14. The resin composition according to claim 6, wherein The total amount of the component (A) and the component (C) is 50% by volume or more based on 100% by volume of the nonvolatile matter in the resin composition.
15. The resin composition according to claim 1, wherein The component (B) contains an epoxy resin.
16. The resin composition according to claim 1, wherein The invention further comprises (D) a thermoplastic resin.
17. The resin composition according to claim 1, which is used to fill a hole.
18. A cured product of the resin composition according to any one of claims 1 to 17. 19 . A magnetic paste comprising the resin composition according to claim 1 .
20. A resin sheet comprising a support and a resin composition layer provided on the support, The resin composition layer contains the resin composition according to any one of claims 1 to 17.
21. A circuit substrate comprising: a substrate having a hole, and A cured product of the resin composition according to any one of claims 1 to 17 filled in the pores. 22 . A circuit board comprising a cured product layer comprising a cured product of the resin composition according to claim 1 . 23 . An inductor substrate comprising the circuit substrate according to claim 21 or 22 .
Citation Information
Cited By
Thermosetting packaging integrated inductor and manufacturing method thereof
CN120149031A