Hydrogen storage material, hydrogen storage container, and hydrogen supply device
By adding specific element composition and heat treatment technology to TiFe-based alloys, multiple R-rich phase sea island structures are formed, which solves the problems of low initial activation and hydrogen release efficiency of TiFe-based alloys and achieves good hydrogen storage and release characteristics.
Patent Information
- Application Number
- CN202380019437.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-08
- Filing Date
- 2023-01-25
- Publication Date
- 2024-10-15
AI Technical Summary
TiFe-based alloys require high temperature and high pressure during the initial activation process, and as the amount of Mn added increases, the starting point and end point of the hydrogen storage and release in the hydrogen pressure-composition isotherm diagram shifts to the right, resulting in insufficient releasable hydrogen, making it difficult to ensure Balance stress.
Using an alloy composed of specific elements including Ti, rare earth elements and Fe, there is an R-rich phase between 0.1 μm and 10 μm in the 1000x COMP image obtained by EPMA. The phase area ratio is between 0.3% and 6.0%. The combination is appropriate. The heat treatment and cooling rate form multiple R-enriched phase sea-island structures to improve the initial activation and hydrogen release characteristics.
It achieves good initial activation and sufficient hydrogen release while suppressing the amount of Mn. It is suitable as a hydrogen storage material and improves the efficiency and balance pressure of hydrogen storage and release.
Smart Images

Figure CN118786232A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a hydrogen storage material, a hydrogen storage container and a hydrogen supply device. Background Art
[0002] Hydrogen absorbing (storage) alloys are alloys that can reversibly absorb and release hydrogen. They have been used as negative electrode materials for nickel-hydrogen secondary batteries. However, in recent years, they have also been expected to be materials that can safely store hydrogen, which has attracted attention as an energy source, and their use in hydrogen storage and supply systems is also being promoted for practical use. Hydrogen absorbing alloys include AB5, AB2, TiFe, TiVCr and other BCC types. Among them, TiFe alloys have the cheapest raw materials and are the most anticipated materials for hydrogen storage applications, where the required amount far exceeds the amount used in batteries.
[0003] However, TiFe alloys are difficult to activate and require a temperature of 400°C or higher and a pressure of 3 MPa or higher for initial activation, making them difficult to use. Adding Mn is known to be effective in improving this, and the following patent documents, for example, are known.
[0004] Patent Document 1 discloses a method of preparing a catalyst having the formula Ti 1+k Fe 1-l Mn l A m (wherein 0≤k≤0.3, 0<l≤0.3, 0<m≤0.1, A is an element consisting of at least one of niobium and rare earth elements). In addition, it is disclosed that by adding Mn and A element (at least one of Nb and rare earth elements) to a TiFe alloy, an alloy that is easy to activate and has a sufficient hydrogen storage capacity can be obtained.
[0005] Patent document 2 discloses a hydrogen absorbing alloy, characterized in that the hydrogen absorbing alloy is composed of a general formula (T 1-a Fe a ) 100-b-c-d La b M c M' d(wherein T is at least one element selected from Ti, Zr and Hf, M is at least one element selected from V, Nb, Ta, Cr, Mo and W, M' is at least one element selected from Mn, Co, Ni, Cu, Zn, B, Al, Ge and Sn, a is 0.45≤a≤0.55 in atomic ratio, b, c and d are 0.01≤b≤10, 0≤c≤20 and 0≤d≤30 in atomic %), wherein a fine crystalline phase having a crystal grain size of 10 μm or less is precipitated in at least a part of the alloy structure. In addition, it is disclosed that the types of elements constituting T component, Fe component, La component, M component and M' component in the general formula and the composition ratio of each component are appropriately set, and after cooling and solidification, heat treatment is performed to precipitate a fine crystalline phase, thereby obtaining a hydrogen absorbing alloy having excellent hydrogen absorption characteristics and corrosion resistance.
[0006] Patent document 3 discloses a hydrogen absorbing alloy, characterized in that the hydrogen absorbing alloy is composed of a general formula A a T b M c M' d (wherein A is at least one element selected from Ti, Zr, Hf and V, T is at least one element selected from Ni, Co, Fe, Cu, Mn and Cr, M is at least one element selected from Al, Si, Ga, Ge, Zn, Sn, In and Sb, M' is at least one element selected from B, C, N and P, a, b, c, d are 20≤a≤70, 30≤b≤60, 5≤c≤40, 0.1≤d≤10, a+b+c+d=100 in atomic %), and a fine crystalline phase with a crystal grain size of 10 μm or less is precipitated in at least a part of the alloy structure. In addition, it is disclosed that the types of elements constituting the A component, T component, M component and M' component in the general formula and the composition ratio of each component are appropriately set, and after cooling and solidification, heat treatment is performed to precipitate a fine crystalline phase, thereby obtaining a hydrogen absorbing alloy excellent in hydrogen absorption characteristics and corrosion resistance.
[0007] Prior art literature
[0008] [Patent Document]
[0009] [Patent Document 1] Japanese Patent Application Laid-Open No. 61-250136
[0010] [Patent Document 2] Japanese Patent Application Laid-Open No. 10-265875
[0011] [Patent Document 3] Japanese Patent Application Laid-Open No. 10-265888 Summary of the invention
[0012] Problems to be solved by the invention
[0013] However, although the initial activation of TiFe-based alloys is improved with the increase in the amount of Mn added, the starting point and end point of hydrogen absorption and release in the hydrogen pressure-composition isotherm diagram (hereinafter sometimes referred to as the PCT curve) are shifted to the right with the increase in the amount of Mn added. As a result, it is confirmed that even if the amount of hydrogen absorption is large, the amount of releasable hydrogen is insufficient as the amount of hydrogen that can be actually used. In addition, since the addition of Mn has the effect of reducing the equilibrium pressure, the addition of excessive Mn may make it difficult to ensure the equilibrium pressure required as a hydrogen storage material. Therefore, the subject of the present invention is to provide a hydrogen storage material, which has a TiFe-based alloy that has good initial activation while suppressing the amount of Mn and has a sufficient amount of releasable hydrogen. In addition, a hydrogen storage container having the hydrogen storage material and a hydrogen supply device having the hydrogen storage container are provided.
[0014] Means for solving problems
[0015] The present inventors have conducted intensive studies to solve the above-mentioned problems and, as a result, have found an alloy having a specific element composition containing Ti, a rare earth element, and Fe, thereby completing the present invention.
[0016] That is, according to the present invention, there is provided a hydrogen storage material, the hydrogen storage material having an alloy composed of elements represented by the following formula (1), wherein in a COMP image of a cross section of the alloy obtained by EPMA at a magnification of 1000, there are 25 or more and 3000 or less R-rich phases having a phase diameter of not less than 0.1 μm and not more than 10 μm in a field of view of 85 μm×120 μm of the COMP image, and the total area S of the phases existing in the field of view is R μm 2 The area S(10200)μm relative to the field of view 2 The R-rich phase area ratio [(S R / S)×100(%)] is 0.3% or more and 6.0% or less.
[0017]
[0018] [In formula (1), R is at least one selected from the rare earth elements and must contain Ce. M1 represents at least one selected from the group consisting of V, Zr, Nb, Ta and Mo, and M2 represents at least one selected from the group consisting of transition metal elements (except rare earth elements, M1, Ti, Fe and Mn), Al, B, Ga, Si and Sn. Here, the rare earth elements include Sc and Y. a is 0.003≤a≤0.15, b is 0≤b≤0.20, c is 0.40≤c≤1.15, d is 0≤d≤0.15, e is 0≤e≤0.20, f is 0≤f≤0.07, and c+d+e is 0.60≤c+d+e≤1.15.]
[0019] According to another aspect of the present invention, there are provided a hydrogen storage container having the above-mentioned hydrogen storage material and a hydrogen supply device having the hydrogen storage container.
[0020] Effects of the Invention
[0021] Since the hydrogen storage material of the present invention comprises an alloy having the above-mentioned specific element composition, it has good initial activation and a sufficient amount of releasable hydrogen, and can be suitably used for hydrogen storage purposes. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] [ Figure 1 ] is a figure showing a COMP image photograph of the cross section of the alloy casting piece after heat treatment in Example 1.
[0023] [ Figure 2 ] is a figure showing a COMP image photograph of a cross section of the alloy casting piece after heat treatment of Comparative Example 1.
[0024] [ Figure 3 ] is a figure showing a COMP image photograph of a cross section of the alloy casting piece after heat treatment of Comparative Example 6.
[0025] [ Figure 4 ] is the hydrogen pressure-composition isotherm diagram (PCT curve) of the alloy powder of Example 1 and the alloy powder of Comparative Example 1 at 0°C.
[0026] [ Figure 5 ] is the hydrogen pressure-composition isotherm diagram (PCT curve) of the alloy powder of Example 1 and the alloy powder of Comparative Example 1 at 50°C. DETAILED DESCRIPTION
[0027] The present invention will be described in detail below. The hydrogen storage material of the present invention is a material having an alloy composed of elements represented by the following formula (1). Preferably, the material is composed of the alloy.
[0028]
[0029] [In formula (1), R is at least one selected from the rare earth elements and must contain Ce. M1 represents at least one selected from the group consisting of V, Zr, Nb, Ta and Mo, and M2 represents at least one selected from the group consisting of transition metal elements (except rare earth elements, M1, Ti, Fe and Mn), Al, B, Ga, Si and Sn. Here, the rare earth elements include Sc and Y. a is 0.003≤a≤0.15, b is 0≤b≤0.20, c is 0.40≤c≤1.15, d is 0≤d≤0.15, e is 0≤e≤0.20, f is 0≤f≤0.07, and c+d+e is 0.60≤c+d+e≤1.15.]
[0030] In formula (1), a, b, c, d, e and f represent the content ratio of each element in terms of molar ratio, which is as follows. Hereinafter, this content ratio may also be referred to as "content" or "amount".
[0031] R in formula (1) is at least one selected from rare earth elements, and must contain Ce. Here, it is assumed that the rare earth elements include Sc (scandium) and Y (yttrium). Therefore, as R, Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb and Lu can be listed. Among them, the preferred rare earth elements other than Ce are La, Pr, Nd, Sm, and these elements can also be contained in addition to Ce. The Ce content in R is preferably 30% by mass or more of the total R amount, and more preferably 50% by mass or more. R is effective for improving initial activation, increasing hydrogen storage, increasing equilibrium pressure during hydrogen storage and release, and eliminating two platforms in the PCT curve. In formula (1), a representing the content of R is 0.003≤a≤0.15, preferably 0.003≤a≤0.10, and more preferably 0.005≤a≤0.08.
[0032] M1 in formula (1) is at least one selected from the group consisting of V, Zr, Nb, Ta and Mo. M1 is not necessarily required, but is an element that mainly helps to adjust various characteristics. For example, by forming an intermetallic compound with Ti, Mn, Fe and the like as main constituent elements and M1 elements, the initial activation has a good effect, and it can be contained when it is necessary to fine-tune the characteristics according to the use conditions during hydrogen storage. In formula (1), b representing the content of M1 is 0≤b≤0.20, preferably 0≤b≤0.05.
[0033] In formula (1), c represents the Fe content. c is 0.40≤c≤1.15, preferably 0.50≤c≤0.95, and more preferably 0.65≤c≤0.95. When the amount of Fe in the TiFe alloy is large and c is greater than 1.15, initial activation becomes difficult, and when used as a hydrogen storage material, it may not be possible to obtain sufficient hydrogen storage. When the amount of Fe in the TiFe alloy is small and c is less than 0.40, the hydrogen storage amount decreases. In addition, the equilibrium pressure of hydrogen absorption and release becomes too low, and when used as a hydrogen storage material, it may not function effectively.
[0034] In formula (1), d represents the content of Mn. d is 0≤d≤0.15, preferably 0≤d≤0.12, more preferably 0≤d<0.05, and particularly preferably 0≤d≤0.045. When the amount of Mn in the TiFe alloy is large and d is greater than 0.15, the starting point of hydrogen absorption and release of the PCT curve shifts to the right, and when used as a hydrogen storage material, hydrogen may not be effectively utilized. When the amount of Mn in the TiFe alloy is small, initial activation becomes difficult in the past. When used as a hydrogen storage material, it may not be possible to obtain sufficient hydrogen absorption or the initial activation requires a lot of labor and time, which lacks practicality. However, in the present application, even if d is 0, it is possible to obtain an initial activation and hydrogen absorption amount that can withstand practical use.
[0035] M2 in formula (1) represents at least one selected from transition metal elements (except rare earth elements, M1, Ti, Fe and Mn), Al, B, Ga, Si and Sn. M2 is preferably selected from at least one selected from Co, Ni, Cu, Cr, Al, B, Ga, Si and Sn. M2 is not necessarily required, but is an element that mainly helps to adjust various characteristics. For example, it can be contained in the case where it is necessary to fine-tune the characteristics according to the conditions of use during hydrogen storage. In formula (1), e representing the content of M2 is 0≤e≤0.20, preferably 0≤e≤0.10.
[0036] In formula (1), f represents the content of C (carbon). f is 0≤f≤0.07, preferably 0.001≤f≤0.05, and more preferably 0.001≤f≤0.035. C is effective for increasing the equilibrium pressure during hydrogen absorption and release and eliminating the two-stage platform in the PCT curve.
[0037] It should be noted that R and C in formula (1) are both elements effective for increasing the equilibrium pressure during hydrogen absorption and release and eliminating the two-stage platform in the PCT curve as described above, and a higher effect can be obtained by combining the two. In formula (1), it is preferred that f is 0.001≤f, and a+f is 0.005≤a+f≤0.11.
[0038] In formula (1), c+d+e represents the total content of Fe, Mn and M2. This value affects the activation and equilibrium pressure of the hydrogen storage material of the present invention. By adjusting it within the following range, an alloy that is easy to initially activate while maintaining the equilibrium pressure required for hydrogen storage can be made. c+d+e is 0.60≤c+d+e≤1.15, preferably 0.70≤c+d+e≤1.10, and more preferably 0.75≤c+d+e≤1.00.
[0039] The elemental composition of the alloy of the present invention represented by the above formula (1) can be confirmed by quantitative analysis using an ICP (Inductively Coupled Plasma) analyzer. It should be noted that in this specification, when referred to as the alloy of the present invention, unless otherwise specified, it refers to the alloy of the elemental composition represented by formula (1).
[0040] The alloy of the present invention has the following structural characteristics. Specifically, in a 1000-fold COMP image obtained by EPMA (Electron Probe Micro Analyzer) of a cross section of the alloy, the R-rich phase (phase enriched in R) is within a specific size range and has the following characteristics. That is, it has the following characteristics: there are 25 or more and 3000 or less R-rich phases with a phase diameter of 0.1 μm or more and 10 μm or less in the 85 μm×120 μm field of view of the COMP image, and when the field area is set to Sμm 2 The total area of the R-rich phase in the field of view is defined as S R μm 2 When (S R / S)×100(%) is 0.3% or more and 6.0% or less. S is 10200(85×120). It should be noted that in this specification, (S R / S)×100(%) is called “R-rich phase area ratio”.
[0041] Here, the cross section of the alloy refers to the cross section formed by embedding the alloy in a room temperature curing resin (e.g., epoxy resin) and curing it, then performing rough grinding and precision grinding using a wet grinder, and finally finishing the ground surface to a mirror surface. It should be noted that there is no particular restriction on the size of the alloy when forming the cross section. For example, an alloy sheet of about 1 cm square, about 1 cm 3 Alloy castings.
[0042] In the observation of the cross section formed in this way, the alloy of the present invention forms a sea island structure in which a plurality of R-rich phases exist in the main phase of the TiFe-based alloy. Since the R-rich phases as islands are dispersed in the main phase of the TiFe-based alloy as the sea as described above, although the detailed mechanism is unclear, it is possible to achieve both good initial activation as a hydrogen storage material and ensuring a good amount of releasable hydrogen. As a result, the absorption and release of hydrogen can be repeatedly carried out efficiently and well. It should be noted that each element in the main phase and the R-rich phase can be confirmed by a mapping image of the contained elements obtained by surface analysis using EPMA.
[0043] In the present application, the initial activation degree is used as an indicator of the quality of the initial activation. In the present application, the initial activation degree indicates the ease of hydrogen absorption when the hydrogen storage material initially absorbs (stores) hydrogen, that is, the time (minutes) required to absorb a certain amount of hydrogen. Therefore, the smaller the value of the initial activation degree, the better the initial activation is judged to be. Specifically, the initial activation degree is measured by the "activation rate test" described below. In the case where the TiFe-based alloy used in the hydrogen storage material contains a large amount of Mn, the value of the initial activation degree is small, and the initial activation becomes good. However, on the other hand, when the amount of Mn is large, there is a problem that the amount of releasable hydrogen is reduced, that is, the absorbed hydrogen cannot be fully released.
[0044] The activation rate test is carried out as follows. About 5 g of a hydrogen storage material having a particle size of 500 μm or less is filled into a sample chamber having a pressure storage portion, a pipeline portion, and a sample filling portion and having a total volume of about 138 ml. As a pretreatment, the chamber is evacuated at 80°C for 2 hours (vacuum degree: about 0.5 Pa to about 2.5 Pa), and then at 25°C and an initial hydrogen pressure of about 0.85 MPa, hydrogen absorption into the hydrogen storage material is started (total hydrogen amount: about 0.05 mol). Next, the time until the hydrogen pressure drops by 60 kPa from the initial hydrogen pressure is measured. The measured time is called the "initial activation degree". The initial activation degree is preferably less than 14.5 hours, and more preferably less than 10 hours. The shorter the initial activation time, the better, but the actual upper and lower limits are more than 0.1 hours.
[0045] In the present application, the releasable hydrogen amount refers to the amount of hydrogen that can be releasable relative to the amount of hydrogen absorbed in the hydrogen storage material, that is, the amount of hydrogen that can be effectively used. Specifically, the difference between the hydrogen absorption amount at 1MPa of the PCT absorption curve at 0°C and the hydrogen absorption amount at 0.1MPa of the PCT release curve at 50°C is taken as the releasable hydrogen amount. The hydrogen absorption amount is a value expressing the amount of hydrogen in the hydrogen storage material in weight percentage (wt%). The releasable hydrogen amount is preferably greater than 1.20 wt%, more preferably greater than 1.40 wt%, and particularly preferably greater than 1.61 wt%. The upper limit of the releasable hydrogen amount is substantially less than 2.5 wt%.
[0046] In addition, in the PCT release curve of the alloy of the present invention at 50°C, the hydrogen release pressure P at a hydrogen storage amount of 0.3 wt% is preferably a1 The hydrogen release pressure P at a hydrogen storage capacity of 0.1 wt% a2 Satisfy[{log 10 (P a1 )-log 10 (P a2)} / 0.2]≤1.10. This is because, by virtue of the PCT curve having the above-mentioned characteristics, the squareness of the curve becomes clear, and more hydrogen can be released when the hydrogen release ends at a predetermined pressure, so that a very suitable hydrogen storage material can be made that does not leave the stored hydrogen in the alloy and can be effectively utilized. The squareness refers to the degree of shoulder shown in the shape at the end of the PCT release curve. The clearer the shoulder, the better the squareness is evaluated. In this application, [{log 10 (P a1 )-log 10 (P a2 )} / 0.2] is used as an indicator of the quality of squareness, and for convenience, this value is called squareness.
[0047] The main phase of TiFe alloys is mainly a phase having a TiFe phase (which may contain substitution elements such as Mn). It is sometimes referred to as the main phase below. The phase diameter of the main phase is preferably less than 200 μm, and more preferably less than 150 μm. In addition, the phase diameter of the main phase is preferably greater than 2 μm. The R-rich phase (a phase enriched with R) refers to a phase that is mostly formed by the R element. In addition, there are cases where C (carbon) is contained therein (it may also contain a small amount of other added elements). In the observation of the R-rich phase in the field of view of the above-mentioned cross section, as shown Figure 1 The microscopic islands of the shape shown are dispersed in the main phase, and the phase diameter is within the range of 0.1 μm to 10 μm. Here, the phase diameter is the value obtained by measuring the major and minor axes of each phase and using the calculation formula "(major axis + minor axis) / 2".
[0048] When the alloy of the present invention contains C (carbon), C is relatively contained in the R-rich phase. Although the detailed mechanism is not clear, it is considered that the R-rich phase dispersed as described above contains C, which can achieve better effects on the increase of the equilibrium pressure during hydrogen absorption and release and the elimination of the two-stage platform in the PCT curve.
[0049] Next, the method for producing the hydrogen storage material of the present invention is described. First, as a method for producing the alloy, for example, a strip continuous casting method such as a single roll method, a twin roll method or a disk method, and a metal mold casting method can be cited.
[0050] For example, in the strip casting method, raw materials are prepared to form a desired alloy composition. Then, the combined raw materials are heated and melted in an inert gas atmosphere such as Ar to form an alloy melt, and then the alloy melt is poured onto a copper water-cooled roll, quenched, and solidified to obtain an alloy casting. As the copper water-cooled roll, a water-cooled roll having a coating layer containing Ni, Cr, other elements, etc. on the surface can also be used. The coating layer can be formed of, for example, metal, alloy, or ceramic.
[0051] In addition, in the metal mold casting method, the alloy melt is obtained by the same operation, and then the alloy melt is poured into a water-cooled copper mold, cooled and solidified to obtain an ingot. In the strip casting method and the metal mold casting method, the cooling rate is different. Generally, in the case of obtaining an alloy with less segregation and uniform composition distribution, the strip casting method is preferred. The alloy of the present invention is an alloy dispersed with a fine R-rich phase different from the main phase of the TiFe alloy, but the composition distribution of the main phase of the TiFe alloy other than the R-rich phase is preferably uniform, so in the present invention, the strip casting method is also a preferred method. In addition, the TiFe alloy is very hard and not easy to crush, so from this point of view, the strip casting method is also preferred.
[0052] In order to reduce the number of R-rich phases with a phase diameter of 0.1 μm or more and 10 μm or less and the R-rich phase area ratio [(S R / S)×100] is controlled within the scope of the present invention described above, and the cooling rate of the alloy melt when manufacturing the alloy flakes is controlled in the following manner. That is, the cooling rate from the cooling start temperature of the alloy melt (for example, the temperature at the moment when the molten metal contacts the roller) to the alloy temperature reaching 950°C is set to 300°C / second or more. Preferably, it is 700°C / second or more, more preferably 1000°C / second or more, and particularly preferably 1500°C / second or more. There is no particular restriction on the upper limit of the cooling rate, and it is actually about 50000°C / second or less. It should be noted that the cooling start temperature of the alloy melt also varies according to the alloy composition, and is in the range of about 1300°C to about 1500°C. There is no particular restriction on the cooling rate less than 950°C. For example, in the case of the strip continuous casting method, it can be adjusted to, for example, below 100°C by natural cooling after being peeled off from the roller and recovered.
[0053] In addition, in order to make an alloy with a more uniform composition distribution of the main phase of the TiFe alloy, it is preferred that the alloy flakes obtained by the above cooling be heat treated. Heat treatment can be carried out in an inert gas atmosphere such as Ar, in a range of more than 700°C and less than 1250°C. The heat treatment temperature is preferably more than 900°C and less than 1150°C, and the heat treatment time is more than 0.35 hours and less than 48 hours, preferably more than 2 hours and less than 24 hours. The heat treatment can be carried out in a known heat treatment furnace that can control the atmosphere. For example, rotary furnaces such as chamber type intermittent furnaces, continuous furnaces, and rotary kiln furnaces can be used.
[0054] Next, the alloy flakes obtained by casting are crushed to obtain alloy powder. The crushing can be carried out using a known crusher. The particle size of the alloy powder is preferably 800 μm or less, and more preferably 500 μm or less. There is no need to specifically stipulate the lower limit of the particle size of the alloy powder, but it is substantially about 0.1 μm. Here, the particle size of the alloy powder refers to the diameter measured using a shaking sieve machine (Rotape type). In addition, the O value of the alloy powder is preferably 3500 ppm or less, and the N value is preferably 1500 ppm or less. "O value" refers to the value in which the total amount of oxygen and oxygen-containing compounds contained in the alloy powder is expressed in the form of the amount of oxygen atoms. "N value" refers to the value in which the total amount of nitrogen and nitrogen-containing compounds contained in the alloy powder is expressed in the form of the amount of nitrogen atoms.
[0055] The hydrogen storage material of the present invention may be the powdered alloy itself, or may be a composite obtained by mixing alloy powder and resin, etc., and forming into any shape such as granules, or a composite obtained by fixing into a material capable of controlling temperature. In this case, the resin acts as a binder for the alloy powder. Mixing can be performed by a known method. For example, mixing can be performed using a mortar, or using a rotating mixer such as a double cone or V-type mixer, or a stirring mixer such as a blade type or a screw type mixer. In addition, a pulverizer such as a ball mill or a grinder may be used to mix the alloy flakes and the binder while pulverizing them.
[0056] The hydrogen storage container of the present invention has the hydrogen storage material manufactured in the above manner, and the material and shape of the container can use known materials and shapes.
[0057] The hydrogen supply device of the present invention includes the above-mentioned hydrogen storage container, and other configurations may use known configurations.
[0058] [Example]
[0059] The present invention is described in detail below by way of examples and comparative examples, but the present invention is not limited thereto. It should be noted that in the description of the present embodiment, the alloy of the present invention of the example and the alloy other than the present invention of the comparative example are both referred to as "alloys". In addition, the alloy obtained in the form of a cast flake by the strip casting method is referred to as an alloy cast flake, and the powder obtained by pulverizing the alloy cast flake is referred to as an alloy powder.
[0060] (Example 1)
[0061] The raw metals were weighed in such a way that the elemental composition of the alloy finally obtained became the composition shown in Table 1, and melted in an argon (Ar) atmosphere using a high-frequency melting furnace to form an alloy melt. Next, the pouring temperature of the melt was set to 1450°C, and the melt was rapidly cooled and solidified by a strip continuous casting method using a single roll casting device using a copper water-cooled roll, to obtain an alloy casting with a thickness deviation of about 0.1mm to about 0.4mm and an average thickness of 0.25mm. The cooling start temperature of the alloy melt, that is, the temperature at the moment of contact with the copper water-cooled roll, was about 1400°C. There was a difference in cooling rate between the roll contact side and the non-contact side of the alloy melt, and the cooling rate from 1400°C to 950°C was between 2000°C / second and 3000°C / second.
[0062] The alloy casting obtained above was heat treated in a heat treatment furnace in an Ar atmosphere at 1050°C for 6 hours. After the heat treatment, the alloy casting was embedded in an epoxy resin and cured, and rough grinding and precision grinding were performed using a wet grinder, and the ground surface was finally finished to a mirror surface to form an alloy cross section. The FE (field emission) type EPMA (manufactured by JEOL Ltd., trade name: JXA-8530F) was used at a magnification of 1000 times, an accelerating voltage of 15 kV, and a current of 1×10 -7 A, beam diameter 1μm, the cross section is analyzed (COMP image, mapping image of each element). The number of R-rich phases with a phase diameter of 0.1μm to 10μm in the field of view of 85μm×120μm of the COMP image is visually counted. The counted number is called the "number of R-rich phases". In addition, the total area S of the phase in the field of view is calculated. R The area ratio of the R-enriched phase relative to the field of view area S [(S R / S)×100(%)]. The results are shown in Table 1. Figure 1 A copy of the COMP image of the alloy cross section is shown in FIG.
[0063] The alloy flakes after the heat treatment were pulverized in a stainless steel mortar and sieved with a sieve having a mesh size of 500 μm to obtain alloy powder having a particle size of 500 μm.
[0064] [Activation speed test]
[0065] PCT was used to measure the activation rate of the obtained alloy powder using an automatic high-pressure Sievert device (manufactured by Hughes Technonet Co., Ltd.). Before the evaluation, about 5 g of alloy powder with a particle size of less than 500 μm was filled into a sample chamber having a pressure storage portion, a pipeline portion, and a sample filling portion and a total volume of about 138 ml. First, vacuum was evacuated at 80°C for 2 hours (vacuum degree: about 0.5 Pa to about 2.5 Pa), and then pressurized at a hydrogen pressure of about 0.85 MPa at 25°C (total hydrogen amount: about 0.05 moles), and placed for 15 hours. The hydrogen pressure was measured during this time, and the time required for the hydrogen pressure to be reduced by 60 kPa from the initial pressure was used as an index of the ease of initial activation of the alloy. This index is referred to as "initial activation degree". The results are shown in Table 1.
[0066] [Determination of Hydrogen Pressure-Composition Isotherm (PCT Curve)]
[0067] The PCT curve was obtained by measuring the hydrogen storage and release characteristics of the obtained alloy powder using an automatic high-pressure Sievert device (manufactured by Hughes Technonet Co., Ltd.). The sample chamber filled with the alloy powder used in the activation rate test was evacuated again at 80°C for 1 hour (vacuum degree: about 0.5Pa to about 2.5Pa), then pressurized with a hydrogen pressure of about 2.5MPa, and finally hydrogen was stored at 0°C until the hydrogen pressure stabilized. Next, evacuated at 80°C for 0.5 hours (vacuum degree: about 0.5Pa to about 2.5Pa), and pressurized with a hydrogen pressure of about 2.5MPa, and finally the operation of storing hydrogen at 0°C until the hydrogen pressure stabilized was performed twice. Next, vacuum was applied at 80°C for 2 hours (vacuum degree: about 0.5Pa to about 2.5Pa), and then the hydrogen pressure was varied between 0.01MPa and about 2MPa at the measurement temperatures of 0°C and 50°C, respectively, to measure the equilibrium pressure of hydrogen absorption and release. Figure 4 and 5 The hydrogen pressure-composition isotherms (PCT curves) at 0°C and 50°C are shown in FIG.
[0068] [Releasable Hydrogen Amount]
[0069] From the obtained PCT curve, the hydrogen storage amount at 1 MPa of the PCT absorption curve at 0°C and the hydrogen storage amount at 0.1 MPa of the PCT release curve at 50°C were read and the difference was calculated. This value was referred to as "releasable hydrogen amount". The results are shown in Table 1.
[0070] [Squareness]
[0071] From the obtained PCT curve, the hydrogen release pressure P at a hydrogen storage amount of 0.3 wt% of the PCT release curve at 50°C was read. a1and the hydrogen release pressure P at a hydrogen storage capacity of 0.1 wt% a2 , find [{log 10 (P a1 )-log 10 (P a2 The results are shown in Table 1.
[0072] (Examples 2 to 28)
[0073] Except for changing the element composition and heat treatment conditions of the final alloy as shown in Table 1 and Table 2, the alloy flakes and alloy powders of each embodiment were made in the same manner as in Example 1, and the surface analysis of the alloy cross section and the number of R-rich phases, the area ratio of R-rich phases, the activation rate test and the PCT curve were carried out. In addition, the initial activation degree, the amount of releasable hydrogen and the squareness were calculated from the activation rate test and the PCT curve. The pouring temperature, the cooling start temperature and the cooling rate of the alloy melts of these embodiments are roughly the same as those in Example 1, which are 1450°C, 1400°C and between 2000°C / second and 3000°C / second. The results are shown in Table 1 and Table 2.
[0074] (Comparative Examples 1 to 5, 7)
[0075] Except for changing the elemental composition and heat treatment conditions of the final alloy as shown in Table 2, the alloy castings and alloy powders of each comparative example were prepared in the same manner as in Example 1, and the surface analysis of the alloy cross section, the activation rate test, and the PCT curve were carried out. In addition, the initial activation degree, the amount of releasable hydrogen, and the squareness were calculated from the activation rate test and the PCT curve. The pouring temperature, cooling start temperature, and cooling rate of the alloy melts of these comparative examples were roughly the same as those in Example 1, which were 1450°C, 1400°C, and between 2000°C / sec and 3000°C / sec. The results are shown in Table 2. A copy of the COMP image of the alloy cross section of Comparative Example 1 is shown in Figure 2 middle.
[0076] (Comparative Example 6)
[0077] The raw metals were weighed in such a way that the elemental composition of the alloy finally obtained became the composition shown in Table 2, and melted in an argon (Ar) atmosphere using a high-frequency melting furnace to form an alloy melt. Then, the pouring temperature of the melt was set to 1450°C, and it was poured and solidified in a copper metal mold to obtain an alloy ingot with a thickness of about 20 mm. The cooling start temperature of the alloy melt, that is, the temperature at the moment of contact with the copper metal mold, was about 1400°C. The cooling rate of the alloy melt was about 10°C / second. The alloy flakes obtained above were heat treated in a heat treatment furnace, in an Ar atmosphere, at 1080°C for 6 hours. In addition, the heat-treated alloy flakes were crushed using a stainless steel mortar, and an alloy powder with a mesh size of 500μm was obtained using a sieve with a mesh size of 500μm. For the alloy flakes and powders obtained, the surface analysis of the alloy cross section and the number of R-rich phases, the area ratio of R-rich phases, the activation rate test and the determination of the PCT curve were carried out in the same manner as in Example 1. In addition, the initial activation degree, the amount of releasable hydrogen and the squareness were calculated from the activation rate test and the PCT curve. The results are shown in Table 2. A copy of the COMP image of the alloy cross section of Comparative Example 6 is shown in Figure 3 middle.
[0078]
[0079]
[0080] As can be seen from the table, the alloys of the examples have a superior amount of releasable hydrogen compared to the alloys of the comparative examples. In addition, the initial activation degree of the alloys of the examples is also good.
Claims
1. A hydrogen storage material, wherein: The hydrogen storage material has an alloy composed of elements represented by the following formula (1): In a COMP image of the cross section of the alloy obtained by EPMA at a magnification of 1000, there are 25 or more and 3000 or less R-rich phases having a phase diameter of 0.1 μm or more and 10 μm or less in a field of view of 85 μm×120 μm of the COMP image, and the total area S of the phases present in the field of view is R μm 2 The area S (10200) μm relative to the field of view 2 The R-rich phase area ratio [(S R / S)×100(%)] is 0.3% or more and 6.0% or less, In formula (1), R is at least one selected from the rare earth elements, but must include Ce; M1 represents at least one selected from the group consisting of V, Zr, Nb, Ta and Mo, M2 represents at least one selected from the group consisting of transition metal elements (except rare earth elements, M1, Ti, Fe and Mn), Al, B, Ga, Si and Sn; here, the rare earth elements include Sc and Y; a is 0.003≤a≤0.15, b is 0≤b≤0.20, c is 0.40≤c≤1.15, d is 0≤d≤0.15, e is 0≤e≤0.20, f is 0≤f≤0.07, and c+d+e is 0.60≤c+d+e≤1.
15.
2. The hydrogen storage material according to claim 1, wherein In the hydrogen pressure-composition isotherm diagram of the alloy at 50°C, the hydrogen release pressure P at a hydrogen storage amount of 0.3 wt% a1 The hydrogen release pressure P at a hydrogen storage capacity of 0.1 wt% a2 Satisfy[{log 10 (P a1 )-log 10 (P a2 )} / 0.2]≤1.
10.
3. The hydrogen storage material according to claim 1 or 2, wherein: The hydrogen storage material includes a composite obtained by mixing the alloy and a resin.
4. A hydrogen storage container, wherein: The hydrogen storage container comprises the hydrogen storage material according to any one of claims 1 to 3.
5. A hydrogen supply device, wherein: The hydrogen supply device includes the hydrogen storage container according to claim 4.