Steel material
By adjusting the chemical composition and microstructure of the steel, fine MC-type carbides are generated, which solves the problem of high susceptibility to hydrogen embrittlement of bolts and achieves high strength and improved durability of bolts.
Patent Information
- Application Number
- CN202380024056.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-04
- Filing Date
- 2023-03-03
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing technology, the steel used for bolts is prone to hydrogen embrittlement sensitivity under high strength conditions, resulting in delayed fracture, and it is difficult to effectively reduce hydrogen embrittlement sensitivity.
By adjusting the chemical composition and microstructure of the steel to ensure the content range of elements such as C, Si, Mn, Mo, and V in the chemical composition, and generating fine MC-type carbides through spheroidizing annealing, quenching and tempering processes, Increase the number density and narrow particle size distribution of cementite to form sufficient MC carbide to reduce hydrogen embrittlement susceptibility.
It effectively reduces the hydrogen embrittlement susceptibility of the bolt, improves its strength and durability, and ensures that delayed fracture is less likely to occur under high-strength conditions.
Smart Images

Figure BDA0005014340590000261 
Figure BDA0005014340590000361 
Figure BDA0005014340590000371
Abstract
Description
Technical Field
[0001] The present disclosure relates to a steel material, and more particularly, to a steel material that can be used as a blank of a bolt. Background Art
[0002] Bolts are used in industrial machinery, automobiles, buildings represented by bridges, etc. In recent years, with the improvement of the performance of industrial machinery and automobiles, and the enlargement of buildings, etc., the bolts are required to have higher strength.
[0003] In a bolt having high strength, there is a possibility that the hydrogen embrittlement sensitivity increases. Hydrogen embrittlement becomes a major cause of delayed fracture of the bolt. Therefore, in a bolt having high strength, it is required to have low hydrogen embrittlement sensitivity.
[0004] International Publication No. 2020 / 162616 (Patent Document 1) proposes a steel material for a bolt having high strength and low hydrogen embrittlement sensitivity.
[0005] The steel material disclosed in Patent Document 1 comprises, in mass%, C: 0.35-0.45%, Si: 0.02-0.10%, Mn: 0.20-0.84%, Cr: 0.60-1.15%, V: 0.30-0.50%, Mo: 0.25-0.99%, Al: 0.010-0.100%, N: 0.0010-0.0150%, P: 0.015% or less, S: 0.015% or less, and the balance: Fe and impurities, and satisfies the following equations (1) and (2).
[0006] 0.48≤Mo / 1.4+V<1.10 (1)
[0007] 0.80<Mo / V<3.00 (2)
[0008] In this steel material, the Mo content and the V content in the chemical composition are adjusted so as to satisfy the formula (1) and the formula (2). As a result, in the bolts manufactured using the steel material as a blank, MC-type carbides are easily dispersed. As a result, the hydrogen embrittlement sensitivity of the bolts is reduced. This is described in Patent Document 1 as above.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: International Publication No. 2020 / 162616 Summary of the invention
[0012] Problem that the invention aims to solve
[0013] The hydrogen embrittlement sensitivity of the bolt produced using the steel material disclosed in Patent Document 1 is low. However, the hydrogen embrittlement sensitivity of the bolt produced using the steel material can be reduced by a scheme different from that of Patent Document 1.
[0014] An object of the present disclosure is to provide a steel material which, when used as a blank of a bolt, can reduce the hydrogen embrittlement sensitivity of the bolt.
[0015] Solutions for solving problems
[0016] The steel material disclosed in the present invention has the following configuration.
[0017] A steel material comprising, by mass%,
[0018] C: 0.30~0.50%,
[0019] Si: 0.01-0.30%,
[0020] Mn: 0.10~1.50%,
[0021] P: 0.030% or less,
[0022] S: 0.030% or less,
[0023] Cr: 0.01~0.80%,
[0024] Mo: 0.70% or more and less than 1.50%,
[0025] V: 0.01~0.50%,
[0026] Al: 0.005~0.100%,
[0027] N: 0.0010~0.0300%、
[0028] Cu: 0-0.40%,
[0029] Ni: 0~0.40%
[0030] B: 0~0.0100%,
[0031] Zr: 0~0.300%,
[0032] Hf: 0~0.100%、
[0033] Ta: 0~0.100%、
[0034] W: 0~0.200%、
[0035] Ti: 0~0.100%,
[0036] Nb: 0~0.100%,
[0037] Ca: 0~0.0050%,
[0038] Mg: 0~0.0050%,
[0039] Bi: 0 to 0.020%, and
[0040] Te: 0~0.010%,
[0041] The balance is Fe and impurities.
[0042] The area ratio of the hard structure of the steel material is more than 90%, and the Vickers hardness is 220 to 400 HV.
[0043] The hard tissue has a 0.0005 μm 2 The number density of cementite in the area above is 4.0 / μm 2 In the above, among the plurality of cementites in the hard structure, the cementites having a diameter of 0.0005 to 0.0100 μm 2 The number ratio of the cementite in the area is 50.0% or more, and the sample standard deviation of the area of the plurality of cementites in the hard structure is 0.070 μm 2 the following.
[0044] Effects of the Invention
[0045] When the steel material of the present disclosure is used as a material for bolts, it is possible to reduce the hydrogen embrittlement sensitivity of the bolts. DETAILED DESCRIPTION
[0046] The present inventors have studied steel materials that can reduce the hydrogen embrittlement sensitivity of bolts when used as a raw material for bolts. As a result, the present inventors have obtained the following findings.
[0047] First, the inventors studied a steel material that can be used as a bolt material and reduce the hydrogen embrittlement sensitivity of the bolt from the viewpoint of chemical composition. As a result, the inventors believed that if a steel material containing, by mass%, C: 0.30-0.50%, Si: 0.01-0.30%, Mn: 0.10-1.50%, P: 0.030% or less, S: 0.030% or less, Cr: 0.01-0.80%, Al: 0.005-0.100%, N: 0.0010-0.0300%, Cu: 0-0.40%, Ni: 0-0.40%, B: 0-0.0100%, Zr: 0 ~0.300%, Hf: 0~0.100%, Ta: 0~0.100%, W: 0~0.200%, Ti: 0~0.100%, Nb: 0~0.100%, Ca: 0~0.0050%, Mg: 0~0.0050%, Bi: 0~0.020%, and Te: 0~0.010%, with the remainder being Fe and impurities, when used as a blank for bolts, there is a possibility that the hydrogen embrittlement sensitivity of the bolts can be reduced.
[0048] The present inventors have also studied a method for reducing hydrogen embrittlement sensitivity from the perspective of the microstructure of the bolt having the above chemical composition. As a result, the present inventors have found that the hydrogen embrittlement sensitivity of the bolt can be reduced by dispersing a plurality of fine MC-type carbides in the bolt.
[0049] Therefore, the inventors of the present invention believed that if the above chemical composition further contains Mo and V, fine MC-type carbides are formed in the bolt, and the hydrogen embrittlement sensitivity of the bolt is reduced. Therefore, the inventors of the present invention further studied the chemical composition of the steel material in consideration of the formation of MC-type carbides in the manufacturing process of the bolt. As a result, it was found that if the steel material of the present embodiment satisfies the chemical composition of the following feature 1, when a bolt using the steel material as a blank is manufactured, the hydrogen embrittlement sensitivity in the bolt is reduced to some extent.
[0050] (Feature 1)
[0051] The chemical composition contains, by mass%, C: 0.30-0.50%, Si: 0.01-0.30%, Mn: 0.10-1.50%, P: 0.030% or less, S: 0.030% or less, Cr: 0.01-0.80%, Mo: 0.70% or more and less than 1.50%, V: 0.01-0.50%, Al: 0.005-0.100%, N: 0.0010-0.0300%, Cu: 0-0 .40%, Ni: 0~0.40%, B: 0~0.0100%, Zr: 0~0.300%, Hf: 0~0.100%, Ta: 0~0.100%, W: 0~0.200%, Ti: 0~0.100%, Nb: 0~0.100%, Ca: 0~0.0050%, Mg: 0~0.0050%, Bi: 0~0.020%, and Te: 0~0.010%, and the balance is Fe and impurities.
[0052] However, even with a steel material having the chemical composition of feature 1, the hydrogen embrittlement sensitivity of the bolt may not be sufficiently low. Therefore, the present inventors have studied a method for further reducing the hydrogen embrittlement sensitivity of the bolt. As a result, the following findings were obtained.
[0053] In the case of a steel material having a chemical composition satisfying feature 1, cementite is generated in the steel material. In addition, in the manufacturing process of a bolt using the above-mentioned steel material as a blank, the steel material is subjected to spheroidizing annealing, quenching and tempering. As a result, the above-mentioned fine MC type carbide containing Mo and / or V is generated in the bolt.
[0054] In order to generate fine MC type carbides in the bolt, it is preferred that cementite in the steel material is fully dissolved during quenching. The cementite in the steel material before quenching contains Mo and V. If a plurality of cementites in the steel material are layered (that is, if a plurality of cementites are part of pearlite (lamellar pearlite)), the cementite in the steel material is not fully dissolved during quenching in the manufacturing process of the bolt. In this case, even if tempering is performed, a sufficient amount of fine MC type carbides will not be generated.
[0055] Therefore, in the steel material of the present embodiment, it is assumed that the microstructure satisfies the following feature 2.
[0056] (Feature 2)
[0057] The area ratio of the hard structure in the microstructure is more than 90%, and the Vickers hardness of the steel is 220-400 HV. Among them, the hard structure refers to the structure formed by ferrite containing carbides, and does not have a layered structure of carbides and ferrite. In other words, the hard structure does not contain pearlite. There are also cases where such a hard structure is called bainite.
[0058] If the area ratio of the hard structure is 90% or more in the microstructure of the steel material having the chemical composition satisfying feature 1, and if the Vickers hardness of the steel material is 220 to 400 HV, the cementite in the microstructure is not in a layered form but is roughly in a granular form. Granular cementite is easier to fully dissolve during quenching than the layered cementite in pearlite. Therefore, the microstructure of the steel material is substantially a hard structure.
[0059] In addition, in the microstructure of the steel material of the present embodiment, when the structure other than proeutectoid ferrite and pearlite is defined as a "hard structure", the area ratio of the hard structure in the microstructure is 90% or more, and if the Vickers hardness of the steel material is 220 to 400 HV, the microstructure of the steel material is substantially a hard structure. Therefore, in the steel material of the present embodiment, it is defined as Feature 2.
[0060] As described above, the present inventors believed that if the steel material satisfies the characteristics 1 and 2, when the bolt is manufactured using the steel material as a blank, the hydrogen embrittlement sensitivity of the bolt can be sufficiently low. However, even if the steel material satisfies the characteristics 1 and 2, there are still cases where the hydrogen embrittlement sensitivity of the bolt manufactured using the steel material as a blank cannot be sufficiently low. Therefore, the present inventors conducted further investigations and obtained the following findings.
[0061] The microstructure of the steel is substantially set as a hard structure. Even if the cementite in the steel is set as a granular state, the amount of fine MC-type carbides generated in the bolt after tempering is also affected by the number density of cementite in the steel and the particle size distribution of cementite. If the number density of cementite in the steel is reduced, the generation site of MC-type carbides cannot be fully obtained. In addition, even if the average grain diameter of the cementite in the steel becomes smaller, if the particle size distribution of the cementite is wider, the size of the cementite in the steel will also fluctuate. In this case, the cementite with a larger size has a larger amount of V and Mo contained in the cementite than the cementite with a smaller size. Therefore, even if the cementite in the steel is fully dissolved by quenching, V and Mo are enriched in the micro-region where the cementite with a larger size is dissolved, compared with other micro-regions (regions where the cementite with a smaller size is dissolved). Therefore, even when the average grain size of cementite is small, if the particle size distribution of cementite is wide, V and Mo enriched areas are locally generated during quenching due to the large cementite. In this case, it is difficult to generate a sufficient amount of fine MC type carbides during tempering. Therefore, in the bolt manufactured using steel as a blank, it is impossible to fully ensure the hydrogen capture site. As a result, the hydrogen embrittlement sensitivity of the bolt does not become sufficiently low.
[0062] Therefore, in the steel material of the present embodiment, in order to suppress the generation of V and Mo enriched regions during quenching, the number density of cementite is increased as much as possible in the steel material. Moreover, the number ratio of fine cementite among the plurality of cementites is increased as much as possible. Moreover, in order to suppress the fluctuation of the size of cementite, the particle size distribution of cementite is narrowed. Specifically, it is assumed that the steel material satisfying the characteristics 1 and 2 also satisfies the following characteristic 3.
[0063] (Feature 3)
[0064] The hard tissue has a 0.0005μm 2 The number density of cementite in the area above is 4.0 / μm 2 As described above, among the plurality of cementites in the hard structure, the cementite having a diameter of 0.0005 to 0.0100 μm 2 The number ratio of cementite in the area is 50.0% or more, and in the hard structure, there is 0.0005μm 2 The sample standard deviation of the cementite area above is 0.070 μm. 2 the following.
[0065] In this case, cementite is sufficiently present in the steel. Moreover, the cementite is sufficiently fine, and the particle size distribution of the cementite is sufficiently narrow. In other words, the fluctuation of the size of the cementite is sufficiently suppressed. Therefore, during quenching in the manufacturing process of manufacturing bolts using the steel as a blank, cementite is sufficiently dissolved, and V and Mo enriched areas are also difficult to be generated. As a result, the hydrogen embrittlement sensitivity of the bolt is sufficiently low.
[0066] The above mechanism is presumed. Therefore, the bolt manufactured using the steel material of the present embodiment as a blank may also have a sufficiently low sensitivity to hydrogen embrittlement due to a mechanism different from the above mechanism. However, as shown in the examples discussed later, for a steel material satisfying characteristics 1 to 3, when a bolt is manufactured using the steel material as a blank, the hydrogen embrittlement sensitivity of the bolt is sufficiently low.
[0067] The steel material of the present embodiment completed based on the above findings has the following structure.
[0068] [1] A steel material containing, by mass%,
[0069] C: 0.30~0.50%,
[0070] Si: 0.01-0.30%,
[0071] Mn: 0.10~1.50%,
[0072] P: 0.030% or less,
[0073] S: 0.030% or less,
[0074] Cr: 0.01~0.80%,
[0075] Mo: 0.70% or more and less than 1.50%,
[0076] V: 0.01~0.50%,
[0077] Al: 0.005~0.100%,
[0078] N: 0.0010~0.0300%、
[0079] Cu: 0-0.40%,
[0080] Ni: 0~0.40%
[0081] B: 0~0.0100%,
[0082] Zr: 0~0.300%,
[0083] Hf: 0~0.100%、
[0084] Ta: 0~0.100%、
[0085] W: 0~0.200%、
[0086] Ti: 0~0.100%,
[0087] Nb: 0~0.100%,
[0088] Ca: 0~0.0050%,
[0089] Mg: 0~0.0050%,
[0090] Bi: 0 to 0.020%, and
[0091] Te: 0~0.010%,
[0092] The balance is Fe and impurities.
[0093] The area ratio of the hard structure of the steel material is more than 90%, and the Vickers hardness is 220 to 400 HV.
[0094] The hard tissue has a 0.0005 μm 2 The number density of cementite in the area above is 4.0 / μm 2 In the above, among the plurality of cementites in the hard structure, the cementites having a diameter of 0.0005 to 0.0100 μm 2The number ratio of the cementite in the area is 50.0% or more, and the sample standard deviation of the area of the plurality of cementites in the hard structure is 0.070 μm 2 the following.
[0095] [2] The steel material according to [1], wherein
[0096] The steel material contains 0.01 to 0.40% Cu,
[0097] Ni: 0.01~0.40%,
[0098] B: 0.0001~0.0100%,
[0099] Zr: 0.001~0.300%,
[0100] Hf: 0.001~0.100%,
[0101] Ta: 0.001~0.100%,
[0102] W: 0.001~0.200%,
[0103] Ti: 0.001~0.100%,
[0104] Nb: 0.001~0.100%,
[0105] Ca: 0.0001~0.0050%,
[0106] Mg: 0.0001~0.0050%,
[0107] Bi: 0.001 to 0.020%, and
[0108] Te: One or more elements of the group consisting of 0.001 to 0.010%.
[0109] [3] The steel material according to [1] or [2], wherein
[0110] The steel material contains 0.01 to 0.40% Cu,
[0111] Ni: 0.01~0.40%,
[0112] B: 0.0001~0.0100%,
[0113] Zr: 0.001~0.300%,
[0114] Hf: 0.001~0.100%,
[0115] Ta: 0.001 to 0.100%, and
[0116] W: at least one element of the group consisting of 0.001 to 0.200%.
[0117] [4] The steel material according to any one of [1] to [3], wherein
[0118] The steel material contains one or more elements selected from the group consisting of Ti: 0.001 to 0.100% and Nb: 0.001 to 0.100%.
[0119] [5] The steel material according to any one of [1] to [4], wherein
[0120] The steel material contains one or more elements selected from the group consisting of Ca: 0.0001 to 0.0050% and Mg: 0.0001 to 0.0050%.
[0121] [6] The steel material according to any one of [1] to [5], wherein
[0122] The steel material contains one or more elements selected from the group consisting of Bi: 0.001 to 0.020% and Te: 0.001 to 0.010%.
[0123] The steel material of the present embodiment will be described in detail below. In addition, "%" related to an element means mass % unless otherwise specified.
[0124] [Features of the Steel Material of the Present Embodiment]
[0125] The steel material of this embodiment has the following characteristics.
[0126] (Characteristic 1) The content of each element in the chemical composition is within the range shown below.
[0127] (Feature 2) The area ratio of the hard structure is 90% or more, and the Vickers hardness is 220 to 400 HV.
[0128] (Feature 3) The hard tissue has a 0.0005 μm 2 The number density of cementite in the area above is 4.0 / μm 2 As described above, among the plurality of cementites in the hard structure, the cementite having a diameter of 0.0005 to 0.0100 μm 2 The number ratio NR of the cementite in the area is 50.0% or more, and the sample standard deviation σ of the area of the plurality of cementites in the hard structure is 0.070 μm 2 the following.
[0129] Hereinafter, features 1 to 3 will be described.
[0130] [(Feature 1) Regarding chemical composition]
[0131] The chemical composition of the steel material of the present embodiment contains the following elements.
[0132] C: 0.30~0.50%
[0133] Carbon (C) improves the hardenability of steel and improves the strength of bolts made from steel as a blank. C also forms cementite and sufficiently increases the number density ND of cementite discussed later. Therefore, the hydrogen embrittlement sensitivity of the bolt is sufficiently low. If the C content is less than 0.30%, even if the content of other elements is within the range of this embodiment, the above effects cannot be fully obtained.
[0134] On the other hand, if the C content exceeds 0.50%, the hydrogen embrittlement sensitivity of the bolt increases even if the contents of other elements are within the ranges of the present embodiment.
[0135] Therefore, the C content is 0.30 to 0.50%.
[0136] The lower limit of the C content is preferably 0.32%, more preferably 0.35%.
[0137] The upper limit of the C content is preferably 0.48%, more preferably 0.45%.
[0138] Si: 0.01~0.30%
[0139] Silicon (Si) improves the hardenability of steel and increases the strength of bolts. If the Si content is less than 0.01%, the above effects cannot be fully obtained even if the contents of other elements are within the ranges of the present embodiment.
[0140] On the other hand, if the Si content exceeds 0.30%, the cold forgeability of the steel material decreases even if the contents of other elements are within the ranges of the present embodiment.
[0141] Therefore, the Si content is 0.01 to 0.30%.
[0142] The lower limit of the Si content is preferably 0.02%, more preferably 0.03%.
[0143] The upper limit of the Si content is preferably 0.25%, more preferably 0.20%, and further preferably 0.15%.
[0144] Mn: 0.10~1.50%
[0145] Manganese (Mn) improves the hardenability of steel and increases the strength of bolts. If the Mn content is less than 0.10%, the above effects cannot be fully obtained even if the contents of other elements are within the ranges of the present embodiment.
[0146] On the other hand, if the Mn content exceeds 1.50%, the hydrogen embrittlement sensitivity of the bolt increases even if the contents of other elements are within the ranges of the present embodiment.
[0147] Therefore, the Mn content is 0.10 to 1.50%.
[0148] The lower limit of the Mn content is preferably 0.15%, more preferably 0.20%.
[0149] The upper limit of the Mn content is preferably 1.30%, more preferably 1.20%, and further preferably 1.10%.
[0150] P: 0.030% or less
[0151] Phosphorus (P) is an impurity. That is, the lower limit of the P content is greater than 0%. If the P content is greater than 0.030%, P will segregate at the grain boundaries even if the contents of other elements are within the range of this embodiment. As a result, the hydrogen embrittlement sensitivity of the bolt increases.
[0152] Therefore, the P content is 0.030% or less.
[0153] The P content is preferably as low as possible. However, an extreme reduction in the P content will significantly increase the manufacturing cost. Therefore, in consideration of industrial production, the preferred lower limit of the P content is 0.001%, more preferably 0.002%, and further preferably 0.003%.
[0154] The upper limit of the P content is preferably 0.025%, more preferably 0.020%.
[0155] S: 0.030% or less
[0156] Sulfur (S) is an impurity. That is, the lower limit of the S content is greater than 0%. If the S content is greater than 0.030%, S will segregate at the grain boundaries even if the contents of other elements are within the range of the present embodiment. As a result, the hydrogen embrittlement sensitivity of the bolt increases.
[0157] Therefore, the S content is 0.030% or less.
[0158] The S content is preferably as low as possible. However, an extreme reduction in the S content will significantly increase the manufacturing cost. Therefore, in consideration of industrial production, the preferred lower limit of the S content is 0.001%, more preferably 0.002%, and further preferably 0.003%.
[0159] The upper limit of the S content is preferably 0.025%, more preferably 0.020%.
[0160] Cr: 0.01~0.80%
[0161] Chromium (Cr) improves the hardenability of steel and increases the strength of bolts. Cr also improves the tempering softening resistance of steel and increases the strength of bolts. If the Cr content is less than 0.01%, even if the contents of other elements are within the range of this embodiment, the above effects cannot be fully obtained.
[0162] On the other hand, when the Cr content is 0.80% or less, even if the contents of other elements are within the ranges of the present embodiment, the intrusion of hydrogen into the steel material is sufficiently suppressed. As a result, the hydrogen embrittlement sensitivity of the bolt is sufficiently suppressed.
[0163] Therefore, the Cr content is 0.01 to 0.80%.
[0164] The lower limit of the Cr content is preferably 0.03%, more preferably 0.05%.
[0165] The upper limit of the Cr content is preferably 0.70%, more preferably 0.60%, and further preferably 0.50%.
[0166] Mo: 0.70% or more and less than 1.50%
[0167] Molybdenum (Mo) increases the temper softening resistance of steel and increases the strength of the bolt. Mo also enriches in MC carbides and increases the hydrogen capture function of MC carbides. As a result, Mo reduces the hydrogen embrittlement sensitivity of high-strength bolts. If the Mo content is 0.70% or more, the above-mentioned effect can be obtained to some extent even if the content of other elements is within the range of this embodiment.
[0168] On the other hand, when the Mo content is less than 1.50%, the steel material can obtain sufficient cold forgeability even if the contents of other elements are within the ranges of the present embodiment.
[0169] Therefore, the Mo content is 0.70% or more and less than 1.50%.
[0170] The lower limit of the Mo content is preferably 0.75%, more preferably 0.80%.
[0171] The upper limit of the Mo content is preferably 1.40%, more preferably 1.30%.
[0172] V: 0.01~0.50%
[0173] Vanadium (V) forms MC type carbides together with Mo to reduce the hydrogen embrittlement sensitivity of the bolt. If the V content is less than 0.01%, the above effects cannot be fully obtained even if the contents of other elements are within the ranges of the present embodiment.
[0174] On the other hand, if the V content exceeds 0.50%, the cold forgeability of the steel material decreases even if the contents of other elements are within the ranges of the present embodiment.
[0175] Therefore, the V content is 0.01 to 0.50%.
[0176] The lower limit of the V content is preferably 0.03%, more preferably 0.05%.
[0177] The upper limit of the V content is preferably 0.45%, more preferably 0.40%, and further preferably 0.35%.
[0178] Al: 0.005~0.100%
[0179] Aluminum (Al) is a deoxidizer during steel refining. Al also combines with N to form Al nitrides. Al nitrides suppress the coarsening of grains through the pinning effect during the quenching process during bolt manufacturing. As a result, the hydrogen embrittlement sensitivity of the bolts becomes lower. If the Al content is less than 0.005%, the above-mentioned effects cannot be fully obtained even if the contents of other elements are within the range of this embodiment.
[0180] On the other hand, if the Al content exceeds 0.100%, even if the contents of other elements are within the range of the present embodiment, coarse Al nitrides are generated. Coarse Al nitrides become the starting point of cracks, thereby reducing the cold forgeability of the steel material.
[0181] Therefore, the Al content is 0.005 to 0.100%.
[0182] The lower limit of the Al content is preferably 0.006%, more preferably 0.007%, and further preferably 0.008%.
[0183] The upper limit of the Al content is preferably 0.090%, more preferably 0.080%, and further preferably 0.070%.
[0184] In the chemical composition of the steel material of the present embodiment, the Al content refers to the total Al (Total-Al) content.
[0185] N: 0.0010~0.0300%
[0186] Nitrogen (N) combines with Al to form Al nitride. Al nitride uses the pinning effect to suppress the coarsening of grains during the quenching process when manufacturing bolts. As a result, the hydrogen embrittlement sensitivity of the bolts becomes lower. If the N content is less than 0.0010%, even if the content of other elements is within the range of this embodiment, the above-mentioned effects cannot be fully obtained.
[0187] On the other hand, if the N content exceeds 0.0300%, even if the contents of other elements are within the ranges of the present embodiment, coarse nitrides are generated. Coarse nitrides become starting points of cracks, and thus the cold forgeability of the steel material is reduced.
[0188] Therefore, the N content is 0.0010 to 0.0300%.
[0189] The lower limit of the N content is preferably 0.0020%, more preferably 0.0025%, and further preferably 0.0030%.
[0190] The upper limit of the N content is preferably 0.0290%, more preferably 0.0280%, more preferably 0.0270%, more preferably 0.0250%, more preferably 0.0200%, more preferably 0.0150%, and still more preferably 0.0100%.
[0191] The balance of the chemical composition of the steel material of this embodiment is Fe and impurities. The impurities in the chemical composition refer to elements mixed from ore and scrap as raw materials or from the manufacturing environment when the steel material is industrially manufactured, and are elements allowed within a range that does not adversely affect the steel material of this embodiment.
[0192] For example, impurities other than the above-mentioned impurities are as follows.
[0193] O: 0.0030% or less
[0194] Sn: 0.100% or less
[0195] Pb: 0.090% or less
[0196] Sb: 0.050% or less
[0197] Zn: 0.050% or less
[0198] Co: 0.050% or less
[0199] Rare earth elements (REM): 0.020% or less
[0200] The content of each of these impurity elements may be 0%.
[0201] [Optional Elements]
[0202] The chemical composition of the steel material of the present embodiment may further contain one or more elements selected from the group consisting of Cu, Ni, B, Zr, Hf, Ta, W, Ti, Nb, Ca, Mg, Bi, and Te to replace a part of Fe. These elements are all arbitrary elements and may not be contained.
[0203] These optional elements are described below.
[0204] [For Group 1: Cu, Ni, B, Zr, Hf, Ta, and W]
[0205] Alternatively, the chemical composition of the steel material of the present embodiment may further contain one or more elements selected from the group consisting of Cu, Ni, B, Zr, Hf, Ta, and W to replace a portion of Fe. These elements are all arbitrary elements and may not be contained. When contained, Cu, Ni, B, Zr, Hf, Ta, and W improve the hardenability of the steel material and improve the strength of the bolt.
[0206] Cu: 0~0.40%
[0207] Copper (Cu) is an arbitrary element and may not be contained. In other words, the Cu content may be 0%.
[0208] When Cu is contained, that is, when the Cu content is greater than 0%, Cu improves the hardenability of the steel material and improves the strength of the bolt. Even if a small amount of Cu is contained, the above effect can be obtained to some extent.
[0209] However, if the Cu content exceeds 0.40%, the steel material becomes brittle even if the contents of other elements are within the ranges of the present embodiment. As a result, the hot workability of the steel material decreases.
[0210] Therefore, the Cu content is 0 to 0.40%, and when contained, the Cu content is 0.40% or less (greater than 0 and 0.40% or less).
[0211] The lower limit of the Cu content is preferably 0.01%, more preferably 0.03%, and further preferably 0.05%.
[0212] The upper limit of the Cu content is preferably 0.35%, more preferably 0.30%, and further preferably 0.25%.
[0213] Ni: 0~0.40%
[0214] Nickel (Ni) is an arbitrary element and may not be contained. In other words, the Ni content may be 0%.
[0215] When Ni is contained, that is, when the Ni content is greater than 0%, Ni improves the hardenability of the steel material and improves the strength of the bolt. Even if a small amount of Ni is contained, the above effect can be obtained to some extent.
[0216] However, if the Ni content exceeds 0.40%, the hardenability becomes too high even if the contents of other elements are within the ranges of the present embodiment. As a result, the hot workability of the steel material decreases.
[0217] Therefore, the Ni content is 0 to 0.40%, and when contained, the Ni content is 0.40% or less (greater than 0 and 0.40% or less).
[0218] The lower limit of the Ni content is preferably 0.01%, more preferably 0.02%, and further preferably 0.03%.
[0219] The upper limit of the Ni content is preferably 0.35%, more preferably 0.30%, and further preferably 0.25%.
[0220] B: 0~0.0100%
[0221] Boron (B) is an arbitrary element and may not be contained. In other words, the B content may be 0%.
[0222] When B is contained, that is, when the B content is greater than 0%, B improves the hardenability of the steel material and improves the strength of the bolt. B also suppresses the grain boundary segregation of P and reduces the hydrogen embrittlement sensitivity of the bolt. Even if a small amount of B is contained, the above effects can be obtained to some extent.
[0223] However, if the B content exceeds 0.0100%, even if the contents of other elements are within the ranges of the present embodiment, coarse B nitrides are generated. Coarse B nitrides become starting points of cracks. As a result, the cold forgeability of the steel material is reduced.
[0224] Therefore, the B content is 0 to 0.0100%, and when contained, the B content is 0.0100% or less (greater than 0 and 0.0100% or less).
[0225] The lower limit of the B content is preferably 0.0001%, more preferably 0.0005%, and further preferably 0.0008%.
[0226] The upper limit of the B content is preferably 0.0090%, more preferably 0.0080%, further preferably 0.0070%, further preferably 0.0060%, further preferably 0.0050%.
[0227] Zr: 0~0.300%
[0228] Zirconium (Zr) is an arbitrary element and may not be contained. In other words, the Zr content may be 0%.
[0229] When Zr is contained, that is, when the Zr content is greater than 0%, Zr improves the hardenability of the steel material and improves the strength of the bolt. Even if a small amount of Zr is contained, the above effect can be obtained to some extent.
[0230] However, if the Zr content exceeds 0.300%, even if the contents of other elements are within the range of the present embodiment, coarse Zr nitrides are generated. Coarse Zr nitrides become the starting point of cracks. As a result, the cold forgeability of the steel material is reduced.
[0231] Therefore, the Zr content is 0 to 0.300%, and when contained, the Zr content is 0.300% or less (greater than 0 and 0.300% or less).
[0232] The lower limit of the Zr content is preferably 0.001%, more preferably 0.010%, and further preferably 0.020%.
[0233] The upper limit of the Zr content is preferably 0.280%, more preferably 0.250%, further preferably 0.200%, further preferably 0.150%, further preferably 0.100%.
[0234] Hf: 0~0.100%
[0235] Hafnium (Hf) is an arbitrary element and may not be contained. In other words, the Hf content may be 0%.
[0236] When Hf is contained, that is, when the Hf content is greater than 0%, Hf improves the hardenability of the steel material and improves the strength of the bolt. Even if a small amount of Hf is contained, the above-mentioned effect can be obtained to some extent.
[0237] However, if the Hf content exceeds 0.100%, even if the contents of other elements are within the range of the present embodiment, coarse Hf nitrides are generated. Coarse Hf nitrides become the starting point of cracks. As a result, the cold forgeability of the steel material is reduced.
[0238] Therefore, the Hf content is 0 to 0.100%, and when contained, the Hf content is 0.100% or less (greater than 0 and 0.100% or less).
[0239] The lower limit of the Hf content is preferably 0.001%, more preferably 0.005%, and further preferably 0.010%.
[0240] The upper limit of the Hf content is preferably 0.080%, more preferably 0.070%, further preferably 0.060%, further preferably 0.050%.
[0241] Ta: 0~0.100%
[0242] Tantalum (Ta) is an arbitrary element and may not be contained. In other words, the Ta content may be 0%.
[0243] When Ta is contained, that is, when the Ta content is greater than 0%, Ta improves the hardenability of the steel material and improves the strength of the bolt. Even if a small amount of Ta is contained, the above effect can be obtained to some extent.
[0244] However, if the Ta content exceeds 0.100%, even if the contents of other elements are within the range of the present embodiment, coarse Ta nitrides are generated. Coarse Ta nitrides become the starting point of cracks. As a result, the cold forgeability of the steel material is reduced.
[0245] Therefore, the Ta content is 0 to 0.100%, and when contained, the Ta content is 0.100% or less (greater than 0 and 0.100% or less).
[0246] The lower limit of the Ta content is preferably 0.001%, more preferably 0.005%, further preferably 0.010%.
[0247] The upper limit of the Ta content is preferably 0.080%, more preferably 0.070%, further preferably 0.060%, further preferably 0.050%.
[0248] W: 0~0.200%
[0249] Tungsten (W) is an arbitrary element and may not be contained. In other words, the W content may be 0%.
[0250] When W is contained, that is, when the W content is greater than 0%, W improves the hardenability of the steel material and improves the strength of the bolt. Even if a small amount of W is contained, the above effect can be obtained to some extent.
[0251] However, if the W content exceeds 0.200%, the hardenability becomes too high even if the contents of other elements are within the ranges of the present embodiment. As a result, the cold forgeability of the steel material decreases.
[0252] Therefore, the W content is 0 to 0.200%, and when contained, the W content is 0.200% or less (greater than 0 and 0.200% or less).
[0253] The lower limit of the W content is preferably 0.001%, more preferably 0.002%, and further preferably 0.010%.
[0254] The upper limit of the W content is preferably 0.150%, more preferably 0.120%, further preferably 0.100%.
[0255] [For Group 2: Ti and Nb]
[0256] The chemical composition of the steel material of the present embodiment may further contain one or more elements selected from the group consisting of Ti and Nb to replace a portion of Fe. These elements are all arbitrary elements and may not be contained. When contained, Ti and Nb form precipitates to refine the grains. As a result, the hydrogen embrittlement sensitivity of the bolt is reduced.
[0257] Ti: 0~0.100%
[0258] Titanium (Ti) is an arbitrary element and may not be contained. In other words, the Ti content may be 0%.
[0259] When Ti is contained, that is, when the Ti content is greater than 0%, Ti forms fine precipitates such as Ti carbides, which refines the crystal grains. As a result, the hydrogen embrittlement sensitivity of the bolt is reduced. Even if a small amount of Ti is contained, the above effect can be obtained to some extent.
[0260] However, if the Ti content exceeds 0.100%, even if the contents of other elements are within the range of the present embodiment, coarse Ti nitrides are generated. Coarse Ti nitrides become the starting point of cracks. As a result, the cold forgeability of the steel material is reduced.
[0261] Therefore, the Ti content is 0 to 0.100%, and when contained, the Ti content is 0.100% or less (greater than 0 and 0.100% or less).
[0262] The lower limit of the Ti content is preferably 0.001%, more preferably 0.003%, and further preferably 0.005%.
[0263] The upper limit of the Ti content is preferably 0.090%, more preferably 0.080%, and further preferably 0.075%.
[0264] Nb: 0~0.100%
[0265] Niobium (Nb) is an arbitrary element and may not be contained. In other words, the Nb content may be 0%.
[0266] When Nb is contained, that is, when the Nb content is greater than 0%, Nb forms fine precipitates such as Nb carbides, which refines the crystal grains. As a result, the hydrogen embrittlement sensitivity of the bolt is reduced. Even if a small amount of Nb is contained, the above effect can be obtained to some extent.
[0267] However, if the Nb content exceeds 0.100%, even if the contents of other elements are within the ranges of the present embodiment, coarse Nb carbides and the like are generated. Coarse Nb carbides and the like become starting points of cracks. As a result, the cold forgeability of the steel material is reduced.
[0268] Therefore, the Nb content is 0 to 0.100%, and when contained, the Nb content is 0.100% or less (greater than 0 and 0.100% or less).
[0269] The lower limit of the Nb content is preferably 0.001%, more preferably 0.003%, further preferably 0.010%, further preferably 0.020%.
[0270] The upper limit of the Nb content is preferably 0.090%, more preferably 0.080%, further preferably 0.070%.
[0271] [For Group 3: Ca and Mg]
[0272] The chemical composition of the steel material of the present embodiment may further contain one or more elements selected from the group consisting of Ca and Mg to replace a portion of Fe. These elements are all arbitrary elements and may not be contained. When contained, Ca and Mg refine MnS in the steel material and reduce the hydrogen embrittlement sensitivity of the bolt.
[0273] Ca: 0~0.0050%
[0274] Calcium (Ca) is an arbitrary element and may not be contained. In other words, the Ca content may be 0%.
[0275] When Ca is contained, that is, when the Ca content is greater than 0%, Ca refines MnS in the steel material and reduces the hydrogen embrittlement sensitivity of the bolt. Even if a small amount of Ca is contained, the above effect can be obtained to some extent.
[0276] However, if the Ca content exceeds 0.0050%, the cold forgeability of the steel material decreases even if the contents of other elements are within the ranges of the present embodiment.
[0277] Therefore, the Ca content is 0 to 0.0050%, and when contained, the Ca content is 0.0050% or less (greater than 0 and 0.0050% or less).
[0278] The lower limit of the Ca content is preferably 0.0001%, more preferably 0.0003%, and further preferably 0.0005%.
[0279] The upper limit of the Ca content is preferably 0.0040%, more preferably 0.0030%.
[0280] Mg: 0~0.0050%
[0281] Magnesium (Mg) is an arbitrary element and may not be contained. In other words, the Mg content may be 0%.
[0282] When Mg is contained, that is, when the Mg content is greater than 0%, Mg refines MnS in the steel material and reduces the hydrogen embrittlement sensitivity of the bolt. Even if a small amount of Mg is contained, the above effect can be obtained to some extent.
[0283] However, if the Mg content exceeds 0.0050%, the cold forgeability of the steel material decreases even if the contents of other elements are within the ranges of the present embodiment.
[0284] Therefore, the Mg content is 0 to 0.0050%, and when contained, the Mg content is 0.0050% or less (greater than 0 and 0.0050% or less).
[0285] The lower limit of the Mg content is preferably 0.0001%, more preferably 0.0002%, and further preferably 0.0005%.
[0286] The upper limit of the Mg content is preferably 0.0040%, more preferably 0.0030%.
[0287] [For Group 4: Bi and Te]
[0288] The chemical composition of the steel material of the present embodiment may further contain one or more elements selected from the group consisting of Bi and Te to replace a portion of Fe. These elements are all arbitrary elements and may not be contained. When contained, Bi and Te improve the machinability of the steel material.
[0289] Bi: 0~0.020%
[0290] Bismuth (Bi) is an arbitrary element and may not be contained. In other words, the Bi content may be 0%.
[0291] When Bi is contained, that is, when the Bi content is greater than 0%, Bi improves the machinability of the steel material. Even if a small amount of Bi is contained, the above-mentioned effect can be obtained to some extent.
[0292] However, if the Bi content exceeds 0.020%, the hot workability of the steel material decreases even if the contents of other elements are within the ranges of the present embodiment.
[0293] Therefore, the Bi content is 0 to 0.020%, and when contained, the Bi content is 0.020% or less (greater than 0 and 0.020% or less).
[0294] The lower limit of the Bi content is preferably 0.001%, more preferably 0.005%, and further preferably 0.010%.
[0295] The upper limit of the Bi content is preferably 0.018%, more preferably 0.015%.
[0296] Te: 0~0.010%
[0297] Tellurium (Te) is an arbitrary element and may not be contained. In other words, the Te content may be 0%.
[0298] When Te is contained, that is, when the Te content is greater than 0%, Te improves the machinability of the steel material. Even if a small amount of Te is contained, the above-mentioned effect can be obtained to some extent.
[0299] However, if the Te content exceeds 0.010%, the hot workability of the steel material decreases even if the contents of other elements are within the ranges of the present embodiment.
[0300] Therefore, the Te content is 0 to 0.010%, and when contained, the Te content is 0.010% or less (greater than 0 and 0.010% or less).
[0301] The lower limit of the Te content is preferably 0.001%, more preferably 0.002%, and further preferably 0.003%.
[0302] The upper limit of the Te content is preferably 0.009%, more preferably 0.008%.
[0303] [(Feature 2) Microstructure of steel]
[0304] The microstructure of the steel material of this embodiment has the following characteristics.
[0305] (Feature 2) The area ratio of the hard structure is 90% or more, and the Vickers hardness of the steel material is 220 to 400 HV.
[0306] Here, the hard structure is a structure other than proeutectoid ferrite and pearlite, and is a structure formed of ferrite containing carbides. Such a hard structure may also be called bainite.
[0307] The microstructure of the steel material of the present embodiment is substantially a hard structure. The hard structure can be easily distinguished from structures other than the hard structure (proeutectoid ferrite and pearlite) by microstructure observation described later.
[0308] When the content of each element in the chemical composition is within the range of the present embodiment, the area ratio of the hard structure in the microstructure is 90% or more, and when the Vickers hardness of the microstructure of the steel material is 220 to 400 HV, the microstructure is substantially formed of the hard structure.
[0309] The steel material of this embodiment is subjected to spheroidizing treatment during the manufacturing process of the bolt. As described above, the microstructure of the steel material of this embodiment is substantially a hard structure. Therefore, in the steel material after spheroidizing treatment, the spheroidization rate of cementite is improved. In this case, the cold forgeability of the steel material can be improved.
[0310] The lower limit of the area ratio of the hard structure in the microstructure of the steel material is preferably 92%, more preferably 94%, and further preferably 96%.
[0311] The preferred lower limit of the Vickers hardness of the steel microstructure is 230 HV, more preferably 240 HV, and further preferably 250 HV. The preferred upper limit of the Vickers hardness of the steel microstructure is 395 HV, further preferably 390 HV, further preferably 380 HV, and further preferably 370 HV.
[0312] [Methods for measuring the microstructure of steel materials]
[0313] The microstructure of this embodiment can be measured by the following method.
[0314] The cross section of the steel material perpendicular to the length direction is defined as the cross section. In the cross section, the center position of the radius connecting the central axis and the surface of the steel material is defined as the "D / 4" position. D refers to the diameter of the cross section.
[0315] Collect a sample including the D / 4 position of the steel. The surface of the sample corresponding to the above-mentioned cross section is defined as the observation surface. The observation surface of the sample is mirror-polished. Use 3% nital (nitric acid ethanol etching solution) to etch the mirror-polished observation surface for 10 seconds at room temperature. In the etched observation surface, the D / 4 position of the steel is set as the observation field P1. In the observation surface, the observation fields P2 to P5 are determined at intervals of 500μm from the observation field P1 in the direction perpendicular to the radial direction of the steel (equivalent to the circumferential direction of the steel). The area of each observation field P1 to P5 is set to 90μm×120μm. Observe each observation field P1 to P5 using a 1000x optical microscope.
[0316] In the observation field, the hard structure can be easily distinguished from the proeutectoid ferrite and pearlite by contrast. Proeutectoid ferrite is observed as a white area. When observed at 1000 times, pearlite is observed as a phase with a layered structure. The hard structure is observed as an area with a brightness lower than that of ferrite. Therefore, proeutectoid ferrite and pearlite are determined based on the contrast. Specifically, when observed at 1000 times, the white structure is identified as proeutectoid ferrite. When observed at 1000 times, the layered structure that can be confirmed is identified as pearlite. In each observation field, the structure other than proeutectoid ferrite and pearlite is regarded as hard structure.
[0317] The total area of proeutectoid ferrite and pearlite in the five observation fields P1 to P5 was calculated based on the determined proeutectoid ferrite and pearlite. The total area of hard structures in the five observation fields was calculated by subtracting the total area of proeutectoid ferrite and pearlite in the five observation fields from the total area of the five observation fields P1 to P5. The area ratio (%) of hard structures was calculated based on the total area of hard structures in the five observation fields and the total area of the five observation fields.
[0318] [Vickers hardness measurement method]
[0319] The Vickers hardness of the microstructure of the steel is calculated using the following method. Collect a sample with the section (cross section) of the steel perpendicular to the length direction as the observation surface. The observation surface of the sample is set as the entire cross section of the steel perpendicular to the length direction. In other words, the diameter of the observation surface of the sample is D. The observation surface is mirror-polished. In the mirror-polished observation surface, any measurement position at a depth of D / 4 from the surface of the steel in the radial direction is set as the measurement position P1. From the measurement position P1, the measurement positions P2 to P12 are determined at intervals of 30° around the center of the observation surface of the sample (that is, equivalent to the center of the cross section of the steel). The Vickers hardness is measured at the measurement positions P1 to P12, which are the D / 4 depth positions of the 12 locations.
[0320] At each of the measurement positions P1 to P12, a Vickers hardness test was performed in accordance with JIS Z 2244: 2020. The test force was set to 0.98 N. The arithmetic mean of the hardness obtained at the 12 measurement positions was defined as the Vickers hardness (HV) of the microstructure of the steel material.
[0321] [(Feature 3) Regarding cementite in steel]
[0322] In the steel material of this embodiment, the hard structure has a thickness of 0.0005 μm. 2 The number density of cementite in the area above is 4.0 / μm 2 Above, the hard tissue has 0.0005μm 2 Among the cementites with an area of more than 0.0005 to 0.0100 μm 2 The number ratio of cementite in the area is 50.0% or more, and the hard structure has 0.0005μm 2 The sample standard deviation σ of the cementite area above is 0.070 μm 2 the following.
[0323] In the steel material of the present embodiment, the V content and the Mo content are high. Therefore, when the bolt is manufactured using the steel material as a blank, a plurality of fine MC type carbides containing Mo are formed due to tempering after quenching in the manufacturing process. These fine MC type carbides are easy to capture hydrogen. Therefore, in the manufactured bolt, the limit amount of hydrogen that causes damage increases. As a result, the hydrogen embrittlement sensitivity of the bolt becomes lower.
[0324] In order to achieve the above effects, in the steel material used as the raw material of the bolt, (1) the number density of cementite in the hard structure is increased, (2) the proportion of fine cementite among the plurality of cementites in the hard structure is increased, and (3) the fluctuation of the size of cementite is suppressed to make the particle size distribution of cementite narrow. These points are described below.
[0325] [Regarding the number density of cementite ((1) above)]
[0326] In the manufacturing process of bolts using steel as a blank, the higher the number density of cementite in the hard structure of the steel, the higher the number density of MC type carbides in the bolt, and the MC type carbides in the bolt are evenly dispersed. As a result, the hydrogen embrittlement sensitivity of the bolt is sufficiently low. Specifically, in a steel satisfying the above-mentioned characteristics 1 and 2, if the number density ND of cementite in the hard structure is 4.0 pieces / μm 2 In the above conditions, the MC type carbides in the bolt are sufficiently finely dispersed, and the hydrogen embrittlement sensitivity of the bolt is sufficiently low.
[0327] The preferred lower limit of the number density ND of cementite in the hard structure is 4.2 pieces / μm 2 , and more preferably 4.5 / μm 2 , and more preferably 4.7 pieces / μm 2 .
[0328] The upper limit of the number density ND of cementite in the hard structure is not particularly limited. The upper limit of the number density ND of cementite in the hard structure is preferably 25.0 pieces / μm. 2 , and more preferably 20.0 pieces / μm 2 , and more preferably 15.0 pieces / μm 2 , and more preferably 10.0 pieces / μm 2 .
[0329] [Regarding the particle size distribution of cementite (the above (2) and (3))]
[0330] Even if the microstructure of the steel satisfying feature 1 is substantially bainite and cementite is granular, the amount of fine MC carbide generated in the bolt after tempering is affected by the particle size distribution of cementite. Specifically, even if the average grain size of a plurality of cementites in the steel is small, if the particle size distribution of cementite is wide, the size of cementite in the steel will fluctuate. In this case, the hydrogen embrittlement sensitivity of the bolt manufactured using the steel as a blank cannot be sufficiently low.
[0331] If the hard tissue has a 0.0005μm 2 Among the cementites with an area of more than 0.0005 to 0.0100 μm 2 The number ratio of cementite in the area is 50.0% or more, and the hard structure has 0.0005μm 2 The sample standard deviation σ of the cementite area above is 0.070 μm 2 Below, the cementite in the steel material is sufficiently fine, and the particle size distribution of the cementite is sufficiently narrow. In this case, during quenching in the manufacturing process of manufacturing bolts using the steel material as a blank, the cementite is sufficiently dissolved, and the segregation region of V and Mo is also difficult to form. As a result, the hydrogen embrittlement sensitivity of the bolt is sufficiently low.
[0332] The lower limit of the number ratio NR is preferably 52.5%, more preferably 55.0%, and further preferably 57.5%.
[0333] The upper limit of the number ratio NR is not particularly limited. The upper limit of the number ratio NR is, for example, 100.0%, for example, 90.0%, for example, 85.0%, for example, 80.0%.
[0334] The preferred upper limit of the sample standard deviation σ is 0.065 μm 2 , and more preferably 0.063 μm 2 , and more preferably 0.061 μm 2 .
[0335] [Method for measuring the number density ND of cementite, the number ratio NR of cementite, and the sample standard deviation σ of the area of cementite]
[0336] The hard tissue has a 0.0005μm 2 The number density ND of cementite in the area above 0.0005 μm 2 Among the cementites with an area of more than 0.0005 to 0.0100 μm 2 The number ratio of cementite in the area of NR, and the number of cementite with 0.0005μm in the hard structure 2The sample standard deviation σ of the areas of a plurality of cementite bodies having the above areas can be measured by the following method.
[0337] In the section (cross section) perpendicular to the longitudinal direction of the steel, a sample including the D / 4 position is collected. The surface of the sample corresponding to the above cross section is defined as the observation surface. After the observation surface of the sample is polished, the observation surface is etched for 20 seconds at room temperature using a 6% picrol etching solution (an etching solution obtained by mixing 6g of picric acid with 94mL of ethanol). Using a field emission scanning electron microscope (FE-SEM: Field Emission Scanning Electron Microscope), the D / 4 position in the etched observation surface is set as the observation field P11. In the observation surface, observation fields P12 to P15 are determined at intervals of 100μm in a direction perpendicular to the radial direction of the steel (equivalent to the circumferential direction of the steel) from the observation field P11. The area of each observation field P11 to P15 is set to 9μm×12μm. Each of the observation fields P11 to P15 was observed at a magnification of 10,000 times, and particles (precipitates and inclusions) in the observation field were photographed to generate a photographic image. The observation field was set to a region within the hard structure.
[0338] In each of the above-mentioned observation fields, an EDS (Energy Dispersive X-ray Spectroscopy) attached to the SEM is used to determine oxides and sulfides using a well-known method. Among the particles in the observation field, particles other than oxides and sulfides are determined as cementite. The area of the determined cementite is calculated. The area of the determined cementite can be calculated, for example, using well-known image processing.
[0339] Based on the observation field at 5 locations with a 0.0005 μm 2 The total number of cementites in the above area and the total area of the observation field at the five locations were used to calculate the number density ND (number / μm 2 ).
[0340] In addition, the cementite with an area of 0.0005 to 0.0100 μm 2 The ratio (%) of the total number of cementites to the total number of cementites determined is defined as the number ratio NR (%). Then, the sample standard deviation σ is calculated based on the area of each determined cementite. The sample standard deviation σ is calculated using the following formula.
[0341] [Mathematical formula 1]
[0342]
[0343] Where n is the value of 0.0005 μm determined at the observation field of view of 5 locations. 2 The total number of cementites above the area. i It is determined to have a 0.0005μm 2 The area of each cementite above is the area of the cementite. μ is determined with a value of 0.0005μm 2 The arithmetic mean of the areas of cementite of the above areas. The formula for the above sample standard deviation σ is a well-known formula.
[0344] [Effects of the Steel Material of the Embodiment]
[0345] As described above, the steel material according to the present embodiment has the following structure.
[0346] (Feature 1) The content of each element in the chemical composition is within the range described in this embodiment.
[0347] (Feature 2) The area ratio of the hard structure is 90% or more, and the Vickers hardness of the steel material is 220 to 400 HV.
[0348] (Feature 3) In the steel material of this embodiment, the hard structure has a thickness of 0.0005 μm. 2 The number density of cementite in the area above is 4.0 / μm 2 Above, the hard tissue has 0.0005μm 2 Among the cementites with an area of more than 0.0005 to 0.0100 μm 2 The number ratio of cementite in the area is 50.0% or more, and the hard structure has 0.0005μm 2 The sample standard deviation σ of the cementite area above is 0.070 μm 2 the following.
[0349] When the steel material having the above-mentioned structure is used as a material for a bolt, the hydrogen embrittlement sensitivity of the bolt can be reduced.
[0350] In this specification, for example, the following method is used to evaluate hydrogen embrittlement sensitivity. The steel material of this embodiment is subjected to wire drawing. The well-known spheroidizing annealing is performed on the wire-drawn steel material. In the spheroidizing annealing, the steel material is heated to 760°C. Then, it is maintained at 760°C for 5.0 hours. After the holding time, the steel material is slowly cooled to 650°C at 7°C / hour. The steel material temperature is air-cooled from 650°C to room temperature.
[0351] The spheroidizing annealed steel is subjected to cold forging (bolt forming) to produce an intermediate product in the shape of a bolt. The produced intermediate product is quenched and tempered under well-known conditions. The quenching temperature is set to 920°C, and the holding time at the quenching temperature is set to 1 hour. The intermediate product after the holding time is water-cooled. The quenched intermediate product is tempered. The tempering temperature is set to 620°C, and the holding time at the tempering temperature is set to 2.0 hours. Bolts are produced using the above process.
[0352] A round bar test piece with a 7mm diameter and 70mm length and an annular notch was collected from the inside of the manufactured bolt at a depth of more than 1mm from the surface. An annular notch was formed in the center of the length direction of the test piece. The notch shape had a notch depth of 1.4mm, a notch angle of 60°, and a curvature radius of the notch bottom of 0.175mm.
[0353] The round bar test piece with an annular notch was charged with hydrogen by the cathode hydrogen charging method. Specifically, a cathode hydrogen charging solution at room temperature was prepared. The cathode hydrogen charging solution was an aqueous solution prepared by adding 3 g of ammonium thiocyanate to 1 L of a 3 mass % sodium chloride aqueous solution.
[0354] The round bar test piece with an annular notch was immersed in the cathode hydrogen charging solution and the cathode current density was controlled to 0.05 mA / cm 2 A constant current of 10000 was generated for 18 hours to add hydrogen to the round bar test piece with a ring-shaped notch. After the cathode hydrogen charging method was implemented, the round bar test piece with a ring-shaped notch was left at room temperature for 96 hours. Thereafter, a zinc coating was formed on the surface of the round bar test piece with a ring-shaped notch that had been charged with hydrogen under the same conditions to prevent the hydrogen in the round bar test piece with a ring-shaped notch from leaking to the outside.
[0355] A constant load test is performed on a round bar test piece with an annular notch formed with a galvanized film, and a constant load is applied at room temperature and atmospheric pressure by applying a load of cross-sectional area × tensile strength × 0.90. The cross-sectional area refers to the cross-sectional area of the section (cross section) perpendicular to the length direction of the test piece at the bottom of the notch. In addition, the tensile strength refers to the tensile strength (MPa) obtained by using a smooth round bar tensile test piece and through the tensile test discussed later.
[0356] In addition, a tensile test using a smooth round rod tensile test piece was carried out using the following method. The smooth round rod tensile test piece was collected from the inside at a depth of more than 1 mm from the surface of the bolt. The diameter of the parallel portion of the smooth round rod tensile test piece was 6 mm, and the length of the parallel portion was set to 70 mm. The central axis of the parallel portion of the smooth round rod tensile test piece was coaxial with the central axis of the bolt. Using the smooth round rod tensile test piece, a tensile test according to JIS Z 2241:2022 was carried out in an atmosphere at room temperature (20±15°C) to determine the tensile strength (MPa).
[0357] In the above-mentioned constant load test, when the round bar test piece with an annular notch is durable without breaking for more than 100 hours, it is determined that the hydrogen embrittlement sensitivity is sufficiently low. In the above-mentioned constant load test, the round bar test piece with an annular notch is durable without breaking for more than 100 hours. Therefore, the hydrogen embrittlement sensitivity of the bolt manufactured using the steel material of the present embodiment as a blank is sufficiently low.
[0358] [Shape of steel]
[0359] The steel material of this embodiment is a steel material having a circular cross section perpendicular to the axial direction (length direction). Specifically, it is a steel bar or wire material having a circular cross section perpendicular to the axial direction. The steel material may be a material rolled into a roll or cut into a predetermined length. The diameter of the cross section of the steel material of this embodiment is not particularly limited, and is, for example, 5 to 30 mm.
[0360] [Use of Steel]
[0361] As described above, the steel material of this embodiment is suitable for the blank of the bolt. The steel material of this embodiment is particularly suitable for the blank of the bolt having a tensile strength of 1300 MPa or more and requiring low hydrogen embrittlement sensitivity. However, the steel material of this embodiment can also be used for other purposes besides the above-mentioned bolts.
[0362] [Method for manufacturing steel materials]
[0363] An example of a method for manufacturing a steel material of the present embodiment is described. The method for manufacturing a steel material described below is an example for manufacturing the steel material of the present embodiment. Therefore, the steel material having the above-mentioned structure can also be manufactured by other manufacturing methods other than the manufacturing method described below. However, the manufacturing method described below is a preferred example of the method for manufacturing a steel material of the present embodiment.
[0364] An example of a method for producing a steel material according to the present embodiment includes the following steps.
[0365] (Process 1) Direct hot working process after casting
[0366] (Process 2) Finishing process
[0367] The main production conditions in the above-mentioned steps 1 and 2 are as follows.
[0368] (Conditions in process 1)
[0369] · When the surface temperature of the casting material during cooling (solidification) is within the range of 1100 to 900°C, the casting material is subjected to hot working (direct hot working)
[0370] (Conditions in process 2)
[0371] Heating temperature HT: 1000~1200℃
[0372] Finishing temperature FT: above 900℃
[0373] · Average cooling rate CR1 from finishing rolling temperature FT to 820°C: 1.0°C / sec or more and less than 2.0°C / sec
[0374] ·820~400℃ average cooling rate CR2: 2.0~4.0℃ / sec
[0375] In the above-mentioned manufacturing process, the grains in the steel are maintained as coarse as possible until the finish rolling is completed. As a result, during cooling after the finish rolling is completed, the bainite front in the continuous cooling phase transformation diagram (CCT line diagram) shifts to the long time side. As a result, the starting temperature of the bainite phase transformation is reduced. If the starting temperature of the bainite phase transformation is reduced, the formation temperature of the cementite precipitated with the bainite phase transformation also becomes lower. If the formation temperature of the cementite becomes lower, the cementite remains fine. Therefore, steel that meets characteristics 1 to 3 can be manufactured. Below, each process is explained.
[0376] [(Process 1) Direct hot working process after casting]
[0377] In the hot working step directly after casting, a cast material is produced, and when the surface temperature of the cast material during cooling (solidification) is in the range of 1100 to 900° C., hot working is started to produce a steel billet. Thus, a steel billet with coarse grains can be produced.
[0378] The direct hot working process after casting includes the following steps.
[0379] (Process 11) Casting process
[0380] (Process 12) Direct heat treatment process
[0381] Hereinafter, each step will be described.
[0382] [(Process 11) Casting process]
[0383] In the casting process, a cast material having a chemical composition satisfying feature 1 is manufactured. Specifically, molten steel having a chemical composition in which the content of each element satisfies feature 1 is prepared. The prepared molten steel is used to manufacture a billet using a well-known casting method. For example, a steel ingot is manufactured using an ingot casting method. Alternatively, a large steel billet is manufactured using a continuous casting method. The cast material (steel ingot or large steel billet) is manufactured using the above process.
[0384] [(Process 12) Direct heat treatment process]
[0385] In the direct hot working step, the cast material is hot worked after the casting step while cooling (solidifying) to produce a steel billet. Specifically, when the cast material is cooling (solidifying) and the surface temperature of the cast material is within the range of 1100 to 900°C, the hot working is started to produce a steel billet.
[0386] Thus, in this specification, hot working performed when the surface temperature of the casting material during cooling reaches 1100 to 900°C without cooling the manufactured casting material to room temperature is referred to as "direct hot working". The hot working method may be hot forging or hot rolling. The cumulative reduction ratio in the direct hot working step is not particularly limited, and is, for example, 35% or more.
[0387] Generally, a cast material produced by a casting method is cooled to room temperature once. Then, the cast material cooled to room temperature is heated to A in a heating furnace. c3 Above the transformation point, initial rolling (rough rolling) is then performed. In this specification, such a conventional manufacturing process is referred to as "hot working after reheating". In the case of hot working after reheating, a reverse phase transformation (phase transformation from α phase to γ phase) occurs in the cast material with respect to the heating before initial rolling. Due to this reverse phase transformation, the grains are refined.
[0388] On the other hand, in this embodiment, the grain refinement caused by the reverse phase transformation is avoided. Specifically, when the surface temperature of the casting material being cooled in the casting process is within the range of 1100 to 900°C, that is, when the surface temperature of the casting material is A r3 In the state above the phase transformation point, the cast material is subjected to hot forging or hot rolling to produce a steel billet. In this case, the cast material is subjected to hot working without reverse phase transformation. Therefore, the grain refinement of the produced steel billet can be suppressed.
[0389] In addition, the upper limit of the cumulative reduction ratio in the direct hot working step is not particularly limited, and is, for example, 80%.
[0390] [(Process 2) Finishing rolling process]
[0391] In the finishing rolling process, the steel slab manufactured in the direct hot working process is heated. The heated steel slab is finish rolled. The finish rolled steel slab is cooled to manufacture a steel material. In the finishing rolling process, the following manufacturing conditions are met.
[0392] The conditions in the finish rolling step are as follows.
[0393] Heating temperature HT: 1000~1200℃
[0394] Finishing temperature FT: above 900℃
[0395] · Average cooling rate CR1 from finishing rolling temperature FT to 820°C: 1.0°C / sec or more and less than 2.0°C / sec
[0396] ·820~400℃ average cooling rate CR2: 2.0~4.0℃ / sec
[0397] Hereinafter, each manufacturing condition will be described.
[0398] [For heating temperature HT]
[0399] The heating temperature HT in the heating furnace in the finish rolling step is 1000 to 1200°C.
[0400] If the heating temperature HT of the heating furnace in the finishing rolling process is less than 1000°C, the precipitates in the steel billet are not fully dissolved. In this case, the undissolved precipitates have a pinning effect, thereby suppressing the coarsening of the grains in the steel billet. In this case, the cementite in the steel material after the finishing rolling process becomes coarse, and characteristic 3 is not satisfied.
[0401] On the other hand, if the heating temperature HT exceeds 1200° C., the manufacturing cost becomes high. Furthermore, cracks are likely to occur in the steel slab during finish rolling.
[0402] Therefore, the heating temperature HT is 1000 to 1200°C.
[0403] The lower limit of the heating temperature HT is preferably 1020°C, more preferably 1040°C, and further preferably 1060°C.
[0404] The upper limit of the heating temperature HT is preferably 1180°C, more preferably 1160°C, and further preferably 1140°C.
[0405] The holding time of the heating temperature HT is not particularly limited and is, for example, 0.5 to 4.0 hours.
[0406] [For finishing rolling temperature FT]
[0407] In the finishing rolling process, hot rolling (finishing rolling) is carried out using a continuous rolling mill having a plurality of rolling mill stands arranged in a row. In hot rolling using a continuous rolling mill, the temperature of the steel at the output side of the stand where the steel is finally pressed is defined as the finishing rolling temperature FT (°C). In addition, the steel temperature refers to the surface temperature of the steel.
[0408] The finishing rolling temperature FT is 900°C or higher.
[0409] If the finishing rolling temperature FT is lower than 900° C., the coarsening of the crystal grains in the steel material is suppressed by the pinning effect of the precipitates. In this case, the cementite of the steel material after the finishing rolling step becomes coarse, and the characteristic 3 is not satisfied.
[0410] If the finish rolling temperature is 900° C. or higher, the grains after the finish rolling can be maintained in a coarse state. As a result, fine cementite can be generated in the cooling step of the next step, satisfying the feature 3.
[0411] [Cooling after finishing rolling]
[0412] After the finish rolling is completed, the finished steel is cooled. The grains in the finished steel are maintained as coarse grains by satisfying the manufacturing conditions in the above process. Therefore, for the steel having the chemical composition of feature 1, the bainite front in the CCT line diagram shifts to the long time side. In other words, the phase transformation start temperature of bainite becomes lower.
[0413] Therefore, for cooling after finish rolling, when the steel material temperature is in the range of the finish rolling temperature FT to 820°C, the cooling rate (average cooling rate CR1) is slowed down as much as possible to keep the grains as coarse as possible. In addition, the steel material temperature range of 820 to 400°C corresponds to the bainite transformation temperature region, so the cooling rate (average cooling rate CR2) is accelerated to suppress the growth of cementite generated with the bainite transformation. The average cooling rates CR1 and CR2 are described below.
[0414] [For average cooling rate CR1]
[0415] The average cooling rate CR1 is the arithmetic mean of the cooling rates within the range of the steel material temperature from the finish rolling temperature FT to 820°C.
[0416] If the average cooling rate CR1 is above 2.0°C / sec, the cooling rate in this temperature range is too fast. In this case, the grains in the steel are refined. Therefore, in the CCT line diagram of the steel with the chemical composition of feature 1, the bainite front is offset to the short time side. In this case, the bainite transformation temperature becomes higher. Therefore, the cementite generated by the bainite transformation grows during the cooling process. As a result, the steel after the finishing rolling process does not meet feature 3.
[0417] The lower limit of the average cooling rate CR1 is not particularly limited, but in consideration of equipment capacity, the lower limit of the average cooling rate CR1 is 1.0° C. / sec.
[0418] The preferred lower limit of the average cooling rate CR1 is 1.1° C. / sec, and more preferably 1.2° C. / sec. The preferred upper limit of the average cooling rate CR1 is 1.9° C. / sec, and more preferably 1.8° C. / sec.
[0419] [For average cooling rate CR2]
[0420] The average cooling rate CR2 is the arithmetic mean of the cooling rates within the range of the steel material temperature from 820°C to 400°C.
[0421] The temperature range of 820 to 400°C for the steel material includes the temperature range that causes bainite transformation in the steel material produced by using the cast material satisfying the chemical composition of feature 1 and satisfying the above-mentioned manufacturing conditions. Therefore, in the temperature range of 820 to 400°C, the cooling rate is accelerated to a degree that martensite is not excessively generated. Thus, the growth of cementite generated during the bainite transformation is suppressed, and the cementite is maintained in a fine state.
[0422] When the average cooling rate CR2 is less than 2.0°C / sec, the cooling rate in the temperature range of 820 to 400°C is too slow. In this case, the generated cementite becomes coarse. Therefore, the steel material after the finish rolling step does not satisfy the feature 3.
[0423] On the other hand, when the average cooling rate CR2 exceeds 4.0°C / sec, the cooling rate in the temperature range of 820 to 400°C is too fast. In this case, martensite is excessively generated. As a result, in the microstructure of the steel material after the finish rolling process, although the area ratio of the hard structure becomes 90% or more, the Vickers hardness exceeds 400 HV.
[0424] If the average cooling rate CR2 is 2.0 to 4.0° C. / sec, the steel material after the finish rolling step satisfies characteristics 1 to 3, assuming that other manufacturing conditions are satisfied.
[0425] The preferred lower limit of the average cooling rate CR2 is 2.2°C / sec, more preferably 2.4°C / sec, and further preferably 2.6°C / sec. The preferred upper limit of the average cooling rate CR2 is 3.8°C / sec, more preferably 3.6°C / sec, and further preferably 3.4°C / sec.
[0426] In addition, the average cooling rate CR1 and the average cooling rate CR2 can be obtained by the following method. The cooling of the steel is carried out by using a cooling equipment line arranged downstream of the continuous rolling mill for finishing rolling. In the cooling equipment line, thermometers are set at multiple locations from upstream to downstream. The temperature and passage time of the steel passing through each thermometer are detected. The average cooling rate CR1 and the average cooling rate CR2 are obtained based on the obtained steel temperature and passage time.
[0427] The steel material of this embodiment is manufactured by the above-mentioned manufacturing steps.
[0428] [Bolt Manufacturing Process]
[0429] As a reference, a manufacturing process of a bolt using the steel material of the present embodiment as a blank will be described. An example of a manufacturing process of a bolt using the steel material of the present embodiment as a blank includes the following steps. In addition, the manufacturing process of a bolt is well known.
[0430] Wire drawing process
[0431] Spheroidizing annealing process
[0432] Cold forging process
[0433] ·Quenching and tempering process
[0434] Hereinafter, each step will be described.
[0435] [Wire drawing process]
[0436] In the wire drawing process, the steel material is subjected to well-known wire drawing to produce a steel wire. The wire drawing process may be performed only once or multiple times such as twice.
[0437] [Spheroidizing annealing process]
[0438] In the spheroidizing annealing process, the steel wire after the wire drawing process is subjected to spheroidizing annealing. The spheroidizing annealing can be carried out under well-known conditions. For example, the steel wire is heated to 720-800°C. Then, it is kept at 720-800°C for 1.0-6.0 hours. Then, it is slowly cooled to 650°C at a cooling rate of 3-10°C / hour. Then, it is cooled to room temperature.
[0439] [Cold forging process]
[0440] In the cold forging step, the steel wire after the spheroidizing annealing step is subjected to well-known cold forging to produce an intermediate product in a bolt shape.
[0441] [Quenching and tempering process]
[0442] In the quenching and tempering step, the intermediate product is quenched and tempered.
[0443] [Quenching]
[0444] The intermediate product after the cold forging process is quenched by a well-known method. The quenching temperature and the holding time of the quenching temperature are not particularly limited. The quenching temperature is, for example, 840 to 970°C. The holding time of the quenching temperature is, for example, 15 minutes to 360 minutes (6 hours). The intermediate product after the holding time is rapidly cooled. Specifically, the intermediate product is water-cooled or oil-cooled.
[0445] [Tempering]
[0446] The intermediate product after quenching is subjected to well-known tempering. For example, the tempering conditions are as follows. The tempering temperature is, for example, 570 to 660° C. The holding time of the tempering temperature is, for example, 0.5 to 6.0 hours.
[0447] The bolt using the steel material of the present embodiment as a raw material can be manufactured by the above-mentioned manufacturing method.
[0448] [For other processes]
[0449] The manufacturing process of the bolt may also include other processes in addition to the above-mentioned processes. For example, a rolling process may be performed after the cold forging process and before the quenching and tempering process to form the thread. In addition, a compressive residual stress imparting process may be performed after the quenching and tempering process. These processes are all arbitrary processes and may not be performed.
[0450] Example
[0451] The effect of the steel material of this embodiment will be described in more detail using examples. The conditions in the following examples are one example of conditions used to confirm the feasibility and effect of the steel material of this embodiment. Therefore, the steel material of this embodiment is not limited to this one example of conditions.
[0452] Steel materials (round bars) serving as bolt materials having the chemical compositions shown in Tables 1-1 and 1-2 were prepared. In the tables, "-" indicates that no intentional addition was made.
[0453] [Table 1-1]
[0454] Table 1-1
[0455]
[0456] [Table 1-2]
[0457] Table 1-2
[0458]
[0459] The steel material of each test number was manufactured by the following method: Steel ingots having the chemical compositions shown in Table 1-1 and Table 1-2 were manufactured by a casting method (casting process).
[0460] In test numbers 1 to 26 and 29 to 36, when the surface temperature of the cast material during cooling after the casting process reached 1100 to 900°C, the cast material was hot forged to produce a steel billet. That is, in these test numbers, direct hot working was performed (recorded as "direct" in the "hot working" column in Table 2). On the other hand, in test numbers 27 and 28, after the cast material was cooled to room temperature, it was reheated to 1200°C in a heating furnace and then hot forged to produce a steel billet (recorded as "after reheating" in the "hot working" column in Table 2). In any hot working method, the cumulative reduction rate in the direct hot working process is in the range of 35 to 60%.
[0461] [Table 2]
[0462] Table 2
[0463]
[0464] The produced steel billet (162 mm×162 mm in cross section) was subjected to a finish rolling process to produce a steel material (round bar) having a diameter of 20 mm.
[0465] The heating temperature HT (°C) in the finishing rolling process, the finishing rolling temperature FT (°C), the average cooling rate CR1 (°C / second) of the steel material temperature from the finishing rolling temperature FT to 820°C, and the average cooling rate CR2 (°C / second) of the steel material temperature from 820°C to 400°C are as shown in Table 2. The steel materials (round bars) of each test number were manufactured by the above manufacturing process.
[0466] [Evaluation test]
[0467] The following evaluation tests were carried out using the manufactured steel materials.
[0468] (Test 1) Microstructure observation test
[0469] (Test 2) Vickers hardness test
[0470] (Test 3) Cementite number density ND, cementite number ratio NR and sample standard deviation σ measurement test
[0471] (Test 4) Wire drawing processability evaluation test of steel materials
[0472] (Test 5) Cold forgeability evaluation test of steel
[0473] (Test 6) Hydrogen embrittlement sensitivity evaluation test of bolts made of steel
[0474] Hereinafter, each evaluation test will be described.
[0475] [(Test 1) Microstructure observation test]
[0476] The area ratio (%) of the hard structure in the microstructure of the steel material of each test number was calculated based on the above-mentioned [Method for measuring the microstructure of steel material]. The obtained results are shown in the "Hard structure area ratio (%)" column of "Microstructure" in Table 2.
[0477] [(Test 2) Vickers hardness test]
[0478] The Vickers hardness (HV) of the steel material of each test number was determined based on the above-mentioned [Vickers hardness measurement method]. The obtained Vickers hardness (HV) is shown in the "Vickers hardness (HV)" column of "Microstructure" in Table 2.
[0479] [(Test 3) Test for measuring the number density ND of cementite, the number ratio NR of cementite and the sample standard deviation σ]
[0480] In the steel material of each test number, the number of cementite density ND, the number ratio NR of cementite, and the sample standard deviation σ of the area of cementite were determined based on the above-mentioned [Method for measuring the number density ND of cementite, the number ratio NR of cementite, and the sample standard deviation σ of the area of cementite]. 2 The number density of cementite in the area above ND (pieces / μm 2 ), among the multiple cementites in the hard structure, those with a diameter of 0.0005 to 0.0100 μm 2 The number ratio NR (%) of cementite in the area, and the number of cementite with 0.0005 μm in the hard structure 2 The sample standard deviation σ(μm 2 The obtained number density ND (number / μm 2 ), number ratio NR (%) and sample standard deviation σ (μm 2 ) respectively represent the “number density ND (pieces / μm)” in the “cementite” column in Table 2 2 )”, “Number ratio NR (%)” and “Sample standard deviation σ (μm 2 )"column.
[0481] [(Test 4) Wire drawing processability evaluation test of steel materials]
[0482] The following wire drawing process was applied to the steel of each test number. After lubrication treatment was applied to 250 kg of steel of each test number under the same conditions, wire drawing was applied. The cumulative cross-sectional shrinkage rate at the die during the wire drawing process was set to 25%. In the case where no wire breakage occurred during the wire drawing process, the wire drawing process was evaluated as excellent (indicated by "P (Pass)" in the "Wire Drawing Processability" column in Table 2). On the other hand, in the case where wire breakage occurred during the wire drawing process, the wire drawing process was evaluated as low (indicated by "F (Fail)" in the "Wire Drawing Processability" column in Table 2). In addition, Tests 5 to 6 were not applied to the steel of the test numbers with low wire drawing processability.
[0483] [(Test 5) Cold forgeability evaluation test of steel material]
[0484] The cold forgeability of the steel material of each test number was evaluated by the following method.
[0485] First, the steel was subjected to spheroidizing annealing. In the spheroidizing annealing, the steel was heated to 760°C and maintained at 760°C for 5.0 hours. After the holding time, the steel was slowly cooled to 650°C at 7°C / hour. The steel was air-cooled from 650°C to room temperature.
[0486] A smooth test piece was collected from the D / 4 depth position in the cross section perpendicular to the length direction of the steel material after spheroidizing annealing. The smooth test piece was cylindrical, with a diameter of 8 mm and a length of 12 mm. The length direction of the smooth test piece was parallel to the length direction of the steel material.
[0487] The smooth test piece was subjected to an ultimate compression test according to the test method described in the Cold Forging Subcommittee Material Research Group: Plasticity and Processing vol.22 No.241 (1981-2), pages 139-144. Specifically, the smooth test piece was cold compressed at a speed of 10 mm / min at room temperature and in the atmosphere using an end-face restraint die. The compression was stopped when a microcrack of 0.5 mm or more was generated on the smooth test piece, and the compression rate (%) at this time was calculated. This measurement was performed a total of 10 times, and the compression rate (%) at which the cumulative probability of breakage became 50% was calculated, and this compression rate was set as the ultimate compression rate (%).
[0488] When the limit compression rate is 70% or more, the cold forgeability is judged to be excellent (indicated by "70 or more" in the "Limit Compression Rate (%)" column in Table 2). On the other hand, when the limit compression rate is less than 70%, the cold forgeability is judged to be low (the "Limit Compression Rate (%)" column in Table 2 indicates the limit compression rate (%)). In addition, for the test number with low cold forgeability, Test 6 was not implemented.
[0489] [(Test 6) Hydrogen embrittlement sensitivity evaluation test of bolts made of steel materials]
[0490] The hydrogen embrittlement sensitivity evaluation test of the bolts using the steel material of each test number as a raw material was evaluated by the following method.
[0491] First, the steel material of each test number was subjected to wire drawing under the same conditions to produce a steel wire with a diameter of 16 mm. The steel wire of each test number was subjected to spheroidizing annealing under the same conditions as those of the spheroidizing annealing performed in [(Test 5) Cold forgeability evaluation test of steel material].
[0492] The steel wire after spheroidizing annealing was subjected to cold forging (bolt forming) under the same conditions to produce intermediate products having the same bolt shape with a thread bottom diameter of 14 mm for each test number.
[0493] The intermediate product thus produced was subjected to quenching and tempering. In the quenching, the quenching temperature was set to 920° C. and the holding time at the quenching temperature was set to 1 hour for each test number. After the holding time, the intermediate product was water-cooled.
[0494] The intermediate product after quenching was tempered at a temperature of 620° C. and a holding time of the tempering temperature of 2.0 hours.
[0495] Bolts of respective test numbers were manufactured using the above-described manufacturing process.
[0496] The following hydrogen embrittlement sensitivity evaluation test was performed on the bolts of each test number.
[0497] A round bar test piece with a 7mm diameter and 70mm length with an annular notch was collected from the inside of the bolt at a depth of 1mm or more from the surface. An annular notch was formed in the center of the length direction of the test piece. The notch shape has a notch depth of 1.4mm, a notch angle of 60°, and a curvature radius of 0.175mm at the notch bottom.
[0498] The round bar test piece with an annular notch was charged with hydrogen by the cathode hydrogen charging method. Specifically, a cathode hydrogen charging solution at room temperature was prepared. The cathode hydrogen charging solution was an aqueous solution prepared by adding 3 g of ammonium thiocyanate to 1 L of a 3 mass % sodium chloride aqueous solution.
[0499] The round bar test piece with an annular notch was immersed in the cathode hydrogen charging solution and the cathode current density was controlled to 0.05 mA / cm 2 A constant current of 1000 Hz was generated for 18 hours while hydrogen was added to the round bar test piece with the annular notch.
[0500] After the cathode hydrogen charging method was implemented, the round bar test piece with an annular notch was left at room temperature for 96 hours. Then, a zinc coating was formed on the surface of the round bar test piece with an annular notch that had been charged with hydrogen under the same conditions to prevent the hydrogen in the round bar test piece with an annular notch from leaking to the outside.
[0501] A constant load test was carried out at room temperature and atmospheric pressure on a round bar test piece with an annular notch formed with a galvanized film by applying a load of cross-sectional area × tensile strength × 0.90. Among them, the cross-sectional area refers to the cross-sectional area of the section (cross section) perpendicular to the length direction of the test piece at the bottom of the notch. The tensile strength refers to the tensile strength (MPa) obtained by the tensile test discussed later using a smooth round bar tensile test piece. The maximum test time is set to 100 hours. In the constant load test, when the round bar test piece with an annular notch is durable without breaking for more than 100 hours, it is evaluated that the hydrogen embrittlement sensitivity is sufficiently low (the "Durability Time (Hours)" column in the "Hydrogen Embrittlement Sensitivity" in Table 2 is indicated by "100 or more"). On the other hand, in the constant load test, when the round bar test piece with an annular notch breaks at less than 100 hours, it is evaluated that the hydrogen embrittlement sensitivity is high (the "Durability Time (Hours)" column in the "Hydrogen Embrittlement Sensitivity" in Table 2 indicates the durability time (hours)).
[0502] In addition, a tensile test using a smooth round bar tensile test piece was performed using the following method. The smooth round bar tensile test piece was collected from the inside of the bolt at a depth of more than 1 mm from the surface of each test number. The diameter of the parallel portion of the smooth round bar tensile test piece was 6 mm, and the length of the parallel portion was 70 mm. The central axis of the parallel portion of the smooth round bar tensile test piece was set to be coaxial with the central axis of the bolt.
[0503] The tensile strength (MPa) was determined by performing a tensile test in accordance with JIS Z2241:2022 using a smooth round bar tensile test piece in air at room temperature (20±15°C). The obtained tensile strength is shown in the "Tensile Strength (MPa)" column of "Hydrogen Embrittlement Susceptibility" in Table 2.
[0504] [Evaluation results]
[0505] Referring to Table 1-1, Table 1-2, and Table 2, in the steel materials of Test Nos. 1 to 23, the chemical composition is appropriate and the manufacturing conditions are also appropriate. Therefore, the area ratio of the hard structure is more than 90%, and the Vickers hardness is 220 to 400 HV. In addition, the steel material has a hard structure of 0.0005 μm. 2 The number density of cementite in the area above is 4.0 / μm 2 As described above, among the plurality of cementites in the hard structure, the cementite having a diameter of 0.0005 to 0.0100 μm 2 The number ratio of cementite in the area is 50.0% or more, and the hard structure has 0.0005μm 2 The sample standard deviation σ of the cementite area above is 0.070 μm 2 Therefore, the wire drawing property is excellent. Moreover, the cold forging property after spheroidizing treatment is excellent. Moreover, the hydrogen embrittlement sensitivity of the bolt manufactured using the steel material as the blank is sufficiently low.
[0506] On the other hand, in Test No. 24, the Mo content was too low. Therefore, the bolt produced using the steel material had a high hydrogen embrittlement sensitivity.
[0507] In test number 25, the V content was too low. Therefore, the bolt manufactured using the steel material had high hydrogen embrittlement sensitivity.
[0508] In Test No. 26, the V content was too high. Therefore, the cold forgeability after spheroidizing treatment was low.
[0509] In test numbers 27 and 28, although the chemical composition was appropriate, the cast material was subjected to hot working after reheating. Therefore, the number density ND of cementite was less than 4.0 pieces / μm. 2, the number ratio NR of cementite is less than 50.0%, and the sample standard deviation σ of the area of cementite exceeds 0.070μm 2 Therefore, bolts made from steel blanks are more sensitive to hydrogen embrittlement.
[0510] In test number 29, although the chemical composition was appropriate, the heating temperature HT in the finishing rolling process was too low and the finishing rolling temperature FT was too low. Therefore, the number density ND of cementite was less than 4.0 pieces / μm. 2 , the number ratio NR of cementite is less than 50.0%, and the sample standard deviation σ of the area of cementite exceeds 0.070μm 2 Therefore, bolts made from steel blanks are more sensitive to hydrogen embrittlement.
[0511] In test numbers 30 and 31, although the chemical composition was appropriate, the average cooling rate CR1 was too fast. Therefore, the number density ND of cementite was less than 4.0 pieces / μm. 2 , the number ratio NR of cementite is less than 50.0%, and the sample standard deviation σ of the area of cementite exceeds 0.070μm 2 Therefore, bolts made from steel blanks are more sensitive to hydrogen embrittlement.
[0512] In test numbers 32 and 33, although the chemical composition was appropriate, the average cooling rate CR2 was too slow. Therefore, the number density ND of cementite was less than 4.0 pieces / μm. 2 , the number ratio NR of cementite is less than 50.0%, and the sample standard deviation σ of the area of cementite exceeds 0.070μm 2 Therefore, bolts made from steel blanks are more sensitive to hydrogen embrittlement.
[0513] In test numbers 34 and 35, although the chemical composition was appropriate, the average cooling rate CR2 was too fast. Therefore, although the area ratio of the hard structure was 90% or more, the Vickers hardness exceeded 400 HV. Therefore, the wire drawability was low.
[0514] In test number 36, the C content was too low. Therefore, the number density ND of cementite was less than 4.0 pieces / μm. 2 Therefore, bolts made from steel materials have a high sensitivity to hydrogen embrittlement.
[0515] The embodiments of the present disclosure have been described above. However, the above embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above embodiments, and the above embodiments can be appropriately modified and implemented within the scope of the present disclosure.
Claims
1. A steel material comprising, by mass%, C:0.30~0.50%、 Si: 0.01-0.30%, Mn: 0.10~1.50%, P: 0.030% or less, S: 0.030% or less, Cr:0.01~0.80%、 Mo: 0.70% or more and less than 1.50%, V:0.01~0.50%、 Al:0.005~0.100%、 N:0.0010~0.0300%、 Cu: 0-0.40%, Ni: 0~0.40% B:0~0.0100%、 Zr:0~0.300%、 Hf: 0~0.100%、 Ta: 0~0.100%、 W:0~0.200%、 Ti: 0~0.100%, Nb: 0~0.100%, Ca: 0~0.0050%, Mg: 0~0.0050%, Bi: 0 to 0.020%, and Te: 0~0.010%, The balance is Fe and impurities. The area ratio of the hard structure of the steel material is more than 90%, and the Vickers hardness is 220 to 400 HV. The hard tissue has a 0.0005 μm 2 The number density of cementite in the area above is 4.0 / μm 2 In the above, among the plurality of cementites in the hard structure, the cementites having a diameter of 0.0005 to 0.0100 μm 2 The number ratio of the cementite in the area is 50.0% or more, and the sample standard deviation of the area of the plurality of cementites in the hard structure is 0.070 μm 2 the following.
2. The steel material according to claim 1, in, The steel material contains 0.01 to 0.40% Cu, Ni: 0.01~0.40%, B:0.0001~0.0100%、 Zr:0.001~0.300%、 Hf: 0.001~0.100%, Ta: 0.001~0.100%, W:0.001~0.200%、 Ti: 0.001~0.100%, Nb: 0.001~0.100%, Ca: 0.0001~0.0050%, Mg: 0.0001~0.0050%, Bi: 0.001 to 0.020%, and Te: One or more elements of the group consisting of 0.001 to 0.010%.