Rhenium-tungsten alloy wire, method for producing same, medical needle, and probe
By controlling the NH4 ion concentration on the surface of the rhenium-tungsten alloy wire and suppressing discoloration, the problem of discoloration of the rhenium-tungsten alloy wire during storage is solved, the stability and yield of the wire are improved, and it is suitable for the manufacture of probes and medical needles.
Patent Information
- Application Number
- CN202380024018.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-15
AI Technical Summary
Rhenium-tungsten alloy wires are prone to discoloration during storage, resulting in changes in resistance, deterioration of mechanical properties and reduction in yield, making them unable to be used stably for a long time.
By controlling the NH4 ion concentration on the wire surface to be below 10 ppm by mass, the formation and discoloration of rhenium oxide is suppressed, and appropriate manufacturing processes and packaging methods are adopted to ensure the stability of the wire.
It effectively suppresses the discoloration of rhenium-tungsten alloy wire, improves long-term storage stability and yield, and is suitable for the manufacture of probes and medical needles.
Smart Images

Figure CN118786255A_ABST
Abstract
Description
Technical Field
[0001] The embodiments described below relate to a rhenium-tungsten alloy wire, a method for producing the same, a medical needle, and a probe. Background Art
[0002] Tungsten alloy (ReW) wire containing a specified amount of rhenium (Re) has improved resistance characteristics and wear resistance compared to ordinary tungsten (W) wire. In addition, the tensile strength in a wide range of temperatures and the ductility after recrystallization are also improved. Therefore, it has been used in semiconductor inspection probes, electron tube heaters, filament materials for earthquake-resistant bulbs, thermocouples, fluorescent display tube filaments, medical needles, etc.
[0003] After the surface mixture layer produced in the manufacturing process is removed by electrolytic polishing, the ReW wire is a white silver color with a metallic luster. As the storage period is extended, the surface becomes, for example, blue, yellow, or magenta. If discoloration occurs, the resistance of the probe may change. For filaments used in display tubes, the uniformity of the coating (electrodeposition surface treatment) of the oxide used to release thermal electrons disappears. For medical needles, if heat treatment is performed in a discolored state, the mechanical properties deteriorate and the wire sometimes breaks during bending. In addition, quality deterioration and impurity such as changes in the friction of the discolored part and the risk of falling off of the discolored part become problems.
[0004] Therefore, the discolored part cannot be used and needs additional treatment such as re-electrolysis. Furthermore, the additional treatment changes the size of the wire, and the resistance and strength change, so it becomes unusable and the yield rate decreases. Therefore, after the electrolysis process, for example, the wire is fully dried, and the wound wire reel is sealed and packaged under reduced pressure and stored in a manner isolated from the external environment. However, there are differences in the occurrence of discoloration in ReW wires stored in the same manner.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 4-308003
[0008] Patent Document 2: Japanese Patent Application Publication No. 2021-95585
[0009] Non-patent literature
[0010] Non-patent literature 1: Saburo Nagakura and five others, "Iwanami Physical and Chemical Dictionary 5th Edition", Iwanami Shoten, February 1998, p. 541 Summary of the invention
[0011] Problems to be solved by the invention
[0012] An object of the present invention is to provide a ReW wire that can be easily stored for a long period of time by suppressing discoloration.
[0013] Means for solving problems
[0014] In order to solve the above problems, the rhenium tungsten alloy wire according to the embodiment is a wire composed of a tungsten alloy containing rhenium, and the amount of NH4 on the wire surface calculated by NH4 ion weight on the wire surface / alloy wire weight is 10 mass ppm or less. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1a This is an example of the result of TDS analysis of the undiscolored portion of the ReW line.
[0016] Figure 1b This is an example of the result of TDS analysis of the color change portion of the ReW line.
[0017] Figure 2 Cross-sectional view of the test device for evaluating the effect of NH4 on ReW wire.
[0018] Figure 3 is a graph showing the color change of the ReW line and its reflection spectrum.
[0019] Figure 4 The figure shows an example of the results of analyzing a sample with discoloration (CW) and a sample without discoloration (NW) by X-ray photoelectron spectroscopy (XPS).
[0020] Figure 5 It is an illustration of particle size distribution. DETAILED DESCRIPTION
[0021] Hereinafter, the rhenium tungsten alloy wire of the embodiment will be described with reference to the drawings. Hereinafter, the rhenium tungsten alloy wire may also be referred to as ReW wire. It should be noted that the drawings are schematic, and for example, the ratio of the dimensions of each part is not limited to the drawings.
[0022] The rhenium-tungsten alloy wire according to the embodiment is a wire made of a tungsten alloy containing rhenium, and the amount of NH 4 on the surface of the wire determined by NH 4 ion weight on the surface of the wire / alloy wire weight is 10 mass ppm or less.
[0023] Among rhenium oxides, Re2O5, also known as rhenium pentoxide, is a blue compound. ReO3, also known as rhenium trioxide, is a red cubic crystal with a metallic luster. Re2O7, also known as rhenium heptoxide, is a yellow orthorhombic crystal (Non-Patent Document 1). Thus, rhenium oxides have colors, and the colors change depending on the type of oxide. As a result of repeated and in-depth studies, the following understanding was obtained: the color change of the ReW line is caused by rhenium oxide, and further, NH4 has an effect.
[0024] exist Figure 1a and Figure 1b An example of the results of TDS analysis of the undiscolored part (A) and the discolored part (B) of the ReW line is shown in FIG. The device used was a TDS1200I I quadrupole mass spectrometer manufactured by Electronic Science Co., Ltd. The length of the evaluation sample was set to 1 cm, and the measurement temperature was in the range of room temperature to 1400°C. Comparing B (discolored part) with the undiscolored part (A), it can be seen that the separation of NH3 (m / z=17, 16) and H2O (m / z=18, 17) is significant.
[0025] In order to confirm the influence of NH4, a mandatory test was carried out by setting up ammonia water in a closed container. Figure 2 The cross section of the test device is shown in . The sample (X) subjected to electrolytic grinding and wound on a reel is placed on the mesh table (Y) of the test device, and the sample (X) is sealed in the device and left for 4 days. When ammonia water is placed in a sealed container (Z) set below the mesh table (Y) and left, the ammonia atmosphere concentration in the device is 3.5%.
[0026] In Experiment 1, a tungsten-doped wire was used that had not changed color after electrolysis. In Experiment 2, a 26% Re-W wire that had changed color after storage was used again by electrolysis. In Experiment 3, a 26% Re-W wire that had not changed color after storage was used again by electrolysis. The test results are shown in Table 1. As for the tungsten-doped (W) wire, there was no color change regardless of the ammonia atmosphere. The ReW wire only changes color in an ammonia atmosphere, and Re has an effect on the color change, which is accelerated by the presence of NH4. In addition, the ammonia-free setting in Table 1 ( Figure 2 The blank shown in FIG. 1 was tested by placing water in a sealed container (Z) instead of ammonia water.
[0027] [Table 1]
[0028]
[0029] ○: No discoloration, ×: Discoloration
[0030] exist Figure 3The color change of the ReW line and its reflection spectrum are shown in . The color change shows the color of the rhenium oxide mentioned above (blue, purple (red and blue), yellow). As for the reflection spectrum of each color-changing part, a spectroscopic system is assembled in the microscope, and a microscopic spectroscopic system (DF-1037 manufactured by Techno Synagi) capable of spectroscopic measurement of tiny points is used to measure under the conditions of a measuring point of about φ10μm, an exposure time of 10ms, and an accumulation number of 200 times. For the visible light wavelength of 400nm to 700nm, if it is a white silver color (metallic color) without color change, the difference between the maximum and minimum values of the reflectivity is less than 5%. On the other hand, the reflectivity of the color-changing part changes, and changes to a spectrum with a peak having a difference of more than 5% from the minimum value in the wavelength portion corresponding to each color. Therefore, the color-changing part is judged based on whether the difference between the maximum and minimum values of the reflectivity in the wavelength of 400nm to 700nm of the visual or reflection spectrum exceeds 5%.
[0031] exist Figure 4 An example of the results of analyzing a discolored sample (CW) and a non-discolored sample (NW) using X-ray photoelectron spectroscopy (XPS) in a 26 wt% Re-W line of φ0.152 mm after electrolytic polishing to give it a metallic luster and storing it for a certain period of time is shown in the figure. The device used was Quantera SXM manufactured by PHI, the X-ray source was single crystal spectroscopic A1Kα rays, the X-ray output power was 12.5 W, and the analysis range was φ50 μm.
[0032] exist Figure 4 W-Metal and tungsten oxide (WO) detected in the NW (sample without discoloration) shown in B x )Compare Figure 4 The CW (discoloration sample) shown in A is more Figure 4 The rhenium oxide (ReO) detected in the CW shown in A x )Compare Figure 4 There are many NWs shown in B. As described above, rhenium oxide has color, and the color changes depending on the type of oxide. That is, it is known that rhenium oxide is the cause of the color change, and the presence of NH4 promotes the generation of rhenium oxide.
[0033] Table 2 shows the results of hot water extraction-ion chromatography for measuring the amount of NH4 in the discolored and non-discolored parts. The amount of NH4 was measured by hot water extraction of 0.5 g of alloy wire in 50 ml of pure water and ion chromatography. The device used was ICS-2000 manufactured by Thermo Fischer Scientific Co., Ltd. The results show that discoloration can be suppressed by limiting the amount of NH4 attached to the surface. Figure 4 The color change sample (A(CW)) shown in the results corresponds to samples 2, 3, and 4. Figure 4The results shown in FIG. 5 correspond to the sample without discoloration (B(NW)).
[0034] The reason for the incorporation of ammonium ions into the rhenium tungsten alloy wire is as follows. The ammonia contained in the atmosphere in the manufacturing process of the rhenium tungsten alloy wire is adsorbed. It is estimated that ammonia in the atmosphere is produced when organic matter such as plants and animals, and ammonium salts are decomposed by bacteria, etc., and it is mainly likely to be naturally produced in soil, oceans, etc. In addition, in cities, it is also considered to be produced based on sewers, feces treatment plants, chemical plants, refineries, and the combustion of fossil fuels. In addition, for the lubricant used in the drawing process of the manufacturing method described later, a suspension of graphite powder dissolved in water can be used. In the lubricant, ammonia water is added to adjust the pH. These are estimated to be the reasons.
[0035] [Table 2]
[0036]
[0037] In the rhenium-tungsten alloy wire of the embodiment, the amount of NH4 on the wire surface, which is obtained by the weight of NH4 ions on the wire surface / the weight of the alloy wire, is 10 mass ppm or less, and further, 5 mass ppm or less. By controlling the amount of NH4 on the surface to 10 mass ppm or less, and further, 5 mass ppm or less, discoloration can be suppressed, and the use as a raw material in a probe or a medical needle can be manufactured with a high yield.
[0038] The amount of NH4 on the surface of the wire can be set to a target value by, for example, adjusting the surface treatment of the rhenium tungsten alloy wire, for example, by adjusting the electrolytic polishing conditions, cleaning conditions, or drying conditions of the rhenium tungsten alloy wire. In addition, the amount of NH4 on the surface of the wire can also be set to a target value by adjusting the storage method or packaging method of the rhenium tungsten alloy wire. As for the adjustment, each of the above methods can be performed individually or in combination.
[0039] The content of rhenium contained in the ReW wire of the embodiment is, for example, 2% by weight or more and less than 30% by weight. In addition, the content of rhenium contained in the ReW wire of the embodiment is, for example, preferably 10% by weight or more and 28% by weight or less. The content of rhenium is a value analyzed by inductively coupled plasma-optical emission spectrometry (ICP-OES). Rhenium improves the elongation of tungsten at high temperatures and improves processability. In addition, strength is improved by solid solution strengthening.
[0040] When the rhenium content is less than 2% by weight, the effect is not sufficient. For example, when using a ReW wire with a rhenium content of less than 2% by weight as a raw material for a probe, the deformation of the completed probe increases with the frequency of use, resulting in poor contact and reduced semiconductor inspection accuracy. If the rhenium content becomes more than 30% by weight, it exceeds the solid solubility limit with tungsten, so it is impossible to diffuse and homogenize (solid dissolve) rhenium in the tungsten matrix. As a result, it is possible to produce a phase region (segregation phase of σ phase) with a locally high rhenium composition ratio. When such a part appears on the surface, it is easy to discolor.
[0041] When ReW wire having a rhenium content of 2 wt% or more and less than 30 wt% is used as a raw material to manufacture a probe or a medical needle, discoloration can be suppressed, and high yield can be achieved. In addition, the mechanical properties (strength, wear resistance) of the manufactured probe or medical needle can be ensured. The rhenium content is preferably 10 wt% or more and 28 wt% or less, for example.
[0042] The ReW wire of the embodiment may contain 30 wtppm or more and 90 wtppm or less of potassium (K) as a doping material. The potassium content is a value analyzed by inductively coupled plasma optical emission spectrometry (ICP-OES). By containing potassium, the tensile strength and creep strength at high temperatures are improved by utilizing the doping effect.
[0043] When the potassium content is less than 30 wtppm, the doping effect becomes insufficient. If the potassium content exceeds 90 wtppm, the processability is reduced, and the yield rate may be greatly reduced. By containing 30 wtppm or more and 90 wtppm or less of potassium as a dopant, for example, a thin wire for a thermocouple or an electron tube heater using the ReW wire of the embodiment as a raw material can be produced with a high yield while ensuring high temperature characteristics (preventing wire breakage and deformation during high temperature use).
[0044] The ReW wire according to the embodiment has a diameter of, for example, 0.1 mm or more and 1.00 mm or less.
[0045] The ReW wire of this embodiment suppresses surface discoloration, greatly contributing to long-term storage and improved yield. In addition, the ReW wire of the embodiment can be applied to medical needles. In addition, it can also be applied to ReW wire applications for thermocouples and probes.
[0046] Next, a method for producing the ReW wire according to the embodiment will be described. The production method is not particularly limited, and examples thereof include the following methods.
[0047] The tungsten powder and the rhenium powder are mixed so that the rhenium content is 2% by weight or more and less than 30% by weight. There is no particular limitation on the mixing method, but a method of mixing the powders in a slurry state using water or an alcohol solution is particularly preferred in order to obtain a powder with good dispersibility. In addition, in order to ensure the homogeneity of the powder batch, it is more preferred to dry-mix the same powder batch after drying the slurry.
[0048] The mixed rhenium powder preferably has an average particle size of less than 8 μm. The particle size distribution preferably has an SD value of less than 11 μm. Figure 5 An explanatory diagram of the particle size distribution is shown in . The horizontal axis is the particle size (μm), the left vertical axis is the frequency (%), and the right vertical axis is the cumulative (%). The SD value is the value obtained by SD = (d(84%) - d(16%)) / 2 when d(84%) is set as the cumulative particle size of 84% and d(16%) is set as the cumulative particle size of 16%, and becomes an indicator of the distribution width of the measured particle size. In addition, the particle size distribution is measured by the laser diffraction method. As for the amount of powder used in one measurement, it is set to be carried out with the amount recommended by the measuring device. Generally, 0.02g is recommended. In addition, the measurement sample is set to be fully stirred before measurement and then measured.
[0049] The tungsten powder is a pure tungsten powder from which inevitable impurities are removed or a doped tungsten powder containing potassium (K) in an amount that takes into account the yield of the wire. The tungsten powder preferably has an average particle size of less than 16 μm. The particle size distribution preferably has an SD value of less than 13 μm. When the average particle size of the rhenium powder is 8 μm or more, when the SD value of the rhenium powder is 11 μm or more, when the average particle size of the tungsten powder is 16 μm or more, or when the SD value of the tungsten powder is 13 μm or more, the diffusion distance of the rhenium atoms or tungsten atoms used to diffuse and homogenize (solid solution) rhenium in the tungsten matrix increases, and the σ phase is easily generated.
[0050] The ratio of the average particle size of the rhenium powder to the average particle size of the tungsten powder (Re average particle size / W average particle size) is preferably 0.4 or more and 2.0 or less. When the ratio of the average particle size of the rhenium powder to the average particle size of the tungsten powder is less than 0.4 or exceeds 2.0, the diffusion distance of the rhenium atoms to the center of the tungsten particles or the diffusion distance of the tungsten atoms to the center of the rhenium particles becomes longer, and there is a possibility that the σ phase is easily generated.
[0051] Next, the mixed powder is placed in a specified mold for compression molding. The compression pressure at this time is preferably 150 MPa or more. For the molded body, in order to facilitate handling, a pre-sintering treatment can be performed at 1200-1400°C in a hydrogen furnace. The obtained molded body is sintered in a hydrogen atmosphere, or in an inert gas atmosphere such as argon, or in a vacuum. The sintering temperature is preferably above 2500°C. When the sintering temperature is less than 2500°C, the diffusion of rhenium atoms and tungsten atoms is not fully carried out during sintering. The upper limit of the sintering temperature is 3400°C (the melting point of tungsten is below 3422°C).
[0052] The relative density of the sintered body (relative density (%) relative to the true density = [sintered body density / true density] × 100%) is preferably 90% or more. In addition, in one sintered body, for example, the ratio of the density of the lowest part such as the lower end during the current sintering to the average density of the entire sintered body is preferably 0.98 or more. By making the relative density of the sintered body 90% or more and making the ratio of the density of the lowest part to the average density of the entire sintered body 0.98 or more, the fluctuation of the rhenium content can be suppressed.
[0053] The sintered body obtained in the main sintering step is subjected to a first swaging process. The first swaging process is preferably performed at a heating temperature of 1300 to 1600° C. The reduction rate of the cross-sectional area (reduction rate) by the first heating treatment (first heating) is preferably 5 to 15%.
[0054] Rolling may be performed instead of the first rotary forging process. The rolling process is preferably performed at a heating temperature of 1200 to 1600°C. The surface reduction rate in the first heating is preferably 40 to 75%. As a rolling mill, a double-roll rolling mill, a four-roll rolling mill, a die roll rolling mill, etc. can be used. The manufacturing efficiency can be greatly improved by rolling. The first rotary forging (SW) process can be combined with the rolling process.
[0055] The sintered body (ReW rod) that has been subjected to the first rotary swaging, rolling, or a combination of the first rotary swaging and rolling is subjected to the second rotary swaging (SW) process. The second rotary swaging process is preferably performed at a heating temperature of 1200 to 1500° C. The area reduction rate in the first heating (first heating) is preferably about 5 to 20%.
[0056] The ReW rod that has completed the second rotary forging step is then subjected to a recrystallization treatment, which can be performed, for example, using a high-frequency heating device in a hydrogen atmosphere, an inert gas atmosphere such as argon, or a vacuum, at a treatment temperature in the range of 1800 to 2600°C.
[0057] The third rotary forging process is performed on the ReW rod that has completed the recrystallization treatment. The third rotary forging process is preferably performed at a heating temperature of 1200 to 1500°C. The surface reduction rate in the first heating is preferably about 10 to 30%. The third rotary forging process is performed until the ReW rod has a diameter that can be processed by wire drawing (preferably a diameter of 2 to 4 mm).
[0058] For the ReW rod that has completed the third rotary forging process, in order to smoothly carry out the wire drawing (DW: drawing) process, a lubricant is applied to the surface and the lubricant is dried. For the wire drawing process, the application of the lubricant, the drying of the lubricant, the heating to a processable temperature, and the drawing process using a drawing die are repeated. As for the lubricant, it is preferred to use a carbon (C)-based lubricant with excellent heat resistance. The processing temperature is set according to the wire diameter of the wire drawing process. The processing temperature is preferably below 1100°C, for example. The surface reduction rate of each die is preferably 10 to 35%. In the middle of the wire drawing process, an annealing process and a surface grinding process (such as an electrolysis process) may be added under known conditions as needed.
[0059] The ReW wire that has completed the wire drawing process is ground. For example, the grinding process includes electrochemical grinding (electrolytic grinding) in a sodium hydroxide aqueous solution with a concentration of 3 to 15% by weight. The surface reduction rate in the grinding process is preferably 10 to 25%. In the case of less than 10%, it may not be possible to remove the mixture of the unevenness on the material surface generated in the rotary forging process and the wire drawing process and the unevenness attached to the material surface. In the case of insufficient surface removal, the mixture layer remains locally, so the presence ratio of rhenium may increase. If it exceeds 25%, the material yield deteriorates.
[0060] In the case of electrolytic polishing, the polishing speed is preferably 0.5 to 3.0 μm / second. If it is slower than 0.5 μm / second, the tungsten on the surface may be preferentially dissolved, and the presence ratio of rhenium on the surface may increase. If it exceeds 3.0 μm / second, the amount of electrolysis per unit time may increase, resulting in rapid electrolysis, and the correction of the cross-sectional shape of the ReW line may become insufficient. For the ReW line after electrolytic polishing, in order to remove the alkali metals, carbon, etc. remaining on the surface, it is cleaned. The cleaning water is preferably pure water with a conductivity of less than 1 μS / cm. In addition, ultrasonic cleaning can be used in combination.
[0061] For the ReW wire that has completed the grinding process, for example, a drying process can be performed. The drying process is carried out, for example, in a vacuum dryer with the temperature inside the box set to a range of 50 to 80°C. The drying time is, for example, more than 1 hour. Then, a prescribed delivery inspection is carried out. When storing the ReW wire after vacuum drying, for example, by placing it in a moisture-proof storage box with a relative humidity of less than 5%, it is possible to prevent the adsorption of moisture. For example, except for the case of performing characteristic and quantity inspections, the ReW wire is placed in the moisture-proof storage box and stored.
[0062] The ReW wire is wound around a reel for shipping, for example, while undergoing a shipping inspection. For the ReW wire that has been inspected for shipping, the outermost surface of the reel for shipping is covered with a protective paper, for example, and fixed with a rubber band or the like. Then, for example, according to the capacity of the aluminum bag, the necessary amount of ammonia adsorbent (for example, SiO2 as the main component) is placed in an aluminum bag, and a degassing treatment is performed to an extent that no tension is applied to the aluminum bag, and the bag is sealed.
[0063] By using an appropriate amount of the ReW wire obtained in the above-mentioned steps and carrying out necessary steps under known conditions, a probe or medical needle having a predetermined wire diameter and necessary properties (strength, hardness, etc.) can be obtained.
[0064] (Example 1)
[0065] A doped tungsten powder having an average particle size of 13 μm and an SD value of 12 μm, containing potassium (K) in an amount of 50 to 80 wtppm in the final wire, and a rhenium powder having an average particle size of 6 μm and an SD value of 7 μm were mixed in a slurry state using an alcohol solution so that the rhenium content was 3 wt%. The obtained slurry was dried to obtain a raw material powder.
[0066] The mixed powder of the raw materials is pressed into a molded body. The molded body is subjected to a pre-sintering treatment at 1300°C in a hydrogen furnace. The molded body is sintered at 3000°C in a hydrogen atmosphere to obtain a sintered body. The sintered body is subjected to a first rotary forging process by heating to a temperature of 1400°C and a reduction rate of 14% in the cross-sectional area of the first heating treatment process. The sintered body subjected to the first rotary forging process is subjected to a second rotary forging process by heating to a temperature of 1300°C and a reduction rate of 15% in the cross-sectional area of the first heating treatment process.
[0067] The ReW rod after the second rotary forging was subjected to recrystallization treatment in a hydrogen atmosphere at a treatment temperature of 2400° C. After the recrystallization treatment, the third rotary forging was performed at a heating temperature of 1300° C. and a cross-sectional area reduction rate of 13% in the first heating treatment, thereby obtaining a rod with a diameter of 2.5 mm.
[0068] A lubricant is applied to the surface of the rod material subjected to the third rotary forging process and dried. The obtained rod material is subjected to wire drawing. The wire drawing process is performed at 1000° C. so that the reduction rate of the cross-sectional area in the first drawing process becomes 10% to 35%. During the wire drawing process, an annealing process is performed at 1300° C.
[0069] The ReW wire that has been drawn is electrolytically polished in an aqueous sodium hydroxide solution with a concentration of 8 wt%. The electrolytic polishing process is performed with a cross-sectional area reduction rate of 15 to 20% and a polishing speed of 2.2 μm / sec. After electrolytic polishing, the ReW wire is washed with pure water with an electrical conductivity of 1 μS / cm. The wire diameter of the obtained ReW wire is 0.8 mm.
[0070] After electrolytic grinding, ReW was dried for 2 hours in a vacuum dryer at 70°C and then stored in a moisture-proof storage box with a relative humidity of 5% or less. The obtained ReW wire was wound on a 100m / reel shipping reel, the outermost surface was covered with protective paper and fixed with a rubber band. The shipping reel on which the ReW wire was wound was placed in an aluminum bag together with an ammonia adsorbent containing SiO2 as the main component, and the aluminum bag was degassed to the extent that no tension was applied to it, and then sealed.
[0071] Three rolls were made from the same roll, and the three roll samples were placed on a 1m high platform in a room with a humidity of less than 60% and a room temperature of less than 30°C and stored side by side for 13 months. Figure 3 The presence or absence of color change was confirmed by the difference between the maximum value and the minimum value of the reflectance in the wavelength range of 400 nm to 700 nm in the reflectance spectrum described above.
[0072] (Example 2)
[0073] The ReW wire was produced in the same manner as in Example 1 except that the raw material tungsten powder was not doped with potassium, the ratio of rhenium was set to 26% by weight, and the wire diameter of the final ReW wire was set to 0.15 mm, and was wound on a 500 m / reel shipping reel, and stored in an aluminum bag together with the ammonia adsorbent using the same packaging method as in Example 1. As in Example 1, three reels were produced for the same reel, and the reels were stored for 13 months using the same method as in Example 1. After 13 months, the presence or absence of discoloration was confirmed.
[0074] (Example 3)
[0075] Using the same raw material powder as in Example 1, the same steps as in Example 1 were carried out until the wire drawing process to manufacture a ReW wire. For the obtained ReW wire, an electrolytic grinding process was carried out at a grinding speed of 4.0 μm / second. After the electrolytic grinding process, it was not stored in a moisture-proof storage box. Except for this, a ReW wire with a wire diameter of 0.8 mm was obtained by the same method as in Example 1. The obtained ReW wire was wound on a shipping reel of 100 m / reel, the outermost surface was covered with protective paper, and fixed with a rubber band. The shipping reel on which the ReW wire was wound was placed in an aluminum bag together with a desiccant containing silica gel, and the aluminum bag was vacuum degassed and sealed. For the same reel, 3 reels were made and stored for 13 months using the same method as in Example 1. After 13 months, the presence or absence of discoloration was confirmed.
[0076] (Comparative Example 2)
[0077] The same raw material powder as in Example 2 was used, and the same steps as in Example 2 were performed until the wire drawing process to manufacture a ReW wire. The obtained ReW wire was subjected to an electrolytic polishing process at a polishing speed of 4.0 μm / sec, and a ReW wire having a wire diameter of 0.15 mm was obtained by the same method as in Example 2, except that the wire was not stored in a moisture-proof storage box after the electrolytic polishing process. The obtained ReW wire was wound on a 500 m / reel shipping reel and packaged by the same method as in Example 3. Three reels were made for the same reel, and the same method as in Example 1 was used to store the reels for 13 months. After 13 months, the presence or absence of discoloration was confirmed.
[0078] (Example 4)
[0079] ReW wire was manufactured in the same manner as in Example 2 and wound on a 500 m / reel shipping reel. The shipping reel of Example 4 was placed in an aluminum bag together with a desiccant containing silica gel, and the aluminum bag was vacuum degassed and sealed. Three reels were manufactured for the same reel and stored for 13 months in the same manner as in Example 1. After 13 months, the presence or absence of discoloration was confirmed.
[0080] Table 3 shows the measurement results of rhenium content, potassium content and NH4 content. The analysis of rhenium content and potassium content was carried out by inductively coupled plasma optical emission spectrometry (ICP-OES). In addition, the lower detection limit of potassium is 5 ppm by weight, and the case where there is no addition and the analysis value is less than 5 ppm by weight is recorded as "-". As for the NH4 amount, 0.5 g of alloy wire was extracted with hot water in 50 ml of pure water and measured by ion chromatography. The device used was ICS-2000 manufactured by Thermo Fischer Scientific Co., Ltd.
[0081] [Table 3]
[0082]
[0083] As can be seen from Table 3, the ReW wire according to the embodiment can suppress discoloration even during long-term storage, and can significantly improve the yield when used as a probe or a medical needle.
[0084] In Examples 1-4, in which the amount of NH4 on the wire surface of at least one of the three reels was less than 10 mass ppm, discoloration after long-term storage was suppressed. In Comparative Example 2, in which the amount of NH4 on the wire surface of all three reels exceeded 10 mass ppm, discoloration occurred due to long-term storage. It is inevitable that there will be some deviations in the amount of moisture or ammonia adsorbed in the working environment from the electrolytic polishing process to the aluminum bag. It is speculated that Example 3 and Comparative Example 2 are easily affected by the deviation in the amount of moisture or ammonia adsorbed. This is believed to be because, in Example 3 and Comparative Example 2, the electrolytic polishing speed was set to 4.0 μm / sec, and in addition, it was not stored in a moisture-proof storage box, and no ammonia adsorbent was used.
[0085] Several embodiments of the present invention are illustrated above, but these embodiments are presented as examples and are not intended to limit the scope of the invention. These new embodiments can be implemented in various other forms, and various omissions, substitutions, changes, etc. can be made without departing from the scope of the main purpose of the invention. The modified examples of these embodiments are included in the scope and main purpose of the invention, and are also included in the invention recorded in the patent claims and the scope equivalent thereto. In addition, the above-mentioned embodiments can be implemented in combination with each other.
[0086] The invention according to the embodiment will be described below.
[0087] <1> The rhenium-tungsten alloy wire is a wire composed of a tungsten alloy containing rhenium, and the amount of NH 4 on the surface of the wire calculated by: NH 4 ion weight on the wire surface / alloy wire weight is 10 mass ppm or less.
[0088] <2> The rhenium tungsten alloy wire according to <1>, wherein a content of the rhenium is 2% by weight or more and less than 30% by weight.
[0089] <3> The rhenium tungsten alloy wire according to <1>, wherein a content of the rhenium is 10 wt % or more and 28 wt % or less.
[0090] <4> The rhenium tungsten alloy wire according to any one of <1> to <3>, wherein a potassium (K) content is 30 wtppm or more and 90 wtppm or less.
[0091] <5> The rhenium tungsten alloy wire according to any one of <1> to <4>, wherein the diameter is 0.1 mm or more and 1.00 mm or less.
[0092] <6> The rhenium tungsten alloy wire according to any one of <1> to <5>, which is used as a wire material for a medical needle.
[0093] <7> The rhenium tungsten alloy wire according to any one of <1> to <5>, which is used as a wire material of a probe.
[0094] <8> The method for producing a rhenium-tungsten alloy wire according to any one of <1> to <7>.
[0095] <9> A medical needle using the rhenium tungsten alloy wire according to any one of <1> to <5>. <10> A probe using the rhenium tungsten alloy wire according to any one of <1> to <5>.
[0096] Description of Reference Numerals
[0097] A…Undiscolored part
[0098] B…Discoloration
[0099] X…Sample Reel
[0100] Y…Mesh table
[0101] Z…Container
[0102] A(CW)…Sample with discoloration
[0103] B(NW)…Sample without discoloration
Claims
1. Rhenium tungsten alloy wire is a wire composed of a tungsten alloy containing rhenium, and the amount of NH4 on the surface of the wire calculated by the weight of NH4 ions on the surface of the wire / the weight of the alloy wire is 10 mass ppm or less.
2. The rhenium-tungsten alloy wire according to claim 1, wherein: The rhenium content is 2% by weight or more and less than 30% by weight.
3. The rhenium-tungsten alloy wire according to claim 1, wherein: The rhenium content is 10 wt % or more and 28 wt % or less.
4. The rhenium-tungsten alloy wire according to claim 1, wherein: The potassium (K) content is 30 wtppm or more and 90 wtppm or less.
5. The rhenium-tungsten alloy wire according to claim 1, wherein: The diameter is 0.1 mm or more and 1.00 mm or less. The rhenium tungsten alloy wire according to any one of claims 1 to 5, which is used as a wire material for a medical needle. 7 . The rhenium-tungsten alloy wire according to claim 1 , which is used as a wire material of a probe. 8 . The method for producing the rhenium-tungsten alloy wire according to claim 1 . 9 . A medical needle using the rhenium tungsten alloy wire according to claim 1 . 10 . A probe using the rhenium-tungsten alloy wire according to claim 1 .