Foam assisted application of uncured starch and dry strength agent to paper products
By using foam-assisted addition technology of unripened starch and dry strength additives in the papermaking process, the problems of uneven distribution and low cost efficiency of traditional wet end additives are solved, and the in-plane and Z-direction stretch of multi-layer paper sheets are significantly improved. Strength and interlayer bonding effect.
Patent Information
- Application Number
- CN202280085599.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-11-22
- Filing Date
- 2022-11-24
- Publication Date
- 2024-10-15
AI Technical Summary
Traditional wet-end additives have problems with uneven additive distribution, low cost efficiency and poor layer adhesion efficiency in the papermaking process. Especially in the production of multi-layer paper sheets, it is difficult to effectively improve the in-plane and Z-direction tensile strength.
By creating a foam of unripened starch and dry strength agent, which is applied to the wet paper web, vacuum pressure is used to retain the particles of unripened starch on the surface of the paper web, and dry strength agent molecules are introduced to improve the internal bonding of the paper. and intensity.
It achieves better additive retention and distribution, increases the in-plane and Z-direction tensile strength of the paper, enhances inter-layer bonding, reduces production costs, and improves layer bonding efficiency.
Smart Images

Figure HDA0004907916700000011 
Figure HDA0004907916700000021 
Figure HDA0004907916700000031
Abstract
Description
Technical Field
[0001] The present invention relates to the field of applying additives to wet paper webs. More specifically, the present invention relates to applying unripened starch and synthetic, bio-based or natural strength agents to a newly formed wet paper web using foam application technology in the production of multi-ply paperboard. Background Art
[0002] In papermaking, additives are introduced into the papermaking process to improve paper properties. For example, known additives increase paper strength, drainage properties, retention properties, etc.
[0003] In a conventional paper machine, pulp is prepared for papermaking in a stock preparation system. From time to time, chemical additives, dyes, and fillers are added to the thick stock section of the stock preparation system, which operates at a consistency of 2.5 to 5% dry solids; the additives may be added to the mixing chest, the machine chest, the pulp suction device associated with one of these chests, or other locations. In the thin stock loop of the stock preparation system, the pulp is diluted from a consistency of 2.5 to 3.5% dry solids to a consistency of 0.5 to 1.0% dry solids before passing through the thin stock cleaner, screen, optional degassing system, and feed pipe. During or after this dilution, additional chemical additives may be added to the pulp in the pump suction device or in the headbox feed pipe. The addition of chemical additives in the thick or thin stock section of the stock preparation system will be considered as "wet end addition" as used herein.
[0004] A well-prepared slurry, typically at a consistency of 0.5 to 1.0% dry solids, is pumped to a headbox, which discharges the slurry onto a moving, continuous forming fabric. The forming fabric may be in the form of a woven mesh screen. When traveling from the headbox to the press section, water is drained through the forming fabric while the fibers remain on the forming fabric to form an embryonic web. As the water is drained away, the moisture content of the embryonic web may drop from 99 to 99.5% water to 70 to 80% water. The water may be further removed by pressing the wet web with a roll press in the press section, and the wet web exiting the roll press may contain only 50 to 60% water (i.e., a consistency of 40 to 50% dry solids). Water is further removed from the web, typically by evaporation in the dryer section, and the web exiting the dryer section may have a consistency of 90 to 94% dry solids. The sheet may then be calendered to improve the surface smoothness of the sheet and control the sheet thickness or density to a target value. The sheets are then typically collected on reels.
[0005] As explained above, chemical additives such as strength agents can be introduced into the pulp in the stock preparation section, which is called "wet-end addition". In some cases, strength agents can also be added by spraying onto the wet paper web in the forming section or applying the additives to the dry paper sheet using a size press. Spray application of additives and size press addition are optional.
[0006] In wet-end application, the chemical additive is distributed throughout the paper web, and the retention of the chemical additive varies depending on the papermaking system and the chemistry being applied. There are other factors to consider when applying additives in the wet end, such as deposits on the forming fabric and other surfaces in the forming section, and potential circulation problems (wet-end additives can accumulate in the circulating water due to poor fixation of the additives to the fibers). Spray application can be somewhat problematic due to accumulation of excess spray on nearby surfaces and clogging of nozzles. Size press application is not performed in the wet end of the paper machine and does not have the advantages of applying chemicals to the wet sheet before or during forming.
[0007] Furthermore, chemical additives applied by conventional wet-end application typically provide a relatively uniform distribution of additive across the Z-direction of the paper web, which may be desirable or may result in less additive than expected in certain Z-direction locations within the paper sheet. Thus, the wet-end approach is not targeted and may result in somewhat cost-inefficient chemical application.
[0008] Specifically, some paperboard products are formed by multiple layers. Each layer can advantageously be composed of different types of fibers. This can improve the performance of the paper or for cost-saving reasons. In a three-layer paper sheet, each layer can be determined as a top layer (usually the preferred printing side), an intermediate layer, and a back layer, which can be printed or not. Usually, due to unbleaching or due to insufficient refining or due to fiber material or pulp production process, the fibers used in the intermediate layer may be lower in cost or larger in volume, while the fibers in the top layer may be brighter and can produce a smoother printable surface. The back layer may be between the top layer and the intermediate layer in terms of cost and characteristics, or if both sides are to be printed, it may be very similar to the top layer. Usually, the mass per unit area of the top layer and the back layer is minimized to reduce the total cost. Usually, the mass per unit area of the intermediate layer is greater than that of the top layer or the back layer, especially when the paper sheet is extremely thick. Usually, all broken paper (broke) from the production process is sent to the intermediate layer to maintain the appearance and printing quality of the top layer, and in some cases, the appearance and printing quality of the back layer is also maintained.
[0009] There are many methods of producing paper sheets with different stock characteristics in the various layers, including specialized headboxes with separate inlets for the separate stock materials and vanes within the headbox that keep the materials separate until they are discharged from the headbox to the forming fabric. This method is sometimes referred to as "wet-on-wet" forming and has been known to those skilled in the art for at least 35 years. This forming technique produces very good bonding between the layers, but the layer purity is not as good as would be preferred and the drain water from the different layers often mixes, which can cause some process problems when the drain water in the forming section is reused. This is especially true when there is a large difference in brightness between the top layer or top and back layers relative to the middle layers.
[0010] Another method well known to those skilled in the art is to use an auxiliary headbox which applies the top layer to the base or center layer when the base or center layer on the forming table is about 8% to 10% solids. This method is sometimes called "wet-on-dry" multilayer forming because the base or center layer is partially dewatered before the very low consistency slurry that will become the top layer is applied. This forming technique generally provides better layer purity and fairly good adhesion between layers, but when the combined sheets are drained, the water from the top layer will still mix somewhat with the water from the base or center layer. The auxiliary headbox method of forming multi-layer (usually two-layer) sheets has also been widely practiced for many years.
[0011] Another widely practiced method of forming a multi-layer paper sheet is to produce the top layer on a paper forming machine and the middle layer on a second paper forming machine. Sometimes, multiple middle layers can be produced on multiple separate paper forming machines. A separate paper forming machine can be used to produce the bottom layer. The layers with a solid content of about 8 to 12% are bonded together by gently pressing one layer into another using a "combining roller", after which the combined paper sheet can be further dewatered by applying additional vacuum to the combined paper sheet. This paper forming section is well known to those skilled in the art, and the technology can be called "dry-on-dry" forming because before the layers are combined, they are separately dewatered to a solid content of 8 to 12%. This forming method can produce excellent layer purity and can also provide optimal separation of the water systems of the mentioned layers. It is also known to those skilled in the art that the "dry-on-dry" forming technology has poor bonding efficiency between the layers, which sometimes leads to delamination of the layer bonding areas during printing.
[0012] The ply bonding of multi-ply formed paper sheets, particularly "dry-on-dry" formed multi-ply paper sheets, can be improved by spraying a suspension of unripened starch on one of the ply surfaces where ply bonding is inadequate. The unripened starch is in the form of small particles which are retained on the ply application surface by filtration. The particles of unripened starch will absorb water over time, particularly when the sheet is heated to elevated temperatures in the dryer section, and in sufficient moisture and temperature will gel and form adhesive bonds between ply fibers with which it contacts, thereby improving ply bonding.
[0013] It should be understood that if a multi-ply paper sheet is to be provided with a unique stock composition for different layers, a separate stock preparation system is required for each layer. The need for separate top, middle and back layer stock preparation and forming sections makes this multi-ply paper sheet forming method complicated and expensive compared to a paper sheet having only one layer or having two or more layers of uniform composition.
[0014] It would be desirable to further improve paper strength parameters related to bonding, such as in-plane and Z-direction tensile strength. Summary of the invention
[0015] This Summary introduces some concepts in a simplified form that are further described below in the Detailed Description.
[0016] In one exemplary embodiment, a method for making a multi-layer paper sheet is provided. The method includes: generating a foam of water, air, a foaming agent, unripened starch, and a dry strength agent; applying the foam to a first surface of a base embryonic ply, wherein the base embryonic ply has a second surface opposite to the first surface; providing an applied embryonic ply having a first surface and an opposite second surface and contacting the first surface of the base embryonic ply with the first surface of the applied embryonic ply at an interface to form a combined layer web; and selectively applying vacuum pressure to the second surface of the base embryonic ply to retain particles of unripened starch on or near the first surface of the base embryonic ply, thereby drawing dry strength agent molecules into the base embryonic ply and / or applying to the first surface of the applied embryonic ply to retain particles of unripened starch in the interface and draw dry strength agent molecules into the applied embryonic ply.
[0017] In another exemplary embodiment, a method of introducing a dry strength agent into a multi-ply paper product is provided, comprising generating foam from a foaming formulation comprising: a foaming agent; unripened starch; a dry strength agent; and water; and applying the foam to a wet germ layer web.
[0018] In another exemplary embodiment, a multi-ply paper product is provided. The multi-ply paper product is made by the following steps: generating a foam of water, air, unripened starch, and a dry strength agent; applying the foam to a first surface of a base germ layer web, wherein the base germ layer web has a second surface opposite to the first surface; providing an application germ layer web having a first surface and an opposite second surface and contacting the first surface of the base germ layer web with the first surface of the application germ layer web at an interface to form a combined layer web; and selectively applying vacuum pressure to the second surface of the base germ layer web to retain particles of unripened starch on or near the first surface of the base germ layer web and introduce dry strength agent molecules into the base germ layer web and / or applying to the first surface of the application germ layer web to retain particles of unripened starch in the interface and introduce dry strength agent molecules into the application germ layer web.
[0019] Other desirable features will become apparent from the following detailed description and the appended claims, taken in conjunction with the drawings and this background. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The subject matter may be more fully understood from the following detailed description taken in conjunction with the accompanying drawings, wherein like reference numerals represent like elements, and wherein:
[0021] Figure 1 is a schematic diagram of a multi-layer papermaking apparatus according to various embodiments;
[0022] Figure 2 is a schematic diagram showing how a multilayer web may be constructed from individually formed layers according to various embodiments;
[0023] Figure 3 Graphing synthetic dry strength agent dose response curves for Scott bond strength values with and without unripened starch for a comparative embodiment and according to one embodiment of the embodiments herein;
[0024] Figure 4 Picture shows Figure 3 The relationship between the Scott bond break position in the middle layer or base layer and the dosage of the synthetic dry strength agent of the embodiment;
[0025] Figure 5 Graphs Scott bond strength for four synthetic dry strength agents, a comparative embodiment using only synthetic dry strength agents, and an embodiment according to embodiments herein using synthetic dry strength agents plus unripened starch;
[0026] Figure 6 Picture shows Figure 5 Scott bond break locations within the middle layer or base layer for embodiments using only synthetic dry strength agents and dry strength agents plus unripened starch for four synthetic dry strength agents;
[0027] Figure 7 Graphs show Z-direction tensile strength (ZDT) for four synthetic dry strength agents, a comparative embodiment using only a synthetic dry strength agent, and an embodiment according to embodiments herein using a dry strength agent plus unripened starch; and
[0028] Figure 8 Pictured Figure 5 Z-direction tensile strength (ZDT) split locations within the middle layer or base layer for four synthetic dry strength agents, a comparative embodiment using only synthetic dry strength agents, and using dry strength agents plus unripened starch. DETAILED DESCRIPTION
[0029] The following specific embodiments are illustrative only and are not intended to limit the embodiments of the subject matter or the application and use of these embodiments. As used herein, the word "exemplary" means "as an example, instance or illustration". Therefore, any embodiment described herein as "exemplary" does not necessarily need to be interpreted as preferred or superior to other embodiments. All embodiments described herein are exemplary embodiments, intended to enable those skilled in the art to make or use the systems and methods defined in the claims. In addition, the present invention is not intended to be bound by any express or implied theory presented in the aforementioned technical field, background technology, technical content or the following specific embodiments. For the sake of brevity, conventional techniques and compositions may not be described in detail herein.
[0030] Unless otherwise stated, "a", "an" or "the" as used herein means one or more. The term "or" can be conjunction or disjunction. Open terms such as "including", "comprising", "containing", "containing" and the like mean "comprising". The term "about" used with numerical values throughout the specification and claims represents an accuracy interval familiar to and accepted by those skilled in the art. Typically, this accuracy interval is ± ten percent. Therefore, "about ten" means nine to eleven. Unless otherwise expressly stated, all numerical values in this specification indicating amounts, material ratios, material physical properties and / or uses should be understood to be modified by the word "about". Unless otherwise stated, "%" as described in the present disclosure as used herein refers to weight percentage.
[0031] Embodiments of the present disclosure relate to the introduction of unripened starch and dry strength agents into a paper substrate via a foam-assisted application technique.
[0032] Applying the immature starch and dry strength agent to the wet paper web by foam application may be advantageous because while the chemicals are applied to the wet end like conventional methods, some of the typical disadvantages are avoided. Foam application can be expected to have better additive retention, thereby reducing or avoiding deposits, and application to the wet paper web surface allows some of the benefits of spray application to be achieved while still being able to penetrate into the web. Embodiments of foam application of immature starch and dry strength agent to the paper substrate have advantages in efficiency, cost, and targeted application compared to standard practice.
[0033] As described herein, unripened starch and dry strength agent are applied to the surface of the layer by foam. The foam is pulled into the web by vacuum or negative pressure, which can provide greater advantages than traditional methods. For example, compared with traditional wet end application, the consistency and surface application in the foam can be optimized to better retain in the web. In addition, the foam is easier to control and manage than spraying, and the foam does not cause the accumulation of spray component droplets on the surface during overspray. And, compared with the typical limitations of spraying application, it is possible to apply higher viscosity chemicals and higher concentrations of chemicals in the foam. In addition, application to the surface of the web allows fine-tuned penetration into the web and controlled distribution from one surface, rather than uniform distribution in the entire Z direction of the web. The exemplary embodiments of this article emphasize the synergistic effect of combining unripened starch with a dry strength agent (DSA) to achieve higher strength performance than when unripened starch or dry strength agent (i.e., not combined with each other) is used alone.
[0034] Exemplary embodiments herein introduce natural, bio-based or synthetic dry strength agents (hereinafter referred to as strength agents or dry strength agents) into multi-ply paper products.
[0035] The embodiments herein achieve improvements in paper strength properties and changes in the weakness of paper products through a new application method (foam-assisted additive addition of unripened starch and dry strength agent). By utilizing a process change of a combination of dry strength agent and unripened starch, strength improvements are achieved compared to the individual components. In addition, this application method allows for fine tuning of the split location in the paper sheet, which is difficult to do using conventional currently available methods.
[0036] Figure 1A schematic diagram of an apparatus 10 is shown for forming a three-layer paper sheet using the previously described "dry-on-dry" method, and for applying a foam formulation to a wet embryonic paper web. The apparatus 10 includes a middle layer stock preparation section 11b, which includes a middle layer thick stock circuit 12b and a middle layer thin stock circuit 13b. In the figure, the flow of the middle layer component stock 20b is shown using solid arrows. In one embodiment, the middle layer thick stock section 12b includes one or more middle layer refiners 21b, which are configured to improve fiber-fiber bonding in the middle layer thick stock component 20b by making the fibers of the middle layer thick stock component 20b more flexible and by increasing its surface area through mechanical action applied to the middle layer thick stock component 20b having a consistency of about 2.0 to 5.0% dry solids. In one embodiment, after the refiner, the middle layer thick stock component 20b enters the middle layer blending tank 22b. In the middle layer blending tank 22b, the stock component 20b can be optionally blended with one or more middle layer stock components 23b from other sources (e.g., broken paper). In addition, the stock component 20b can be blended with chemical additives 24b in the middle layer blending tank 22b. After leaving the middle layer blending tank 22b, the middle layer stock components 20b and 23b can be diluted by adding water 25b to control the consistency of the middle layer stock components 20b and 23b within a predetermined target range; the blended and consistency-adjusted middle layer stock can now be referred to as 26b. The middle layer stock 26b then enters the middle layer paper machine tank 27b, where additional chemical additives 28b can be added. In one embodiment, as the stock exits the middle layer machine pool 27b, the middle layer stock 26b is diluted with a large amount of water 29b to control the consistency of the middle layer stock 26b to be about 0.5 to 1.0% dry solids when the middle layer stock 26b exits the middle layer thick stock circuit 12b. The middle layer stock 26b having a consistency of 0.5 to 1.0% dry solids when entering the middle layer thin stock circuit 13b can now be referred to as 30b.
[0037] In an exemplary embodiment, within the middle layer thin stock loop 13b, the middle layer slurry 30b can pass through a low consistency cleaning, screening and degassing device. In an exemplary embodiment, additional chemical additives 32b can be added to the slurry 30b at any number of locations within the middle layer cleaning, screening and degassing area 31b, such as at location 32b and at location 33b in the feed flow conduit 34b leading to the middle layer forming section 35b. When the middle layer slurry 30b enters the middle layer forming section 35b, it can now be referred to as 37b. In an exemplary embodiment, in the middle layer forming section 35b, the middle layer headbox 36b distributes the middle layer slurry 37b onto a moving woven fabric (middle layer "forming fabric") 40b. In an exemplary embodiment, the middle layer forming fabric 40b delivers the middle layer slurry 37b to one or more boxes of hydrofoils 41b, which are used to remove water from the middle layer slurry 37b, thereby increasing the consistency of the slurry 37b to form an embryonic middle layer paper web 42b. In an exemplary embodiment, when the consistency of the embryonic middle layer paper web 42b is 2% to 3% dry solids, the paper web 42b then passes through one or more low vacuum boxes 43b, which are configured to apply a "low" vacuum to the embryonic middle layer paper web 42b to remove additional water from the paper web. The embryonic middle layer paper web 42b can also be further dewatered by an optional additional dewatering unit 44b installed above the middle layer forming fabric 40b. The embryonic middle layer paper web 42b can then pass through one or more "high" vacuum boxes 45b, where a higher vacuum (i.e., a stronger negative pressure) force will remove additional water until the consistency of the paper web 42b reaches 6% to 12% dry solids. The wet middle layer web, no longer in embryonic form, is now referred to as 46b.
[0038] In an exemplary embodiment, unripened starch 50b, one or more dry strength agents 51b, and foaming agent 52b (if required) (collectively referred to as foaming formulation 53b) are mixed with gas 54b (usually air) in a middle layer foam generator 55b to produce foam 56b. In an exemplary embodiment, after the gas 54b is incorporated into the foaming formulation 53b, the resulting middle layer foam 56b is transported to a middle layer foam dispenser 58b via a pipe or hose 57b, where the middle layer foam 56b is applied to a wet middle layer paper web 46b. In an exemplary embodiment, the foam 56b is applied between the high vacuum box 45b and the post-application high vacuum box 47b. The vacuum generated by the high vacuum box 47b after the foam is applied introduces the foam 56b into the wet middle layer paper web 46b. Due to the influence of the vacuum of the high vacuum box 47b, the consistency of the foam-coated and vacuum-treated middle layer paper web (now referred to as 48b) is also generally slightly higher, at 8% to 12%.
[0039] The above describes the middle layer production capability of the apparatus 10 (middle layer stock preparation system 11b, middle layer paper forming system 35b and middle layer foam addition system 53b-58b). It works in conjunction with the top layer former 35a and the base layer former 35c (equivalent to the middle layer former 35b). The top layer former 35c and the back layer former are composed of the corresponding top layer and back layer stock preparation systems ( Figure 1 The top layer wet paper web 48a produced by the top layer former 35a is combined with the middle layer wet paper web 48b by the combining roller 60b, and the combining roller 60b transfers the wet middle layer paper web to the top layer wet paper web on the top layer forming fabric 40a between the initial high vacuum box 45a and the final top layer high vacuum box 47a.
[0040] The wet top layer 48a and the wet middle layer 48b (referred to as 61 when combined) are transferred to the wet back layer web 48c by the combining roll 60c, which presses the combined wet top and middle layer web 61 to the wet back layer web 48c immediately after the back layer high vacuum box 45c and before the back layer subsequent high vacuum box 47c on the back layer former 35c. Web 71 is composed of the combined wet top layer web 48a, the wet middle layer web 48b and the wet back layer web 48c. The combined wet web 71 can be further dewatered to about 20 to 25% solids by the additional high vacuum box 47c on the back layer former 35c, and is now referred to as 72.
[0041] The combined web 72 enters a press section 80 where press rolls squeeze additional water from the wet web 72. The wet web 72 exits the press section at a consistency of about 40 to 55% dry solids and is referred to as web 73. The wet web 73 enters a dryer section 81 where the web 73 is heated by a heated dryer drum and additional water is evaporated from the web 73. The heat from the dryer and the remaining moisture in the wet sheet swell the particles of unripened starch which form a gel and adhere the top layer 48a to the middle layer 48b as the wet layer continues to dry. The wet web 73 is dried in the dryer section to a consistency of 6 to 10% (90 to 94% dry matter) and is now referred to as a dry sheet 74. After the dryer section 81, the dry web 74 may go directly to a calender 84 and reel 85, or may be treated with a surface sizing agent in an optional size press 82; if so treated, it is then dried again with an additional dryer 83. After the drying section 81 or optional size press 82 and additional dryer 83 , the paper sheet 74 may be treated with a calender 84 to improve surface smoothness and control sheet thickness and may then be taken up by a reel 85 .
[0042] It should be understood that the description of the middle layer stock preparation system 11b and the middle layer former 35b for producing the wet middle layer paper web 48b is also applicable to the top and back layer stock preparation systems ( Figure 235c). In addition, the description of the middle layer forming section 35b is also a good general description of the top layer forming section 35a and the back layer forming section 35c, respectively. Each numbered item in each web forming system is numbered correspondingly, with the components of the middle layer forming system 35b using the suffix "b", the corresponding numbered components of the top layer system using the suffix "a", and the corresponding numbered components of the back layer forming system 35c using the suffix "c". For example, the top layer headbox 36a corresponds to the middle layer headbox 36b and the back layer headbox 36c, and so on.
[0043] It is also clearly understood by those skilled in the art that many variations of the details may vary from one manufacturing plant location to another, but the same objectives are achieved, and therefore these variations are considered to be part of the system described and claimed herein. For example, the intermediate layer slurry preparation thick slurry system 12b shows a refiner that acts on the slurry component 20b but does not act on one or more additional slurry components 23b. In some cases, other slurry components may be blended with the slurry component 20b before the refiner 21b and refined together with the slurry component 20b. Before adding the foamed paper additive 56b, there may be fewer or more foil boxes 41b, low vacuum boxes 43b or high vacuum boxes 45b. For example, the additional dewatering step 44b is determined to be optional. The foam dispenser 58b can advantageously apply the foam 56b at any accessible position after the first low vacuum box 43b and before the last high vacuum box 45b. In some embodiments, there may be only two layers, while in other embodiments, there may be three or more layers. Foam can be advantageously applied between any two adjacent layers to enhance layer bonding and other Z-direction strength properties. The combination of size press 82 and additional dryer 83 is likewise shown as optional within the scope of the system described herein, ie, they may be present in some cases and may not be present in other cases. Many other similar variations are possible within the scope of the system described herein.
[0044] It has been unexpectedly discovered that applying unripened starch and dry strength agent by foam-assisted addition technology improves (or in some cases, at least performs equivalently) the bonding-related strength properties of a multi-ply paper product compared to a multi-ply paper product to which the dry strength agent is added by wet-end addition and the unripened starch is added via spraying. Foaming agents were previously known to reduce paper strength properties because they disrupt the bonds between pulp fibers. However, when a dry strength agent is added with foam, the negative effects of the foaming agent may be reduced or the bond strength may be significantly improved.
[0045] Additionally, adjusting process variables (the amount of wet foam coating per unit sheet area, the time and intensity of vacuum application before and after the addition of the foaming additive, layer thickness, % dry solids of the layer when the foaming additive is applied, and many other variables) can change the distribution of the dry strength agent. This can select for a more uniform distribution of the dry strength agent within the sheet, or a higher concentration of the dry strength agent closer to the surface to which the foam is applied. Without being bound by theory, it is believed that the dry strength agent can provide overall strength to the layer, especially the bond strength of the portion of the web closest to the surface to which the foaming additive is applied, while the unripened starch can improve the layer adhesion (bonding between two adjacent layers) after gelling in the dryer section. The bond strength within the top layer may not be very important because the top layer is usually made of refined kraft fibers, which usually bond relatively well. The bonding within the middle layer is usually lower because fibers with lower bonding potential and larger volume are used in the middle layer, such as bleached chemi-thermomechanical pulp (BCTMP). Since the top layer is usually the printing surface, the bonding within the back layer and the layer bonding between the middle layer and the back layer are usually not a big problem. Exceptions may occur, especially if two-sided printing is to be performed.
[0046] By strengthening the bonds within the middle layer with dry strength agents and by strengthening the ply bonds between the top and middle layers with unripened starch, the entire multi-ply sheet can achieve considerable internal bond strength. The process described herein allows this to be achieved with relatively good chemical efficiency by selectively increasing strength where improvement is most needed.
[0047] It is meaningless to add unripened starch in the middle layer wet end (paper machine pool 27b addition or thin stock cleaning, screening and degassing system 31b addition) because the unripened starch will be distributed throughout the middle layer paper web and thus cannot effectively improve layer bonding.
[0048] exist Figure 2 In the exemplary embodiment shown diagrammatically in A, a layer of foaming additive 62b (i.e., unripened starch 50b, dry strength agent 51b, foaming agent 52b (if necessary), and gas 54b that form foam 56b) can be applied to wet middle layer web 46b. The foam layer 62b is applied when the wet middle layer web 46b carried by the middle layer forming fabric 40b is transferred from vacuum box 45b to 47b. Water is removed from the wet middle layer web 46b and particles of unripened starch 63b are absorbed onto and retained on the first surface of the wet middle layer web 46b, while molecules of dry strength agent 51b, foaming agent 52b (if necessary), and gas 54b (in the form of bubbles) are introduced into or passed through the wet middle layer web 46b and retained in the web by the action of vacuum box 47b through a combination of electrostatic and physical means, such as Figure 2B. The actual distribution of the dry strength agent molecules depends on the factors previously described, but it is expected that all or most of the dry strength agent molecules from 56b will be in the wet middle layer web under the action of one or more middle layer high vacuum boxes 47b. In addition, the thickness of the wet middle layer web may be slightly reduced by removing some of the water through one or more middle layer vacuum boxes 47b. Particles 63b of unripened starch from foam layer 62b remain on the surface of the wet middle layer web, now referred to as 48b.
[0049] In the same exemplary embodiment, Figure 2 As shown in FIG. 3 , the wet top layer 48a carried by the top forming fabric 40a passes through the combination roller 60b ( Figure 2 c) is applied to the first surface of the wet middle layer 48b and then treated with the vacuum box 47a. Since the particles 63b of unripened starch are located on or near the first foam application surface of the wet middle layer web 48b, the particles 63b of unripened starch are located between the wet top layer 48a and the wet middle layer 48b after the top layer 48a is applied. Therefore, when the particles 63b of unripened starch absorb water and gel when heated in the drying section 81, these particles 63b of unripened starch are ideally arranged to adhere the top layer to the middle layer. When the combined webs 48b and 48a pass through one or more top layer high vacuum boxes 47a, additional water can also be removed by the one or more top layer high vacuum boxes 47a.
[0050] In the same exemplary embodiment, a wet backing layer 48c is added to the opposite side (forming fabric side) of the wet middle layer 48b at combining roll 60a, thereby producing Figure 1 and Figure 2 D shows a three-layer structure of a paper sheet 71. The combined paper sheet 71 is composed of a top layer 48a, a middle layer 48b, and a back layer 48c. The particles 63b of the unripened starch are trapped in the layer bonding area between the top layer 48a and the middle layer 48b, while the other components of the foaming formulation 53b are mostly contained in the middle layer 48b. The vacuum from one or more top layer high vacuum boxes 47a after the combining roll 60a can remove additional water and further compact and consolidate the combined paper sheet 71 (solids content is 20% to 25%), and can also draw some of the wet strength agent 51b molecules back to the top layer 48a.
[0051] It should be understood that the system described herein is not limited to Figure 1The precise configuration shown. For example, a foaming additive corresponding to 56b applied with an applicator corresponding to 58b can be added to the top paper web 48a immediately before the high vacuum suction box 45a. In this embodiment, the high vacuum suction boxes 45a and 47a will introduce dry strength agent molecules into the wet top layer 48a, but particles of unripened starch will remain in the layer bonding area between the wet top layer 48a and the wet middle layer 48b. Similarly, a foaming additive corresponding to 56b applied with a foam dispenser corresponding to 58b can be added to the top paper web 48a immediately before the high vacuum box 45c. High vacuum boxes 45c and 47c will introduce dry strength agent molecules into the back layer 48c, while particles of unripened starch corresponding to 62b will remain in the layer bonding area between the base layer 48c and the middle layer 48b. The choice of where to apply the foam containing dry strength agent and unripened starch should be based on the forming section configuration, which layer needs internal bonding improvement, and which layer bond joints need to be strengthened.
[0052] Foaming agent
[0053] As used herein, the term "foaming agent" defines a substance that reduces the surface tension of the liquid medium in which it is dissolved, and / or the interfacial tension with other phases, thereby being absorbed at the liquid / vapor interface (or other such interface). Foaming agents are generally used to generate or stabilize foam.
[0054] Foaming agents generally reduce bonding-related paper strength parameters by disrupting the bonds between pulp fibers. It has been observed that the minimum amount of foaming agent in the foaming formulation used is sufficient to produce foam in a manner that minimizes bonding-related paper strength parameters. Specifically, it has been observed that the amount of foaming agent required to effectively disperse a certain amount of immature starch and dry strength agent in a foam having an average maximum size or diameter of bubbles of 50 to 150 microns and a gas content of 70% to 90% may vary depending on the type and amount of immature starch and dry strength agent, the temperature and pH of the foaming formulation. This amount of foaming agent is defined herein as a "minimum sufficient amount" of foaming agent dosage, which is intended to reduce the negative effects of many foaming agents on fiber bonding while reducing costs and reducing subsequent foaming problems that may occur elsewhere in the paper machine white water circuit.
[0055] It has been determined that not all types of blowing agents are satisfactory in all situations. Certain blowing agents, such as the anionic blowing agent sodium dodecyl sulfate (SDS), tend to result in a decrease in the adhesion-related strength parameters of the final paper product. SDS is generally considered to be a preferred blowing agent because of its low cost and the fact that only a small dosage is generally required to achieve the target gas content in the foam. However, it has been found that the anionic charge of SDS may interfere with certain dry strength agents having cationic functional groups and result in the formation of gel-like associations (i.e., coacervates). Such associations may cause foam handling problems and inhibit the migration of the foam strength agent into the embryonic paper web. Even in an ideal situation (no charge interference between SDS and the dry strength agent containing a cationic group), SDS will still reduce strength due to adhesion interference. It has been determined in the development of the system described herein that certain other types of blowing agents are unable to produce foams in the target gas content range unless a blowing agent concentration that is too costly is used.
[0056] For the foam-assisted application of certain strength agents, it was investigated which foaming agents produced foams with the desired gas content and bubble size range. It was observed that the physical parameters of the investigated paper samples were improved when the gas content of the foam applied to the samples was 40% to 95% (e.g., 70% to 90%). In an exemplary embodiment, the gas is air. In various exemplary embodiments, the foam is formed by shearing the foam formulation in the presence of sufficient gas or by injecting the gas into the foaming solution or by injecting the foaming solution into the gas stream.
[0057] It was also observed that when the foaming formulation contained one or more foaming agents in an amount of 0.001% to 10% by weight based on the total weight of the foaming formulation, such as 0.01% to 1% based on the total weight of the foaming formulation, the physical properties of the paper samples were improved. In addition, it was also observed that when the amount of foaming agent was minimized to just enough to produce foam with a target gas content and bubble size, the physical properties of the paper samples were improved.
[0058] Typically, the desired concentration of blowing agent is such that substantially all of the bubbles in the foam are within the preferred range of 50 to 150 microns in diameter. Adding blowing agent in excess of the minimum sufficient amount of blowing agent required to produce a foam having the target gas content increases the likelihood of loss of strength properties associated with adhesion and, therefore, increases the magnitude of the loss of strength parameters. Using excess blowing agent beyond that required to produce the foam, such as using excess blowing agent in excess of 10% by weight of the foaming solution, also increases the overall cost of the process.
[0059] It is observed that the preferred foaming agent for foam-assisted application of uncooked starch with a dry strength agent having a cationic functional group is a foaming agent selected from the following: a subset of nonionic, zwitterionic, amphoteric or cationic foaming agents, or a combination of the same type or more than one type of these foaming agents. In particular, the preferred foaming agent is selected from nonionic foaming agents, zwitterionic foaming agents, amphoteric foaming agents and combinations thereof.
[0060] Without wishing to be bound by theory, it is believed that the improved strength parameter results obtained with nonionic and zwitterionic or amphoteric blowing agents are due to the lack of electrostatic interactions between these types of blowing agents and the pulp fibers and cationic strength agents. In particular, improved results are obtained by using a nonionic blowing agent selected from the group consisting of ethoxylates, alkoxylated fatty acids, polyethoxylates, glycerides, polyol esters, hexitol esters, fatty alcohols, alkoxylated alcohols, alkoxylated alkylphenols, alkoxylated glycerols, alkoxylated amines, alkoxylated diamines, fatty amides, fatty acid alkanolamides, alkoxylated amides, alkoxylated imidazoles, fatty amide oxides, alkanolamines, alkanolamides, polyethylene glycols, ethylene oxide and propylene oxide, EO / PO copolymers and derivatives thereof, polyesters, alkyl saccharides, alkyl polysaccharides, alkyl glucosides, alkyl polyglucosides, alkyl glycol ethers, polyoxyalkylene alkyl ethers, polyvinyl alcohols, alkyl polysaccharides, derivatives thereof, and combinations thereof.
[0061] Improved strength parameter results are also obtained by using zwitterionic or amphoteric foaming agents selected from the group consisting of lauryl dimethylamine oxide, cocoamphoacetate, cocoamphodiacetate, cocoamphopropionate, cocamidopropyl betaine, alkyl betaines, alkylamidobetaines, hydroxysultaines, cocamidopropyl hydroxysultaine, alkyliminodipropionate, amine oxides, amino acid derivatives, alkyldimethylamine oxides, and nonionic surfactants such as alkylpolysaccharides and polyalkylpolysaccharides, and combinations thereof.
[0062] It has been observed that anionic blowing agents can also produce improved results in strength parameters when combined with strength agents having cationic functional groups (having relatively low cationic charge, e.g., molar concentrations of cationic functional groups of less than about 16%). Preferred anionic blowing agents are those selected from the group consisting of alkyl sulfates and derivatives, alkyl sulfonates and sulfonic acid derivatives, alkali metal sulfonates, sulfonated fatty acid glycerides, sulfonated alcohol esters, fatty acid salts and derivatives, alkyl amino acids, aminosulfonic acid amides, sulfonated fatty acid nitriles, ether sulfates, sulfate esters, alkylnaphthalenesulfonic acids and salts, sulfosuccinates and sulfosuccinic acid derivatives, aminosulfonic acid amides, sulfonated fatty acid nitriles, ether sulfates, sulfate esters, alkylnaphthalenesulfonic acids and salts, sulfosuccinates and sulfosuccinic acid derivatives, phosphates and phosphonic acid derivatives, alkyl ether phosphates and phosphate esters, and combinations thereof.
[0063] It has been observed that cationic blowing agents can also produce improved results in strength parameters when combined with strength agents having cationic functional groups (having relatively low cationic charge, e.g., molar concentrations of cationic functional groups less than about 16%). Preferred cationic blowing agents are blowing agents selected from the group consisting of alkylamines and amides and derivatives thereof, alkylammonium, alkoxylated amines and amides and derivatives thereof, fatty amines and fatty amides and derivatives thereof, quaternary ammonium, alkylquaternary ammonium and derivatives thereof and salts thereof, imidazoline derivatives, carbonyl ammonium salts, carbonyl phosphonium salts, polymers and copolymers of the above structures, and combinations thereof.
[0064] Combinations of the above-mentioned foaming agents are also disclosed herein. Combining certain different types of foaming agents allows for a combination of different benefits. For example, anionic foaming agents are generally cheaper than other foaming agents and are generally effective in preparing foams, but may not be as effective in improving the strength properties of paper related to bonding. Nonionic, zwitterionic or amphoteric foaming agents are generally more expensive than anionic foaming agents, but are generally more effective in improving strength properties together with strength agents having cationic functional groups. Thus, a combination of anionic and nonionic, zwitterionic and / or amphoteric foaming agents can provide a dual benefit of improving paper strength properties while also achieving cost-effectiveness, or at least provide a compromise between these two properties. Foaming agents can also be combined to utilize the high foaming ability of one type of foaming agent and the better bonding improvement performance of another type of foaming agent. For certain combinations, there is a synergistic improvement in strength properties related to bonding when using certain foaming agents and certain strength agents (e.g., cationic or amphoteric strength agents) having cationic functional groups. Anionic or nonionic strength agents can also show synergy with certain foaming agents or combinations thereof.
[0065] In an exemplary embodiment, the blowing agent is poly(vinyl alcohol), also known as polyvinyl alcohol, PVA, PVOH or PVAl and its derivatives. It has been observed that the use of a PVOH blowing agent in combination with a strength agent having a cationic functional group improves the strength properties of the sample compared to the addition of the same cationic strength agent in the wet end. Polyvinyl alcohol blowing agents with higher molecular weights, lower hydrolysis degrees and no defoamers generally provide good strength properties through foam-assisted application of strength agents. In an exemplary embodiment, the polyvinyl alcohol has a degree of hydrolysis between about 70% and 99.9%, such as between about 86% and about 90%. In an exemplary embodiment, the polyvinyl alcohol blowing agent has a number average molecular weight of about 5,000 to about 400,000, resulting in a viscosity of about 3 to 75 cP at 4% solid content and 20°C. In an exemplary embodiment, the polyvinyl alcohol blowing agent has a number average molecular weight of about 70,000 to about 100,000, resulting in a viscosity of 45 to 55 cP at 4% solid content and 20°C. It is also noted that polyvinyl alcohol based blowing agents advantageously do not impair paper strength parameters by disrupting the bonds between pulp fibers of the paper web. Combinations of nonionic, zwitterionic or amphoteric blowing agents with polyvinyl alcohol blowing agents (or their derivatives) of other molecular weights and degrees of hydrolysis, together with cationic strength agents, also provide good foam quality and good strength enhancement.
[0066] It was also observed that improved physical parameters in the samples were obtained when the foaming agent used had a hydrophilic-lipophilic balance (HLB) above about 8. An HLB balance above about 8 facilitates the ability to produce foam in aqueous compositions.
[0067] Unripened starch
[0068] Unripened starch is used herein to provide improved ply adhesion for the manufactured paper product. Unripened starch is introduced to the surface of the wet paper web before the wet paper web contacts another wet paper web to form an interface between the plies. The purpose of the unripened starch is to help the adhesion between the plies, also known as ply adhesion. The unripened starch will gel in the dryer section under heating and in the presence of water. This helps adhesion between different plies. The purpose of the unripened starch is not necessarily to increase the strength of any ply itself, but to increase the adhesion between the plies.
[0069] In an exemplary embodiment, the uncooked starch is provided in the form of granules, and the granules have an average maximum dimension of 5 to 50 microns.
[0070] Starch is a natural polymer derived from corn, wheat, rice, tapioca, potato, cassava or other plants, consisting of straight-chain molecules (amylose) and branched molecules (amylopectin). The diameter of natural starch granules from corn may be 5 to 25 μm, while the diameter of natural starch granules from potato may be 15 to 100 μm, and the diameter of natural starch granules from wheat may be 5 to 25 μm. When heated in water, the granules swell, gel, break and dissolve into single molecules with characteristic molecular weight. The temperature at which the granules gel also depends on the source of the starch granules. Corn starch granules gel at 72 to 75°C, while potato starch granules gel at 62 to 65°C and wheat starch granules gel at 62 to 80°C. Native (unmodified) starch solutions generally contribute more to paper strength than modified (degraded) starch, but native starch solutions may be difficult to handle due to their higher viscosity. Starch can be selectively degraded by oxidation with sodium hypochlorite or other oxidants. The degree of oxidation affects the viscosity of the starch solution and the starch's potential contribution to improved adhesion. Starch can also be modified by chemical derivatization (ethylation of starch is the most common derivatization). Commercially available starch products may contain blends of starches from different plant sources. Starch sales contracts sometimes allow for substitution of one plant source for another as market prices or supply fluctuate.
[0071] Starch has limited or no adhesive properties in its uncooked state. However, when the starch slurry is heated sufficiently, the starch granules will absorb the available suspension liquid and swell, resulting in gelatinization of the starch granules. In this state, the starch has excellent adhesive capabilities and will form bonds between many substrates, including paper.
[0072] Unripened starch has been applied to the surface of the multi-layer paperboard plies in the forming section for the purpose of improving ply bonding. Current practice is to apply the unripened starch to the wet plies via nozzles mounted on spray booms across the forming section. This method improves ply bonding, but overspray from the nozzles creates a risk to workers and accumulates on exposed surfaces. Oversprayed starch can exacerbate slippery conditions and biological growth, resulting in corrosion and slippery walking conditions. In addition, nozzle clogging can occur in certain locations depending on the starch granule size and nozzle size.
[0073] Dry strength agent
[0074] As used herein, "dry strength agents" improve the strength properties of the final paper product, as measured when the paper is conditioned to an equilibrium of 23°C + / - 1°C and 50% + / - 2% relative humidity. Dry strength agents generally work by increasing the total bond area of fiber-fiber bonds rather than by making the individual fibers of the paper web stronger. The increase in fiber bond area and the subsequent increase in paper strength properties associated with bonding can also be achieved by other techniques. For example, increased fiber refining, paper wet pressing, and improved forming can be used to increase the fiber bond area. In some cases, the improvement in paper strength properties associated with fiber bonding achieved by foam-assisted application of dry strength agents is shown to be greater than that achieved by wet-end addition of the same strength agent. In particular, one advantage associated with the foam-assisted application of dry strength agents is that higher concentrations of dry strength agents can be introduced into wet-formed paper sheets, while the practical dosage range of dry strength agents limits the concentration of wet-end additives in the extremely low consistency environment of traditional wet-end addition. In traditional wet-end addition, the dosage limitation of dry strength agents results in a "plateau" of paper strength properties related to adhesion in the dose-response curve at relatively low dosages, while foam-assisted addition of dry strength agents results in a sustained dose response, where an increase in the concentration of dry strength agent applied to the wet paper sheet results in an increase in the strength properties of the resulting paper product, even much higher than normal dosage application.
[0075] In an exemplary embodiment, the dry strength agent is a synthetic dry strength agent comprising a cationic functional group, such as a cationic strength agent or an amphoteric strength agent. As explained in more detail below, it is noteworthy that synthetic strength agents having cationic functional groups improve the bonding-related strength properties of the final paper sheet.
[0076] In an exemplary embodiment, the foam-assisted application is performed using a foam formulation comprising at least one dry strength agent in an amount of 0.01 to 50 weight percent based on the total weight of the foam formulation, such as 0.1 to 10 weight percent based on the total weight of the foam formulation.
[0077] Without being bound by theory, the reason that foam-assisted application of certain strength agents can improve strength properties related to paper bonding compared to wet-end addition of the same strength agent may be that the strength agent is better retained when foam-assisted application is performed. Specifically, because the foam application is performed when the paper sheet has a higher fiber concentration (relative to water, where the water content is typically 70% to 90%) than when the strength agent is added to the paper pulp in the stock preparation section (where the water content is typically 95% to 99% or higher), less strength agent is lost when the pulp passes through the subsequent dewatering section. In an exemplary embodiment, the step of applying the foam to the wet-formed embryonic paper web is performed when the wet-formed embryonic paper web has a pulp fiber consistency of 5% to 45% (e.g., 5% to 30%).
[0078] Without wishing to be bound by theory, it is believed that the reason that foam-assisted application of certain strength agents can improve paper strength parameters compared to wet-end addition of the same agent is that contaminants / pollutants that interfere with additive adsorption of the strength agent onto the fibers may be present in large quantities in the stock preparation section, particularly in the thin stock section, as will be explained in more detail below.
[0079] Without wishing to be bound by theory, it is believed that the reason that foam-assisted application of certain strength agents can improve paper parameters compared to wet-end addition of the same agent is that the strength agent is at least partially physically bound to the sheet rather than solely by surface charge, and the lack of remaining available charged sites in the formed web does not limit the amount of strength agent that can be incorporated into the sheet. When additives are introduced by wet-end addition, especially when large amounts of additives are introduced in this manner, a lack of remaining available charged binding sites, such as a lack of remaining available anionic charged sites, can occur in the formed web. Alternatively or additionally, without wishing to be bound by theory, the improved strength may be due to the unique distribution of DSA in the sheet provided by embodiments herein. It is believed that foam application concentrates the distribution of DSA in the sheet in targeted areas rather than being uniformly distributed throughout.
[0080] In an exemplary embodiment, the dry strength agent comprises a synthetic dry strength agent. It should be noted that the term "synthetic" strength agent as used herein excludes natural strength agents. In an exemplary embodiment, the synthetic dry strength agent comprises a synthetic strength agent having a cationic functional group. In other embodiments, the synthetic dry strength agent comprises a synthetic strength agent having an anionic functional group. In yet another embodiment, the synthetic dry strength agent comprises a synthetic strength agent having an amphoteric functional group.
[0081] In an exemplary embodiment, the synthetic strength agent comprises a graft copolymer of a vinyl monomer and a functionalized vinyl amine, a vinyl amine-containing polymer, or an acrylamide-containing polymer. In an exemplary embodiment, the at least one synthetic dry strength agent having a cationic functional group is selected from: acrylamide-diallyldimethylammonium chloride copolymer; glyoxylated acrylamide-diallyldimethylammonium chloride copolymer; vinyl amine-containing polymers and copolymers; polyamidoamine-epichlorohydrin polymers; glyoxylated acrylamide polymers; polyethyleneimine; acryloyloxyethyltrimethylammonium chloride. An exemplary synthetic strength agent comprises a graft copolymer of a vinyl monomer and a functionalized vinyl amine.
[0082] Additionally or alternatively, in an exemplary embodiment, the at least one synthetic strength agent having a cationic functional group is selected from: DADMAC-acrylamide copolymers, which may or may not be glyoxylated; polymers and copolymers of acrylamides having cationic groups, including AETAC, AETAS, METAC, METAS, APTAC, MAPTAC, DMAEMA, or combinations thereof, which may or may not be glyoxylated; polymers and copolymers containing vinylamine; PAE polymers; polyethylene imine; poly-DADMAC; polyamine ; and polymers based on dimethylaminomethyl substituted acrylamides, wherein: DADMAC is diallyldimethylammonium chloride; DMAEMA is dimethylaminoethyl methacrylate; AETAC is acryloxyethyltrimethyl chloride; AETAS is acryloxyethyltrimethylsulfate; METAC is methacryloyloxyethyltrimethyl chloride; METAS is methacryloyloxyethyltrimethylsulfate; APTAC is acrylamidopropyltrimethylammonium chloride; MAPTAC is acrylamidopropyltrimethylammonium chloride; and PAE is a polyamidoamine-epichlorohydrin polymer.
[0083] It was also observed that synthetic dry strength agents having cationic functional groups and also containing primary amine functional units (in the form of polyvinylamine polymer units) were effective in improving strength parameters compared to synthetic strength agents without primary amine functional units. In an exemplary embodiment, the synthetic strength agent having cationic functional groups included in the foaming formulation has a primary amine functionality of 1 to 100%.
[0084] In another embodiment, natural material based strength agents are used as dry strength agents in foaming formulations. Natural material based strength aids include cooked starch, guar gum, chitosan, microfibrillated cellulose (MFC), and many other materials known to those skilled in the art. Foam application provides a unique opportunity to apply MFC, which is difficult to apply via spraying because of the potential for nozzle clogging and which typically must be diluted to very low solids content for conventional handling and application.
[0085] In yet another embodiment, the biobased strength agent is comprised of polymers synthesized from biobased versions of fossil-based materials to create a more sustainable version of known synthetic strength agents.
[0086] Foam assisted application
[0087] In an exemplary embodiment, the air content of the foam when the foam assists in applying the unripened starch and the dry strength agent is 40% to 95%, such as 70% to 90%, based on the total volume of the foam. The foam can be formed by injecting gas into the foaming formulation, by shearing the foaming formulation in the presence of sufficient gas, by injecting the foaming formulation into a gas stream, or by other suitable means.
[0088] In an exemplary embodiment, the foam density of the produced foam is from 50 to 300 g / L, for example from 100 to 300 g / L, such as from 150 to 300 g / L.
[0089] In an exemplary embodiment, when the foam is applied to the wet layer of paper web, the foam is applied at a rate of 30 to 300 g / m 2 (based on wet weight), such as less than 200g / m 2 (based on wet weight), for example 60 to 150 g / m 2 (by wet weight) of foam coverage is applied horizontally.
[0090] In an exemplary embodiment, when the foam is applied to the layer paper web, the foam is applied so that the dosage of the dry mass of uncooked starch to the wet layer paper web is 0.1 to 4 g / m 2 , for example at least 0.75 g / m 2 , or at least 1g / m 2 , and not more than about 3g / m 2 , or not more than about 2.5g / m 2 .
[0091] In an exemplary embodiment, when the foam is applied to the layer web, the foam is applied so that the dosage of the one or more dry strength agents to the wet layer web is at least 0.075% (on an active basis), such as at least 0.2% (on an active basis), and no more than 1.2% (on an active basis), such as no more than 0.8% (on an active basis), all based on layer dry weight.
[0092] In an exemplary embodiment, when the foam is applied to the layer paper web, the layer paper web has a solids content of 5 to 20%, for example, a solids content of 5 to 15% or a solids content of 8 to 15%.
[0093] Without wishing to be bound by theory, it is noteworthy that when a small batch of foamable formulations is foamed by incorporating air into a liquid using a high speed homogenizer in an open top container, the amount of gas dispersed into fine bubbles of maximum size (such as diameter) of 10 to 300 micrometers (μm) is limited by the nature and concentration of the foaming agent and its interaction with particles of unripened starch and molecules of the dry strength agent. As the air content increases, the foam becomes more viscous, and at a certain air content, the foam cannot effectively fall back into the vortex created by the homogenizer. For a given type and concentration of foaming agent, the maximum gas content is usually reached in less than one minute. Further homogenization does not entrain more gas in the form of bubbles of 10 to 300 micrometer diameter because any additional gas introduced into the vortex will be dispersed in the form of larger bubbles, which have a maximum diameter of 2 to 20 millimeters (mm). Bubbles of this size will quickly coalesce and float to the top of the foam, where they will usually burst and the gas will escape from the foam. The actual air content achieved when equilibrium is reached (after 30 to 60 seconds of homogenization) varies with the amount and type of dry strength additive and / or starch incorporated into the foaming formulation.
[0094] Without wishing to be bound by theory, it is noteworthy that commercially available foam generators can be used to produce foam suitable for foam auxiliary additive addition at pilot scale or industrial scale. Suitable commercially available foam generators sometimes produce foam by tight gaps in a rotating device, by an oscillating device, by air induction or by high shear induced by other suitable means. Most are pressurized, which facilitates feeding the foam into a foam dispenser above the layer forming device. When excess gas is added to a pressurized foam generator, if the acceptable quality of foam (10 to 300 μm bubbles) that can be dispersed by the foam generator is exceeded, the excess gas will be discharged (along with the foam) in the form of large bubbles with a diameter of 2 to 20 mm, which are dispersed in the foam. The diameter of bubbles with a diameter of 2 to 20 mm is much larger than the typical thickness of a wet layer paper web or foam layer. Since the particles of unripened starch and dry strength agent are only present in the liquid film in the foam and the interstitial areas of the bubbles, if most areas of the paper sheet are only covered by the film on the single bubble, the bubbles with very large diameters cannot deliver the particles of unripened starch and dry strength agent to the fiber intersection area. In order to distribute the unripened starch and dry strength agent more evenly, gas bubbles smaller than the thickness of the foam layer or the thickness of the wet paper web are preferred. For this application, gas bubbles with a diameter of 20 to 300 μm, especially gas bubbles with a diameter of 50 to 150 μm, are preferred because bubbles of this size can carry the unripened starch onto the wet layer paper web and carry the dry strength agent into the wet layer paper web without damaging the paper web, thereby distributing the unripened starch and strength agent more effectively. Foam containing gas bubbles with a diameter of 50 to 150 μm and an air content of 70 to 80% is convenient because it can be easily poured from an open-top container. Foam containing up to 90% to 95% air can be conveyed by pressure through a hose to a foam dispenser and discharged, and the foam dispenser can be used to apply the foam to the layer paper web. Most foam generators cannot reliably produce foams of acceptable quality for the purpose with an air content of more than about 90%.
[0095] Example
[0096] A Noble & Wood Handsheet Mold was used to make two-ply handsheets, which were used to mold the top and middle plies of a three-ply paperboard sheet. Bleached chemi-thermomechanical pulp (BCTMP) and mill-supplied waste paper with a basis weight of about 120 g / m2 were prepared in the mold by standard wet-end addition of sizing agent, cooked starch and retention aid. 2The wet paper sheet was removed from the setter frame and placed on the vacuum plate of the Gardco suction device connected to a vacuum pump. The exposed area of the vacuum plate was covered with an impermeable material to avoid loss of vacuum force due to air leakage around the hand sheet. An initial vacuum was applied to remove water and compact the paper sheet. A foaming formulation was prepared by combining a foaming agent, a synthetic dry strength agent and unripened starch (when used) with water. Air was incorporated into the foaming formulation using a handheld homogenizer under atmospheric conditions, and the foam produced in the process was considered to have an air content of about 70%. The foam was then poured onto the suction device adjacent to the paper sheet and a uniform coating of the foaming additive was distributed on the surface of the paper sheet using a coating blade. The foam addition level is noted in the following experiments. A vacuum force was applied to suck the applied foaming additive onto the surface of the wet middle layer paper sheet (particles of unripened starch) or introduced into the paper sheet (synthetic dry strength agent). A final basis weight of about 40 g / m was then prepared from refined kraft pulp in a Noble & Wood hand sheet mold. 2 The middle sheet into which the foaming additive has been introduced is placed on a press felt with the foamed side facing upward. The top sheet is removed from the deckle of the Noble & Wood handsheet mold and placed face down on the middle sheet plywood against the surface of the middle sheet to which the foam was previously applied. Another press felt is applied over the combined sheets and the sheets are pressed and dried in the usual manner.
[0097] The data collected from the testing of the exemplary embodiments using two layers of handsheets produced as described above indicate that when the two chemistries (i.e., unripened starch and synthetic dry strength agent) are applied in combination, strength properties are improved compared to the use of either chemistries alone (i.e., unripened starch alone or synthetic dry strength agent alone). Without wishing to be bound by theory, it is believed that the unripened starch will remain at or near the interface, providing strength between the two layers, while the synthetic dry strength agent is able to penetrate into the sheet and provide strength within each layer. This combined approach provides increased paper strength and shifts the location of cracks (weak points in the sheet) from those observed with standard papermaking methods.
[0098] Example 1
[0099] In this experiment, Xelorex TM F 3000 is used as a synthetic dry strength agent and in some cases with uncured 30067 starch. Starch at 0.75g / m 2 The synthetic dry strength agent was dosed at three levels (in terms of active substance) based on the dry weight of the simulated middle layer portion of the two-layer paper sheet. The foam was dosed at 122 g / m 2The air content of the foam was 70% at a liquid addition level of 1.20.20. The two graphs are presented comparing the results of adding a synthetic dry strength agent with and without the addition of uncured starch. Figure 3 Results are shown for dosing the synthetic dry strength agent alone and for dosing the dry strength agent plus a constant dose of unripened starch. Addition of both unripened starch and the synthetic dry strength agent increased the Scott Bond (internal bond test) value compared to the strength results obtained with the synthetic dry strength agent alone. Figure 4 It shows that the addition of synthetic dry strength agent alone (lower line) does not change the location of the Z-direction crack, and the crack remains at or near the interface of the two paper layers. The combination of unripened starch and synthetic dry strength agent moves the crack zone deeper into the middle layer of the paper sheet. Since the use of dry strength agent alone does not change the Z-direction crack, we confirm that the failure point is located at the bond between the top layer and the middle layer without the addition of unripened starch. With the addition of unripened starch, as the dosage of synthetic dry strength agent increases, the Z-direction failure point moves deeper into the paper sheet, far below the top layer-middle layer area. This shows that the joint is now stronger than the internal bond of the middle layer without the addition of synthetic dry strength agent, while the synthetic dry strength agent significantly increases the internal bond of the middle layer, and the overall Scott bond value is much higher.
[0100] Example 2
[0101] Four synthetic dry strength agents were used alone at single dosage levels and in combination with 0.75 g / m 2 The unripened starch was combined with the double-layer paper sheets prepared as described in the previous examples, all at 122 g / m 2 A foam addition level of 1000 ng / ml was applied to the paper sheet (air content 70%). Figure 5 The Scott bond strength of each synthetic dry strength agent is shown with and without unripened starch. In all cases, the Scott bond test values for the combination of synthetic dry strength agent plus unripened starch were much higher than when unripened starch was not used. Figure 6 The Z-direction crack location is shown by indicating the mass percentage in the top of the torn sheet. For all sheets with only synthetic dry strength agents, the crack location in the combined sheet is the same, 30% of the sheet thickness, in or near the ply bond area. The addition of unripened starch increases the depth of the Z-direction crack, with the synthetic dry strength agent having the largest change in crack location and the largest increase in Scott bond value. This again indicates that starch only reinforces the ply bond joint, while the synthetic dry strength agent reinforces the middle ply internally.
[0102] Figure 7 and Figure 8 They are shown respectively with Figure 5 and Figure 6 The same trend, but quantified by the Z-direction tensile strength (ZDT) test, is another common test method for internal bonding of paper and paperboard.
[0103] Although at least one exemplary embodiment has been presented in the foregoing specific embodiments, it should be understood that there are numerous variations. It should also be understood that one or more exemplary embodiments described herein are not intended to limit the scope, applicability or configuration of the claimed subject matter in any way. On the contrary, the foregoing specific embodiments will provide a convenient roadmap for implementing the one or more embodiments described for those skilled in the art. It should be understood that, without departing from the scope specified in the appended claims, various changes may be made to the function and arrangement of the elements described in the exemplary embodiments.
Claims
1. A method of making a multi-ply paper product, the method comprising: Producing foam of water, air, foaming agent, unripened starch and dry strength agent; applying a foam to a first surface of a base germ layer web, wherein the base germ layer web has a second surface opposite the first surface; providing an application layer web having a first surface and an opposing second surface and contacting the first surface of the base layer web with the first surface of the application layer web at an interface to form a composite layer web; as well as Vacuum pressure is selectively applied to the second surface of the base germ layer web to retain particles of unripened starch on or near the first surface of the base germ layer web, thereby introducing dry strength agent molecules into the base germ layer web and / or to the first surface of the application germ layer web to retain particles of unripened starch in the interface and introduce dry strength agent molecules into the application germ layer web.
2. The method of claim 1 , wherein selectively applying vacuum pressure to the second surface of the base germ layer web to retain particles of uncooked starch on or near the first surface comprises: Vacuum pressure is applied to the second surface of the base germ layer web at least prior to contacting the first surface of the base germ layer web with the first surface of the application germ layer web.
3. The method according to claim 1 further includes providing a tertiary germ layer web having a first surface and an opposite second surface and contacting the first surface of the tertiary germ layer web with the second surface of the base germ layer web, wherein the combined layer web includes an application germ layer web, a base germ layer web and a tertiary germ layer web.
4. The method of claim 3, further comprising applying a foam to the second surface of the base germ layer web, to the application germ layer web, and / or to the tertiary germ layer web.
5. The method of claim 1, further comprising pressing the combined layer web in one or more stages to further distribute the dry strength agent molecules within the base germ layer web and / or the application germ layer web.
6. The method of claim 1 further comprising drying the combined layer webs under sufficient layer moisture, temperature and time conditions to gelatinize and distribute the particles of uncooked starch within the interface and to increase the layer bond strength between the base interlayer web and the applied layer web.
7. The method of any one of claims 1 to 6, wherein generating a foam of water, air, unripened starch, and a dry strength agent comprises generating a foam having a foam density of 50 to 300 g / L.
8. A method according to any one of claims 1 to 6, wherein the particles of the uncooked starch have an average maximum dimension of 5 to 50 microns and the foam coverage level is 30 to 300 g / m 2 , measured by wet weight.
9. The method of any one of claims 1 to 6, wherein applying the foam to the first surface of the base germ web comprises applying the foam to the base germ web such that the dosage of the uncooked starch relative to the base germ web is 0.1 to 4 g / m 2 .
10. The method of any one of claims 1 to 6, wherein applying the foam to the first surface of the base germ web comprises applying the foam to the base germ web such that the dosage of the dry strength agent is 0.05 to 5 g / m 2 .
11. The method according to any one of claims 1 to 6, wherein: When the foam is applied to the first surface of the base germ layer web, the base germ layer web has a solids content of 5% to 20%.
12. The method according to any one of claims 1 to 6, wherein the foam is produced from water, air, uncooked starch, a dry strength agent and a foaming agent.
13. A method of introducing a dry strength agent into a multi-ply paper product, comprising: The foam is produced from a foaming formulation comprising: Foaming agent; Unripened starch; Dry strength agent; and Water; and The foam is applied to the wet germ layer web.
14. A multi-ply paper product, produced by the following steps: Produces a foam of water, air, unripened starch and dry strength agent; applying a foam to a first surface of a base germ layer web, wherein the base germ layer web has a second surface opposite the first surface; providing an application layer web having a first surface and an opposing second surface, and contacting the first surface of the base layer web with the first surface of the application layer web at an interface to form a composite layer web; as well as Vacuum pressure is selectively applied to the second surface of the base germ layer web to retain particles of unripened starch on or near the first surface of the base germ layer web and introduce dry strength agent molecules into the base germ layer web and / or to the first surface of the application germ layer web to retain particles of unripened starch in the interface and introduce dry strength agent molecules into the application germ layer web.
Citation Information
Patent Citations
Playing card paperboard and processing method thereof
CN102733267A
Hydrophobically sized fibrous web and a method for the preparation of a sized web layer
CN104285006A
Foam assisted application of strength additives to paper products
CN112218930A
Compositions and processes for renewable rigid foam
CN113631774A
Method of applying a foam composition to a tissue product
US20030221808A1
Cited By
Paper reinforcing agent and application thereof
CN121629801A