Nanocomposite barrier paper laminates
By using a paper laminate with a water-dispersible nanocomposite barrier layer in paper packaging, the contradiction between recyclability and biodegradability of paper packaging in the existing technology when improving barrier performance and sealing properties is solved, and the paper packaging is realized. Recycling and environmentally friendly paper packaging solutions.
Patent Information
- Application Number
- CN202380015745.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-27
- Filing Date
- 2023-01-27
- Publication Date
- 2024-10-15
AI Technical Summary
When improving barrier properties and sealing properties of existing paper packaging, it is difficult to maintain recyclability and biodegradability. In particular, the polyethylene coating does not degrade in the environment and forms microplastics, which affects environmental safety.
Paper laminates employing water-dispersible nanocomposite barrier layers, including recyclable and biodegradable paper layers, adhesive layers, and sealing layers, prepared through coating and drying steps of aqueous nanocomposite dispersions to create nanoscale orderly spaced structure to improve barrier performance.
It achieves recyclability in industrial paper recycling facilities and home composting, while being biodegradable when improperly disposed of, reducing environmental pollution and improving the moisture barrier and sealing properties of paper packaging.
Smart Images

Figure CN118786266A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a paper laminate comprising a water-dispersible nanocomposite barrier for use in flexible packaging applications or product delivery systems such as pouches, sachets, bags, the paper laminate comprising paper combined with an adhesive layer, a water-dispersible nanocomposite barrier layer and a sealant layer, the paper laminate providing several advantages over prior art paper-based flexible packaging; and a method for producing a paper laminate with an integrated water-dispersible nanocomposite barrier. Background Art
[0002] Paper packaging is becoming increasingly popular among consumers because it is perceived as more natural, more recyclable and more biodegradable. However, uncoated paper has poor barrier properties, and attempts to improve barrier properties by adding coatings often result in reduced recyclability of the packaging in commercial paper recycling systems and also reduce its ability to biodegrade in various environments.
[0003] Uncoated paper packaging is very easy to recycle in commercial paper recycling systems and is usually biodegradable in certain environments. However, paper without coatings or adhesives at all cannot easily form a complete functional package. Moreover, uncoated paper packaging can only be used to contain dry products that do not require any type of moisture or gas or fragrance or grease barrier. If the dry product is sensitive to moisture, it will be damaged because moisture will quickly enter the package. If it is sensitive to oxygen, it will oxidize. If the product is greasy, the grease will migrate through the paper and leave unsightly stains on the outside of the package. If the product contains fragrance, the fragrance will escape from the package and change the nature of the expected smell of the product. However, if a coating is added to the paper to improve the barrier properties and / or make it sealable, great care must be taken to avoid adversely affecting the recyclability of the packaging in the commercial paper recycling system. In addition, in the case of improper disposal, it is hoped that the coating does not affect the ability of the entire package to biodegrade within the most desired range of environmental conditions. Failure to degrade may have adverse environmental impacts, such as microplastics that persist in seawater.
[0004] A common approach to address the poor barrier properties of paper and make it sealable is to add a polyethylene-based or ethylene copolymer-based or other non-biodegradable polymer coating to the surface of the paper by coating, printing or lamination. However, if the polyethylene coating is too thick, it will adversely affect the recyclability of the paper laminate in a typical commercial paper recycling system. There are many examples of polyethylene coatings that have caused problems in paper recycling processes, especially where thicker coatings are used to enhance seal strength and / or enhance barrier properties. Examples of such problems are, but are not limited to: i) coatings that clog repulping tanks and filters in the system; ii) coatings that remain tightly on the paper fibers and prevent a high percentage of the paper fibers from being released into the water of the repulping system; iii) coatings that are ultimately incorporated into the recycled paper and adversely affect the appearance or performance of the resulting recycled paper.
[0005] If such polyethylene coating is made very thin, it can be stripped and sent to landfill or burned to provide fuel to the factory, leaving paper fibers to collect and recycle into paper, then the overall structure can be considered to be recyclable in the paper recycling stream. However, such structure still has some disadvantages, because if it is improperly abandoned in the environment, paper will biodegrade, but the polyethylene coating cannot. This will instead form a persistent microplastic that has an adverse effect on the environment, becoming a non-nutritional food source for some animals. In addition, many consumers may notice the appearance of the shiny polyethylene layer on the inner surface of the paper laminate and negatively regard it as a non-natural material. The polyethylene coating will also have an adverse effect on the ability of the packaging to be composted via industrial or home composting, unless the consumer can easily remove the polyethylene coating before composting.
[0006] On the contrary, if biodegradable materials are used instead of polyethylene, such as those described in patent application US2002 / 0127358, the barrier properties of the barrier paper laminate to moisture vapor permeation will be adversely affected, since biodegradable materials are known to be moisture vapor permeable. Coatings made of biodegradable materials will need to be thick coatings, leading to problems in the paper recycling process.
[0007] Thus, there is an unmet need for paper laminates for flexible packaging applications having moisture barrier and sealant layers, having improved recycling efficiency in industrial paper repulping systems, having enhanced biodegradation kinetics, and having reduced environmental impacts such as impacts on soil and aquatic environments. Summary of the invention
[0008] A paper laminate comprising a water-dispersible nanocomposite barrier is provided, the paper laminate being capable of being recycled in an industrial paper recycling facility, being suitable for use in a home or industrial composting facility, and being biodegradable when improperly disposed of in the environment. The paper laminate is made of the following layers: a recyclable and / or biodegradable paper layer having an outer surface and an inner surface; an adhesive layer having an outer surface and an inner surface, the outer surface being disposed on the inner surface of the paper layer; a water-dispersible nanocomposite barrier layer having an outer surface and an inner surface, the outer surface being disposed on the inner surface of the adhesive layer; and a sealing layer having an outer surface and an inner surface, the outer surface being disposed on the inner surface of the water-dispersible nanocomposite barrier layer.
[0009] A method for preparing a paper laminate including a water-dispersible nanocomposite barrier is provided, the method comprising applying an adhesive layer to paper or board; applying an aqueous nanocomposite dispersion to a surface of the adhesive layer; removing water from the nanocomposite dispersion to obtain a water-dispersible nanocomposite barrier layer; and applying a sealing layer to the nanocomposite barrier layer.
[0010] A method for preparing a paper laminate including a water-dispersible nanocomposite barrier is provided, the method comprising using a sealable film; applying an aqueous nanocomposite dispersion to a surface of the sealable film; removing water from the nanocomposite dispersion to obtain a water-dispersible nanocomposite barrier layer; applying an adhesive layer to the nanocomposite barrier layer; and laminating paper or board to the adhesive layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 A cross section of a paper or board layer 10 is shown.
[0012] Figure 2 A cross section of an adhesive layer 20 applied to a paper or board layer 10 is shown.
[0013] Figure 3 A cross section of a water dispersible nanocomposite barrier layer 30 coated on an adhesive layer 20 coated on a paper or board layer 10 is shown.
[0014] Figure 4 A cross-section of a paper laminate including a water-dispersible nanocomposite barrier according to the present invention is shown, the paper laminate including a sealant layer 40 coated on a water-dispersible nanocomposite barrier layer 30, the water-dispersible nanocomposite barrier layer being coated on an adhesive layer 20, which is coated on a paper or board layer 10.
[0015] Figure 5A cross-sectional image obtained via scanning electron microscopy (SEM) of a paper laminate including a water-dispersible nanocomposite barrier according to the present invention is shown, the paper laminate including a sealing layer 40 coated on a water-dispersible nanocomposite barrier layer 30, the water-dispersible nanocomposite barrier layer being coated on an adhesive layer 20, which is coated on a paper or board layer 10.
[0016] Figure 6 A cross-sectional image obtained via transmission electron microscopy (TEM) of a water-dispersible nanocomposite barrier according to the present invention is shown, showing nanoscale (<100 nm) ordered spacing of hydrophilic hectorite nanosheets (1 nm thick dark lines) and intercalated polyethylene glycol (PEG) fillers (0.8 nm thick light lines).
[0017] Figure 7 A schematic diagram of a method for preparing a paper laminate including a water dispersible nanocomposite barrier according to the present invention is shown.
[0018] Figure 8 A schematic diagram showing the use of a paper laminate comprising a water dispersible nanocomposite barrier according to the present invention is shown. DETAILED DESCRIPTION
[0019] A paper laminate including a water-dispersible nanocomposite barrier is described that provides several advantages over prior art paper barrier laminates, and a method for preparing a paper laminate including a water-dispersible nanocomposite barrier is described.
[0020] As used herein, the term "water dispersible" means breaking into small fragments less than one tenth of a millimeter in water. These fragments may, but need not, be stably suspended in water.
[0021] As used herein, the term "nanocomposite" refers to a heterogeneous material comprising nanoscale, orderly spaced hydrophilic nanosheets and intercalated polymer fillers; "nanoscale" means less than 100 nanometers.
[0022] As used herein, the term "water vapor transmission rate" or "WVTR" refers to the rate at which water vapor passes through paper when measured according to the Water Vapor Transmission Rate Test Method set forth in the Test Methods section.
[0023] As used herein, the term "copolymer" refers to a polymer formed from two or more types of monomer repeating units. As used herein, the term "copolymer" also encompasses terpolymers, such as terpolymers having a distribution of vinyl alcohol monomer units, vinyl acetate monomer units, and possibly butene glycol monomer units; however, if the copolymer is substantially completely hydrolyzed, the vinyl acetate monomer units may be substantially absent.
[0024] As used herein, the term "degree of hydrolysis" refers to the mole percentage of vinyl acetate units that are converted to vinyl alcohol units when polymerized vinyl alcohol is hydrolyzed.
[0025] As used herein, when the term "about" modifies a particular value, the term refers to a range equal to the particular value plus or minus twenty percent (+ / -20%). For any of the embodiments disclosed herein, in various alternative embodiments, any disclosure of a particular value may also be understood to be a disclosed range approximately equal to the particular value (i.e., + / -20%).
[0026] As used herein, when the term "about" modifies a particular value, the term refers to a range equal to the particular value plus or minus fifteen percent (±15%). For any of the embodiments disclosed herein, in various alternative embodiments, any disclosure of a particular value may also be understood to be a disclosed range approximately equal to the particular value (i.e., ±15%).
[0027] As used herein, when the term "substantially" modifies a particular value, the term refers to a range equal to the particular value plus or minus ten percent (±10%). For any of the embodiments disclosed herein, in various alternative embodiments, any disclosure of a particular value may also be understood to be approximately equal to the disclosed range of the particular value (i.e., ±10%).
[0028] As used herein, when the term "almost" modifies a particular value, the term refers to a range equal to the particular value plus or minus five percent (±5%). For any of the embodiments disclosed herein, in various alternative embodiments, any disclosure of a particular value may also be understood as a disclosed range approximately equal to the particular value (i.e., ±5%).
[0029] Figure 1 A cross section of a paper or board layer 10 is shown. The paper or board layer 10 has a first surface 12 and a second surface 14 opposite the first surface 12, a thickness 116 between the surfaces 12 and 14, and a grammage obtained from the density and the thickness 116.
[0030] The grammage of the paper layer 10 may be about 20 g / m 2 About 200g / m 2 , preferably about 40g / m 2 About 120g / m 2 , more preferably about 50 g / m 2 About 100g / m 2 , and more preferably about 60 g / m 2 Up to 85g / m 2 The weight of the board layer 10 may be about 150 g / m2 About 500g / m 2 , preferably about 190g / m 2 About 380g / m 2 , more preferably about 230 g / m 2 About 260g / m 2 within the range.
[0031] Figure 2 A cross-section of an adhesive layer 20 is shown, the adhesive layer having a first surface 22 and a second surface 24 opposite the first surface 22 and a thickness 216 between the first surface 22 and the second surface 24, the adhesive layer being applied to substantially cover at least one of the first surface 12 or the second surface 14 of the paper or board layer 10.
[0032] The thickness 216 of the adhesive layer 20 may range from about 1 μm to about 120 μm, preferably about 1 μm to about 25 μm, more preferably about 1 μm to about 10 μm, and even more preferably between 1 μm and about 5 μm.
[0033] The adhesive layer 20 may include at least one water-soluble polymer. Depending on the application, the water-soluble polymer may be selected from the available options to dissolve in water at 23° C. in seconds, minutes, or hours. A polymer that takes more than 24 hours to dissolve in water at 23° C. will not be considered water-soluble.
[0034] Figure 3 A cross-section of a water-dispersible nanocomposite barrier layer 30 is shown, the water-dispersible nanocomposite barrier layer having a first surface 32 and a second surface 34 opposite the first surface 32 and a thickness 316 between the first surface 32 and the second surface 34, the water-dispersible nanocomposite barrier layer being applied to substantially cover at least one of the first surface 22 or the second surface 24 of the adhesive layer 20.
[0035] The thickness of the water-dispersible nanocomposite barrier layer 30 is in the range of about 0.1 μm to about 20 μm, preferably about 0.1 μm to about 10 μm, and more preferably about 0.1 μm to about 5 μm.
[0036] The water-dispersible nanocomposite barrier layer 30 is a nanocomposite comprising nanoscale ordered spaced hydrophilic nanosheets and intercalated polymer fillers, wherein the basal spacing measured by XRD is less than Preferably less than More preferably, less than
[0037] Figure 6A cross-sectional image obtained via transmission electron microscopy (TEM) of one embodiment of a water-dispersible nanocomposite barrier according to the present invention is shown, wherein the basal spacing measured via XRD is equal to Showing the ordered spacing of hydrophilic hectorite nanosheets ( Thick dark lines) and intercalated polyethylene glycol (PEG) fillers ( Thick bright lines), which repeat regularly at the nanoscale.
[0038] Nanosheets are flaky nanoparticles characterized by a high aspect ratio between diameter and orthogonal height. The high aspect ratio enables the formation of a "brick wall" in which the nanosheets are laid parallel to the surface of the underlying water-soluble polymer layer, overlapping each other and placed on top of each other, thus significantly reducing the migration of molecules (whether gaseous or liquid) through the nanosheet layer. The higher the aspect ratio, the higher the barrier properties that can be obtained. The typical aspect ratio of montmorillonite exfoliated nanosheets is about 100 or greater (Cadène et al., JCIS 285 (2): 719-30, June 2005).
[0039] The water-dispersible nanocomposite barrier layer 30 according to the present invention can be optically opaque, preferably translucent, and even more preferably transparent, depending on the nanocomposite (nanosheet exfoliation level, polymer intercalation between nanosheets, impurity level) and the nanocomposite application process (nanocomposite orientation).
[0040] Preferably, the water-dispersible nanocomposite barrier layer 30 is flexible. When the paper laminate of the present disclosure is converted through a production line for printing, sheeting, slitting, rewinding and other typical converting operations, or when an article such as a pouch containing the paper laminate of the present disclosure is prepared, the entire structure is typically folded, bent and sometimes slightly stretched. This can cause defects in the barrier layer, reducing the barrier properties. Therefore, it is preferred that the barrier layer 30 is slightly flexible and can be stretched without breaking as the rest of the structure is stretched. Preferably, the barrier layer 30 can be stretched by at least 1%, at least 2%, at least 5% as the paper layer, adhesive layer and sealing layer stretch. In some cases, it may be necessary for the barrier layer to stretch up to 10% or even up to 20% without breaking. In one embodiment, this is achieved by dividing the water-dispersible nanocomposite barrier layer into a plurality of different water-dispersible nanocomposite barrier sublayers separated by a plurality of different water-soluble polymer sublayers.
[0041] Figure 4A cross section of a paper laminate of the present disclosure is shown, the paper laminate comprising a paper or board layer 10 having a first surface 12 and a second surface 14 opposite the first surface 12 and a thickness 116 between the first surface 12 and the second surface 14. Attached to the paper or board layer 10 is an adhesive layer 20 having a first surface 22 and a second surface 24 opposite the first surface 22 and a thickness 216 between the first surface 22 and the second surface 24 and substantially covering at least one of the first surface 12 or the second surface 14 of the paper or board layer 10. Attached to the adhesive layer 20 is a water-dispersible nanocomposite barrier layer 30 having a first surface 32 and a second surface 34 opposite the first surface 32 and a thickness 316 between the first surface 32 and the second surface 34 and substantially covering the second surface 24 of the adhesive layer 20. Attached to the water-dispersible nanocomposite barrier layer is a sealing layer 40 having a first surface 42 and a second surface 44 opposite the first surface 42 and a thickness 416 between the first surface 42 and the second surface 44, and substantially covering the surface 32 of the water-dispersible nanocomposite barrier layer 30. Adhesion between the layers is provided by the interaction between the adhesive layer 20 or the sealing layer 40 and the water-dispersible nanocomposite barrier layer 30.
[0042] The thickness of the sealing layer 40 between the first surface 42 and the second surface 44 may be in the range of about 1 μm to about 1000 μm, preferably about 1 μm to about 200 μm, more preferably about 1 μm to about 40 μm.
[0043] The sealing layer 40 may include at least one water-soluble polymer. Depending on the application, the water-soluble polymer may be selected from the available options to dissolve in water at 23° C. in seconds, minutes, or hours. A polymer that takes more than 24 hours to dissolve in water at 23° C. will not be considered water-soluble.
[0044] Each layer according to the present invention is distinct and separate from each other. By distinct, it is meant that the water-dispersible nanocomposite barrier layer 30 within the adhesive layer 20 and the sealant layer 40 comprises substantially only the nanocomposite barrier material, and that the boundary between the water-dispersible nanocomposite barrier layer 30 and the surrounding adhesive layer 20 and the sealant layer 40 is distinguished by a large composition change over a small distance, thereby producing a sharp boundary that is easily seen by microscopy techniques known in the art. The boundary layer, i.e., the intermediate layer of intermediate composition between the water-dispersible nanocomposite barrier layer and the adjacent adhesive layer and the sealant layer, is no more than 2 μm thick, as seen by microscopy techniques known in the art.
[0045] Figure 5A cross-sectional image obtained via scanning electron microscopy (SEM) of a paper laminate of the present disclosure is shown, the paper laminate comprising a paper layer or board layer coated with an adhesive layer, a water-dispersible nanocomposite barrier layer, and a sealant layer.
[0046] In one embodiment, the adhesive layer and sealing layer of the present invention are water soluble. When immersed in water (e.g., if the waste is managed, it is a paper recycling process; or if the waste is improperly discarded, it is an aquatic environment), the adhesive layer and sealing layer will be dissolved and their components will be digested by bacteria (if recycled, it occurs in a water treatment plant; or if collected, it is composted in a home or industrial composting facility; or if improperly discarded, it is in an aquatic environment (river, ocean)). In the absence of surrounding and supporting water-soluble adhesive layers and sealing layers, the water-dispersible nanocomposite barrier layer will decompose after immersion in water, and the nanocomposite barrier material will be digested as organic material, or will be dispersed as mineral-enriched soil, whether the waste is preferably managed or improperly discarded. This makes the paper or board completely uncoated and easy to recycle and / or biodegrade, because the paper or board is preferably selected from recyclable and / or biodegradable grades.
[0047] If properly handled in a paper recycling system, the water-soluble adhesive layer and sealant layer must dissolve readily when stirred into large quantities of warm water. For a typical current industrial repulping facility, paper packaging must fall apart within 5 to 20 minutes of soaking in warm water under constant vigorous agitation.
[0048] If improperly discarded in the environment, the water-soluble adhesive layer and the sealing layer must also quickly fall apart, thereby exposing the maximum surface area to the bacteria responsible for biodegradation, ensuring complete digestion within a reasonable time. Preferably, the package will biodegrade within 6 to 12 months. And if the paper laminate of the present disclosure is composted, it must undergo complete disintegration and digestion according to established standards.
[0049] The paper laminates of the present disclosure may include a printed area. Printing may be achieved using standard printing techniques such as flexographic printing, gravure printing, or inkjet printing. The paper laminates of the present disclosure may include a surface coating for appearance protection purposes to prevent accidental water or for matte / high gloss effects.
[0050] Paper or board
[0051] Cellulosic fibers used to make paper or board can be derived from softwoods, hardwoods, and non-tree fibers, which generally have shorter fibers, including bamboo, grass, kenaf, flax, corn husks, cotton stalks, coffee grounds, bagasse, rice straw, wheat straw, algae, abaca, sabia grass, esparto grass, milkweed fibers, pineapple leaf fibers, wood fibers, pulp fibers, and the like.
[0052] The paper or board layers used to prepare the paper laminates according to the present disclosure are preferably recyclable in a typical paper recycling stream, and are also preferably biodegradable, leaving no persistent materials in the environment. In practice, paper and board are not made of only 100% cellulose fibers, but also contain polymer binders, mineral adhesives, brighteners, surfactants and other additives. These other ingredients must be appropriately selected to ensure that (a) the paper or board will disintegrate in a repulping unit at a recycling facility and release a maximum amount of cellulose fibers for making recycled paper or board, or (b) the paper or board will biodegrade if improperly disposed of in the environment.
[0053] The effectiveness of the recycling process can be determined via the recyclable percentage. The recyclable percentage of the paper laminate of the present disclosure is determined via the test method PTS-RH:021 / 97 (draft in October 2019) under Category II, performed by Papiertechnische Stiftung (Pirnaer Strasse 37, 01809 Heidenau, Germany). Together with the recyclable percentage, the total percentage of defectives is determined via PTS-RH:021 / 97 (draft in October 2019) under Category II. The total percentage of defectives of the packaging material of the present disclosure may be 40% or less, 30% or less, or 10% or less, specifically including all values within these ranges and any ranges formed therein or thereby. For example, the total percentage of defectives of the packaging material of the present disclosure may be from about 0.5% to about 40%, from about 0.5% to about 30%, or from about 0.5% to about 10%, specifically listing all values within these ranges and any ranges formed therein or thereby.
[0054] It is believed that the percentage of non-recyclable material does not necessarily have a 1:1 correlation with the total reject percentage. For example, dissolvable adhesives and / or coatings are designed to dissolve during the recycling process. In theory, these adhesives may not affect the total reject percentage; however, they will increase the weight percentage of non-recyclable material.
[0055] Test method PTS-RH:021 / 97 (draft October 2019) under Category II also includes a visual component. Trained screeners inspect one or more sheets of recycled packaging material for cosmetic defects. If the number of cosmetic defects is too high, the packaging material is rejected. If the number of visual defects according to test method PTS-RH:021 / 97 (draft October 2019) under Category II is acceptable, the packaging material is approved for additional processing. The paper laminates of the present invention can produce an acceptable level of visual defects during this step of the method.
[0056] The paper laminates of the present disclosure can produce the previously mentioned recyclable percentages and pass the visual screening method. Therefore, when subjected to the test method PTS-RH:021 / 97 (October 2019 draft) under Category II, the paper laminates of the present disclosure can achieve an overall score or final result of "pass".
[0057] It is also worth noting that there are alternative methods for determining the recyclable percentage of the paper laminates of the present disclosure. A test method known as the Repulpability Test Method performed by the University of Western Michigan can provide a percentage yield of recyclable materials. Although there are slight differences between the Repulpability Test Method performed by Western Michigan and the test method PTS-RH:021 / 97 (October 2019 draft) under Category II, it is believed that the percentage yield of the Repulpability Test Method will be similar to the recyclable percentage provided by the test method PTS-RH:021 / 97 (October 2019 draft) under Category II.
[0058] For commercial reasons it is also important that the recycling facility can obtain at least 50 wt. % cellulose fibers from an incoming batch of waste paper or board. For this purpose it is preferred that the paper or board comprises at least between 50 wt. % and 100 wt. % cellulose fibers, more preferably between 65 wt. % and 90 wt. % cellulose fibers, most preferably between 75 wt. % and 95 wt. % cellulose fibers.
[0059] It is contemplated that the paper laminates of the present disclosure, while being recyclable, may themselves contain recycled materials. For example, the paper or board of the present invention may contain greater than 10 wt. %, preferably greater than 20 wt. %, more preferably greater than 30 wt. % recycled materials, with all values within these ranges and any ranges derived therefrom being specifically recited. The paper or board may contain between 0% and 100% virgin or recycled cellulose fibers or mixtures thereof.
[0060] The presence of recycled materials can be detected by visual inspection of the packaging. Typically, manufacturers often promote the use of recycled materials to prove their eco-friendly image. To this end, they may use a logo such as a leaf and text indicating that recycled materials are used in the packaging. Manufacturers may also specify the percentage of recycled materials used, such as more than 50%, more than 70%, etc.
[0061] The visual inspection may simply utilize the human eye to search for signs of the use of recycled materials. Additionally or alternatively, the visual inspection may include microscopy, such as optical microscopy, scanning electron microscopy, or other suitable methods known in the art. For example, packaging materials containing recycled cellulosic fibers may appear different under a microscope due to the presence of a wider range of natural fibers than packaging materials containing 100% virgin fibers.
[0062] It is preferred that the paper or board is as flat as possible on at least one side, which is then coated with an adhesive layer. The paper can be flattened via "sizing", which means in the industry that it can be coated with an aqueous polymer suspension containing various inorganic fillers (such as clay, calcium carbonate and / or titanium dioxide), the suspension is then dried, and the paper is calendered to obtain a flatter surface than before sizing, because the inorganic fillers and binders are dehydrated to fill the porous rough surface of the paper. Alternatively, the paper can be mechanically glazed during the papermaking process by a mechanical ironing / pressing step, which sometimes involves heating, in which case the cellulose fibers are squeezed together and flattened in order to densify the paper surface and remove porosity. In some cases, sizing and mechanical glazing are combined to obtain an even flatter, more perfect surface during the papermaking process, which is then coated with an adhesive layer. In other cases, kraft paper or glass paper or tracing paper that is already naturally very flat can be used, such papers are made by a method that densifies the paper structure throughout its thickness during the manufacturing process, and no further sizing or glazing is required.
[0063] Examples of suitable papers for preparing paper laminates according to the present disclosure include, but are not limited to: Leine Paper (weight 85g / m 2 ), mechanically glossy paper with "OK Home Compost" certification; NiklaSelect V natural linen paper (99 g / m 2 ), paper with sizing on only one side; PackPro 7.0 paper (65 g / m 2 ), paper sized on both sides; obtained from Axello paper (Solna, Sweden); (including Axello tough white paper, 80g / m2 ), which is designed to be tougher than many other papers and therefore may have some advantages in the distribution chain; SCG glassine paper (58 g / m 2 Examples of suitable boards for preparing paper laminates according to the present disclosure include, but are not limited to, Cupforma Natura boards (170 g / m 2 Up to 330g / m 2 ) and Natura board (233g / m 2 Up to 350g / m 2 ).
[0064] As shown in Table 1 below, these papers have all passed the paper recycling programs of Western Michigan University in the United States and the PTS Institute in Germany. These papers have also passed the OECD 301B biodegradation screening test, undergoing at least 60% biodegradation within 28 days.
[0065] Table 1
[0066]
[0067] In order to withstand the stresses of a high speed manufacturing process where a product is placed in a package made from the paper laminates of the present disclosure, as well as the stresses of transportation, the paper layers must be sufficiently strong and resilient. There are numerous ways to specify paper layers. The metrics discussed below are MD tensile strength in kN / m, CD tensile strength in kN / m, MD stretch in percent, CD stretch in percent, MD burst strength in kPa, thickness in μm, MD tensile energy absorption in J / g, CD tensile energy absorption in J / g, and g / m 2 Although all of the metrics can be used in combination to select the appropriate paper in the present invention, some of the metrics alone or in combination with other metrics may also meet the requirements.
[0068] In cases where a very strong paper is required to maintain the physical integrity of the water dispersible nanocomposite barrier layer, it is preferred to use paper available from of For example, Table 2 below shows the of Properties of a tough white paper grade or Advantage Smooth White Strong paper from Mondi.
[0069] Table 2
[0070]
[0071] Water dispersible nanocomposites
[0072] The nanocomposite material comprises nanoscale ordered hydrophilic nanosheets and intercalated polymer fillers, wherein the basal spacing measured by XRD is less than Preferably less than More preferably, less than
[0073] Nanosheets are solid flaky nanoparticles characterized by a high aspect ratio between diameter and orthogonal height. The high aspect ratio provides parallel arrangement of nanosheets and a longer diffusion path length for chemicals through the nanosheets, thus providing a barrier function. It is desirable that the nanosheets have no defects such as cracks and holes that reduce barrier properties. It is also desirable that the nanosheets are easily peeled off in water for both application purposes (e.g., wet coating) and end-of-life situations (e.g., wastewater treatment plants), but have high viscosity when dried. Nanosheets are currently used in industry as rheology modifiers, flame retardants, anti-corrosion coatings, and / or chemical barriers. Nanosheets can be obtained from natural sources and used as is, or can be purified and modified from natural sources, or can be synthesized in a furnace for purity and performance reasons.
[0074] Natural phyllosilicates (such as serpentine, clay, chlorite and mica) consist of nanosheets stacked together. Natural clays (such as montmorillonite and vermiculite) consist of nanosheets stacked together and swell in the presence of water. Smectites (such as montmorillonite and hectorite) consist of nanosheets stacked together and swell most easily in the presence of water. Natural montmorillonite can be purified and modified, such as sodium Crosette from BYK, which is made of bentonite (a natural mineral containing 60% to 80% montmorillonite) and cation exchanged with monovalent sodium for stripping purposes. Montmorillonite can also be synthesized, such as synthetic hectorite from BYK and sodium hectorite from the University of Bayreuth.
[0075] Water soluble polymer
[0076] In some embodiments, the adhesive layer and / or the sealing layer are made of a water-soluble polymer. Such water-soluble polymers are selected from polyvinyl alcohol (PVOH), polyvinyl alcohol copolymers (such as butene glycol-vinyl alcohol copolymer (BVOH)), which are produced by copolymerization of butene glycol and vinyl acetate, followed by hydrolysis of vinyl acetate, and suitable butene glycol monomers are selected from 3,4-diol-1-butene, 3,4-diacyloxy-1-butene, 3-acyloxy-4-ol-1-butene, 4-acyloxy-3-ol-1-butene, etc.; polyvinyl pyrrolidone; polyalkylene oxides, such as polyethylene oxide or polyethylene glycol (PEG); poly(methacrylic acid), polyacrylic acid, polyacrylic acid Esters, acrylate copolymers, maleic acid / acrylic acid copolymers; polyacrylamide; poly(2-acrylamido-2-methyl-1-propane sulfonic acid (polyAMPS); polyamides, poly-N-vinylacetamide (PNVA); polycarboxylic acids and salts; cellulose derivatives such as cellulose ethers, methylcellulose, hydroxyethylcellulose, carboxymethylcellulose; hydroxypropyl methylcellulose; natural gums such as xanthan gum and carrageenan; sodium alginate; maltodextrin, low molecular weight dextrin; polyamino acids or peptides; proteins such as casein and / or caseinates (e.g., as commercialized by Lactips).
[0077] Preferred water-soluble polymers are polyvinyl alcohol, polyethylene oxide, methylcellulose and sodium alginate. For applications requiring a "plastic-free" product, the water-soluble polymer layer may be a naturally derived water-soluble polymer such as sodium alginate. Preferably, the content of polymer in the water-soluble adhesive layer and the sealing layer is at least 60%.
[0078] The average molecular weight of the water-soluble polymer (measured by gel permeation chromatography) is about 1,000Da to about 1,000,000Da, or any integer value of about 1,000Da to about 1,000,000Da, or any range formed by any of the aforementioned values, such as about 10,000Da to about 300,000Da, about 20,000Da to about 150,000Da, etc. More specifically, the molecular weight of polyvinyl alcohol will have a molecular weight in the range of 20,000Da to 150,000Da. The molecular weight of polyethylene oxide will be in the range of 50,000Da to 400,000Da. The molecular weight of methylcellulose will be in the range of 10,000Da to 100,000Da. The molecular weight of sodium alginate will be in the range of 10,000Da to 240,000Da.
[0079] If a homopolymer polyvinyl alcohol is used, the degree of hydrolysis can be from 70% to 100%, or any integer percentage value between 70% and 100%, or any range formed by any of these values, such as 80% to 100%, 85% to 100%, 90% to 100%, 95% to 100%, 98% to 100%, 99% to 100%, 85% to 99%, 90% to 99%, 95% to 99%, 98% to 99%, 80% to 98%, 85% to 98%, 90% to 98%, 95% to 98%, 80% to 95%, 85% to 95%, 90% to 95%, etc.
[0080] Optional Ingredients
[0081] The adhesive layer and sealant layer of the paper laminate of the present disclosure may contain disintegrants, plasticizers, surfactants, lubricants / release agents, fillers, extenders, antiblocking agents, anti-adhesive agents, defoaming agents, or other functional ingredients.
[0082] Certain applications may require that the adhesive layer and sealing layer of the present disclosure include disintegrants to increase their dissolution rate in water. Suitable disintegrants are, but are not limited to, corn / potato starch, methylcellulose, mineral clay powders, cross-linked carboxymethyl cellulose (cross-linked cellulose), crospovidone (cross-linked polyvinyl N-pyrrolidone or PVP), sodium starch glycolate (cross-linked starch). Preferably, the adhesive layer and sealing layer include between 0.1% and 15% by weight, more preferably about 1% to about 15% by weight of disintegrant.
[0083] In some embodiments, the adhesive layer and sealing layer of the present disclosure may include a water-soluble plasticizer. Preferably, the water-soluble plasticizer is selected from water, polyols, sugar alcohols and mixtures thereof. Suitable polyols include polyols selected from the group consisting of glycerol, diglycerol, ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol of up to 400Da molecular weight, neopentyl glycol, 1,2-propylene glycol, 1,3-propylene glycol, dipropylene glycol, polypropylene glycol, 2-methyl-1,3-propanediol, methylene glycol, trimethylolpropane, hexylene glycol, neopentyl glycol and polyether polyols, or mixtures thereof. Suitable sugar alcohols include sugar alcohols selected from the group consisting of isomalt, maltitol, sorbitol, xylitol, erythritol, ribitol, galactitol, pentaerythritol and mannitol, or mixtures thereof. In some cases, the plasticizer may be selected from the following list: ethanolamine, alkyl citrate, isosorbide, pentaerythritol, glucosamine, N-methylglucosamine or sodium cumene sulfonate. Less mobile plasticizers such as sorbitol or polyethylene oxide may promote the formation of a water-soluble polymer layer with greater barrier properties than a water-soluble polymer layer including a more mobile plasticizer such as glycerol. In some cases, when it is desired to use as much naturally derived materials as possible, the following plasticizers may also be used: vegetable oils, polysorbate, polydimethylsiloxane, mineral oil, paraffin, C1-C3 alcohols, dimethyl sulfoxide, N,N-dimethylacetamide, sucrose, corn syrup, fructose, dioctyl sodium sulfosuccinate, triethyl citrate, tributyl citrate, 1,2-propylene glycol, monoacetate, diacetate or triacetate of glycerol, natural gums, citrates and mixtures thereof. More preferably, the water-soluble plasticizer is selected from glycerol, 1,2-propylene glycol, 20 dipropylene glycol, 2-methyl-1,3-propanediol, trimethylolpropane, triethylene glycol, polyethylene glycol, sorbitol, or mixtures thereof, most preferably selected from glycerol, sorbitol, trimethylolpropane, dipropylene glycol, and mixtures thereof. Preferably, the water-soluble polymer layer comprises between 5 wt % and 50 wt %, preferably between 10 wt % and 40 wt %, even more preferably about 12 wt % to about 30 wt % of plasticizer.
[0084] In some embodiments, the adhesive layer and sealing layer of the present disclosure include surfactants. Suitable surfactants can belong to nonionic, cationic, anionic or zwitterionic categories. Suitable surfactants are but not limited to poloxamer (polyoxyethylene polyoxypropylene glycol), alcohol ethoxylates, alkylphenol ethoxylates, tertiary acetylenic glycols and alkanolamides (nonionic), polyoxyethylene amines, quaternary ammonium salts and polyoxyethylene quaternary amines (cationic) and amine oxides, N-alkyl betaines and sulfobetaines (zwitterionic). Other suitable surfactants are acylated fatty acid esters of sodium sulfosuccinate, glycerol and propylene glycol, fatty acid lactyl fat, alkyl sodium sulfate, polysorbate 20, polysorbate 60, polysorbate 65, polysorbate 80, lecithin, glycerol and propylene glycol and acetylated esters of 5 kinds of fatty acids and their combinations. Preferably, the water-soluble polymer layer includes a surfactant between 0.1% by weight and 2.5% by weight, more preferably about 1% by weight to about 2% by weight.
[0085] In some embodiments, the adhesive layer and the sealing layer of the present disclosure contain a lubricant / stripping agent. Suitable lubricants / stripping agents are, but are not limited to, fatty acids and their salts, fatty alcohols, fatty acid esters, fatty amines, fatty amine acetates, and fatty amides. Preferred lubricants / stripping agents are fatty acids, fatty acid salts, fatty amine acetates, and mixtures thereof. Preferably, the water-soluble polymer layer contains 0.02 wt % to 1.5 wt %, preferably about 0.1 wt % to about 1 wt % of the lubricant / stripping agent.
[0086] In some embodiments, adhesive layer and sealing layer of the present disclosure comprise filler, extender, anti-adhesive agent, release agent.Suitable filler, extender, anti-adhesive agent, release agent are but not limited to starch, modified starch, cross-linked polyvinyl pyrrolidone, cross-linked cellulose, microcrystalline cellulose, silicon dioxide, metal oxide, calcium carbonate, talc and mica.Preferably, water-soluble polymer layer is included in filler, extender, anti-adhesive agent, release agent between 0.1 % by weight and 25 % by weight, more preferably about 1 % by weight to about 15 % by weight.In the absence of starch, water-soluble polymer layer comprises filler, extender, anti-adhesive agent preferably between 1 % by weight and 5 % by weight.
[0087] In some embodiments, the adhesive layer and the sealing layer of the present disclosure include a defoamer. Suitable defoamers are, but are not limited to, polydimethylsiloxane and hydrocarbon blends. Preferably, the water-soluble polymer layer includes between 0.001 wt % and 0.5 wt %, more preferably between about 0.01 wt % and about 0.5 wt % of the defoamer.
[0088] Water-insoluble biodegradable polymer
[0089] In some embodiments, the sealable layer is made of a water-insoluble biodegradable polymer.
[0090] In one case, biodegradable aliphatic polyesters and copolyesters can be produced by large-scale bacterial fermentation. Collectively referred to as polyhydroxyalkanoates, also known as "PHAs," these polymers can be harvested in fermentation plants by plants or bacteria fed with specific substrates, such as glucose. In many cases, the structure or mechanical properties of PHAs can be customized to meet the specifications of the desired application. PHAs and their copolymers can be degraded aerobically and anaerobically. This makes them particularly suitable for composting or rapid and complete degradation in the environment. Such bioplastics are typically suspended in aqueous emulsions and can be dried into films on various substrates, although they can also be extruded into films and coatings.
[0091] PHA is available as a copolymer, which is commercially available as a film grade for extrusion and blow molding from ShenZhen Ecomann Biotechnology Co., Danimer Scientific, Inc., which produces poly(β-hydroxyalkanoate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (NODAXTM), or Kaneka, which produces poly(3-hydroxybutyrate-co-3-hydroxyhexanoate). Non-limiting examples of PHA copolymers include those described in U.S. Pat. No. 5,498,692. Other PHA copolymers can be synthesized by methods known to those skilled in the art, such as by microorganisms, ring-opening polymerization of β-lactones, dehydration polycondensation of hydroxyalkanoic acids, and dealcoholization polycondensation of hydroxyalkanoic acid alkyl ethers, as described in Volova, "PolyhydroxyAlkanoates Plastic Materials of the 21" Century: Production, Properties, and Application, Nova Science Publishers, Inc., (2004), which is incorporated herein by reference.
[0092] Other possible biodegradable water-insoluble polymers may include biodegradable thermoplastic materials selected from the group consisting of aliphatic aromatic polyesters such as those sold under the trade name Polybutylene adipate terephthalate (PBAT) was purchased from BASF (Germany), or under the trade name Biodegradable blends of polybutylene adipate terephthalate (PBAT) and polylactic acid (PLA) available from BASF (Germany); the group of thermoplastic starches, such as blends of aliphatic polyesters and starch available under the trade name Mater-Bi from Novamont (Italy) or Plantic (Australia); the group of polybutylene succinate adipate (PBSA), which is available under the trade name BioPBS TM Purchased from Mitsubishi Chemicals (Japan).
[0093] Method for preparing nanocomposite barrier paper laminate
[0094] There are many non-limiting embodiments of methods of making the paper laminates described herein including the water-dispersible nanocomposite barriers. Figure 7 As shown, paper laminates comprising a water-dispersible nanocomposite barrier can be produced by multiple steps of coating and drying of the aqueous dispersion under specific conditions.
[0095] In one non-limiting embodiment, a method of preparing a paper laminate including a water dispersible nanocomposite barrier consists of:
[0096] a) applying a first aqueous polymer dispersion to the surface of a paper or board layer 10 which is sized, glazed, or both sized and glazed
[0097] b) Removing water from the polymer dispersion to obtain an adhesive layer 20
[0098] c) applying an aqueous nanocomposite dispersion onto the surface of the adhesive layer 20
[0099] d) removing water from the nanocomposite dispersion to obtain a water dispersible nanocomposite barrier layer 30
[0100] e) applying a second aqueous polymer dispersion onto the surface of the water-dispersible nanocomposite barrier layer 30
[0101] f) removing water from the second polymer dispersion to obtain a sealing layer 40
[0102] This method provides better bond strength between the paper or board layer 10 and the water-dispersible nanocomposite barrier layer 30. It is also simpler to practice from an industrial point of view. However, it limits the choice of paper or board to those suitable for coating with aqueous dispersions, such as paper sizing on at least one side, or paper mechanically glazed on at least one side, or kraft paper or glassine paper. In some cases, sizing and mechanical glazing can be combined to obtain a flatter surface of the paper or board.
[0103] In another non-limiting embodiment, a method of preparing a paper laminate comprising a water dispersible nanocomposite barrier consists of:
[0104] a) Applying the aqueous nanocomposite dispersion to the surface of the sealable film 40
[0105] b) Removing water from the nanocomposite dispersion to obtain a water dispersible nanocomposite barrier layer 30
[0106] c) applying an aqueous polymer dispersion onto the surface of the water-dispersible nanocomposite barrier layer 30
[0107] d) removing water from the polymer dispersion to obtain an adhesive layer 20
[0108] e) Laminating the paper layer or board layer 10 onto the surface of the adhesive layer 20
[0109] The method provides better barrier properties, since the sealable film can be manufactured with a completely flat surface. It also offers the advantage of being rather insensitive to the porosity and surface roughness of the paper or board layer. Thus, a paper laminate comprising a water-dispersible nanocomposite barrier can be obtained according to this method starting from a paper or board layer that has neither surface glazing nor sizing.
[0110] In order to prepare the adhesive layer 20 and / or the sealing layer 40 from an aqueous polymer dispersion, the starting materials must first be dissolved or dispersed in water. The resulting aqueous polymer dispersion will typically contain 20% to 40% solids, depending on the coating process selected for the application. The aqueous polymer dispersion is then coated onto a given substrate and the water is removed via an IR, convection or diffusion drying process.
[0111] Without being limited by theory, it is believed that the most important material properties of the aqueous polymer dispersion are: a) the solids content at a given temperature between 20°C and 95°C; b) the viscosity of the aqueous polymer dispersion obtained at that temperature, with higher viscosities being better for maximum differentiation / separation between layers; c) the wetting of the aqueous polymer dispersion on a flat paper or board, or on a water-dispersible nanocomposite barrier layer, with higher wetting being more advantageous.
[0112] To prepare the water-dispersible nanocomposite barrier layer 30, an aqueous nanocomposite dispersion is typically formed by taking water-dispersible nanosheets in solid form and exfoliating them first in water. The aqueous nanosheet dispersion is then further mixed with an aqueous polymer solution under moderate stirring. The resulting aqueous nanocomposite dispersion will typically contain 1% to 10% solids, depending on the coating process selected for the application. The aqueous nanocomposite dispersion is then coated onto a given substrate, and the water is subsequently removed via an IR, convection or diffusion drying process.
[0113] Without being limited by theory, it is believed that the most important material properties of the nanocomposite are: a) the aspect ratio of the nanosheets (higher aspect ratio is better for barrier performance); b) the overall exfoliation and dispersion of the nanosheets in water to maximize barrier properties; c) the choice of polymer filler and the weight ratio between nanosheets and polymer filler to minimize the basal spacing between nanosheets without phase separation, thereby maximizing barrier properties.
[0114] Without being limited by theory, it is also believed that the most important processability properties of the aqueous nanocomposite dispersion are: a) the viscosity of the aqueous nanocomposite dispersion, with higher viscosity favoring maximum differentiation / separation between the layers and, therefore, maximum barrier properties; b) the wetting of the aqueous nanocomposite dispersion on the adhesive layer, or on another aqueous dispersible nanocomposite layer, or on the sealant layer; c) the shear applied to the aqueous nanocomposite dispersion, with higher shear favoring parallel nanosheet orientation with respect to the barrier plane; d) the removal of water from the dispersion via diffusion drying without creating defects (such as pinholes or cracks) in the nanocomposite barrier layer.
[0115] Many processes for coating aqueous nanocomposite dispersions were tested: wire rod coating, anilox roll coating, reverse roll coating, slot die extrusion coating, roll-to-roll coating, and spray coating. Aqueous extrusion coating via a customized slot die (e.g., FMP Technology, Coatema) proved to be the most reliable process for providing the correct transverse feed of aqueous nanocomposite dispersions. Coating processes that provide excellent shear of the aqueous nanocomposite dispersions are preferred because the excellent shear provides excellent parallel orientation of the nanosheets within the nanocomposite barrier layer, resulting in excellent barrier properties. However, the barrier properties also depend on the total thickness of the water-dispersible nanocomposite barrier layer. Typically, the thickness of the water-dispersible nanocomposite barrier layer is in the range of 0.1 μm to 10 μm to provide sufficient barrier properties while maintaining sufficient mechanical flexibility and mechanical resistance.
[0116] In another non-limiting embodiment of the method, the water-dispersible nanocomposite barrier layer 30 is obtained by multiple application steps of coating and drying an aqueous nanocomposite dispersion, each nanocomposite sublayer masks the assumed defects in the underlying nanocomposite sublayer, thereby providing maximum barrier properties. To this end, a first water-dispersible nanocomposite barrier sublayer is formed on the adhesive layer 20 according to any of the above methods; subsequently, one or more additional water-dispersible nanocomposite barrier sublayers can be added until the desired water-dispersible nanocomposite layer thickness is obtained. According to this method, a relatively thick water-dispersible nanocomposite layer can be formed. In the case of increasing optical transparency and mechanical flexibility, additional water-dispersible nanocomposite barrier sublayers can be separated by additional thinner water-soluble polymer sublayers. Various polymer sublayers or barrier sublayers can have substantially the same chemical composition or different chemical compositions to provide different properties to the overall structure. Adhesion between sublayers is provided by molecular interactions between water-soluble polymer sublayers and water-dispersible nanocomposite barrier sublayers. Similarly, cohesion between water-dispersible nanocomposite barrier sublayers is provided only by molecular interactions between nanocomposite barrier materials.
[0117] The drying step is usually performed by a conveyor dryer, such as Those sold under the trade name Drytec, those sold by Coatema under the trade name ModulDry and / or those sold by FMP Technologies GmbH (Erlangen, Germany) under the trade name SenDry or PureDry. In some embodiments, the drying substrate is guided through a hot air tunnel by a running belt (belt dryer), by a plurality of idler wheels (roller dryer) or by a plurality of hot air nozzles (contactless hot air dryer). Without being limited by theory, it is believed that the most important parameters of the drying process are: a) the residence time of the drying substrate in the hot air tunnel, which is typically about 50 s for a 60 μ thick aqueous polymer dispersion (wherein the polymer is water soluble and contains 25% solids); b) the temperature profile of the hot air in the tunnel, which is typically up to about 95° C.; c) the flow velocity of the hot air over the substrate, which is typically about 25 m / s. The heating system can be electric, hot oil, steam or gas.
[0118] The paper laminates of the present disclosure may contain residual moisture, which depends on the hygroscopicity and isotherms of the paper laminate components at given temperature and humidity conditions as measured by Karl Fischer titration. For example, paper may contain about 3% to 5% residual moisture at 23°C and 50% relative humidity.
[0119] Inks, Labels and Decorations
[0120] The paper laminates of the present disclosure may be opaque or translucent.The paper laminates of the present disclosure may include a printed area.Printing may be achieved using standard printing techniques such as flexographic printing, gravure printing, or inkjet printing.
[0121] The paper laminates of the present disclosure can be arranged as packages in countless configurations. For example, a package may include multiple sheets that encapsulate multiple articles. Each of these sheets includes an inner surface and an outer surface. The outer surface and / or inner surface of one or more sheets may include ink or dyes that form a trademark, packaging information, and / or background color on the package. Trademarks and / or other packaging information associated with the products in the package are set on the outer surface of at least one sheet. Trademarks may include logos, trade names, trademarks, icons, etc. related to the products in the package. Trademarks are used to inform consumers of the products in the package. The packaging information may include the size of the products related to the products in the package, the number of products in the package, exemplary images of the products contained in the package, recyclability logos, etc.
[0122] In all aspects of the invention, the deposited ink can be solvent-based or water-based, and the pigment in the ink can be organic or inorganic, or a combination of the two. In some embodiments, the ink is highly wear-resistant. For example, a highly wear-resistant ink may include a coating cured by ultraviolet radiation (UV) or electron beam (EB). In some embodiments, any organic pigment in the ink is derived from a petroleum source. In some embodiments, any organic pigment in the ink is derived from a renewable resource, such as soybeans, plants. In some embodiments, if the pigment is organic, any organic pigment in the ink will be biodegradable. In other embodiments, any inorganic pigment in the ink will be made of dispersible and environmentally friendly inorganic metal oxides.
[0123] Non-limiting examples of inks include ECO-SUREITM from Gans Ink & Supply Co. and solvent-based and BioVu™ inks, which are derived entirely from renewable resources (e.g., corn). Other examples include SunVisto AquaGreen, available from Sun Chemicals (Parsippany-Troy Hills, New Jersey).
[0124] The ink is present at a thickness of about 0.5 μm to about 20 μm, preferably about 1 μm to about 10 μm, more preferably about 2.5 μm to about 3.5 μm.
[0125] The paper laminate of the present disclosure may include ink and / or dye to provide a background color to the packaging of the present disclosure. To further illustrate the background color, it is worth noting that the paper layer or board layer includes a base color. The base color of the paper layer or board layer is the color of the packaging without ink or dye. For example, the color of bleached paper is white, the color of unbleached is brown, the color of paper derived from grass is green, and the color of paper including recyclable content is gray. The background color is any color that is not a base color, such as blue, red, green, yellow, purple, orange, black or a combination thereof. However, if the color is obtained by ink and / or dye, the background color may also include white, brown or gray.
[0126] In order to reduce the use of ink / dye to facilitate the recycling process, the natural color of the paper or board layer can be utilized. For example, the ink / dye can be used to define the background color of only the consumer-facing sheet, while the natural color of the paper or board layer will be used as the background color of the other panels of the flexible packaging.
[0127] Surface coating
[0128] Preferably, the printed surface of the paper laminate of the present disclosure is surface coated to protect the ink layer from its physical and chemical environment, to enhance the durability of the paper layer and to provide a high gloss or matte finish. This optional surface coating may be referred to as a paint or varnish or an anti-splash layer. In some embodiments, the surface coating is made of nitrocellulose paint, acrylic paint, water-based paint, reactive two-component polyurethane paint. In some preferred embodiments, the surface coating is made of a natural wax that passes the OECD301B biodegradation screening test, such as beeswax, rapeseed wax or candelilla wax, provided that the exposure temperature does not exceed the melting point of the wax. Since the thickness of the surface coating affects the ability to recycle and the biodegradability of the packaging made of the paper laminate of the present disclosure, a thinner surface coating is preferred. The thickness of the surface coating is preferably between 1 μm and 25 μm, more preferably less than 10 μm, and even more preferably less than 5 μm.
[0129] Method for preparing nanocomposite barrier paper laminate packaging
[0130] The paper laminates comprising a water-dispersible nanocomposite barrier described herein can be formed into articles, including but not limited to articles in which a typical film or sealable paper would be used as a packaging material. Such articles include but are not limited to bags, pouches, bags, flow wraps, pillow bags, and other containers. Pouches, pouches, bags, flow wraps, pillow bags, and other such containers incorporating the paper laminates comprising a water-dispersible nanocomposite barrier described herein can be prepared in any suitable manner known in the art.
[0131] The paper laminates of the present disclosure can be converted into packages and articles using a form-fill-seal method (FFS). Traditional FFS methods generally involve three consecutive steps, wherein the package or article is formed, filled, and then sealed or closed by the paper laminate, as described in U.S. Patent No. 6,293,402, which is incorporated herein by reference. In the heat sealing method, there is a temperature range above which the seal will be burned, and below which the seal will not be strong enough. The seal is provided in any sealing manner known to those skilled in the art. Sealing may include applying a continuously heated element to the paper laminate, which is then removed after sealing. The heating element may be a hot rod comprising a rotating jaw or a heating wheel. Different seal types include fin seals and overlapping seals.
[0132] Single-channel method
[0133] A well-known single-pass method of sealing using a vertical forming and filling machine is described in U.S. Pat. No. 4,521,437, which is incorporated herein by reference. In this method, a flat web material is unwound from a roll and formed into a continuous tube by sealing the longitudinal edges on the film together to form a lap seal (i.e., a fin seal). The resulting tube is pulled vertically downward to the filling station and collapsed on the cross section of the tube, the location of such a cross section is at the sealing device below the filling station. A transverse heat seal is formed by the sealing device at the collapsed portion of the tube, thereby forming an airtight seal across the tube. After the transverse seal is formed, a predetermined volume of the material to be packaged (e.g., a flowable material) enters the tube at the filling station and fills the tube upward from the above-mentioned transverse seal. Then, under the influence of the weight of the material in the tube and the weight of the film advancing mechanism on the machine, the tube falls a predetermined distance. The jaws of the sealing device are closed, collapsing the tube at a second cross section located above the air / material interface in the tube. The sealing device seals and cuts the tube transversely at the second cross section. The material-filled portion of the tube is now in the form of a pillow-shaped pouch. In this way, the sealing device seals the top of the filled pouch, seals the bottom of the next pouch to be formed, and separates the filled pouch from the next pouch to be formed in one operation.
[0134] Multi-channel approach
[0135] The package of the present disclosure may also be processed using a multi-channel pouch packaging machine (such as the VEGA PACK300S produced by QuadroPack (Nijeveen, the Netherlands). A high-speed multi-channel pouch processing machine is also described in U.S. Patent No. 6,966,166, which is incorporated herein by reference. The machine used in the method includes two rollers for distributing sheets of web film of equal size, a plurality of sealing devices suitable for such substrates and devices, such as a pump station described below for inserting contents (e.g., liquids, viscous materials, powders and other substances) into the film package. Multiple packages can be produced by utilizing one or more movable reciprocating brackets traveling with the film flow through the machine, which support each of the sealing and cross-cutting stations. The sealing device is applied to all edges except one edge, thereby forming a bag with a cavity and an opening. The desired contents of the package are inserted into the cavity through the opening. The opening is then sealed and separated from the substrate. A pair of substrate rollers are provided at the substrate roller station. Alternatively, a cutter can be placed in the middle of a single nip roller to divide the substrate width into two equal parts. The sheet of paper laminate is pushed through the equipment by the traction wheel station and used to form the front and back sheets of the package. The paper laminate from each roller is guided so that when the two sheets of paper laminate advance through the machine, the two sheets of paper laminate are very close to each other and in a parallel relationship. The sealing and cutting equipment includes: a longitudinal sealing strip for sealing the vertical edge of the package, a one-way roller for keeping the paper laminate in place and preventing it from sliding backward, a vertical cutter for cutting the torn slit into the package in the vertical direction, and a transverse sealing strip for sealing the package in the horizontal direction. The pump station includes a plurality of filling dispensers connected to a storage structure for containing consumer products in the package. These dispensers can extract a predetermined amount of consumer products from a reservoir and deposit it into the cavity of the paper laminate package formed by the machine. In a preferred embodiment, the pump station and dispenser can be driven by one or more motion-controlled servo motors connected to a cam system. The amount of consumer products can be changed by exchanging dispensers (different dispensers with different capacities), changing the stroke of the pump cycle, changing the timing of the pump cycle, etc. Thus, depending on the size and capacity of the packages to be formed by the machine, different amounts of consumer product may be dispensed.
[0136] The sealing mechanism may be a heat seal, a water seal, a moisture seal, an ultrasonic seal, an infrared seal, or any other type of seal deemed suitable.
[0137] Products
[0138] like Figure 8As shown, the present disclosure also includes an article comprising a product composition and a paper laminate comprising a water-dispersible nanocomposite barrier, which paper laminate can be formed into a container, such as a pouch, a sachet, a capsule, a bag, etc., to hold the product composition. For simplicity, the articles of interest herein will be described in terms of paper laminate pouches, but it should be understood that the discussion herein is also applicable to other types of containers.
[0139] The pouch formed by the foregoing method can be any form and shape suitable for holding the composition contained therein until it is desired to release the composition from the paper laminate pouch, such as by tearing it open. The pouch can include one compartment or two or more compartments (i.e., the pouch can be a multi-compartment pouch). In one embodiment, the paper laminate pouch can have two or more compartments.
[0140] In one embodiment, the paper laminate of the present disclosure can be sealed to a film without an attached paper. This can form a window into the package so that the consumer can see the product without changing the recyclability of the package.
[0141] The pouch or other container can hold a unit dose of one or more compositions from a range of products, which may include, but is not limited to, holding consumer products. As used herein, "consumer products" refers to materials such as those used for hair care, beauty care, oral care, health care, personal cleaning, and household cleaning. Non-limiting examples of consumer products include shampoo, conditioner, mousse, facial soap, hand soap, body soap, liquid soap, bar soap, moisturizer, body lotion, shaving lotion, toothpaste, mouthwash, hair spray, hand disinfectant, laundry detergent composition, dishwashing detergent, automatic dishwasher detergent composition, hard surface cleaner, stain remover, fabric enhancer and / or fabric softener, cosmetics and over-the-counter drugs, electronics, drugs, candy, pet health products, CBD-based products, other products derived from non-cannabis drugs, vitamins, non-drug natural / herbal "health" products, razors, absorbent articles, wipes, hair spray, food and beverages, animal food products, and new product forms. Typical absorbent articles of the present invention include, but are not limited to, diapers, adult incontinence briefs, training pants, diaper holders, catamenial pads, incontinence pads, liners, absorbent inserts, sanitary pads, tampons, and the like.
[0142] The composition in the pouch can be in any suitable form, including but not limited to: powder, solid foam, fiber, solid, granule, liquid, gel, paste, cream, capsule, pill, dragee, solid foam, fiber, absorbent article, nonwoven fabric, etc. Except containing less than 30% water, more preferably less than some paste, gel, liquid products of 20% water, the pouch is particularly suitable for dry products. The packaging and articles of the present invention are tolerant to consumer products. As used herein, "tolerant" refers to the ability of packaging and articles to maintain their mechanical properties and appearance on their surfaces when designed and not to diffuse through the packaging material via consumer products causing the packaging and articles to deteriorate.
[0143] Additional product forms (articles) include disposable aprons, laundry bags, disposable medical bedding, skin patches, face masks, disposable gloves, disposable medical gowns, medical devices, skin wraps, agricultural covers, shopping bags, refill bags, reloadable components in durable systems, sandwich bags, trash bags, emergency blankets and clothing, building / structural wraps and moisture-barrier liners, primary packaging for shipping such as envelopes and mailing bags, non-absorbent clothing articles that can be used to package clothing such as dresses, shirts, suits and shoes.
[0144] The different compartments of a multi-compartment pouch can be used to separate incompatible ingredients. For example, it may be desirable to separate dry shampoo and dry conditioner or laundry detergent and laundry additives into separate compartments.
[0145] Due to the improvements in water vapor and oxygen barriers, dyes and fragrances commonly used in some products should be more stable inside pouches made from the paper laminates of the present disclosure than pouches made from non-barrier paper laminates. Also, the barrier to migration of oils, surfactants, and other chemicals contained within the package may be improved compared to packages made from non-barrier paper laminates.
[0146] At the end of the life of the packaging, the consumer can recycle the packaging in a conventional paper recycling system. In a specific embodiment, the structure will be broken in a repulping system so that the paper fibers can be recycled. The adhesive layer and the sealing layer will dissolve in water and eventually biodegrade. The water-dispersible nanocomposite barrier material will be dispersed in water, the organic fraction will dissolve in water and eventually biodegrade, and the mineral fraction will be deposited in the environment as an inert, harmless and compatible material. However, if discarded, the packaging will biodegrade within 6 to 12 months.
[0147] In order to facilitate and promote the recyclability of packaging, the packaging made of the structure of the present disclosure may contain less than 50% by weight of ink, dye, barrier layer, polymer layer, glue and / or synthetic fiber. The weight percentage of ink, dye, barrier layer, polymer layer, glue and / or synthetic fiber in the packaging may be less than 50% by weight, more preferably less than 30% by weight, or most preferably less than 10% by weight, specifically listing all values within these ranges and any ranges resulting therefrom. For example, the weight percentage of ink, dye, barrier layer, polymer layer, glue and / or synthetic fiber in the packaging material may be between 0.1% by weight and 50% by weight, more preferably between 0.1% by weight and 30% by weight, or most preferably between 0.1% by weight and 10% by weight, specifically listing all values within these ranges and any ranges resulting therefrom. In a specific example, the amount of ink, dye, barrier layer, polymer layer, glue and / or synthetic fiber is 5% by weight or less, or between 0.1% by weight and 5% by weight, specifically listing all values within these ranges and any ranges resulting therefrom.
[0148] Preferably, the resulting overall package made from the paper laminate of the present disclosure contains at least 50 wt% natural cellulosic fibers, at least 70 wt% natural cellulosic fibers, or at least 90 wt% natural cellulosic fibers, specifically reciting all values within these ranges and any ranges derived therefrom.
[0149] The recyclability of packaging according to the present invention can be determined by a recyclable percentage. The paper laminates of the present disclosure can exhibit a recyclable percentage of 50% or greater, more preferably 70% or greater, or most preferably 80% or greater, with all values within these ranges and any ranges derived therefrom being specifically recited. The paper laminates of the present disclosure can have a recyclable percentage yield of 50% to about 99%, more preferably about 85% to about 99%, or most preferably about 90% to about 99%.
[0150] Test Method
[0151] When testing and / or measuring materials, if the relevant test method does not specify a specific temperature, the specimens are tested and / or measured at a temperature of 23°C (±3°C), wherein such specimens are pre-conditioned to such temperature. When testing and / or measuring materials, if the relevant test method does not specify a specific humidity, the specimens are tested and / or measured at a humidity of 35% (±5%), wherein such specimens are pre-conditioned to such humidity. The tests and / or measurements should be performed by trained, skilled and experienced personnel in accordance with good laboratory practice via properly calibrated equipment and / or instruments.
[0152] 1) Water Vapor Transmission Rate (WVTR)
[0153] The test method is carried out according to ASTM F1249-13 under the following test conditions: temperature is 40°C (±0.56°C) and relative humidity is 50% (±3%). If tropical conditions are required, the temperature is set to 38°C (±0.56°C) and the relative humidity is set to 90% (±3%). The water vapor transmission rate is expressed in [g / m 2 For materials outside the scope of ASTM F-1249-13 (§1.1), the water vapor transmission rate test method is not applicable.
[0154] 2) Scanning electron microscopy (SEM)
[0155] SEM images were recorded by an instrument Zeiss Ultra Plus from Carl Zeiss AG (Oberkochen, Germany) operated at 5.0 kV and equipped with an in-lens secondary electron detector. The sample specimens were prepared by cutting paper cross sections via a surgical scalpel under room temperature conditions.
[0156] 3) Transmission electron microscopy (TEM)
[0157] TEM images of the interlayer film cross sections were recorded using a microscope JEOL-JEM-2200FS (JEOL GmbH, Germany). Cross sections were prepared from paper by applying a JEOL EM-09100IS Cryo Ion Slicer (JEOL GmbH, Germany).
[0158] 4) Basal spacing obtained by X-ray diffraction (XRD)
[0159] The CuKα radiation was used on a Bragg-Brentano-type instrument (Empyrean Malvern Panalytical BV, The Netherlands). X-ray diffraction was measured using a PIXcel-1D detector. The X-ray diffraction patterns were analyzed using Malvern Panalytical's Highscore Plus software to determine the basal spacing (d 001 ).
[0160] 5) Small-angle X-ray scattering (SAXS)
[0161] As a preparatory work, the birefringent optical properties of the dispersion were checked with homemade orthogonal polarizers. SAXS analysis of nematic dispersions was then performed at 23°C in 1 mm glass capillaries (Hilgenberg, Germany) by using the system Ganesha Air (SAXSLAB, Denmark). The system was equipped with a rotating anode copper X-ray source MicroMax 007HF (RigakuCorp., Japan) and a position sensitive detector PILATUS 300K (Dectris, Switzerland). The sample to detector position was adjustable, covering a wide range of scattering vectors q.
[0162] 6) Biodegradation test
[0163] Aerobic biodegradation is measured by the generation of carbon dioxide (CO2) from sample specimens according to Test Method 301B and Test Guide 306 of Section 3 of the OECD Chemical Testing Guide. OECD 301B applies to both the primary components (paper, barrier layer, sealant) and the final packaging. The final packaging includes all primary and secondary (ink, varnish) components and is open to simulate its disposal after consumption. OECD 306 applies to the final packaging tested in seawater. The pass / fail success criteria are as follows:
[0164]
[0165] *Fully formed bag represents the final form of the bag (containing all dyes and coatings) that will be disposed of in the environment. The bag will be cut open to simulate being torn open by a consumer.
[0166] The samples should biodegrade by at least 60% within 60 days, preferably by at least 60% within 28 days.
[0167] Example
[0168] Preparation of paper or board prior to water dispersible nanocomposite barrier integration
[0169] In one embodiment, PackPro 7.0 grade recyclable and biodegradable 80 g / m2 of polymer available from Birgl & Bergmeister (B&B) was coated with a solution of polymer in water (30% solids) via an anilox roll process at 40 m / min to 50 m / min at Jura-Tech GmbH (Germany). 2 In another embodiment, Natura grade recyclable and biodegradable 257 g / m 2 from Stora Enso (Finland) was coated with a solution of polymer in water (30% solids) at 40 m / min to 50 m / min at Jura-Tech GmbH (Germany).2 In both cases, the resulting dried layer of water-soluble polymer was 5 μ thick and composed of 80% Selvol 205 grade PVOH from Sekisui Chemicals (Japan), 10% CremerGLYC 3109921 grade glycerol from Cremer Oleo (Germany) and 10% PEGylated from Roquette (France). P 100T grade sorbitol.
[0170] Preparation of water-soluble polyvinyl alcohol (PVOH) solution (30% solids)
[0171] 700 g of double distilled water was heated to 85° C. in a beaker. 240 g of solid PVOH powder (Selvol 205, purchased from Sekisui Chemical in Japan), 30 g of glycerol (Cremer GLYC 3109921, purchased from Cremer Oleo in Germany) and 30 g of sorbitol ( P 100T, Roquette, France). The solution was kept at reflux for 2 hours at 85°C with stirring at up to 200 rpm to dissolve all solid components. Before use, the PVOH solution was homogenized and defoamed under vacuum (50 mbar) for 10 min with stirring at up to 2500 rpm using a SpeedMixer DAC 400.2VAC-P device from Hauschild (Germany).
[0172] Preparation of water dispersible hectorite dispersion (6% solids)
[0173] Sodium hectorite [Na 0.5 ] inter [Mg 2.5 Li 0.5 ] oct [Si4] tet O 10F2: The high purity reagents SiO2 (Merck, fine particles, washed and calcined quartz), LiF (ChemPur, 99.9%, powder), MgF2 (ChemPur, 99.9%, 3 mm to 6 mm blocks, molten), MgO (Alfa Aesar, 99.95%, 1 mm to 3 mm molten agglomerates) and NaF (Alfa Aesar, 99.995%, powder) were carefully weighed according to the composition in the recipe. Crucibles made of molybdenum (25 mm outer diameter, 21 mm inner diameter, 180 mm long) were provided by Plansee SE (Reutte, Austria). For cleaning purposes, these crucibles were first heated to 1600° C. in a quartz tube placed in a copper-based high-frequency induction heating coil. The reagents were then added to the crucible under an argon atmosphere (glove box) and heated to 1200° C. under vacuum to remove any residual water. The crucible was then sealed with a molybdenum lid by heating both parts to the melting point of the molybdenum. Therefore, the sealed crucible was placed horizontally in a graphite heating furnace under an argon atmosphere and rotated at 1750°C for 80 minutes. Then, the crucible was opened, the resulting sodium hectorite was collected, ground via a planetary ball mill, and dried in a clean crucible at 250°C under an argon atmosphere for 14 hours. Then, the crucible was sealed with a molybdenum lid and annealed in a graphite heating furnace at 1045°C for 6 weeks to increase the homogeneity of the sodium hectorite. Then, the material was placed in a desiccator at (23°C, 43% relative humidity) to achieve a hydrated form [Na 0.5 ] inter [Mg 2.5 Li 0.5 ] oct [Si4] tet O 10 F2·[H2O]2. Then, double distilled water was added to reach a 6% hectorite dispersion in water. Finally, the dispersion was placed at 23°C for 1 week to allow the hectorite nanosheets to spontaneously delaminate, thereby obtaining the maximum aspect ratio of the hectorite nanosheets. The aspect ratio ranged between 400 and 40,000.
[0174] Preparation of water dispersible hectorite / PEG nanocomposite dispersion (1% solids)
[0175] First, 117g of 6% hectorite water dispersion was diluted with 583g of double distilled water at 23°C to obtain 700g of 1% hectorite water dispersion. 3g of PEG 10,000g / mol provided by Sigma-Aldrich was dissolved separately with 297g of double distilled water at 23°C to obtain 300g of 1% PEG 10000 solution. The dispersion and solution were mixed together at 23°C to obtain 1000g of 1% hectorite / PEG 10000 water dispersion (ratio 70:30). The birefringent optical properties indicate that the hectorite nanosheets are self-oriented parallel to each other in the dispersion. 1D small angle X-ray scattering (SAXS) analysis confirmed the nematic liquid crystal state of the dispersion.
[0176] Preparation of water dispersible hectorite / PEO nanocomposite dispersion (1% solids)
[0177] First, 117g of 6% hectorite water dispersion was diluted with 583g of double distilled water at 23°C to obtain 700g of 1% hectorite water dispersion. 3g of PEO 2000000g / mol provided by Sigma-Aldrich was dissolved separately with 297g of double distilled water at 80°C under stirring to obtain 300g of 1% PEO 2000000 solution. The dispersion and solution were mixed together at 23°C to obtain 1000g of 1% hectorite / PEO 2000000 water dispersion (ratio 70:30). The birefringent optical properties indicate that the hectorite nanosheets are self-oriented parallel to each other in the dispersion. 1D small angle X-ray scattering (SAXS) analysis confirmed the nematic liquid crystal state of the dispersion.
[0178] Preparation of water dispersible hectorite / PVOH nanocomposite dispersion (5% solids)
[0179] First, 333 g of 6% hectorite aqueous dispersion was diluted with 67 g of double distilled water at 23 ° C to obtain 400 g of 5% hectorite aqueous dispersion. 30 g of PVOH grade Poval 10-98 provided by Kuraray was dissolved separately with 570 g of double distilled water at 80 ° C under stirring to obtain 600 g of 5% PVOH solution. The dispersion and solution were mixed together at 23 ° C to obtain 1000 g of 5% hectorite / PVOH aqueous dispersion (ratio 40:60). The birefringent optical properties indicate that the hectorite nanosheets are self-oriented parallel to each other in the dispersion. 1D small angle X-ray scattering (SAXS) analysis confirmed the nematic liquid crystal state of the dispersion.
[0180] Laboratory-scale preparation of paper laminates with integrated water-dispersible nanocomposite barriers
[0181] All aqueous solutions / dispersions were homogenized at 2500 rpm using a SpeedMixer DAC 400.2VAC-P from Hauschild & Co KG (Hamm, Germany) and degassed for 5 minutes at (23° C., 50 mbar) before using them. 36 μ thick polyethylene terephthalate (PET) film grade purchased from Bleher Folientechnik GmbH (Germany) was 501 was used as a carrier and further surface treated. As a next step, the carrier film (as previously described) was coated with a 30% PVOH solution using an automatic knife coating device (ZAA 2300, Zehntner GmbH Testing Instruments, Switzerland). The speed was set to 15 mm / s and the blade height was set to 250 μm. The wet coating was dried at 60° C. for 30 min, and the resulting dry layer was about 28 μm thick and consisted of 80% PVOH grade Selvol 205, 10% glycerol, 10% sorbitol.
[0182] 1. Paper laminate with integrated water-dispersible hectorite / PEG nanocomposite barrier
[0183] In one embodiment, the hectorite / PEG nanocomposite barrier is applied by spraying using a fully automatic spraying system (SATA 4000LAB HVLP1.0mm spray gun purchased from SATA, Germany). The distance between the nozzle and the PET film coated with PVOH is set to 17cm. Subsequently, 1% hectorite / PEG nanocomposite dispersion (as previously described) is fed into the nozzle under a constant 4bar pressure and applied to the PET film coated with PVOH. The wet coating is dried at 50°C for 30min, and the resulting dried layer is 40nm thick. The spraying and drying cycle is repeated 100 times, and the resulting dried layer is 4 μm thick and is composed of 70% hectorite and 30% PEG 10000g / mol. As a next step, the nanocomposite barrier was coated with a 30% PVOH solution (as described previously) using an automated knife coating apparatus (as described previously), and the resulting dry layer was about 26 μm thick and consisted of 80% PVOH, 10% glycerol, 10% sorbitol. As a next step, the nanocomposite barrier was coated with 1.0 g / m PVOH using a spray coating apparatus (as described previously). 2 Up to 1.5g / m 2 Bi-distilled water coated the PVOH surface and was pressed against the PVOH surface of a PVOH coated PackPro 7.0 grade paper purchased from Birgl & Bergmeister. At this point, the carrier PET film was removed, resulting in a paper laminate including a nanocomposite barrier.
[0184] 2. Paper laminate with integrated water-dispersible hectorite / PEO nanocomposite barrier
[0185] In one embodiment, the hectorite / PEO nanocomposite barrier is applied by spraying using a fully automatic spraying system (SATA 4000LAB HVLP1.0mm spray gun purchased from SATA, Germany). The distance between the nozzle and the PET film coated with PVOH is set to 17cm. Subsequently, 1% hectorite / PEO nanocomposite dispersion (as previously described) is fed into the nozzle under a constant 4bar pressure and applied to the PET film coated with PVOH. The wet coating is dried at 50°C for 30min, and the resulting dried layer is 40nm thick. The spraying and drying cycle is repeated 100 times, and the resulting dried layer is 4 μm thick and is composed of 70% hectorite and 30% PEO 2000000g / mol. As a next step, the nanocomposite barrier was coated with a 30% PVOH solution (as described previously) using an automated knife coating apparatus (as described previously), and the resulting dry layer was about 26 μm thick and consisted of 80% PVOH, 10% glycerol, 10% sorbitol. As a next step, the nanocomposite barrier was coated with 1.0 g / m PVOH using a spray coating apparatus (as described previously). 2 Up to 1.5g / m 2 Double distilled water coated the PVOH surface and was pressed against the PVOH surface of the PVOH coated PackPro 7.0 grade paper purchased from Birgl & Bergmeister. At this point, the carrier PET film was removed, resulting in a water soluble film with an integrated nanocomposite barrier.
[0186] 3. Paper laminate with integrated water-dispersible hectorite / PVOH nanocomposite barrier
[0187] In one embodiment, the hectorite / PVOH nanocomposite barrier is applied by a knife coating device (ZAA 2300, Zehntner GmbH TestingInstruments, Switzerland). The speed is set to 15 mm / s and the blade height is set to 100 μm. A 5% hectorite / PVOH nanocomposite dispersion (as previously described) is applied to a PVOH-coated PET film. The wet coating is dried at 60°C for 4 hours and consists of 40% hectorite and 60% PVOH grade Poval 10-98. As a next step, the nanocomposite barrier is coated with a 30% PVOH solution (as previously described) using the same equipment, and the resulting dry layer is about 26 μm thick and consists of 80% PVOH, 10% glycerol, and 10% sorbitol. As a next step, a spray coating device (as previously described) is used to coat the nanocomposite barrier with 1.0 g / m 2 Up to 1.5g / m 2Double distilled water coated the PVOH surface and was pressed against the PVOH surface of the PVOH coated PackPro 7.0 grade paper purchased from Birgl & Bergmeister. At this point, the carrier PET film was removed, resulting in a water soluble film with an integrated nanocomposite barrier.
[0188] Table 1
[0189]
[0190] Table 1 provides the barrier properties (WVTR) of the above embodiments.
[0191] Table 2
[0192]
[0193] Table 2 provides the recyclability and biodegradability of the above embodiments.
[0194] Comparative Example
[0195] A. Barrier paper laminates based on paper, polyvinyl alcohol and beeswax
[0196] Preparation of sealing layer composition
[0197] Polyvinyl alcohol flakes (Selvol 1205, obtained from Sekisui Chemicals) and sorbitol solution (E420 USP / FCC grade, obtained from Archer Daniels Midland, 71% D sorbitol content in water) were pumped into a CT-25 twin-screw compounder (obtained from Baker & Perkins, Saginaw, Michigan, USA) with an L / D ratio of 52, a co-rotating screw speed of 340 rpm, and a molding temperature of 25°C (inlet), 170°C (melting and metering zone), and 150°C (extrusion die). Water was added as a processing aid and removed via a vacuum pump to produce essentially water-free polymer strands. The strands were then air-cooled and chopped to produce pellets of 80% PVOH and 20% sorbitol composition. Separately, polyvinyl alcohol flakes (Selvol 205, available from Sekisui Chemicals), glycerol (GL99.7 USP grade, available from Peter Cremer Oleo Division) and silicate antiblock particles ( 820A grade, available from Evonik Industries AG, Essen, Germany) was compounded by a similar procedure to produce pellets of 74% PVOH, 20% glycerol, and 6% antiblock composition.
[0198] As the next step, the pellets from the two batches were each dosed 50% by weight and put into the extruder barrel of a pilot scale cast film production line, with an L / D ratio of 30, a single 30mm diameter screw designed for PE blends. The screw speed was set to 30rpm, and the extruder barrel temperature was set to 25°C (inlet), 200°C (melting and metering zone) and 195°C (extrusion die head). The polymer melt extruded from the slit die was cooled on a chill roll and calendered to produce a 20 μm thick film of 77% PVOH, 10% glycerol, 10% sorbitol and 3% anti-blocking composition. Therefore, the film was rewound into a film roll under constant tension control.
[0199] Preparation of barrier layer composition
[0200] Beeswax (white beeswax) off-white pastille grade 442 was obtained from Strahl & Pitsch (West Babylon, New York, USA) and used as received. The melting point was in the range of 62°C to 65°C.
[0201] Preparation of barrier paper laminates based on paper, polyvinyl alcohol and beeswax
[0202] The 80 g / m 2 The less glossy side of an A4 size paper of Paper Grade Packaging Pro 7.0 was thermally laminated to an A4 size sheet of 20 μm thick PVOH film as described in the above seal layer composition paragraph. The lamination step was performed using a laboratory scale equipment model 480R6 professional laminator from Sky DSB (Seoul, South Korea), using a temperature of 140°C and a feed speed of 575 mm / min (setting 3 in the 1 to 6 levels, and the maximum setting 6 corresponds to 1150 mm / min).
[0203] As a next step, an A4 size paper laminate was coated with beeswax on a brighter, larger size Pack Pro 7.0 paper surface. For this purpose, a laboratory scale equipment model C-14 adhesive wax coater from Schaefer Machine Company (Clinton, Connecticut, USA) was modified by replacing the original blade with a Mayer bar of different wire rod diameters to enable different molten wax coating thicknesses. The temperature of the molten wax in the well was set to 90°C.
[0204] Table 3
[0205]
[0206] Table 3 provides the barrier properties (WVTR) of the above embodiments.
[0207] Although beeswax coated paper moisture barrier is interesting for some applications, the problem with applying beeswax to paper is the trade-off between the desired barrier to moisture penetration and the desired ability to recycle the paper. As shown in Table 4 below, all of the comparative examples produced failed the PTS recyclability test, with the main problem being that wax spots were detected as unacceptable optical defects despite the high recycled fiber content.
[0208] Table 4
[0209]
[0210] Table 4 provides the recyclability and biodegradability of the above embodiments.
[0211] The dimensions and values disclosed herein are not to be understood as being strictly limited to the exact numerical values cited. Instead, unless otherwise indicated, each such dimension is intended to represent the stated value and a functionally equivalent range around that value. For example, a dimension disclosed as "40 mm" is intended to mean "about 40 mm".
[0212] Unless expressly excluded or otherwise limited, each document cited herein, including any cross-referenced or related patent or patent application and any patent application or patent to which this application claims priority or the benefit of, is hereby incorporated by reference in its entirety. The citation of any document is not an admission that it is prior art to any of the present invention disclosed or claimed herein, or an admission that it, by itself or in combination with any one or more of the references, proposes, suggests, or discloses any such invention. In addition, to the extent that any meaning or definition of a term in this invention conflicts with any meaning or definition of the same term in a document incorporated by reference, the meaning or definition assigned to that term in this invention shall govern.
[0213] Although specific embodiments of the present invention have been illustrated and described, it will be apparent to those skilled in the art that various other changes and modifications may be made without departing from the spirit and scope of the present invention. Therefore, it is intended that all such changes and modifications within the scope of the present invention be covered in the appended claims.
Claims
1. A paper laminate, comprising: a) a paper or board layer having an outer surface and an inner surface; b) an adhesive layer having an outer surface and an inner surface, the outer surface being disposed on the inner surface of the paper layer; c) a water-dispersible nanocomposite barrier layer having an outer surface and an inner surface, the outer surface being disposed on the inner surface of the adhesive layer; d) a sealing layer having an outer surface and an inner surface, the outer surface being disposed on the inner surface of the water-dispersible nanocomposite barrier layer.
2. The paper laminate according to claim 1, wherein the grammage of the paper laminate is about 20 g / m 2 About 1000g / m 2 , preferably about 20 g / m 2 About 200g / m 2 .
3. The paper laminate of claim 1, wherein the WVTR of the paper laminate is about 0.01 g / m 2 / day to about 100g / m 2 / sky.
4. The paper laminate according to any one of claims 1 to 3, wherein the paper laminate is recyclable and exhibits a recyclability percentage of at least 50% as determined by test method PTS-RH:021 / 97 (draft October 2019).
5. A paper laminate according to any of the preceding claims, wherein the paper laminate comprises between about 50% and about 100% by weight natural fibers, preferably between about 65% and about 99% by weight natural fibers, more preferably between about 75% and about 95% by weight natural fibers.
6. The paper laminate according to any one of the preceding claims, wherein the paper is made from natural fibers including at least one of the following: cellulose-based fibers, bamboo fibers, cotton, abaca, kenaf, ramie, flax, North African grass, straw, jute, bagasse, milkweed fibers, pineapple leaf fibers, wood fibers, pulp fibers, or combinations thereof.
7. A paper laminate according to any one of the preceding claims, wherein the paper is sized and / or mechanically glazed on at least one surface, or is glassine paper, or is kraft paper.
8. The paper laminate according to any one of the preceding claims, wherein the paper is produced via a foam forming process, which is a papermaking process that replaces water with a water-based foam.
9. The paper laminate according to any one of the preceding claims, wherein the water dispersible nanocomposite barrier layer is distinct from the adhesive layer and distinct from the sealant layer as observed via scanning electron microscopy (SEM).
10. The paper laminate according to any one of the preceding claims, wherein the water dispersible nanocomposite barrier layer has an average thickness of about 0.1 μm to about 20 μm.
11. The paper laminate according to any one of the preceding claims, wherein the water-dispersible nanocomposite barrier layer comprises more than one water-dispersible nanocomposite barrier sublayer.
12. The paper laminate according to any one of the preceding claims, wherein the water dispersible nanocomposite barrier layer is a nanocomposite comprising nanoscale ordered spaced hydrophilic nanoplatelets and intercalated polymer fillers, wherein the basal spacing measured via XRD is less than Preferably less than More preferably, less than 13. The paper laminate according to claim 12, wherein the average aspect ratio of the hydrophilic nanoplatelets is greater than about 100, preferably greater than about 1000, more preferably greater than about 10000.
14. The paper laminate according to claim 12, wherein the hydrophilic nanoplatelets are clay nanoplatelets, preferably wherein the hydrophilic nanoplatelets are at least one of natural, modified or synthetic smectite or natural, modified or synthetic vermiculite.
15. The paper laminate according to any one of the preceding claims, wherein the adhesive layer and the sealing layer comprise at least one water-soluble polymer, such as polyvinyl alcohol, polyethylene oxide, methylcellulose or sodium alginate.
16. A method of preparing the paper laminate according to claim 1, the method comprising: a) applying the polymer composition to paper or board for use as an adhesive layer; b) applying an aqueous nanocomposite material onto the surface of the adhesive layer; c) removing water to obtain a water-dispersible nanocomposite barrier layer; d) applying a polymer composition onto the barrier layer to act as a sealing layer.
Citation Information
Patent Citations
Barrier paper
JP2019177586A
Packaging laminate, method for manufacturing of the packaging laminate and packaging container produced therefrom
US20110132975A1
Biodegradable paper barrier laminate
US20220033158A1
A multi-layer flexible packaging material
WO2021165290A1
Cited By
Paper-based water-based barrier packaging material for pet food as well as preparation method and application thereof
CN121473171A